PVB (polyvinyl butyral) composite film, preparation method thereof, laminated glass and automobile

By using PVB composite film with cesium tungsten bronze composite particles in automotive ceiling glass, the problem of insufficient thermal insulation performance of ceiling glass is solved, better thermal insulation effect and visible light transmittance are achieved, and the comfort and energy efficiency of the car are improved.

CN120192623APending Publication Date: 2025-06-24NIO TECH ANHUI CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202510336981.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-03-19
Publication Date
2025-06-24

AI Technical Summary

Technical Problem

The insulating performance of the car's ceiling glass is insufficient, causing the temperature inside the car to rise sharply, affecting the comfort of the ride and increasing energy consumption.

Method used

A PVB composite film is used, which includes a PVB base film and cesium tungsten bronze composite particles. The cesium tungsten bronze composite particles have a core-shell structure, the core material includes cesium tungsten bronze and titanium dioxide, and the shell material is polyvinyl butyral. The composite film is prepared by hydrolysis reaction and coating process to ensure the uniform distribution of cesium tungsten bronze composite particles in the PVB base film.

Benefits of technology

The thermal insulation performance and visible light transmittance of the PVB composite film are significantly improved, forming laminated glass with good thermal insulation performance and good light transmittance, thereby improving the thermal insulation effect and visual comfort of the car.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120192623A_ABST
    Figure CN120192623A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of automobiles, and provides a PVB composite film and a preparation method thereof, laminated glass and an automobile, the PVB composite film comprises a PVB base film and cesium-tungsten bronze composite particles distributed in the PVB base film, each cesium-tungsten bronze composite particle comprises an inner core and a shell layer coating the surface of the inner core, the inner core is made of cesium-tungsten bronze and titanium dioxide, and the shell layer is made of titanium dioxide. And the material of the shell layer comprises polyvinyl butyral. According to the PVB composite film provided by the invention, the material of the cesium-tungsten bronze composite particle shell layer is consistent with that of the PVB base film, so that the compatibility of the cesium-tungsten bronze composite particles and the PVB base film is remarkably improved, the distribution uniformity of the cesium-tungsten bronze composite particles in the PVB base film is favorably improved, and the heat insulation performance of the PVB composite film is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the technical field of automobiles, and particularly relates to a PVB composite film, a preparation method thereof, laminated glass, and an automobile. Background Art

[0002] At present, with the booming development of the automotive industry, affected by factors such as appearance and cost, more and more automobiles abandon single skylights or panoramic skylights and instead adopt sunroof glass. Sunroof glass does not require an additional switching mechanical structure, has a simple structure, can effectively control costs, and is more technologically aesthetic in appearance, meeting the current trend of automotive design.

[0003] However, the area of automotive sunroof glass is large and unobstructed. When the vehicle is exposed to strong sunlight outdoors, a large amount of heat will enter the vehicle through heat transfer and thermal radiation via the sunroof glass, causing the temperature inside the vehicle to rise sharply, especially in the top area near the sunroof glass. This not only reduces the comfort of passengers but also increases the energy consumption of the vehicle, bringing many adverse effects to the use of the vehicle. Therefore, the research on the heat insulation performance of automotive sunroof glass is extremely crucial and urgent. Summary of the Invention

[0004] The purpose of this application is to provide a PVB composite film, a preparation method thereof, laminated glass, and an automobile, aiming to solve the technical problem that the heat insulation performance of current sunroof glass needs to be improved.

[0005] To achieve the above application purpose, the technical solution adopted in this application is as follows:

[0006] In a first aspect, a PVB composite film includes a PVB base film and cesium tungsten bronze composite particles distributed in the PVB base film. The cesium tungsten bronze composite particles include a core and a shell layer covering the core. The material of the core includes cesium tungsten bronze and titanium dioxide, and the material of the shell layer includes polyvinyl butyral.

[0007] In some embodiments, in the above core, at least part of the titanium dioxide is coated on the surface of the cesium tungsten bronze to form a coating layer.

[0008] In some embodiments, the mass ratio of the PVB base film to the cesium tungsten bronze composite particles is 100:(8 - 10).

[0009] In some embodiments, the mass ratio of cesium tungsten bronze to titanium dioxide is (1 - 3):(1.1 - 3.6).

[0010] In some embodiments, the mass ratio of the core to the shell layer is (1 - 3):(0.1 - 0.3).

[0011] In some embodiments, the particle size of the cesium tungsten bronze composite particles is 100nm - 1μm.

[0012] In some embodiments, the PVB composite film further comprises vanadium dioxide composite particles, which are distributed in the PVB base film. The vanadium dioxide composite particles include a vanadium dioxide core and a polyvinyl butyral shell layer coated on the surface of the vanadium dioxide core.

[0013] In some embodiments, the particle size of the vanadium dioxide composite particles is 1 nm - 100 nm.

[0014] In some embodiments, the mass ratio of the PVB base film, the cesium tungsten bronze composite particles, and the vanadium dioxide composite particles is 100:(4 - 5):(4 - 5).

[0015] In some embodiments, the mass ratio of the vanadium dioxide core to the polyvinyl butyral shell layer is 1:(0.1 - 0.3).

[0016] In some embodiments, the thickness of the PVB composite film is 0.5 mm - 1 mm.

[0017] In a second aspect, the present application provides a method for preparing a PVB composite film, comprising the following steps:

[0018] Disperse cesium tungsten bronze and a titanium source in a first solvent, and obtain a cesium tungsten bronze - titanium dioxide inner core through a hydrolysis reaction;

[0019] Coat a first polyvinyl butyral on the surface of the cesium tungsten bronze - titanium dioxide inner core to obtain cesium tungsten bronze composite particles;

[0020] Add the cesium tungsten bronze composite particles and a second polyvinyl butyral to a second solvent, and obtain a precursor solution after heat treatment;

[0021] Perform a film - forming treatment on the precursor solution to obtain a PVB composite film.

[0022] In some embodiments, the step of coating the first polyvinyl butyral on the surface of the cesium tungsten bronze - titanium dioxide inner core includes:

[0023] Add the cesium tungsten bronze - titanium dioxide inner core and the first polyvinyl butyral to a third solvent, and perform a grinding treatment;

[0024] Alternatively, add the cesium tungsten bronze - titanium dioxide inner core, vanadium dioxide particles, and the first polyvinyl butyral to a third solvent, and perform a grinding treatment.

[0025] In some embodiments, the hydrolysis reaction includes reacting at 40°C - 60°C for 12 h - 24 h.

[0026] In some embodiments, the heat treatment includes heating at 40°C - 70°C for 3 h - 6 h.

[0027] In some embodiments, the film-forming treatment includes coating a precursor solution to form a film, and then performing a curing treatment for 2 h - 6 h under the conditions of a temperature of 40°C - 70°C and a vacuum degree of -55 KPa to -45 KPa.

[0028] In a third aspect, the present application provides a laminated glass, including at least two glass substrates, and a PVB composite film provided in the first aspect and / or a PVB composite film prepared by the preparation method provided in the second aspect is disposed between adjacent glass substrates.

[0029] In a fourth aspect, the present application provides a vehicle, including the laminated glass provided in the third aspect.

[0030] The PVB composite film provided in the first aspect of the present application includes a PVB base film and cesium tungsten bronze composite particles. Among them, the cesium tungsten bronze composite particles have a core-shell structure. Specifically, the cesium tungsten bronze composite particles include cesium tungsten bronze as the core, titanium dioxide, and polyvinyl butyral forming the outer shell layer. On the one hand, since the material of the outer shell layer of the cesium tungsten bronze composite particles is the same as that of the PVB base film, it means that the surface properties of the cesium tungsten bronze composite particles are more similar to those of the PVB base film. This similarity significantly improves the compatibility between the cesium tungsten bronze composite particles and the PVB base film, thereby helping to improve the uniformity of the distribution of the cesium tungsten bronze composite particles in the PVB base film. This uniform distribution makes the PVB composite film not easily prone to problems such as light scattering and uneven refraction, so that the PVB composite film can better exert its optical properties, especially the good absorption or reflection ability of infrared rays, thereby greatly improving its heat insulation performance; on the other hand, cesium tungsten bronze and titanium dioxide together serve as the inner core, which promotes the more uniform distribution of titanium dioxide in the PVB base film. The uniformly distributed titanium dioxide can fully exert its antireflection effect, thereby helping to improve the consistency of the visible light transmittance of the PVB composite film in different regions, making the PVB composite film exhibit a stable and uniform visible light transmittance. Based on this, by distributing the core-shell structured cesium tungsten bronze composite particles in the PVB base film, the present application can obtain a PVB composite film with good heat insulation performance and good light transmittance.

[0031] The preparation method of the PVB composite film provided in the second aspect of the present application decomposes a titanium source into titanium dioxide by hydrolysis to form a cesium tungsten bronze - titanium dioxide inner core, and then coats the first polyvinyl butyral on the surface of the cesium tungsten bronze - titanium dioxide inner core, thus forming cesium tungsten bronze composite particles with a core-shell structure. Then, the solution blending method is used to make the cesium tungsten bronze composite particles relatively uniformly distributed in the PVB base film, and then effectively prepare a PVB composite film with the performance as described in the PVB composite film of the present application above. In addition, the preparation method of the PVB composite film of the present application has a simple process, and has high reliability and repeatability, and is suitable for industrial promotion and application.

[0032] The laminated glass provided in the third aspect of the present application contains the PVB composite film provided in the present application, and this PVB composite film has good heat insulation performance and high visible light transmittance. Therefore, the laminated glass of the present application has excellent heat insulation ability and high-quality lighting effect at the same time.

[0033] The vehicle provided in the fourth aspect of the present application contains the laminated glass provided in the present application, which greatly improves the heat insulation effect of the vehicle, thereby reducing the air conditioning load of the vehicle. At the same time, it can also create a bright and comfortable space environment and provide a high-permeability visual experience for passengers. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following will briefly introduce the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings in the following description are only some embodiments of the present application. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative efforts.

[0035] Figure 1 is the microscopic morphology diagram of the PVB composite film provided in Embodiment 1 of the present application;

[0036] Figure 2 is the microscopic morphology diagram of the PVB composite film provided in Embodiment 2 of the present application;

[0037] Figure 3 is the transmittance spectrum diagram of the laminated glass provided in Embodiments S1-S2 of the present application;

[0038] Figure 4 is the transmittance spectrum diagram of the laminated glass provided in Comparative Examples DS1-DS2 of the present application;

[0039] Figure 5 is the transmittance spectrum diagram of the laminated glass provided in Comparative Examples DS3-DS4 of the present application;

[0040] Figure 6 is the heat insulation test device diagram of the present application;

[0041] Figure 7 is the temperature change diagram of the laminated glass provided in Embodiments S1-S2 of the present application;

[0042] Figure 8 is the temperature change diagram of the laminated glass provided in Comparative Examples DS1-DS2 of the present application;

[0043] Figure 9 is the temperature change diagram of the laminated glass provided in Comparative Example DS4 of the present application. DETAILED DESCRIPTION OF THE EMBODIMENTS

[0044] In order to make the technical problems, technical solutions and beneficial effects to be solved by this application more clear and understandable, the following further details this application in combination with embodiments. It should be understood that the specific embodiments described herein are only used to explain this application and are not used to limit this application.

[0045] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist simultaneously, and B exists alone. Where A and B can be singular or plural. The character " / " generally represents an "or" relationship between the front and back associated objects.

[0046] In this application, "at least one" means one or more, and "a plurality" means two or more. "At least one (item)" or its similar expression refers to any combination of these items, including any combination of single item (item) or plural items (items). For example, "at least one (item) of a, b, or c", or, "at least one (item) of a, b, and c" can both represent: a, b, c, a - b (that is, a and b), a - c, b - c, or a - b - c, where a, b, and c can be single or multiple respectively.

[0047] It should be understood that in various embodiments of this application, the size of the serial numbers of the above processes does not mean the order of execution. Some or all steps can be executed in parallel or sequentially. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation to the implementation process of the embodiments of this application.

[0048] The terms used in the embodiments of this application are only for the purpose of describing specific embodiments, and are not intended to limit this application. The singular forms of "a", "the" and "said" used in the embodiments of this application and the appended claims are also intended to include the plural forms, unless the context clearly indicates otherwise.

[0049] The weight of the relevant components mentioned in the specification of the embodiments of this application not only can refer to the specific content of each component, but also can represent the proportional relationship of the weights between each component. Therefore, as long as the content of the relevant components in the specification of the embodiments of this application is scaled up or down proportionally, it is within the scope disclosed in the specification of the embodiments of this application. Specifically, the mass described in the specification of the embodiments of this application can be mass units well known in the chemical industry such as μg, mg, g, kg, etc.

[0050] The term "PVB" is the abbreviation of "Polyvinyl Butyral", representing polyvinyl butyral.

[0051] A panoramic sunroof glass mainly refers to a large-area transparent glass material applied to positions such as the roof of a vehicle or the top of a building. In the automotive field, it usually covers a large part or even the entire roof of the vehicle to provide a broad view and good lighting effect. Although panoramic sunroof glass offers a highly transparent visual experience and has a relatively low cost advantage, due to its large area, it is prone to allowing a large amount of heat to enter the vehicle through heat transfer and thermal radiation in summer, causing the interior temperature to rise sharply. This not only affects the comfort of passengers but also increases the energy consumption of air conditioning refrigeration, which is not conducive to energy conservation.

[0052] To address the heat insulation problem of automotive panoramic sunroof glass, the solution commonly adopted in the industry is to use Low-e glass technology. Specifically, this technology precisely deposits two or three layers of silver films on the inner surface of the glass by magnetron sputtering, taking advantage of the strong reflection of silver elements to sunlight to achieve good heat insulation performance. However, this widely used Low-e glass heat insulation strategy has many limitations that cannot be ignored. For example, the process flow of magnetron sputtering technology is extremely cumbersome, resulting in a high product price. Additionally, silver, as a precious metal, has a relatively high market price, further increasing the production cost burden. Moreover, when the glass is coated with two or three layers of silver films, although certain heat insulation effects are achieved, it inevitably leads to a significant reduction in the visible light transmittance, reducing the visual comfort.

[0053] To reduce the process cost of panoramic sunroof glass and optimize its performance, due to its unique physical and chemical properties, PVB film has become one of the ideal materials for making laminated glass, especially panoramic sunroof glass. Usually, heat-insulating fillers are added to the PVB film to endow the panoramic sunroof glass with excellent heat insulation performance. However, there are significant differences in the chemical structure and surface properties between most fillers and the PVB film, resulting in poor compatibility between the two. In the actual preparation process, due to the difficulty of their good combination, the fillers are not easily uniformly dispersed in the PVB film and tend to agglomerate, forming particle clusters of different sizes. From the application effect perspective, this problem of poor compatibility, on the one hand, makes the heat insulation performance of the panoramic sunroof glass uneven in different regions, leading to uneven temperature distribution inside the vehicle, with local temperatures being too high or too low, affecting the driving and riding comfort. On the other hand, in terms of optical performance, when light passes through the uneven PVB film, problems such as inconsistent light transmittance, local blurring, or glare are likely to occur, seriously affecting the visual experience.

[0054] Based on this, in the first aspect of the embodiments of the present application, a PVB composite film is provided, which includes a PVB base film and cesium tungsten bronze composite particles distributed in the PVB base film. The cesium tungsten bronze composite particles include a core and a shell layer covering the core. The material of the core includes cesium tungsten bronze and titanium dioxide, and the material of the shell layer includes polyvinyl butyral.

[0055] In the technical solution of this application, the PVB composite film includes a PVB base film and cesium tungsten bronze composite particles. Among them, the cesium tungsten bronze composite particles have a core-shell structure, and the material of its outer shell layer is polyvinyl butyral. Since the material of the outer shell layer of the cesium tungsten bronze composite particles is the same as that of the PVB base film, it means that the surface properties of the cesium tungsten bronze composite particles are more similar to those of the PVB base film. This similarity significantly improves the compatibility between the cesium tungsten bronze composite particles and the PVB base film, thereby helping to improve the uniformity of the distribution of the cesium tungsten bronze composite particles in the PVB base film. This uniform distribution makes it less likely for the PVB composite film to have problems such as light scattering and uneven refraction. In this way, the PVB composite film can better exhibit its optical properties, especially its good absorption or reflection ability for infrared rays, thus greatly improving its heat insulation performance.

[0056] At the same time, due to the good compatibility between the cesium tungsten bronze composite particles and the PVB base film, the interfacial bonding force between the cesium tungsten bronze composite particles and the PVB base film is significantly improved. In this way, the cesium tungsten bronze composite particles can be better fixed in the PVB base film, reducing the possibility of the particles falling off from the film. This good interfacial bonding helps to maintain the stability of the PVB composite film, and during long-term use, it helps the cesium tungsten bronze composite particles to continuously exert their functions.

[0057] In addition, cesium tungsten bronze and titanium dioxide together serve as the inner core, which promotes the more uniform distribution of titanium dioxide in the PVB base film. The uniformly distributed titanium dioxide can fully exert its antireflection effect, thereby helping to improve the consistency of the visible light transmittance of the PVB composite film in different regions, making the PVB composite film exhibit a stable and uniform visible light transmittance. Based on this, by distributing the core-shell structured cesium tungsten bronze composite particles in the PVB base film, this application can obtain a PVB composite film with good heat insulation performance and good light transmittance.

[0058] Cesium tungsten bronze and titanium dioxide together serve as the inner core. In one embodiment, cesium tungsten bronze and titanium dioxide are mixed with each other to form the inner core; in another embodiment, titanium dioxide coats the surface of cesium tungsten bronze to form a coating layer.

[0059] In some embodiments, the mass ratio of the PVB base film to the cesium tungsten bronze composite particles is 100:(8 - 10). Exemplarily, the mass ratio of the PVB base film to the cesium tungsten bronze composite particles can be 100:8, 100:8.5, 100:9, 100:9.5, 100:10 and other typical but non-limiting values.

[0060] The PVB base film itself has good light transmittance. Therefore, within the above mass ratio range, on the one hand, an appropriate amount of cesium tungsten bronze composite particles can exert its heat insulation function without significantly reducing the light transmittance, effectively absorbing and reflecting infrared rays, achieving a balance between light transmittance and heat insulation; on the other hand, the cesium tungsten bronze composite particles can be evenly distributed in the PVB base film, and it is not easy to have problems such as uneven light scattering and refraction caused by uneven particle distribution. In this way, the light passing through the PVB composite film is more uniform, improving the visual quality.

[0061] In some embodiments, the mass ratio of the core to the outer shell layer is (1 - 3):(0.1 - 0.3). Exemplarily, the mass ratio of the core to the outer shell layer can be 1:0.1, 1:0.2, 1:0.3, 2:0.1, 2:0.3, 3:0.1, 3:0.2 and other typical but non-limiting values.

[0062] Within the above mass ratio range, it means that a stable and uniform outer shell layer can be constructed on the surface of the core, so that the cesium tungsten bronze composite particles can better integrate into the PVB base film, prompting the cesium tungsten bronze composite particles to be more evenly dispersed in the PVB base film. In this way, the PVB composite film has better consistency and stability.

[0063] In some embodiments, the particle size of the cesium tungsten bronze composite particles is 100nm - 1μm. Exemplarily, the particle size of the cesium tungsten bronze composite particles can be 100nm, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, 1μm and other typical but non-limiting values.

[0064] Controlling the particle size of the cesium tungsten bronze composite particles within the above range means that an appropriate amount of cesium tungsten bronze composite particles are contained in the PVB composite film, which prompts the cesium tungsten bronze composite particles to be more evenly distributed in the PVB base film. In this way, not only does the refraction and reflection behavior of light at different positions of the PVB composite film become more consistent, improving the uniformity of the optical properties of the PVB composite film, but also this arrangement and appropriate spacing between particles can more effectively reflect infrared rays, forming a good heat insulation barrier, making the PVB composite film exhibit excellent heat insulation performance.

[0065] In some embodiments, in the above core, at least part of the titanium dioxide is coated on the surface of the cesium tungsten bronze to form a coating layer.

[0066] Titanium dioxide coats the surface of cesium tungsten bronze particles to form a core-shell structure. Among them, the refractive index matching degree between titanium dioxide and cesium tungsten bronze is relatively high. This reduces the reflection loss at the interface when light enters cesium tungsten bronze particles from the air and then reaches the PVB base film. In this way, light can enter the PVB composite film more smoothly, thereby improving the visible light transmittance of the PVB composite film. At the same time, the coating of titanium dioxide reduces the light scattering of light, making the light propagation more orderly, improving the uniformity of the transmitted light while increasing the visible light transmittance, and significantly enhancing the visual experience of the PVB composite film.

[0067] In addition, cesium tungsten bronze has good absorption and reflection capabilities for infrared rays, and can effectively block the infrared heat in solar radiation. Titanium dioxide also has certain absorption characteristics in the near-infrared band. The combination of the two effectively broadens the infrared blocking range of cesium tungsten bronze composite particles. Specifically, the PVB composite film can block infrared rays in the wavelength range of 750nm - 2500nm, which significantly enhances the heat insulation effect of the PVB composite film.

[0068] In some embodiments, the mass ratio of cesium tungsten bronze to titanium dioxide is (1 - 3):(1.1 - 3.6). Exemplarily, the mass ratio of cesium tungsten bronze to titanium dioxide can be typical but non-limiting values such as 1:1.1, 1:2, 1:3, 1:3.6, 2:1.1, 2:3.6, 3:1, 3:2, 3:3.6, etc.

[0069] Controlling the mass ratio of cesium tungsten bronze to titanium dioxide within the above range enables the cesium tungsten bronze composite particles to have good heat insulation performance while achieving a relatively high visible light transmittance. In addition, at this ratio, titanium dioxide can better play its role in uniformly scattering light, cooperate with cesium tungsten bronze, reduce the glare phenomenon, and optimize the light scattering and reflection characteristics of the cesium tungsten bronze composite particles, thereby providing a comfortable visual experience.

[0070] In some embodiments, the PVB composite film further includes vanadium dioxide composite particles. The vanadium dioxide composite particles are distributed in the PVB base film. The vanadium dioxide composite particles include a vanadium dioxide core and a polyvinyl butyral shell layer coated on the surface of the vanadium dioxide core.

[0071] Vanadium dioxide has metal-insulator phase transition characteristics. Among them, vanadium dioxide presents an insulating state below the phase transition temperature. At this time, vanadium dioxide can block infrared rays to a certain extent by absorbing and scattering infrared rays, providing a heat insulation effect. Vanadium dioxide presents a metallic state above the phase transition temperature. At this time, the reflectivity of vanadium dioxide to infrared rays increases significantly, thereby effectively blocking the transmission of infrared rays and endowing the PVB composite film with good heat insulation performance.

[0072] Since the vanadium dioxide composite particles have a core-shell structure and include a polyvinyl butyral shell layer with the same material as the PVB base film, it means that the vanadium dioxide composite particles have good compatibility with the PVB base film. By virtue of good affinity, the vanadium dioxide composite particles can be evenly dispersed in the PVB base film, and it is not easy to appear agglomeration phenomenon caused by poor compatibility. This uniform distribution makes the PVB composite film not easy to have problems of light scattering and uneven refraction, so that the PVB composite film can better exert its optical properties, thereby significantly improving its heat insulation performance.

[0073] Both the vanadium dioxide composite particles and the cesium tungsten bronze composite particles have a core-shell structure. And because the materials of the outer shell layers of the two composite particles are the same, the surface properties of the vanadium dioxide composite particles and the cesium tungsten bronze composite particles are more similar. In addition, due to the existence of the outer shell layer, a steric hindrance effect is generated, which makes the composite particles not easy to agglomerate with each other, thus being more conducive to the uniform dispersion of the composite particles in the PVB base film.

[0074] In some embodiments, the mass ratio of the vanadium dioxide core to the polyvinyl butyral shell layer is 1:(0.1 - 0.3). Exemplarily, the mass ratio of the vanadium dioxide core to the polyvinyl butyral shell layer can be 1:0.1, 1:0.2, 1:0.3 and other typical but non-limiting values.

[0075] Within the above mass ratio range, it means that a stable and uniform polyvinyl butyral shell layer can be constructed on the surface of the vanadium dioxide core. This helps the vanadium dioxide composite particles to be more evenly dispersed in the PVB base film by virtue of their good compatibility with the PVB film, making the refraction and reflection behaviors of light at different positions of the PVB base film more consistent, thereby improving the consistency and stability of the optical performance of the PVB composite film and exerting good heat insulation ability.

[0076] In some embodiments, the particle size of the vanadium dioxide composite particles is 1nm - 100nm. Exemplarily, the particle size of the vanadium dioxide composite particles can be 1nm, 5nm, 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm and other typical but non-limiting values.

[0077] Controlling the particle size of the vanadium dioxide composite particles within the above range enables the vanadium dioxide composite particles to better exert their metal-insulator phase transition characteristics in the PVB composite film, enhance the reflection of infrared rays, and thus improve its heat insulation ability.

[0078] In some embodiments, the mass ratio of the PVB base film, the cesium tungsten bronze composite particles, and the vanadium dioxide composite particles is 100:(4-5):(4-5). Exemplarily, the mass proportion of the cesium tungsten bronze composite particles can be typical but non-limiting values such as 4, 4.2, 4.5, 4.8, 5, etc., and the mass proportion of the vanadium dioxide composite particles can be typical but non-limiting values such as 4, 4.2, 4.5, 4.8, 5, etc.

[0079] The cesium tungsten bronze composite particles mainly insulate heat by absorbing and reflecting infrared rays. The vanadium dioxide composite particles mainly exert their heat insulation efficiency by utilizing their own phase change characteristics and absorption and scattering mechanisms. The two composite particles and the PVB base film are combined in the above-mentioned ratio, enabling the two composite particles to play a synergistic effect. That is, when the temperature is lower than the phase transition temperature of vanadium dioxide, it is mainly the cesium tungsten bronze composite particles that exhibit heat insulation performance, reducing heat transfer by absorbing and reflecting infrared rays; when the temperature is higher than the phase transition temperature of vanadium dioxide, vanadium dioxide transforms into a metallic state, rapidly enhancing the infrared reflection ability and jointly playing a heat insulation role with the cesium tungsten bronze composite particles. In addition, due to the differences in the structures of the two composite particles themselves, their abilities to absorb, reflect, and scatter infrared rays of different wavelengths have their own emphases, and their mutual cooperation broadens the effective wavelength range of heat insulation, thus having good barrier performance for the near-infrared band of 700nm-2500nm. Therefore, within the above range, the two composite particles exert a synergistic effect, enabling the PVB composite film to exhibit high heat insulation ability under different temperature environments, light intensities, and other conditions, meeting diverse heat insulation requirements.

[0080] In some embodiments, the thickness of the PVB composite film is 0.5mm-1mm. Exemplarily, the thickness of the PVB composite film can be typical but non-limiting values such as 0.5mm, 0.6mm, 0.7mm, 0.8mm, 0.9mm, 1mm, etc.

[0081] When the thickness of the PVB composite film is within the above range, it can simultaneously have good heat insulation performance and high visible light transmittance. In this way, the formed laminated glass can exhibit excellent heat insulation ability and high-quality daylighting effect.

[0082] The second aspect of the embodiments of the present application provides a preparation method of a PVB composite film, including the following steps:

[0083] Step S10: Disperse cesium tungsten bronze and a titanium source in a first solvent, and obtain a cesium tungsten bronze-titanium dioxide core through a hydrolysis reaction;

[0084] Step S20: Coat the surface of the cesium tungsten bronze-titanium dioxide core with a first polyvinyl butyral to obtain cesium tungsten bronze composite particles;

[0085] Step S30: Add cesium tungsten bronze composite particles and the second polyvinyl butyral into a second solvent, and obtain a precursor solution after heat treatment;

[0086] Step S40: Perform film-forming treatment on the precursor solution to obtain a PVB composite film.

[0087] The method for preparing the PVB composite film provided in the second aspect of the embodiments of the present application decomposes the titanium source into titanium dioxide through hydrolysis to form a cesium tungsten bronze-titanium dioxide core, and then coats the polyvinyl butyral on the surface of the cesium tungsten bronze-titanium dioxide core, thus forming cesium tungsten bronze composite particles with a core-shell structure. Then, the solution blending method is used to make the cesium tungsten bronze composite particles relatively uniformly distributed in the PVB base film, thereby effectively preparing a film with the performance of the PVB composite film as described above in the present application. In addition, the method for preparing the PVB composite film in the present application has a simple process, and has high reliability and repeatability, and is suitable for industrial promotion and application.

[0088] In some embodiments, in step S10, the specific steps of dispersing cesium tungsten bronze and a titanium source in a first solvent and obtaining a cesium tungsten bronze-titanium dioxide core through a hydrolysis reaction are as follows:

[0089] Add cesium tungsten bronze into the first solvent I, then add the titanium source and the first solvent II to carry out a hydrolysis reaction to obtain a cesium tungsten bronze-titanium dioxide core.

[0090] Specifically, the first solvent I includes but is not limited to at least one of ethanol, acetone, and N-methylpyrrolidone.

[0091] Specifically, the first solvent II includes but is not limited to water.

[0092] Specifically, the titanium source includes but is not limited to tetrabutyl titanate.

[0093] Specifically, the particle size of cesium tungsten bronze is 0.1 μm - 10 μm, and the average particle size is 3 μm.

[0094] Specifically, the mass ratio of cesium tungsten bronze, the first solvent I, the titanium source, and the first solvent II is (1 - 3):(20 - 60):(5 - 15):(0.1 - 0.3).

[0095] In some embodiments, in step S10, the hydrolysis reaction includes reacting at 40°C - 60°C for 12h - 24h. Exemplarily, the temperature of the hydrolysis reaction can be typical but non-limiting values such as 40°C, 45°C, 50°C, 55°C, 60°C, etc., and the time of the hydrolysis reaction can be typical but non-limiting values such as 12h, 14h, 16h, 20h, 22h, 24h, etc.

[0096] The surface of cesium tungsten bronze has more active sites. Therefore, during the hydrolysis reaction of the titanium source, the intermediates generated gradually adsorb on the surface of cesium tungsten bronze particles. As the hydrolysis reaction proceeds, the intermediates form titanium dioxide, and the titanium dioxide continuously grows around the cesium tungsten bronze particles, so that the titanium dioxide coats the surface of cesium tungsten bronze to form a coating layer, forming a cesium tungsten bronze-titanium dioxide core.

[0097] In some embodiments, in step S20, the step of coating the surface of the cesium tungsten bronze-titanium dioxide core with the first polyvinyl butyral includes:

[0098] Adding the cesium tungsten bronze-titanium dioxide core and the first polyvinyl butyral to a third solvent and performing a grinding treatment.

[0099] During the grinding treatment, not only is the cesium tungsten bronze-titanium dioxide core refined to make it easier to disperse uniformly in subsequent steps, but also the first polyvinyl butyral gradually coats the surface of the cesium tungsten bronze-titanium dioxide core to form an outer shell layer, obtaining cesium tungsten bronze composite particles with a core-shell structure. At this time, the prepared PVB composite film only includes cesium tungsten bronze composite particles.

[0100] Specifically, the third solvent includes but is not limited to at least one of ethanol, acetone, and N-methylpyrrolidone.

[0101] Specifically, the mass ratio of the cesium tungsten bronze-titanium dioxide core, the first polyvinyl butyral, and the third solvent is (1 - 3):(0.1 - 0.3):(20 - 60).

[0102] In some embodiments, in step S20, the step of coating the surface of the cesium tungsten bronze-titanium dioxide core with the first polyvinyl butyral includes:

[0103] Adding the cesium tungsten bronze-titanium dioxide core, vanadium dioxide particles, and the first polyvinyl butyral to a third solvent and performing a grinding treatment.

[0104] Specifically, the mass ratio of the cesium tungsten bronze-titanium dioxide core, vanadium dioxide particles, the first polyvinyl butyral, and the second solvent is (0.5 - 1.5):(0.5 - 1.5):(0.1 - 0.3):(20 - 60).

[0105] During the grinding treatment, the first polyvinyl butyral gradually coats the surface of the cesium tungsten bronze-titanium dioxide core and the surface of the vanadium dioxide particles, respectively forming cesium tungsten bronze composite particles and vanadium dioxide composite particles. At this time, the prepared PVB composite film simultaneously includes cesium tungsten bronze composite particles and vanadium dioxide composite particles.

[0106] In some embodiments, in step S20, the grinding treatment includes treating at a rotational speed of 300 rpm - 400 rpm for 4 h - 6 h. Exemplarily, the rotational speed can be typical but non-limiting values such as 300 rpm, 310 rpm, 320 rpm, 330 rpm, 340 rpm, 350 rpm, 360 rpm, 370 rpm, 380 rpm, 390 rpm, 400 rpm, etc., and the time can be typical but non-limiting values such as 4 h, 4.5 h, 5 h, 5.5 h, 6 h, etc.

[0107] In some embodiments, in step S30, the specific process of adding the cesium tungsten bronze composite particles and the second polyvinyl butyral into the second solvent and obtaining the precursor solution after heat treatment is as follows:

[0108] Add the second polyvinyl butyral into the second solvent, fully dissolve it for 3 h - 6 h under heat treatment conditions, and then add the cesium tungsten bronze composite particles and mix evenly to obtain the precursor solution.

[0109] Specifically, the cesium tungsten bronze composite particles are added in the form of a dispersion liquid containing the cesium tungsten bronze composite particles, and the solid content of this dispersion liquid is 10% - 35%.

[0110] In some embodiments, in step S30, it further includes vanadium dioxide composite particles, and the specific process is as follows:

[0111] Add the second polyvinyl butyral into the second solvent, fully dissolve it for 3 h - 6 h under heat treatment conditions, and then add the cesium tungsten bronze composite particles and the vanadium dioxide composite particles and mix evenly to obtain the precursor solution.

[0112] Specifically, the cesium tungsten bronze composite particles and the vanadium dioxide composite particles are added in the form of a dispersion liquid containing the cesium tungsten bronze composite particles and the vanadium dioxide composite particles, and the solid content of this dispersion liquid is 10% - 35%.

[0113] Specifically, the second solvent includes but is not limited to at least one of ethanol, acetone, and N-methylpyrrolidone.

[0114] Specifically, the mass ratio of the second polyvinyl butyral to the second solvent can be 10:(50 - 70).

[0115] In some embodiments, in step S30, the heat treatment includes heating at 40°C - 70°C for 3 h - 6 h. Exemplarily, the temperature of the heat treatment can be typical but non-limiting values such as 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, etc., and the time can be typical but non-limiting values such as 3 h, 4 h, 5 h, 6 h, etc.

[0116] Under heat treatment conditions, the second polyvinyl butyral can be fully dissolved, thus making it easier to form a uniform and continuous film.

[0117] In some embodiments, in step S40, the film-forming treatment includes coating the precursor solution into a film and then curing it for 2 h - 6 h under the conditions of a temperature of 40°C - 70°C and a vacuum degree of -55 KPa to -45 KPa.

[0118] Exemplarily, the temperature of the curing treatment can be typical but non-limiting values such as 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, etc., the vacuum degree can be typical but non-limiting values such as -55 KPa, -50 KPa, -45 KPa, etc., and the time can be typical but non-limiting values such as 2 h, 3 h, 4 h, 5 h, 6 h, etc.

[0119] Under the above curing treatment conditions, it is easier to form a continuous, uniform and flat PVB composite film.

[0120] The third aspect of the embodiments of the present application provides a laminated glass, including at least two glass substrates, and a PVB composite film provided by the first aspect and / or a PVB composite film prepared by the preparation method provided by the second aspect is disposed between adjacent glass substrates.

[0121] For the laminated glass provided by the third aspect of the embodiments of the present application, since it contains the PVB composite film provided by the present application, and this PVB composite film has good heat insulation performance and high visible light transmittance, therefore, the laminated glass of the present application simultaneously has excellent heat insulation ability and high-quality lighting effect.

[0122] In some embodiments, the preparation process of the laminated glass is as follows:

[0123] Provide at least two glass substrates (such as white glass bare glass), clean and dry them; then fix the PVB composite film between two glass substrates through a high-temperature tape, put the fixed glass into a high-temperature and high-pressure autoclave, perform cold pumping for 2 h, then raise the temperature to 140°C, keep the pressure for 2 h, and then cool down and take it out to obtain the laminated glass.

[0124] The fourth aspect of the embodiments of the present application provides a vehicle, including the laminated glass provided by the third aspect.

[0125] The laminated glass can be used for the sunroof glass, rear window glass, and window glass of the driver's and passenger's seats in a vehicle.

[0126] For the vehicle provided by the fourth aspect of the embodiments of the present application, since it contains the laminated glass provided by the present application, the heat insulation effect of the vehicle is greatly improved, thereby reducing the air-conditioning load of the vehicle. At the same time, it can also create a bright and comfortable space environment and provide a high-transparency visual experience for the passengers.

[0127] The following is an illustration in conjunction with specific embodiments.

[0128] Examples of PVB composite films and their preparation methods:

[0129] Example 1

[0130] This example provides a PVB composite film with a thickness of 0.5 mm. The PVB composite film comprises a PVB base film and cesium tungsten bronze composite particles (with a particle size of 500 nm) in a mass ratio of 100:10. Among them, the cesium tungsten bronze composite particles include a core and a shell layer bonded successively from the inside to the outside along the radial direction. The mass ratio of the core to the shell layer is 1:0.1. The material of the shell layer includes polyvinyl butyral, and the core includes cesium tungsten bronze and titanium dioxide in a mass ratio of 1:1.17, and the titanium dioxide coats the surface of the cesium tungsten bronze to form a coating layer.

[0131] A method for preparing a PVB composite film includes the following steps:

[0132] Step 1: Add 1 g of cesium tungsten bronze particles into 20 g of ethanol, then add 5 g of tetrabutyl titanate and 0.1 g of deionized water, and then carry out a hydrolysis reaction at 50 °C for 12 h to obtain cesium tungsten bronze - titanium dioxide cores.

[0133] Step 2: Add 1 g of cesium tungsten bronze - titanium dioxide cores into 20 g of ethanol, then add 0.1 g of PVB powder (polyvinyl butyral), and carry out ball milling treatment at 400 rpm for 5 h to obtain a dispersion liquid containing cesium tungsten bronze composite particles. The solid content of this dispersion liquid is 35%.

[0134] Step 3: Add 10 g of PVB powder (polyvinyl butyral) into 60 g of ethanol, fully dissolve it at 60 °C, and then add 2.8 g of the dispersion liquid and mix evenly to obtain a precursor solution.

[0135] Step 4: Place the precursor solution in a mold, and carry out a curing treatment at a vacuum degree of -50 Kpa and a temperature of 60 °C for 4 h to obtain a PVB composite film.

[0136] Example 2

[0137] This embodiment provides a PVB composite film with a thickness of 0.5 mm. The PVB composite film comprises a PVB base film, cesium tungsten bronze composite particles (with a particle size of 500 nm), and vanadium dioxide composite particles in a mass ratio of 100:5:5. Among them, the cesium tungsten bronze composite particles include a core and a shell layer bonded in sequence from the inside to the outside along the radial direction. The mass ratio of the core to the shell layer is 1:0.1. The material of the shell layer includes polyvinyl butyral. The core includes cesium tungsten bronze and titanium dioxide in a mass ratio of 1:1.17, and the titanium dioxide coats the surface of the cesium tungsten bronze to form a coating layer. The vanadium dioxide composite particles include a vanadium dioxide core and a polyvinyl butyral shell layer coated on the surface of the vanadium dioxide core. The mass ratio of the vanadium dioxide core to the polyvinyl butyral shell layer is 1:0.1.

[0138] A preparation method of a PVB composite film includes the following steps:

[0139] Step 1: The same as Step 1 in Example 1.

[0140] Step 2: Add 0.5 g of cesium tungsten bronze - titanium dioxide core and 0.5 g of vanadium dioxide to 20 g of ethanol, and then add 0.1 g of PVB powder (polyvinyl butyral). Perform ball milling treatment at 400 rpm for 5 h to obtain a dispersion liquid containing cesium tungsten bronze composite particles and vanadium dioxide composite particles. The solid content of this dispersion liquid is 35%.

[0141] Step 3: Add 10 g of PVB powder (polyvinyl butyral) to 60 g of ethanol, fully dissolve it at 60 °C, and then add 2.8 g of the dispersion liquid and mix evenly to obtain a precursor liquid.

[0142] Step 4: The same as Step 4 in Example 1.

[0143] Example 3

[0144] This embodiment provides a PVB composite film, which is different from Example 1 in that the mass ratio of the PVB base film to the cesium tungsten bronze composite particles is 100:8.

[0145] A preparation method of a PVB composite film is different from Example 1 in that Step 3 is different. Specifically:

[0146] Step 3: Add 10 g of PVB powder (polyvinyl butyral) to 60 g of ethanol, fully dissolve it at 60 °C, and then add 2.3 g of the dispersion liquid and mix evenly to obtain a precursor liquid.

[0147] Example 4

[0148] This embodiment provides a PVB composite film, which is different from Example 1 in that in the cesium tungsten bronze composite particles, the mass ratio of cesium tungsten bronze to titanium dioxide is 1:2.4.

[0149] A preparation method of a PVB composite film, which is different from that of Example 1 in that: Step 1 is different, specifically:

[0150] Step 1: Add 1 g of cesium tungsten bronze particles to 20 g of ethanol, then add 10 g of tetrabutyl titanate and 0.1 g of deionized water, and then carry out a hydrolysis reaction at 50 °C for 12 h to obtain a cesium tungsten bronze-titanium dioxide core.

[0151] Example 5

[0152] This example provides a PVB composite film, which is different from that of Example 1 in that: in the cesium tungsten bronze composite particles, the mass ratio of cesium tungsten bronze to titanium dioxide is 1:3.5.

[0153] A preparation method of a PVB composite film, which is different from that of Example 1 in that: Step 1 is different, specifically:

[0154] Step 1: Add 1 g of cesium tungsten bronze particles to 20 g of ethanol, then add 15 g of tetrabutyl titanate and 0.1 g of deionized water, and then carry out a hydrolysis reaction at 50 °C for 12 h to obtain a cesium tungsten bronze-titanium dioxide core.

[0155] Example 6

[0156] This example provides a PVB composite film, which is different from that of Example 1 in that: in the cesium tungsten bronze composite particles, the mass ratio of the core to the outer shell layer is 1:0.3.

[0157] A preparation method of a PVB composite film, which is different from that of Example 1 in that: Step 2 is different, specifically:

[0158] Step 2: Add 1 g of cesium tungsten bronze-titanium dioxide core to 20 g of ethanol, then add 0.3 g of PVB powder (polyvinyl butyral), and carry out ball milling treatment at 400 rpm for 5 h to obtain a dispersion liquid containing cesium tungsten bronze composite particles, and the solid content of this dispersion liquid is 35%.

[0159] Example 7

[0160] This example provides a PVB composite film, which is different from that of Example 1 in that: in the cesium tungsten bronze composite particles, the mass ratio of the core to the outer shell layer is 3:0.1.

[0161] A preparation method of a PVB composite film, which is different from that of Example 1 in that: Step 2 is different, specifically:

[0162] Step 2: Add 3 g of cesium tungsten bronze - titanium dioxide core into 20 g of ethanol, then add 0.1 g of PVB powder (polyvinyl butyral), and perform ball milling treatment at 400 rpm for 5 h to obtain a dispersion liquid containing cesium tungsten bronze composite particles, and the solid content of this dispersion liquid is 35%.

[0163] Example 8

[0164] This example provides a PVB composite film, and the difference from Example 2 is that the mass ratio of the PVB base film, cesium tungsten bronze composite particles, and vanadium dioxide composite particles is 100:4:4.

[0165] A preparation method of a PVB composite film, and the difference from Example 2 is that Step 3 is different. Specifically:

[0166] Step 3: Add 10 g of PVB powder (polyvinyl butyral) into 60 g of ethanol, fully dissolve it at 60 °C, then add 2.3 g of the dispersion liquid and mix evenly to obtain a precursor solution.

[0167] Comparative Example 1

[0168] This comparative example provides a PVB composite film, and the difference from Example 1 is that the mass ratio of the PVB base film and cesium tungsten bronze composite particles is 10:0.5.

[0169] A preparation method of a PVB composite film, and the difference from Example 1 is that:

[0170] In Step 3, add 10 g of PVB powder (polyvinyl butyral) into 60 g of ethanol, fully dissolve it at 60 °C, then add 1.4 g of the dispersion liquid and mix evenly to obtain a precursor solution.

[0171] Comparative Example 2

[0172] This comparative example provides a PVB composite film, and the difference from Example 2 is that the mass ratio of the PVB base film, cesium tungsten bronze composite particles (particle size of 500 nm), and vanadium dioxide composite particles is 10:0.25:0.25.

[0173] A preparation method of a PVB composite film, and the difference from Example 2 is that:

[0174] In Step 3, add 10 g of PVB powder (polyvinyl butyral) into 60 g of ethanol, fully dissolve it at 60 °C, then add 1.4 g of the dispersion liquid and mix evenly to obtain a precursor solution.

[0175] Comparative Example 3

[0176] This comparative example provides a PVB film with a thickness of 0.5 mm. The preparation method of this PVB film includes the following steps:

[0177] 10 g of polyvinyl butyral powder (PVB) was added to 60 g of ethanol and fully dissolved at 60 °C. Then the obtained solution was placed in a mold and cured for 4 h under the conditions of a vacuum degree of -50 KPa and a temperature of 60 °C to obtain a PVB film.

[0178] Comparative Example 4

[0179] This comparative example provides a Low-e glass, and a three-silver-coated Low-e glass produced by Jiangsu Tiemao Technology Co., Ltd. was selected, that is, the three-silver Low-E glass of this company.

[0180] Laminated glass examples:

[0181] The PVB composite films provided in the above Examples 1-8 and Comparative Examples 1-2 were respectively assembled into laminated glass according to the following method:

[0182] The white glass bare glass was cleaned and dried, and then two pieces of bare glass with a specification of 10 cm × 10 cm were taken. The PVB composite film provided in the above examples, the PVB composite film of the comparative example, the PVB film or the Low-e glass were fixed in the middle of the two pieces of glass by high-temperature tape. The thicknesses of the PVB composite film and the PVB film were both 0.5 mm. The fixed glass was placed in a high-temperature and high-pressure autoclave. After cold pumping for 2 h, the temperature was raised to 140 °C, and after maintaining the pressure for 2 h, it was cooled and taken out to obtain the laminated glass for sky curtain glass. The laminated glasses containing the PVB composite films provided in Examples 1-8 were respectively denoted as Examples S1-S8, and the laminated glasses containing the PVB composite films, PVB films, and Low-e glasses provided in Comparative Examples 1-4 were respectively denoted as Comparative Examples DS1-DS4.

[0183] Performance characterization

[0184] (1) Microscopic morphology

[0185] The PVB composite film prepared in Example 1 was analyzed for microscopic morphology by a scanning electron microscope (SEM) and an energy-dispersive X-ray spectrometer (EDS), and the results are as Figure 1 shown.

[0186] Figure 1 In (a) is the SEM image of the surface of the PVB composite film prepared in Example 1, Figure 1 In (b) is the SEM image of the cross-section of the PVB composite film prepared in Example 1. It can be seen from the combination that the prepared PVB composite film has a highly uniform surface morphology. The surface of the film is overall continuous, uniform and flat, and there are no local protrusions or recessed areas formed due to the aggregation of microscopic particles, which means that good dispersion and fusion have been achieved among the components during the preparation of the PVB composite film. Figure 1Among them, (c) is the EDS diagram of the PVB composite film prepared in Example 1. From the figure, the distribution of elements can be observed. Specifically, the elements corresponding to cesium tungsten bronze are evenly dispersed inside the film, showing a uniformly dispersed state. In the entire EDS spectrum, the intensity of the element signal peaks representing cesium tungsten bronze is relatively stable in different regions, without obvious fluctuations in signal strength or local aggregation phenomena.

[0187] The PVB composite film prepared in Example 2 was analyzed for its microscopic morphology using a scanning electron microscope (SEM) and an energy dispersive X-ray spectrometer (EDS). The results are as Figure 2 shown.

[0188] Figure 2 Among them, (a) is the SEM diagram of the surface of the PVB composite film prepared in Example 2. Figure 2 Among them, (b) is the SEM diagram of the cross-section of the PVB composite film prepared in Example 2. It can be seen from the combination that the surface of the PVB composite film is overall continuous, uniform, and flat, without any local protrusions or recessed areas formed due to the aggregation of microscopic particles. Figure 2 Among them, (c) is the EDS diagram of the PVB composite film prepared in Example 2. From the figure, it can be observed that the elements corresponding to cesium tungsten bronze are evenly dispersed inside the film, showing a uniformly dispersed state.

[0189] (2) Optical property testing

[0190] The laminated glasses provided in Examples S1 - S8 and Comparative Examples DS1 - DS4 were respectively subjected to transmittance spectrum testing. The specific testing process was as follows: At room temperature, a Cary 5000 UV-Vis-NIR spectrophotometer (Agilent) was used to test the transmittance of the laminated glass in the ultraviolet-visible-near-infrared band (wavelength from 300 nm to 2500 nm).

[0191] The transmittance spectrum diagrams of Examples S1 - S2 are as Figure 3 shown. Among them, Figure 3 Among them, (a) is the transmittance spectrum diagram of Example S1. From the figure, it can be seen that the transmittance of the laminated glass provided in Example S1 in the near-infrared band with a wavelength of 750 nm to 2500 nm is 0, and the transmittance in the visible light wavelength range of 380 nm to 750 nm is 2.9%. Figure 3Among them, (b) is the transmittance spectrogram of Example S2. It can be seen from the figure that the laminated glass provided by Example S2 has a transmittance of 0 in the near-infrared band with a wavelength of 750 nm - 2500 nm, and a transmittance of 1.5% in the visible light wave range with a wavelength of 380 nm - 750 nm. Thus, it can be seen that the presence of cesium tungsten bronze composite particles and vanadium dioxide composite particles enables the PVB composite film to effectively block infrared rays, thereby endowing the laminated glass with good heat insulation performance.

[0192] The transmittance spectrograms of Comparative Examples DS1 - DS2 are as Figure 4 shown. Among them, Figure 4 in (a) is the transmittance spectrogram of Comparative Example DS1. It can be seen from the figure that the laminated glass provided by Comparative Example DS1 has a transmittance of 0 in the near-infrared band with a wavelength of 750 nm - 2500 nm, and a transmittance of 10% at the visible light wavelength with a wavelength of 380 nm - 750 nm. Figure 4 in (b) is the transmittance spectrogram of Comparative Example DS2. It can be seen from the figure that the laminated glass provided by Comparative Example DS2 has a transmittance of 0 in the near-infrared band with a wavelength of 750 nm - 2500 nm, and a transmittance of 5.9% at the visible light wavelength with a wavelength of 380 nm - 750 nm. Thus, it can be seen that after the addition amount of cesium tungsten bronze composite particles and vanadium dioxide composite particles decreases, its visible light transmittance has a certain increase.

[0193] The transmittance spectrograms of Comparative Examples DS3 - DS4 are as Figure 5 shown. Among them, Figure 5 in (a) is the transmittance spectrogram of Comparative Example DS3. It can be clearly seen that the laminated glass prepared from the PVB film has a transmittance of about 75% in the near-infrared band with a wavelength of 750 nm - 2500 nm, indicating that the PVB film has a weak ability to block infrared rays and a low heat insulation effect, but the visible light transmittance is at a relatively high level. Figure 5 in (b) is the transmittance spectrogram of Comparative Example DS4. It can be seen from the figure that the Low-e glass has an infrared transmittance of 0 in the 1400 nm - 2500 nm band, and its visible light transmittance is about 2.3%, indicating that Low-e cannot cover the entire near-infrared band, and its heat insulation performance needs to be improved.

[0194] (3) Heat insulation test

[0195] The laminated glasses provided by Examples S1 - S8 and Comparative Examples DS1 - DS4 were respectively subjected to heat insulation tests. Specifically: an infrared lamp with a power of 120 W was used to irradiate the laminated glass at a distance of 40 cm, and the changes in the external environment temperature, internal environment temperature, outer surface temperature of the glass, and inner surface temperature of the glass within 1 h were recorded. The test device is as Figure 6 shown.

[0196] The temperature change curves of Examples S1 - S2 are as shown in Figure 7 the following. Among them, Figure 7 (a) in it is the temperature change curve of Example S1. It can be seen from the figure that after 1 hour of infrared lamp irradiation, the temperature difference between the external environment temperature and the internal environment temperature of the laminated glass provided by Example S1 is 3°C. Figure 7 (b) in it is the temperature change curve of Example S2. It can be seen from the figure that after 1 hour of infrared lamp irradiation, the temperature difference between the external environment temperature and the internal environment temperature of the laminated glass provided by Example S2 is 3.5°C. This shows that the laminated glass provided by Examples S1 - S2 exhibits good heat insulation performance.

[0197] The temperature change curves of Comparative Examples DS1 - DS2 are as shown in Figure 8 the following. Among them, Figure 8 (a) in it is the temperature change curve of Comparative Example DS1. It can be seen from the figure that after 1 hour of infrared lamp irradiation, the temperature difference between the external environment temperature and the internal environment temperature of the laminated glass provided by Comparative Example DS1 is 1°C. Figure 8 (b) in it is the temperature change curve of Comparative Example DS2. It can be seen from the figure that after 1 hour of infrared lamp irradiation, the temperature difference between the external environment temperature and the internal environment temperature of the laminated glass provided by Comparative Example DS2 is 1.2°C. This shows that after the addition amount of cesium tungsten bronze composite particles and vanadium dioxide composite particles is reduced, the heat insulation effect of the laminated glass drops significantly.

[0198] The temperature change curve of Comparative Example DS4 is as shown in Figure 9 the following. It can be seen from Figure 9 the figure that after 1 hour of infrared lamp irradiation, the temperature difference between the external environment temperature and the internal environment temperature of the laminated glass provided by Comparative Example DS4 is 3.3°C, indicating that the laminated glass containing PVB composite film provided by this application has a heat insulation effect comparable to that of the laminated glass containing Low - e glass.

[0199] The results of the light performance test and heat insulation performance test of the laminated glass provided by Examples S1 - S8 and Comparative Examples DS1 - DS4 are listed in Table 1 below.

[0200] Table 1 Test Results

[0201]

[0202]

[0203] In Table 1, the wavelength of visible light is 380nm - 750nm.

[0204] In Table 1, the heat insulation performance test refers to the temperature difference between the external environment and the internal environment after 1 hour of infrared lamp irradiation. The higher the difference, the better the heat insulation performance of the laminated glass.

[0205] Combined with the spectral performance test and the heat insulation performance test results, it can be seen that the PVB composite film provided by this application can not only effectively block infrared rays in the 750nm - 2500nm band, has good heat insulation effect, but also has good visible light transmittance.

[0206] The above are only the preferred embodiments of this application, and are not intended to limit this application. Any modifications, equivalent replacements, and improvements made within the spirit and principle of this application shall be included in the protection scope of this application.

Claims

1. A PVB composite film, characterized in that: The invention comprises a PVB base film and cesium tungsten bronze composite particles distributed in the PVB base film. The cesium tungsten bronze composite particles comprise a core and an outer shell layer covering the core. The material of the core comprises cesium tungsten bronze and titanium dioxide, and the material of the outer shell layer comprises polyvinyl butyral.

2. The PVB composite film according to claim 1, characterized in that: In the core, at least a portion of the titanium dioxide is coated on the surface of the cesium tungsten bronze to form a coating layer.

3. The PVB composite film according to claim 1, characterized in that: The mass ratio of the PVB base film to the cesium tungsten bronze composite particles is 100:(8-10); and / or, The mass ratio of the cesium tungsten bronze to the titanium dioxide is (1-3): (1.1-3.6); and / or, The mass ratio of the inner core to the outer shell is (1-3):(0.1-0.3); and / or, The particle size of the cesium tungsten bronze composite particles is 100nm-1μm.

4. The PVB composite film according to claim 1, characterized in that: The PVB composite film further comprises vanadium dioxide composite particles, the vanadium dioxide composite particles are distributed in the PVB base film, and the vanadium dioxide composite particles comprise a vanadium dioxide core body and a polyvinyl butyral shell layer coated on the surface of the vanadium dioxide core body.

5. The PVB composite film according to claim 4, characterized in that: The particle size of the vanadium dioxide composite particles is 1 nm-100 nm; and / or, The mass ratio of the PVB base film, the cesium tungsten bronze composite particles and the vanadium dioxide composite particles is 100:(4-5):(4-5); and / or, The mass ratio of the vanadium dioxide core to the polyvinyl butyral shell is 1:(0.1-0.3).

6. The PVB composite film according to any one of claims 1 to 5, characterized in that: The thickness of the PVB composite film is 0.5 mm-1 mm.

7. A method for preparing a PVB composite film, characterized in that: The following steps are involved: Dispersing cesium tungsten bronze and titanium source in a first solvent, and obtaining a cesium tungsten bronze-titanium dioxide core through a hydrolysis reaction; coating the surface of the cesium tungsten bronze-titanium dioxide core with a first polyvinyl butyral to obtain cesium tungsten bronze composite particles; Adding the cesium tungsten bronze composite particles and the second polyvinyl butyral into a second solvent, and performing heat treatment to obtain a precursor solution; The precursor solution is subjected to film-forming treatment to obtain a PVB composite film.

8. The method for preparing the PVB composite film according to claim 7, characterized in that: The step of coating the first polyvinyl butyral on the surface of the cesium tungsten bronze-titanium dioxide core comprises: Adding the cesium tungsten bronze-titanium dioxide core and the first polyvinyl butyral into a third solvent for grinding; Alternatively, the cesium tungsten bronze-titanium dioxide core, the vanadium dioxide particles and the first polyvinyl butyral are added to a third solvent for grinding.

9. The method for preparing the PVB composite film according to claim 7 or 8, characterized in that: The hydrolysis reaction comprises reacting at 40°C-60°C for 12h-24h; and / or, The heat treatment comprises heating at 40°C-70°C for 3h-6h; and / or, The film forming process comprises coating the precursor solution to form a film and then curing the film for 2h-6h at a temperature of 40°C-70°C and a vacuum degree of -55KPa to -45KPa.

10. A laminated glass, characterized in that: The method comprises at least two glass substrates, wherein the PVB composite film according to any one of claims 1 to 6 and / or the PVB composite film prepared by the preparation method according to any one of claims 7 to 9 is arranged between adjacent glass substrates.

11. A car, characterized in that: Comprising the laminated glass as claimed in claim 10.

Citation Information

Cited By

  • Composite material based on Field metal and PVB as well as preparation method and application of composite material

    CN121718113A