N-type Bi-Sb-Se-Te thermoelectric material and preparation method and application thereof
By forming nanolayer sheets with optimal arrangement directions and large surface area in Bi-Sb-Se-Te thermoelectric materials, the problem of poor electrical transport performance is solved, the thermoelectric performance and conversion efficiency are significantly improved, and its application in thermoelectric devices is promoted.
Patent Information
- Application Number
- CN202510468814.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-14
- Publication Date
- 2025-07-18
AI Technical Summary
The existing Bi-Sb-Se-Te thermoelectric materials have poor electrical transport performance, which limits their application in thermoelectric devices.
By adjusting the temperature, deformation size and number of deformations, nanolayer sheets with optimal arrangement direction and large surface area are formed in Bi-Sb-Se-Te thermoelectric materials to improve electrical transport performance and improve thermoelectric performance.
The conductivity and thermoelectric properties of Bi-Sb-Se-Te thermoelectric materials have been significantly improved, making their thermoelectric conversion efficiency close to the level of single crystal samples, and promoting their application in the field of thermoelectric devices.
Smart Images

Figure CN120329042A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of thermoelectric materials, and particularly to an n-type Bi-Sb-Se-Te thermoelectric material, a preparation method thereof, and an application thereof. Background Art
[0002] According to the type of carriers transported, thermoelectric materials can be divided into two major categories: p-type and n-type. However, so far, for the same matrix thermoelectric material, the corresponding p-type and n-type thermoelectric arms are mostly obtained by doping donors or acceptors at different positions of the matrix material to generate electrons or holes, so as to obtain n-type and p-type thermoelectric materials respectively. This will lead to large differences in chemical composition, composition structure, etc. between the obtained n-type and p-type thermoelectric materials, thus affecting the mechanical strength and conversion efficiency of the thermoelectric devices assembled and prepared using them. Therefore, if an n-type and a p-type thermoelectric material with the same chemical composition can be prepared, it will be of great significance for the subsequent design and development of thermoelectric devices.
[0003] Bi-Sb-Se-Te-based thermoelectric materials have great potential in manufacturing high-efficiency thermoelectric conversion devices. However, due to the poor electrical transport properties of n-type Bi-Sb-Se-Te thermoelectric materials, their thermoelectric properties are not very excellent, which greatly limits their application in thermoelectric devices. Summary of the Invention
[0004] The purpose of the present invention is to provide an n-type Bi-Sb-Se-Te thermoelectric material, a preparation method thereof, and an application thereof, which can significantly improve the thermoelectric properties of n-type thermoelectric materials and promote their application in the field of thermoelectric devices.
[0005] In order to achieve the above-mentioned invention purpose, the present invention provides the following technical solutions:
[0006] The present invention provides a preparation method of an n-type Bi-Sb-Se-Te thermoelectric material, including the following steps:
[0007] According to the chemical composition of the thermoelectric material being Bi y Sb 2-y Se 3-x Te x , where 0.5 ≤ x ≤ 1.75, 0.5 ≤ y ≤ 1.75, mix elemental Bi, elemental Sb, elemental Se, and elemental Te, and perform alloying sintering under vacuum conditions to obtain alloyed powder;
[0008] Perform hot-pressing sintering on the alloyed powder to obtain an n-type alloy block;
[0009] Perform hot-pressing deformation on the n-type alloy block to obtain an n-type Bi-Sb-Se-Te thermoelectric material;
[0010] The number of hot press deformations is 1 to 4 times, the temperature of each hot press deformation is independently 400 to 450 °C, the deformation direction is perpendicular to the pressure direction, and the diameter of the mold used for the hot press deformation is 15 to 25 mm.
[0011] Preferably, x is 0.75 to 1.5 and y is 0.75 to 1.5.
[0012] Preferably, x is 1 to 1.25 and y is 1 to 1.25.
[0013] Preferably, the vacuum degree of the vacuum condition is < 1.0×10 -3 Pa; the alloying sintering includes first alloying sintering and second alloying sintering carried out in sequence.
[0014] Preferably, the temperature of the first alloying sintering is 300 to 500 °C, and the heat preservation time is 0.5 to 1 h; the temperature of the second alloying sintering is 700 to 900 °C, and the heat preservation time is 6 to 10 h; the heating rate for heating to the first alloying sintering and the second alloying sintering is independently 5 to 8 °C / min; the particle size of the alloying powder is 1 to 100 μm.
[0015] Preferably, the diameter of the graphite mold used for the hot press sintering is 10 to 15 mm.
[0016] Preferably, the temperature of the hot press sintering is 400 to 450 °C, the heat preservation time is 0.5 to 1 h, and the pressure is 30 to 50 MPa.
[0017] Preferably, the pressure of each hot press deformation is independently 50 to 100 MPa, and the heat preservation time is independently 0.5 to 1 h.
[0018] The present invention provides an n-type Bi-Sb-Se-Te thermoelectric material prepared by the preparation method described in the above technical solution.
[0019] The present invention provides the application of the n-type Bi-Sb-Se-Te thermoelectric material described in the above technical solution in thermoelectric devices.
[0020] The present invention provides an n-type Bi y Sb 2-y Se 3-x Te x Preparation method of a thermoelectric material, the chemical formula of the n-type thermoelectric material is Bi y Sb 2-y Se 3-x Te x where 0.5 ≤ x ≤ 1.75 and 0.5 ≤ y ≤ 1.75, and Bi y Sb 2-ySe 3-x Te x Thermoelectric materials, p-type and n-type thermoelectric materials with the same chemical composition can be prepared through point defect engineering. The preparation method provided by the present invention performs hot pressing deformation perpendicular to the pressure direction, and by adjusting the temperature of the thermal deformation, the magnitude of the deformation, the number of deformation times, etc., in the n-type Bi y Sb 2-y Se 3-x Te x nanolamellae with a preferred orientation direction and a large surface area can be formed inside the thermoelectric material, that is, without changing the Bi y Sb 2-y Se 3-x Te x conduction type, nanolamellae with a preferred orientation direction (perpendicular to the pressure direction) and a large surface area can be formed inside it, making it textured, effectively improving the grain preferred orientation, improving the electrical transport performance, enhancing its thermoelectric performance, providing an additional high-speed path for the carrier transport, being beneficial to the improvement of its electrical properties, making the n-type Bi y Sb 2-y Se 3-x Te x have good electrical and thermal properties, and can significantly improve the conversion efficiency of thermoelectric devices. The results of the examples show that through the way of thermal deformation, the preferred orientation of the grains of the n-type Bi y Sb 2-y Se 3- x Te x thermoelectric material can be effectively improved, and the conductivity of the n-type thermoelectric material can be greatly improved, and even it is expected to increase its power factor to a level close to that of single crystal samples, thereby effectively enhancing its thermoelectric performance, which is of great significance for the subsequent design and development of thermoelectric devices.
[0021] The n-type Bi y Sb 2-y Se 3-x Te x thermoelectric material prepared by the present invention is a multi-layered lamellar thermoelectric material, and there is an oriented texture with a preferred orientation inside it, which can significantly improve the carrier mobility of the material, greatly improve the conductivity of the n-type thermoelectric material, and optimize its electrical transport performance.
[0022] The preparation method adopted by the present invention has the advantages of simple equipment method, short preparation period, low production cost, environmental protection and suitability for large-scale popularization and application, etc., for improving the n-type Bi y Sb 2-y Se 3-xThe thermoelectric properties of Te thermoelectric materials are of great significance for promoting their applications in the field of thermoelectric devices and for developing thermoelectric materials with n-type and p-type conduction types in different regions. Description of the Drawings
[0023] Figure 1 XRD patterns of samples at different stages obtained in Example 13 of the present invention;
[0024] Figure 2 SEM images of samples at different stages obtained in Example 13 of the present invention; among them, (a), (c), (e) and (g) are SEM images of the fracture surfaces of the undeformed alloy bulk, the samples deformed 1, 2 and 3 times respectively, and (b), (d), (f) and (h) are the 3D reconstructed images corresponding to the fracture surfaces of the undeformed alloy bulk, the samples deformed 1, 2 and 3 times respectively;
[0025] Figure 3 Trend diagram of the Seebeck coefficient of samples at different stages obtained in Example 13 of the present invention varying with temperature;
[0026] Figure 4 Trend diagram of the electrical conductivity of samples at different stages obtained in Example 13 of the present invention varying with temperature;
[0027] Figure 5 Trend diagram of the power factor of samples at different stages obtained in Example 13 of the present invention varying with temperature;
[0028] Figure 6 Trend diagram of the total thermal conductivity of samples at different stages obtained in Example 13 of the present invention varying with temperature;
[0029] Figure 7 Figure of the dimensionless thermoelectric figure of merit of samples at different stages obtained in Example 13 of the present invention. Detailed Embodiments
[0030] In the present invention, unless otherwise specified, the raw materials or reagents required for preparation are all commercially available products well-known to those skilled in the art.
[0031] The present invention provides a method for preparing an n-type Bi-Sb-Se-Te thermoelectric material, comprising the following steps:
[0032] According to the chemical composition of the thermoelectric material being Bi y Sb 2-y Se 3-x Te x , 0.5 ≤ x ≤ 1.75, 0.5 ≤ y ≤ 1.75, mix elemental Bi, elemental Sb, elemental Se and elemental Te, and carry out alloying sintering under vacuum conditions to obtain alloyed powder;
[0033] Hot press sinter the alloyed powder to obtain an n-type alloy bulk;
[0034] Hot press deform the n-type alloy bulk to obtain an n-type Bi-Sb-Se-Te thermoelectric material;
[0035] The number of times of hot press deformation is 1 to 4 times, the temperature of each hot press deformation is independently 400 to 450 °C, the deformation direction is perpendicular to the pressure direction, and the diameter of the mold used for hot press deformation is 15 to 25 mm.
[0036] In the present invention, the chemical composition of the thermoelectric material is Bi y Sb 2-y Se 3-x Te x , where 0.5 ≤ x ≤ 1.75, 0.5 ≤ y ≤ 1.75, x is more preferably 0.75 to 1.5, x is further preferably 1 to 1.25, y is preferably 0.75 to 1.5, and y is more preferably 1 to 1.25. In the present invention, x is 0.5, 0.75, 1, 1.25, 1.5, 1.75, and more preferably 1.75; y is 0.5, 0.75, 1, 1.25, 1.5, 1.75, and more preferably 1.
[0037] In the present invention, Bi elemental substance, Sb elemental substance, Se elemental substance and Te elemental substance are mixed to obtain a mixture.
[0038] In the present invention, the atomic ratio of the Bi elemental substance to the Sb elemental substance is preferably (0.5 to 1.75):(0.25 to 1.5), more preferably (0.75 to 1.5):(0.5 to 1.25), and further preferably 1:1; the atomic ratio of the Bi elemental substance to the Se elemental substance is preferably (0.5 to 1.75):(1.25 to 2.5), more preferably (0.75 to 1.5):(1.5 to 2.0), and further preferably 1:1.25; the atomic ratio of the Bi elemental substance to the Te elemental substance is preferably (0.5 to 1.75):(0.5 to 1.75), more preferably (0.75 to 1.5):(1.0 to 1.75), and further preferably 1:1.75.
[0039] In the present invention, the purity of the Bi elemental substance, Sb elemental substance, Se elemental substance and Te elemental substance is independently > 99.999%; the Bi elemental substance, Sb elemental substance, Se elemental substance and Te elemental substance are all preferably elemental metal particles; the particle size of the Se elemental substance particles is preferably 2 to 5 mm; the particle size of the Sb elemental substance particles is preferably 2 to 6 mm; the Sb elemental substance particles are spherical-like; the particle size of the Bi elemental substance particles is preferably 1 to 6 mm; the Bi elemental substance particles are irregular; the particle size of the Te elemental substance particles is preferably 1 to 10 mm.
[0040] In the present invention, preferably, a mixture of raw materials is charged into a quartz tube according to a stoichiometric ratio. After fully shaking to make it uniformly mixed, it is evacuated, and then sealed under vacuum conditions using a hydrogen flame gun and placed in a muffle furnace for alloying sintering. The obtained alloy ingot is ground and crushed to obtain an alloyed powder.
[0041] In the present invention, the degree of vacuum of the vacuum condition (i.e., the vacuum degree of the quartz tube) is preferably < 1.0×10 -3 Pa, more preferably 5.0×10 -4 Pa; the alloying sintering preferably includes first alloying sintering and second alloying sintering carried out in sequence; the temperature of the first alloying sintering is preferably 300 - 500 °C, more preferably 300 - 400 °C, further preferably 300 °C, and the holding time is preferably 0.5 - 1 h, more preferably 0.5 h; the temperature of the second alloying sintering is preferably 700 - 900 °C, more preferably 800 - 900 °C, and the holding time is preferably 6 - 10 h, more preferably 8 - 9 h; the heating rate for heating to the first alloying sintering and the second alloying sintering is independently preferably 5 - 8 °C / min, more preferably 6 °C / min; the particle size of the alloyed powder is preferably 1 - 100 μm, more preferably 20 - 50 μm.
[0042] During the alloying sintering process, Bi element, Sb element, Se element, and Te element form an alloy ingot.
[0043] The present invention has no special limitation on the grinding and crushing, and the required particle size can be obtained according to the process well-known in the art. In the examples of the present invention, the crushing is preferably carried out using an agate mortar and grinding is also carried out.
[0044] The present invention charges the alloyed powder into a graphite mold for hot-pressing sintering to obtain an n-type alloy block.
[0045] In the present invention, the diameter of the graphite mold used for the hot-pressing sintering is preferably 10 - 15 mm, more preferably 13 - 15 mm.
[0046] In the present invention, the temperature of the hot-pressing sintering is preferably 400 - 450 °C, more preferably 420 - 450 °C, the holding time is preferably 0.5 - 1 h, more preferably 0.5 h, and the pressure is preferably 30 - 50 MPa, more preferably 35 - 50 MPa.
[0047] The present invention preferably places the n-type alloy block into a graphite mold for hot-pressing deformation to obtain an n-type Bi-Sb-Se-Te thermoelectric material.
[0048] In the present invention, the number of hot-pressing deformations is 1 to 4 times, more preferably 2 to 3 times. The temperature of each hot-pressing deformation is independently 400 to 450 °C, more preferably 420 to 450 °C. The diameter of the mold used for hot-pressing deformation is 15 to 25 mm, more preferably 20 mm.
[0049] In the present invention, the pressure of each hot-pressing deformation is independently preferably 50 to 100 MPa, more preferably 50 to 80 MPa, and further preferably 50 to 60 MPa; the heat preservation time is independently preferably 0.5 to 1 h, more preferably 0.5 h.
[0050] After completing one hot-pressing deformation, the present invention preferably uses electric discharge machining to cut the sample after one deformation into the size before deformation, and repeats the steps of hot-pressing deformation until the set number of hot-pressing deformations is reached.
[0051] Through multiple hot deformations of the hot-pressed sample, the present invention can form nano-lamellae with a preferred orientation and a large surface area in the n-type Bi y Sb 2-y Se 3-x Te x thermoelectric material, making it have good electrical and thermal properties.
[0052] The steps of hot-pressing sintering and hot-pressing deformation in the present invention are specifically as follows: The powder obtained by grinding in an agate mortar is loaded into a graphite mold with a diameter of 13 mm, and the graphite mold is placed in a hot-pressing furnace for hot-pressing sintering. After maintaining the temperature at 450 °C for 30 min under an axial pressure of 50 MPa, an undeformed bulk material HD0 is obtained; the HD0 sample with a diameter of 13 mm is loaded into a graphite mold with a diameter of 20 mm, and hot deformation is carried out under the conditions of an axial pressure of 50 MPa and a temperature of 450 °C for 30 min to obtain a bulk material HD1; the obtained HD1 sample with a diameter of 20 mm is cut into a cylinder with a diameter of 13 mm by electric discharge machining, and it is loaded into a graphite mold with a diameter of 20 mm again, and the cut HD1 cylindrical sample is sequentially subjected to secondary and tertiary hot deformations using the same process to obtain bulk materials HD2 and HD3 respectively.
[0053] The present invention provides an n-type Bi-Sb-Se-Te thermoelectric material prepared by the preparation method described in the above technical solution.
[0054] The present invention provides the application of the n-type Bi-Sb-Se-Te thermoelectric material described in the above technical solution in thermoelectric devices. The present invention has no special limitation on the application method of the thermoelectric material in thermoelectric devices, and the well-known application methods in the art can be adopted.
[0055] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the protection scope of the present invention. The experimental methods described in the embodiments of the present invention are conventional methods unless otherwise specified.
[0056] The following experimental methods and detection methods, unless otherwise specified, are conventional methods; the following reagents and raw materials, unless otherwise specified, are commercially available.
[0057] In the following embodiments, the purity of Bi, Sb, Se and Te is independently greater than 99.999%; the particle size of Bi particles is 1 to 6 mm; the particle size of Se particles is 2 to 5 mm; the particle size of Sb particles is preferably 2 to 6 mm; and the particle size of Te particles is 1 to 10 mm.
[0058] Example 1
[0059] (1) Ingredients: According to Bi 0.75 Sb 1.25 To determine the atomic ratio of Se2Te, weigh metal particles Bi, Sb, Se and Te with a purity of more than 99.999% and place them in a quartz tube. After shaking them thoroughly to mix them evenly, place them in a vacuum tube at a temperature of 5.0×10 - 4 Under the condition of Pa, the tube is sealed using a hydrogen flame gun;
[0060] (2) Alloying sintering: The sealed quartz tube is placed in a muffle furnace for alloying sintering, and the temperature is increased to 500°C at a heating rate of 6°C / min, and kept at this temperature for 0.5 h. Then, the temperature is increased to 900°C at a heating rate of 6°C / min, and kept at this temperature for 9 h, and then cooled with the furnace;
[0061] (3) crushing: crushing and grinding the obtained alloyed sintered product with an agate mortar to obtain an alloyed powder with a particle size of 1 to 100 μm;
[0062] (4) Hot pressing sintering: The alloyed powder was loaded into a graphite mold with a diameter of 13 mm, and hot pressed for 0.5 h at a sintering pressure of 50 MPa and a temperature of 450 ° C. The alloyed powder was cooled in the furnace to obtain an n-type alloy block.
[0063] (5) Hot pressing deformation sintering: The n-type alloy block sample with a diameter of 13 mm was placed in a graphite mold with a diameter of 20 mm and hot-deformed at a sintering pressure of 50 MPa and a temperature of 450 °C for 0.5 h.
[0064] (6) Electric spark cutting: Use electric spark to cut the Bi with a diameter of 20 mm after primary deformation. 0.75 Sb 1.25 Se2Te was cut into samples with a diameter of 13 mm.
[0065] (7) Repeated hot pressing deformation: Repeat steps (5) and (6) twice in sequence, and perform repeated hot pressing deformation on the sample to obtain a 3-times hot-deformed n-type Bi 0.75 Sb 1.25 Se2Te sample.
[0066] Example 2
[0067] (1) Ingredients: According to Bi 0.75 Sb 1.25 Se 2.5 Te 0.5 The atomic stoichiometric ratio of metal single substance particles Bi, Sb, Se and Te with a purity of more than 99.999% were weighed and placed in a quartz tube. After being shaken thoroughly to mix them evenly, the mixture was placed in a vacuum tube with a degree of 5.0×10 -4 Under the condition of Pa, the tube is sealed using a hydrogen flame gun;
[0068] (2) Alloying sintering: The sealed quartz tube is placed in a muffle furnace for alloying sintering, and the temperature is increased to 500°C at a heating rate of 6°C / min, and kept at this temperature for 0.5 h. Then, the temperature is increased to 900°C at a heating rate of 6°C / min, and kept at this temperature for 9 h, and then cooled with the furnace;
[0069] (3) crushing: crushing and grinding the obtained alloyed sintered product with an agate mortar to obtain alloyed powder;
[0070] (4) Hot pressing sintering: The alloyed powder is loaded into a graphite mold with a diameter of 13 mm, and hot pressing sintered for 0.5 h at a sintering pressure of 50 MPa and a temperature of 450 ° C. The alloy is then cooled in the furnace to obtain an n-type alloy block.
[0071] (5) Hot pressing deformation sintering: The n-type alloy block sample with a diameter of 13 mm was placed in a graphite mold with a diameter of 20 mm and hot-deformed at a sintering pressure of 50 MPa and a temperature of 450 °C for 0.5 h.
[0072] (6) Electric spark cutting: Use electric spark to cut the Bi with a diameter of 20 mm after primary deformation. 0.75 Sb 1.25 Se 2.5 Te 0.5 Cut into samples with a diameter of 13 mm;
[0073] (7) Repeated hot pressing deformation: Repeat steps (5) and (6) twice, and perform repeated hot pressing deformation on the sample to obtain a 3-times hot-deformed n-type Bi0.75 Sb 1.25 Se 2.5 Te 0.5 Sample.
[0074] Example 3
[0075] (1) Ingredients: According to the atomic stoichiometric ratio of Bi 0.75 Sb 1.25 Se 2.25 Te 0.75 , respectively weigh metal single - element particles Bi, Sb, Se, and Te with a purity higher than 99.999% and place them in a quartz tube. After fully shaking to make them evenly mixed, under the condition of a vacuum degree of 5.0×10 -4 Pa, use a hydrogen - flame gun to seal the tube;
[0076] (2) Alloying sintering: Put the sealed quartz tube into a muffle furnace for alloying sintering. Heat it at a heating rate of 6 °C / min to 500 °C, hold for 0.5 h, then heat it at a heating rate of 6 °C / min to 900 °C, hold for 9 h, and then cool it with the furnace;
[0077] (3) Crushing: Crush and grind the obtained alloying sintering product with an agate mortar to obtain an alloying powder with a particle size of 1 - 100 μm;
[0078] (4) Hot - pressing sintering: Load the alloying powder into a graphite mold with a diameter of 13 mm, and carry out hot - pressing sintering for 0.5 h under the conditions of a sintering pressure of 50 MPa and a temperature of 450 °C, and cool it with the furnace to obtain an n - type alloy block;
[0079] (5) Hot - pressing deformation sintering: Load the n - type alloy block sample with a diameter of 13 mm into a graphite mold with a diameter of 20 mm, and carry out hot deformation for 0.5 h under the conditions of a sintering pressure of 50 MPa and a temperature of 450 °C;
[0080] (6) Electrical - discharge machining: Use electrical - discharge machining to cut the Bi 0.75 Sb 1.25 Se 2.25 Te 0.75 with a diameter of 20 mm after the first deformation into a sample with a diameter of 13 mm;
[0081] (7) Repeat hot - pressing deformation: Repeat steps (5) and (6) 2 times to carry out repeated hot - pressing deformation on the sample to obtain an n - type Bi 0.75 Sb 1.25 Se 2.25 Te 0.75 sample.
[0082] Example 4
[0083] (1) Ingredients: According to the atomic stoichiometric ratio of Bi 0.75 Sb 1.25 Se 1.75 Te 1.25 , weigh out the metal elemental particles Bi, Sb, Se, and Te with a purity higher than 99.999% respectively and place them in a quartz tube. After fully shaking to mix them evenly, under the condition of a vacuum degree of 5.0×10 -4 Pa, use a hydrogen flame gun to seal the tube;
[0084] (2) Alloying sintering: Put the sealed quartz tube into a muffle furnace for alloying sintering. Heat it up to 500 °C at a heating rate of 6 °C / min, hold for 0.5 h, then heat it up to 900 °C at a heating rate of 6 °C / min, hold for 9 h, and then cool it with the furnace;
[0085] (3) Crushing: Crush and grind the obtained alloying sintering product with an agate mortar to obtain an alloying powder with a particle size of 1 - 100 μm;
[0086] (4) Hot - pressing sintering: Load the alloying powder into a graphite mold with a diameter of 13 mm, and carry out hot - pressing sintering for 0.5 h under the conditions of a sintering pressure of 50 MPa and a temperature of 450 °C, then cool it with the furnace to obtain an n - type alloy block;
[0087] (5) Hot - pressing deformation sintering: Load the n - type alloy block sample with a diameter of 13 mm into a graphite mold with a diameter of 20 mm, and carry out hot deformation for 0.5 h under the conditions of a sintering pressure of 50 MPa and a temperature of 450 °C;
[0088] (6) Electrical discharge machining: Use electrical discharge to cut the Bi 0.75 Sb 1.25 Se 1.75 Te 1.25 with a diameter of 20 mm after the first deformation into samples with a diameter of 13 mm;
[0089] (7) Repeat hot - pressing deformation: Repeat steps (5) and (6) 2 times to carry out repeated hot - pressing deformation on the sample to obtain an n - type Bi 0.75 Sb 1.25 Se 1.75 Te 1.25 sample.
[0090] Example 5
[0091] (1) Ingredients: According to Bi 0.75 Sb 1.25 Se 1.5 Te 1.5For the atomic stoichiometric ratio, metallic elemental particles of Bi, Sb, Se, and Te with a purity higher than 99.999% were respectively weighed and placed in a quartz tube. After fully shaking to make them evenly mixed, under the condition of a vacuum degree of 5.0×10 -4 Pa, a hydrogen flame gun was used for sealing the tube;
[0092] (2) Alloying sintering: The sealed quartz tube was placed in a muffle furnace for alloying sintering. It was heated to 500 °C at a heating rate of 6 °C / min, held for 0.5 h, then heated to 900 °C at a heating rate of 6 °C / min, held for 9 h, and then cooled with the furnace;
[0093] (3) Crushing: The obtained alloying sintering product was crushed and ground with an agate mortar to obtain an alloying powder with a particle size of 1 - 100 μm;
[0094] (4) Hot - pressing sintering: The alloying powder was loaded into a graphite mold with a diameter of 13 mm. Under the conditions of a sintering pressure of 50 MPa and a temperature of 450 °C, hot - pressing sintering was carried out for 0.5 h, and then cooled with the furnace to obtain an n - type alloy block;
[0095] (5) Hot - pressing deformation sintering: The n - type alloy block sample with a diameter of 13 mm was loaded into a graphite mold with a diameter of 20 mm. Under the conditions of a sintering pressure of 50 MPa and a temperature of 450 °C, hot deformation was carried out for 0.5 h;
[0096] (6) Electrical discharge machining: Using electrical discharge, the Bi 0.75 Sb 1.25 Se 1.5 Te 1.5 with a diameter of 20 mm after the first deformation was cut into samples with a diameter of 13 mm;
[0097] (7) Repeating hot - pressing deformation: Steps (5) and (6) were repeated 2 times to perform repeated hot - pressing deformation on the samples, and 3 - time hot - deformed n - type Bi 0.75 Sb 1.25 Se 1.5 Te 1.5 samples were obtained.
[0098] Example 6
[0099] (1) Batching: According to the atomic stoichiometric ratio of Bi 0.75 Sb 1.25 Se 1.25 Te 1.75 metallic elemental particles of Bi, Sb, Se, and Te with a purity higher than 99.999% were respectively weighed and placed in a quartz tube. After fully shaking to make them evenly mixed, under the condition of a vacuum degree of 5.0×10 -4 Pa, a hydrogen flame gun was used for sealing the tube;
[0100] (2) Alloying sintering: Put the sealed quartz tube into a muffle furnace for alloying sintering. Heat it at a heating rate of 6 °C / min to 500 °C, hold for 0.5 h, then heat it at a heating rate of 6 °C / min to 900 °C, hold for 9 h, and then cool it in the furnace;
[0101] (3) Crushing: Crush and grind the obtained alloying sintering product with an agate mortar to obtain alloying powder with a particle size of 1 - 100 μm;
[0102] (4) Hot - pressing sintering: Load the alloying powder into a graphite mold with a diameter of 13 mm, and carry out hot - pressing sintering for 0.5 h under the conditions of a sintering pressure of 50 MPa and a temperature of 450 °C, then cool it in the furnace to obtain an n - type alloy block;
[0103] (5) Hot - pressing deformation sintering: Load the n - type alloy block sample with a diameter of 13 mm into a graphite mold with a diameter of 20 mm, and carry out hot deformation for 0.5 h under the conditions of a sintering pressure of 50 MPa and a temperature of 450 °C;
[0104] (6) Electrical discharge machining: Use electrical discharge to cut the Bi 0.75 Sb 1.25 Se 1.25 Te 1.75 with a diameter of 20 mm after the first deformation into a sample with a diameter of 13 mm;
[0105] (7) Repeated hot - pressing deformation: Repeat steps (5) and (6) 2 times to carry out repeated hot - pressing deformation on the sample to obtain an n - type Bi 0.75 Sb 1.25 Se 1.25 Te 1.75 sample after 3 - time hot deformation.
[0106] Example 7
[0107] (1) Batching: According to the atomic stoichiometric ratio of BiSbSe2Te, respectively weigh metal single - element particles Bi, Sb, Se, and Te with a purity higher than 99.999% and place them in a quartz tube. After fully shaking to make them mixed evenly, under the condition of a vacuum degree of 5.0×10 -4 Pa, use a hydrogen flame gun to seal the tube;
[0108] (2) Alloying sintering: Put the sealed quartz tube into a muffle furnace for alloying sintering. Heat it at a heating rate of 6 °C / min to 500 °C, hold for 0.5 h, then heat it at a heating rate of 6 °C / min to 900 °C, hold for 9 h, and then cool it in the furnace;
[0109] (3) Crushing: The obtained alloyed sintered product was crushed and ground in an agate mortar to obtain an alloyed powder with a particle size of 1 - 100 μm;
[0110] (4) Hot pressing sintering: The alloyed powder was loaded into a graphite mold with a diameter of 13 mm, and hot pressing sintering was carried out for 0.5 h under the conditions of a sintering pressure of 50 MPa and a temperature of 450 °C, and then cooled in the furnace to obtain an n-type alloy block;
[0111] (5) Hot pressing deformation sintering: The n-type alloy block sample with a diameter of 13 mm was loaded into a graphite mold with a diameter of 20 mm, and hot deformation was carried out for 0.5 h under the conditions of a sintering pressure of 50 MPa and a temperature of 450 °C;
[0112] (6) Electrical discharge machining: BiSbSe2Te with a diameter of 20 mm after the first deformation was cut into samples with a diameter of 13 mm by electrical discharge machining;
[0113] (7) Repeated hot pressing deformation: Steps (5) and (6) were repeated 2 times to perform repeated hot pressing deformation on the samples to obtain a 3-time hot deformed n-type BiSbSe2Te sample.
[0114] Example 8
[0115] (1) Batching: According to the atomic stoichiometric ratio of BiSbSe 2.5 Te 0.5 , metallic single-element particles Bi, Sb, Se, and Te with a purity higher than 99.999% were respectively weighed and placed in a quartz tube. After fully shaking to mix them evenly, the tube was sealed under the condition of a vacuum degree of 5.0×10 -4 Pa using a hydrogen flame gun;
[0116] (2) Alloying sintering: The sealed quartz tube was placed in a muffle furnace for alloying sintering. It was heated to 500 °C at a heating rate of 6 °C / min, held for 0.5 h, then heated to 900 °C at a heating rate of 6 °C / min, held for 9 h, and then cooled in the furnace;
[0117] (3) Crushing: The obtained alloyed sintered product was crushed and ground in an agate mortar to obtain an alloyed powder with a particle size of 1 - 100 μm;
[0118] (4) Hot pressing sintering: The alloyed powder was loaded into a graphite mold with a diameter of 13 mm, and hot pressing sintering was carried out for 0.5 h under the conditions of a sintering pressure of 50 MPa and a temperature of 450 °C, and then cooled in the furnace to obtain an n-type alloy block;
[0119] (5) Hot press deformation sintering: Load an n-type alloy bulk sample with a diameter of 13 mm into a graphite mold with a diameter of 20 mm, and under the conditions of a sintering pressure of 50 MPa and a temperature of 450 °C, perform hot deformation for 0.5 h;
[0120] (6) Electrical discharge machining: Use electrical discharge to cut BiSbSe with a diameter of 20 mm after the first deformation 2.5 Te 0.5 into samples with a diameter of 13 mm;
[0121] (7) Repeat hot press deformation: Repeat steps (5) and (6) twice to perform repeated hot press deformation on the samples to obtain n-type BiSbSe 2.5 Te 0.5 samples after 3 times of hot deformation.
[0122] Example 9
[0123] (1) Batching: According to the atomic stoichiometric ratio of BiSbSe 2.25 Te 0.75 , respectively weigh metal single crystal particles Bi, Sb, Se, and Te with a purity higher than 99.999% and place them in a quartz tube. After fully shaking to mix them evenly, under the condition of a vacuum degree of 5.0×10 - 4 Pa, use a hydrogen flame gun to seal the tube;
[0124] (2) Alloying sintering: Put the sealed quartz tube into a muffle furnace for alloying sintering. Heat it up to 500 °C at a heating rate of 6 °C / min, hold for 0.5 h, then heat it up to 900 °C at a heating rate of 6 °C / min, hold for 9 h, and then cool it down with the furnace;
[0125] (3) Crushing: Crush and grind the obtained alloying sintering product with an agate mortar to obtain an alloying powder with a particle size of 1 - 100 μm;
[0126] (4) Hot press sintering: Load the alloying powder into a graphite mold with a diameter of 13 mm, and under the conditions of a sintering pressure of 50 MPa and a temperature of 450 °C, perform hot press sintering for 0.5 h, and cool it down with the furnace to obtain an n-type alloy bulk;
[0127] (5) Hot press deformation sintering: Load an n-type alloy bulk sample with a diameter of 13 mm into a graphite mold with a diameter of 20 mm, and under the conditions of a sintering pressure of 50 MPa and a temperature of 450 °C, perform hot deformation for 0.5 h;
[0128] (6) Electrical discharge machining: Use electrical discharge to cut BiSbSe with a diameter of 20 mm after the first deformation 2.25 Te 0.75 into samples with a diameter of 13 mm;
[0129] (7) Repeated hot pressing deformation: Repeat steps (5) and (6) twice to perform repeated hot pressing deformation on the sample to obtain a sample of n-type BiSbSe 2.25 Te 0.75 with three times of hot deformation.
[0130] Example 10
[0131] (1) Batching: According to the atomic stoichiometric ratio of BiSbSe 2.15 Te 0.85 , weigh the metal single-element particles Bi, Sb, Se, and Te with a purity higher than 99.999% respectively and place them in a quartz tube. After fully shaking to mix them evenly, under the condition of a vacuum degree of 5.0×10 - 4 Pa, use a hydrogen flame gun to seal the tube;
[0132] (2) Alloying sintering: Put the sealed quartz tube into a muffle furnace for alloying sintering. Heat it up to 500°C at a heating rate of 6°C / min, hold for 0.5 h, then heat it up to 900°C at a heating rate of 6°C / min, hold for 9 h, and then cool it with the furnace;
[0133] (3) Crushing: Crush and grind the obtained alloying sintering product with an agate mortar to obtain an alloying powder with a particle size of 1 - 100 μm;
[0134] (4) Hot pressing sintering: Load the alloying powder into a graphite mold with a diameter of 13 mm, and perform hot pressing sintering for 0.5 h under the conditions of a sintering pressure of 50 MPa and a temperature of 450°C, and cool it with the furnace to obtain an n-type alloy block;
[0135] (5) Hot pressing deformation sintering: Load the n-type alloy block sample with a diameter of 13 mm into a graphite mold with a diameter of 20 mm, and perform hot deformation for 0.5 h under the conditions of a sintering pressure of 50 MPa and a temperature of 450°C;
[0136] (6) Electrical discharge machining: Use electrical discharge to cut the BiSbSe 2.15 Te 0.85 with a diameter of 20 mm after the first deformation into a sample with a diameter of 13 mm;
[0137] (7) Repeated hot pressing deformation: Repeat steps (5) and (6) twice to perform repeated hot pressing deformation on the sample to obtain a sample of n-type BiSbSe 2.15 Te 0.85 with three times of hot deformation.
[0138] Example 11
[0139] (1) Batching: According to the atomic stoichiometric ratio of BiSbSe1.75 Te 1.25 The atomic ratio of Bi, Sb, Se and Te with a purity of more than 99.999% was weighed and placed in a quartz tube. After being shaken thoroughly to mix them evenly, the mixture was placed in a vacuum tube with a vacuum degree of 5.0×10 - 4 Under the condition of Pa, the tube is sealed using a hydrogen flame gun;
[0140] (2) Alloying sintering: The sealed quartz tube is placed in a muffle furnace for alloying sintering, and the temperature is increased to 500°C at a heating rate of 6°C / min, and kept at this temperature for 0.5 h. Then, the temperature is increased to 900°C at a heating rate of 6°C / min, and kept at this temperature for 9 h, and then cooled with the furnace;
[0141] (3) crushing: crushing and grinding the obtained alloyed sintered product with an agate mortar to obtain an alloyed powder with a particle size of 1 to 100 μm;
[0142] (4) Hot pressing sintering: The alloyed powder was loaded into a graphite mold with a diameter of 13 mm, and hot pressed for 0.5 h at a sintering pressure of 50 MPa and a temperature of 450 ° C. The alloyed powder was cooled in the furnace to obtain an n-type alloy block.
[0143] (5) Hot pressing deformation sintering: The n-type alloy block sample with a diameter of 13 mm was placed in a graphite mold with a diameter of 20 mm and hot-deformed at a sintering pressure of 50 MPa and a temperature of 450 °C for 0.5 h.
[0144] (6) Electric spark cutting: The BiSbSe with a diameter of 20 mm after primary deformation is cut by electric spark. 1.75 Te 1.25 Cut into samples with a diameter of 13 mm;
[0145] (7) Repeated hot pressing deformation: Repeat steps (5) and (6) twice, and perform repeated hot pressing deformation on the sample to obtain 3 times hot-deformed n-type BiSbSe 1.75 Te 1.25 sample.
[0146] Example 12
[0147] (1) Ingredients: BiSbSe 1.5 Te 1.5 The atomic ratio of Bi, Sb, Se and Te with a purity of more than 99.999% was weighed and placed in a quartz tube. After being shaken thoroughly to mix them evenly, the mixture was placed in a vacuum tube with a vacuum degree of 5.0×10 -4 Under the condition of Pa, the tube is sealed using a hydrogen flame gun;
[0148] (2) Alloying sintering: Put the sealed quartz tube into a muffle furnace for alloying sintering. Heat it up to 500 °C at a heating rate of 6 °C / min, hold for 0.5 h, then heat it up to 900 °C at a heating rate of 6 °C / min, hold for 9 h, and then cool it down with the furnace;
[0149] (3) Crushing: Crush and grind the obtained alloying sintering product with an agate mortar to obtain alloying powder with a particle size of 1 - 100 μm;
[0150] (4) Hot pressing sintering: Load the alloying powder into a graphite mold with a diameter of 13 mm, and carry out hot pressing sintering for 0.5 h under the conditions of a sintering pressure of 50 MPa and a temperature of 450 °C, and then cool it down with the furnace to obtain an n-type alloy block;
[0151] (5) Hot pressing deformation sintering: Load the n-type alloy block sample with a diameter of 13 mm into a graphite mold with a diameter of 20 mm, and carry out hot deformation for 0.5 h under the conditions of a sintering pressure of 50 MPa and a temperature of 450 °C;
[0152] (6) Electrical discharge machining: Use electrical discharge to cut BiSbSe 1.5 Te 1.5 with a diameter of 20 mm after the first deformation into samples with a diameter of 13 mm;
[0153] (7) Repeat hot pressing deformation: Repeat steps (5) and (6) twice to carry out repeated hot pressing deformation on the sample to obtain a 3-time hot-deformed n-type BiSbSe 1.5 Te 1.5 sample.
[0154] Example 13
[0155] (1) Batching: According to the atomic stoichiometric ratio of BiSbSe 1.25 Te 1.75 , respectively weigh the metal single-element particles Bi, Sb, Se, and Te with a purity higher than 99.999% and place them in a quartz tube. After fully shaking to mix them evenly, under the condition of a vacuum degree of 5.0×10 - 4 Pa, use a hydrogen torch to seal the tube;
[0156] (2) Alloying sintering: Put the sealed quartz tube into a muffle furnace for alloying sintering. Heat it up to 500 °C at a heating rate of 6 °C / min, hold for 0.5 h, then heat it up to 900 °C at a heating rate of 6 °C / min, hold for 9 h, and then cool it down with the furnace;
[0157] (3) Crushing: Crush and grind the obtained alloying sintering product with an agate mortar to obtain alloying powder with a particle size of 1 - 100 μm;
[0158] (4) Hot pressing sintering: Load the alloyed powder into a graphite mold with a diameter of 13 mm, and carry out hot pressing sintering for 0.5 h under the conditions of a sintering pressure of 50 MPa and a temperature of 450 °C, and then cool it in the furnace to obtain an n-type alloy block;
[0159] (5) Hot deformation sintering: Load the n-type alloy block sample with a diameter of 13 mm into a graphite mold with a diameter of 20 mm, and carry out hot deformation for 0.5 h under the conditions of a sintering pressure of 50 MPa and a temperature of 450 °C;
[0160] (6) Electrical discharge machining: Use electrical discharge to cut BiSbSe with a diameter of 20 mm after the first deformation 1.25 Te 1.75 into samples with a diameter of 13 mm;
[0161] (7) Repeated hot pressing deformation: Repeat steps (5) and (6) twice to carry out repeated hot pressing deformation on the sample, and obtain an n-type BiSbSe 1.25 Te 1.75 sample after 3 times of hot deformation.
[0162] Example 14
[0163] (1) Batching: According to the atomic stoichiometric ratio of Bi 1.25 Sb 0.75 Se2Te, weigh out metal single crystal particles Bi, Sb, Se and Te with a purity higher than 99.999% respectively and place them in a quartz tube. After fully shaking to mix them evenly, under the condition of a vacuum degree of 5.0×10 - 4 Pa, use a hydrogen flame gun to seal the tube;
[0164] (2) Alloying sintering: Put the sealed quartz tube into a muffle furnace for alloying sintering. Heat it up to 500 °C at a heating rate of 6 °C / min, keep it warm for 0.5 h, then heat it up to 900 °C at a heating rate of 6 °C / min, keep it warm for 9 h, and then cool it in the furnace;
[0165] (3) Crushing: Crush and grind the obtained alloying sintering product with an agate mortar to obtain an alloyed powder with a particle size of 1 - 100 μm;
[0166] (4) Hot pressing sintering: Load the alloyed powder into a graphite mold with a diameter of 13 mm, and carry out hot pressing sintering for 0.5 h under the conditions of a sintering pressure of 50 MPa and a temperature of 450 °C, and then cool it in the furnace to obtain an n-type alloy block;
[0167] (5) Hot pressing deformation sintering: Load an n-type alloy bulk sample with a diameter of 13 mm into a graphite mold with a diameter of 20 mm, and perform hot deformation at a sintering pressure of 50 MPa and a temperature of 450 °C for 0.5 h;
[0168] (6) Electrical discharge machining: Use electrical discharge to cut Bi with a diameter of 20 mm after the first deformation 1.25 Sb 0.75 Se2Te into samples with a diameter of 13 mm;
[0169] (7) Repeat hot pressing deformation: Repeat steps (5) and (6) successively 2 times to perform repeated hot pressing deformation on the samples, and obtain n-type Bi with 3 times of hot deformation 1.25 Sb 0.75 Se2Te samples.
[0170] Example 15
[0171] (1) Batching: According to the atomic stoichiometric ratio of Bi 1.25 Sb 0.75 Se 2.5 Te 0.5 , respectively weigh metal single-element particles Bi, Sb, Se, and Te with a purity higher than 99.999% and place them in a quartz tube. After fully shaking to mix them evenly, under the condition of a vacuum degree of 5.0×10 -4 Pa, use a hydrogen flame gun to seal the tube;
[0172] (2) Alloying sintering: Put the sealed quartz tube into a muffle furnace for alloying sintering. Heat it up to 500 °C at a heating rate of 6 °C / min, hold for 0.5 h, then heat it up to 900 °C at a heating rate of 6 °C / min, hold for 9 h, and then cool it with the furnace;
[0173] (3) Crushing: Crush and grind the obtained alloying sintering product with an agate mortar to obtain an alloying powder with a particle size of 1 - 100 μm;
[0174] (4) Hot pressing sintering: Load the alloying powder into a graphite mold with a diameter of 13 mm, and perform hot pressing sintering for 0.5 h at a sintering pressure of 50 MPa and a temperature of 450 °C, and cool it with the furnace to obtain an n-type alloy bulk;
[0175] (5) Hot pressing deformation sintering: Load an n-type alloy bulk sample with a diameter of 13 mm into a graphite mold with a diameter of 20 mm, and perform hot deformation at a sintering pressure of 50 MPa and a temperature of 450 °C for 0.5 h;
[0176] (6) Electrical discharge machining: Use electrical discharge to cut Bi with a diameter of 20 mm after the first deformation 1.25 Sb 0.75 Se2.5 Te 0.5 Cut into samples with a diameter of 13 mm;
[0177] (7) Repeated hot pressing deformation: Repeat steps (5) and (6) twice, and perform repeated hot pressing deformation on the sample to obtain a 3-times hot-deformed n-type Bi 1.25 Sb 0.75 Se 2.5 Te 0.5 sample.
[0178] Example 16
[0179] (1) Ingredients: According to Bi 1.25 Sb 0.75 Se 2.25 Te 0.75 The atomic stoichiometric ratio of metal single substance particles Bi, Sb, Se and Te with a purity of more than 99.999% were weighed and placed in a quartz tube. After being shaken thoroughly to mix them evenly, the mixture was placed in a vacuum tube with a degree of 5.0×10 -4 Under the condition of Pa, the tube is sealed using a hydrogen flame gun;
[0180] (2) Alloying sintering: The sealed quartz tube is placed in a muffle furnace for alloying sintering, and the temperature is increased to 500°C at a heating rate of 6°C / min, and kept at this temperature for 0.5 h. Then, the temperature is increased to 900°C at a heating rate of 6°C / min, and kept at this temperature for 9 h, and then cooled with the furnace;
[0181] (3) crushing: crushing and grinding the obtained alloyed sintered product with an agate mortar to obtain an alloyed powder with a particle size of 1 to 100 μm;
[0182] (4) Hot pressing sintering: The alloyed powder is loaded into a graphite mold with a diameter of 13 mm, and hot pressing sintered for 0.5 h at a sintering pressure of 50 MPa and a temperature of 450 ° C. The alloy is cooled in the furnace to obtain an n-type alloy block;
[0183] (5) Hot pressing deformation sintering: The n-type alloy block sample with a diameter of 13 mm was placed in a graphite mold with a diameter of 20 mm and hot-deformed at a sintering pressure of 50 MPa and a temperature of 450 °C for 0.5 h.
[0184] (6) Electric spark cutting: Use electric spark to cut the Bi with a diameter of 20 mm after primary deformation. 1.25 Sb 0.75 Se 2.25 Te 0.75 Cut into samples with a diameter of 13 mm;
[0185] (7) Repeated hot pressing deformation: Repeat steps (5) and (6) twice, and perform repeated hot pressing deformation on the sample to obtain a 3-times hot-deformed n-type Bi1.25 Sb 0.75 Se 2.25 Te 0.75 Sample.
[0186] Example 17
[0187] (1) Ingredients: According to the atomic stoichiometric ratio of Bi 1.25 Sb 0.75 Se 1.75 Te 1.25 , respectively weigh metal single - element particles Bi, Sb, Se and Te with a purity higher than 99.999% and place them in a quartz tube. After fully shaking to make them evenly mixed, under the condition of a vacuum degree of 5.0×10 -4 Pa, use a hydrogen - flame gun to seal the tube;
[0188] (2) Alloying sintering: Put the sealed quartz tube into a muffle furnace for alloying sintering. Heat it at a heating rate of 6℃ / min to 500℃, hold for 0.5 h, then heat it at a heating rate of 6℃ / min to 900℃, hold for 9 h, and then cool it with the furnace;
[0189] (3) Crushing: Crush and grind the obtained alloying - sintering product with an agate mortar to obtain an alloying powder with a particle size of 1 - 100 μm;
[0190] (4) Hot - press sintering: Load the alloying powder into a graphite mold with a diameter of 13 mm, and carry out hot - press sintering for 0.5 h under the conditions of a sintering pressure of 50 MPa and a temperature of 450℃, then cool it with the furnace to obtain an n - type alloy block;
[0191] (5) Hot - press deformation sintering: Load an n - type alloy block sample with a diameter of 13 mm into a graphite mold with a diameter of 20 mm, and carry out hot deformation for 0.5 h under the conditions of a sintering pressure of 50 MPa and a temperature of 450℃;
[0192] (6) Electrical - discharge cutting: Use electrical - discharge to cut the Bi 1.25 Sb 0.75 Se 1.75 Te 1.25 with a diameter of 20 mm after the first deformation into a sample with a diameter of 13 mm;
[0193] (7) Repeat hot - press deformation: Repeat steps (5) and (6) 2 times to carry out repeated hot - press deformation on the sample to obtain an n - type Bi 1.25 Sb 0.75 Se 1.75 Te 1.25 sample.
[0194] Example 18
[0195] (1) Ingredients: According to the atomic stoichiometric ratio of Bi 1.25 Sb 0.75 Se 1.5 Te 1.5 respectively weigh the metal single - element particles Bi, Sb, Se and Te with a purity higher than 99.999% and place them in a quartz tube. After fully shaking to make them evenly mixed, under the condition of a vacuum degree of 5.0×10 -4 Pa, use a hydrogen flame gun to seal the tube;
[0196] (2) Alloying sintering: Put the sealed quartz tube into a muffle furnace for alloying sintering. Heat it at a heating rate of 6 °C / min to 500 °C, keep it warm for 0.5 h, then heat it at a heating rate of 6 °C / min to 900 °C, keep it warm for 9 h, and then cool it with the furnace;
[0197] (3) Crushing: Crush and grind the obtained alloying sintering product with an agate mortar to obtain an alloying powder with a particle size of 1 - 100 μm;
[0198] (4) Hot - pressing sintering: Load the alloying powder into a graphite mold with a diameter of 13 mm, and carry out hot - pressing sintering for 0.5 h under the conditions of a sintering pressure of 50 MPa and a temperature of 450 °C, and cool it with the furnace to obtain an n - type alloy block;
[0199] (5) Hot - pressing deformation sintering: Load the n - type alloy block sample with a diameter of 13 mm into a graphite mold with a diameter of 20 mm, and carry out hot deformation for 0.5 h under the conditions of a sintering pressure of 50 MPa and a temperature of 450 °C;
[0200] (6) Electrical discharge machining: Use electrical discharge to cut the Bi 1.25 Sb 0.75 Se 1.5 Te 1.5 with a diameter of 20 mm after the first deformation into a sample with a diameter of 13 mm;
[0201] (7) Repeat hot - pressing deformation: Repeat steps (5) and (6) 2 times to carry out repeated hot - pressing deformation on the sample to obtain a 3 - time hot - deformed n - type Bi 1.25 Sb 0.75 Se 1.5 Te 1.5 sample.
[0202] Example 19
[0203] (1) Ingredients: According to Bi 1.25 Sb 0.75 Se 1.25 Te 1.75For the atomic stoichiometric ratio, metallic elemental particles of Bi, Sb, Se, and Te with a purity higher than 99.999% were respectively weighed and placed in a quartz tube. After fully shaking to mix them evenly, the tube was sealed under the condition of a vacuum degree of 5.0×10 -4 Pa using a hydrogen flame gun;
[0204] (2) Alloying sintering: The sealed quartz tube was placed in a muffle furnace for alloying sintering. It was heated to 500°C at a heating rate of 6°C / min, held for 0.5 h, then heated to 900°C at a heating rate of 6°C / min, held for 9 h, and then cooled with the furnace;
[0205] (3) Crushing: The obtained alloying sintering product was crushed and ground with an agate mortar to obtain an alloying powder with a particle size of 1 - 100 μm;
[0206] (4) Hot - pressing sintering: The alloying powder was loaded into a graphite mold with a diameter of 13 mm. Under the conditions of a sintering pressure of 50 MPa and a temperature of 450°C, hot - pressing sintering was carried out for 0.5 h, and then cooled with the furnace to obtain an n - type alloy block;
[0207] (5) Hot - pressing deformation sintering: The n - type alloy block sample with a diameter of 13 mm was loaded into a graphite mold with a diameter of 20 mm. Under the conditions of a sintering pressure of 50 MPa and a temperature of 450°C, hot deformation was carried out for 0.5 h;
[0208] (6) Electrical discharge machining: Using electrical discharge, the Bi 1.25 Sb 0.75 Se 1.25 Te 1.75 sample with a diameter of 20 mm after the first deformation was cut into a sample with a diameter of 13 mm;
[0209] (7) Repeating hot - pressing deformation: Steps (5) and (6) were repeated 2 times to perform repeated hot - pressing deformation on the sample, and a sample of n - type Bi 1.25 Sb 0.75 Se 1.25 Te 1.75 with 3 - time hot deformation was obtained.
[0210] Performance testing
[0211] In the following tests, HD0 represents the undeformed alloy block sample, HD1 represents the sample deformed once, HD2 represents the sample deformed twice, and HD3 represents the sample deformed three times
[0212] (1) XRD tests were carried out on the alloying powder, the undeformed alloy block sample (HD0), and the deformed samples (HD1, HD2, HD3) obtained in Example 13. The test results are as Figure 1 shown, where F is the preferred orientation factor.
[0213] It can be seen from Figure 1 that single-phase samples were obtained in each stage of Example 13. The F value of the samples gradually increased from 0.19 of the undeformed sample HD0 to 0.28 of the HD3 sample, indicating that the orientation texture of the samples was enhanced after hot deformation.
[0214] (2) SEM tests were carried out on the samples at different stages obtained in Example 13, and the test results are as Figure 2 shown, where (a), (c), (e) and (g) are the SEM fracture diagrams of the undeformed alloy block, the samples deformed 1, 2 and 3 times respectively, and (b), (d), (f) and (h) are the 3D reconstruction diagrams corresponding to the fractures of the undeformed alloy block, the samples deformed 1, 2 and 3 times respectively.
[0215] It can be seen from Figure 2 that in the examples of the present invention, with the increase of the number of hot deformations, plate-shaped grains with a layered structure and obvious stripes gradually appeared in the samples.
[0216] (3) Using an LSR-3 type comprehensive electrical property test system, Seebeck coefficient tests were carried out on the samples at different stages obtained in Example 13, and the measurement results are as Figure 3 shown.
[0217] It can be seen from Figure 3 that after hot deformation, within the entire test range, the Seebeck coefficient of the samples was significantly improved. At 323K, the Seebeck coefficient of the samples increased from -127.7 μV / K (HD0) to -153.6 μV / K (HD3), an increase of about 20%; the peak Seebeck coefficient increased from -150.2 μV / K (HD0) to -176.3 μV / K (HD1), an increase of about 17%.
[0218] (4) Using an LSR-3 type comprehensive electrical property test system, conductivity tests were carried out on the samples at different stages obtained in Example 13, and the results are shown in Figure 4 . It can be seen from Figure 4 that after hot deformation, the conductivity of the samples was significantly improved within the entire test range. At 323K, the conductivity increased from 2.93×10 4 S / m (HD0) to 4.30×10 4 S / m (HD3), an increase of about 47%.
[0219] (5) Using an LSR-3 type comprehensive electrical property test system, power factor tests were carried out on the samples at different stages obtained in Example 13, and the results are shown in Figure 5 .
[0220] It can be seen from Figure 5It can be seen that by using the method provided by the present invention, the Seebeck coefficient and electrical conductivity of the n-type thermoelectric material sample can be improved simultaneously, and the power factor of the thermally deformed sample is greatly improved in the entire test temperature range, thereby effectively improving its electrical performance.
[0221] (6) The thermal diffusion coefficient and specific heat capacity of the samples obtained at different stages in Example 13 were tested using NETZSCH LFA457 and DSC404F3, and the total thermal conductivity of the thermoelectric material was calculated. The results are shown in Figure 6 .
[0222] Depend on Figure 6 It can be seen that the total thermal conductivity of the thermally deformed sample is greatly reduced in the entire test temperature range. At 323K, the total thermal conductivity of the thermally deformed sample is about 0.82W / m K, which is about 15% lower than the HD0 (0.97W / mK) sample. At about 420K, the total thermal conductivity of the sample is reduced from 0.94W / m K (HD0) to 0.77W / m K (HD3), which is about 18% lower. Using the method provided by the present invention, the thermal conductivity of the n-type thermoelectric material sample can be significantly reduced, and its thermal performance can be effectively improved.
[0223] (7) According to the formula ZT = S 2 σT / κ total (where S, σ, κ total and T are Seebeck coefficient μV / K, electrical conductivity S / cm, thermal conductivity W / m K and absolute temperature K, respectively. 2 σ is also called power factor, mW / m K 2 ) The dimensionless thermoelectric merit of the samples at different stages of Example 13 was calculated and the results are shown in Figure 7 .
[0224] Depend on Figure 7 It can be seen that at 323K, the thermoelectric figure of merit of the HD3 sample is 0.40, which is 2.5 times that of the HD0 sample (0.16). At around 470K, the thermoelectric figure of merit of the HD3 sample is 0.60, which is 2.1 times that of the HD0 sample (0.29). Using the method provided by the present invention, the thermoelectric figure of merit of the sample can be greatly improved in the entire test temperature range, achieving an effective improvement in its thermoelectric performance.
[0225] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A preparation method of an n-type Bi-Sb-Se-Te thermoelectric material, characterized in that, Comprising the following steps: According to the chemical composition of the thermoelectric material being Bi y Sb 2-y Se 3-x Te x , 0.5 ≤ x ≤ 1.75, 0.5 ≤ y ≤ 1.75, mix elemental Bi, elemental Sb, elemental Se, and elemental Te, and perform alloying sintering under vacuum conditions to obtain an alloyed powder; Hot-press sintering the alloyed powder to obtain an n-type alloy block; Performing hot-press deformation on the n-type alloy block to obtain an n-type Bi-Sb-Se-Te thermoelectric material; The number of times of the hot-press deformation is 1 to 4 times, the temperature of each hot-press deformation is independently 400 to 450 °C, the deformation direction is perpendicular to the pressure direction, and the diameter of the die used for the hot-press deformation is 15 to 25 mm.
2. The preparation method according to claim 1, wherein x is 0.75 to 1.5, and y is 0.75 to 1.
5.
3. The preparation method according to claim 2, wherein x is 1 to 1.25, and y is 1 to 1.
25.
4. The preparation method according to claim 1, characterized in that, The degree of vacuum of the vacuum condition < 1.0×10 - 3 Pa; the alloying sintering includes first alloying sintering and second alloying sintering carried out in sequence.
5. The preparation method according to claim 4, characterized in that, The temperature of the first alloying sintering is 300 to 500 °C, and the heat preservation time is 0.5 to 1 h; the temperature of the second alloying sintering is 700 to 900 °C, and the heat preservation time is 6 to 10 h; the heating rate for rising to the temperatures of the first alloying sintering and the second alloying sintering is independently 5 to 8 °C / min; the particle size of the alloyed powder is 1 to 100 μm.
6. The preparation method according to claim 1, wherein The diameter of the graphite die used for the hot-press sintering is 10 to 15 mm.
7. The preparation method according to claim 1 or 6, wherein The temperature of the hot-press sintering is 400 to 450 °C, the heat preservation time is 0.5 to 1 h, and the pressure is 30 to 50 MPa.
8. The preparation method according to claim 1, characterized in that, The pressure of each hot-press deformation is independently 50 to 100 MPa, and the heat preservation time is independently 0.5 to 1 h.
9. An n-type Bi-Sb-Se-Te thermoelectric material prepared by the preparation method according to any one of claims 1 to 8.
10. Application of the n-type Bi-Sb-Se-Te thermoelectric material according to claim 9 in a thermoelectric device.
Citation Information
Cited By
High-performance n-type room temperature doped thermoelectric material and preparation method thereof
CN121085224A