High-hardness wear-resistant composite material as well as preparation method and application thereof

By introducing specific elements and additives into the self-healing material for metal wear, a protective film and a dense layer are formed, which solves the problems of material dispersion and stability in lubricating oil, and improves wear resistance and self-healing performance under high temperature and high load conditions, thus meeting the needs of practical applications.

CN120399775AActive Publication Date: 2025-08-01ZHONGKE BAOLU NEW MATERIALS (LIAONING) CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202510448637.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-04-10
Publication Date
2025-08-01
Estimated Expiration
2045-04-10

AI Technical Summary

Technical Problem

Existing self-healing materials for metal wear have poor dispersibility in lubricating oil, are prone to sedimentation or agglomeration, have unstable long-term performance, and have unstable friction coefficients under high temperature and high load conditions, resulting in poor self-healing performance and failing to meet the needs of practical applications.

Method used

Iron-based alloys of Mn, Mo, Co, Cr, Fe and Ni are introduced, and benzotriazole-6-sulfonic acid and 7-methyl-(1,2,4)triazolo(1,5-a)pyridine-2(3H)-imine are added to form a protective film, which enhances adhesion and wear resistance. The addition of amino urea polymer improves dispersibility and forms a dense protective layer, maintaining the stability of the material under high temperature and high load.

Benefits of technology

It significantly improves the wear resistance of materials, reduces the coefficient of friction, extends the service life of equipment, reduces energy consumption, improves self-healing ability, and ensures long-term reliability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a high-hardness wear-resistant composite material as well as a preparation method and application thereof. The high-hardness wear-resistant composite material comprises an iron-based alloy, a polymer containing amino urea and an additive, the additive comprises 7-methyl-(1, 2, 4) triazolo (1, 5-a) pyridine-2 (3H)-imine and benzotriazole-6-sulfonic acid; the iron-based alloy is composed of Mn, Mo, Co, Cr, Fe and Ni. The iron-based alloy, the polymer containing the amino urea and the composite additive are introduced to achieve a synergistic effect, functional groups of the iron-based alloy, the polymer containing the amino urea and the composite additive are coordinated with the metal surface to form a protective film, dispersity, adhesive force and abrasion resistance are enhanced, a corrosive medium is isolated, the self-repairing capacity is improved, the stability under the high-temperature and high-load conditions is maintained, and the actual application requirement is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of self - healing materials, and more specifically, to a high - hardness anti - wear composite material, its preparation method and application. Background Art

[0002] Wear is one of the main modes of material failure, accounting for about 80% of equipment damage and failure. According to the investigation and analysis in the United States, the United Kingdom, Japan, and Germany in the past 20 years, the economic losses caused by wear failure are huge, accounting for about 2% of the gross national economic output value of each country. At present, to solve the problem of wear failure, anti - wear technology, friction - reduction technology, and repair technology are mainly adopted, but most of these technologies are independent, and their effectiveness, reliability, and versatility are limited.

[0003] The metal wear self - repair technology (ART) is a new surface engineering technology and product that integrates anti - wear, friction - reduction, and dynamic self - repair functions. The core of this technology is to utilize the force - chemical reaction conditions on the metal friction surface to transfer micro - nano powder materials with special components to the metal surface and form a metal - like ceramic protective layer. This protective layer can significantly improve the hardness and smoothness of the friction surface, reduce the friction coefficient, and restore the worn part to its original size.

[0004] Although the metal wear self - repair technology has achieved remarkable application effects in the industrial field, it still faces some technical problems in practical applications. Existing metal wear self - repair materials usually consist of multiple mineral components and various additives. The dispersibility of these materials in lubricating oil is poor, and they are prone to precipitation or agglomeration. This not only affects the uniform distribution of the materials but also may lead to increased local wear. Secondly, over time, the self - repair materials will exhibit unstable phenomena, affecting long - term performance and reliability, ultimately resulting in poor self - repair performance, low repair efficiency, and inability to meet the actual application requirements. Secondly, under high - temperature and high - load conditions, the friction coefficient of the materials is unstable, it is difficult to resist high - load wear, and it is unable to effectively reduce the friction coefficient, resulting in increased energy consumption and wear. Summary of the Invention

[0005] The object of the present invention is to overcome the above - mentioned defects existing in the prior art, and provide a high - hardness anti - wear composite material, its preparation method and application. By introducing Mn, Mo, Co, Cr, Fe, and Ni to enhance the iron - based alloy to improve wear resistance, adding benzotriazole - 6 - sulfonic acid and 7 - methyl - (1,2,4) triazolo (1,5 - a) pyridin - 2(3H) - imine to act synergistically, using their functional groups to coordinate with the metal surface to form a protective film, enhancing adhesion and wear resistance, and isolating corrosive media. The imine group modifies the alloy particles, improves the dispersibility, and enhances the self - repair ability. The amino - urea - containing polymer forms an uneven surface, maintains stability under high - temperature and high - load conditions, ensures the reliability of long - term use, improves the repair efficiency, and meets the actual application requirements.

[0006] To achieve the above object, the technical solution of the present invention is as follows:

[0007] A high-hardness anti-wear composite material, the high-hardness anti-wear composite material comprising an iron-based alloy, a polymer containing semicarbazide, and an additive; the additive comprising 7-methyl-(1,2,4)-triazolo(1,5-a)pyridin-2(3H)-imine and benzotriazole-6-sulfonic acid in a mass ratio of 1:(0.1-0.5); the iron-based alloy is composed of Mn, Mo, Co, Cr, Fe, and Ni, wherein the atomic percentage of Fe is 20%-40%, the atomic percentage of Mn is 5%-10%, the atomic percentage of Mo is 15%-30%, the atomic percentage of Co is 5%-20%, the atomic percentage of Cr is 5%-15%, and the atomic percentage of Ni is 5%-10%; by mass parts, the mass parts of the iron-based alloy is 100 parts, the mass parts of the polymer containing semicarbazide is 1 part to 3 parts, and the mass parts of the additive is 10 parts to 25 parts.

[0008] Optionally, the polymer containing semicarbazide is alkyl dimethyl ammonium chloride.

[0009] Optionally, the Mn, Mo, Co, Cr, Fe, and Ni are pure metal powders with a purity of ≥99.5%.

[0010] Optionally, the average particle size of the iron-based alloy is <1 μm.

[0011] The present invention also discloses a preparation method of a high-hardness anti-wear composite material as described above, comprising the following steps:

[0012] (1) Formulating raw materials of Mn, Mo, Co, Cr, Fe, and Ni according to the atomic percentage to obtain a metal raw material;

[0013] (2) Coarsely grinding and finely grinding the metal raw material in sequence to obtain the iron-based alloy with an average particle size less than 1 μm;

[0014] (3) Adding the iron-based alloy and the polymer containing semicarbazide into an aqueous solution containing an additive for homogeneous dispersion, and then obtaining a solid by centrifugal separation and drying to prepare the high-hardness anti-wear composite material.

[0015] Optionally, in step (2), the time for coarse grinding is 5 h to 8 h; the time for fine grinding is 10 h to 15 h.

[0016] Optionally, in step (2), the liquid medium for fine grinding is alcohol.

[0017] The present invention also discloses an application of the high-hardness anti-wear composite material as described above in lubricating oil, and the lubricating oil includes base lubricating oil and the high-hardness anti-wear composite material.

[0018] Optionally, the volume ratio of the high-hardness anti-wear composite material to the base lubricating oil is (0.1 - 0.5):100.

[0019] Implementing the embodiments of the present invention will have the following beneficial effects:

[0020] The present invention first introduces Mn, Mo, Co, Cr, Fe, and Ni. Through the synergistic action of different mechanisms, it can significantly improve the wear resistance of the material. Further, by adding a composite synergistic dispersant to the iron-based alloy, multiple nitrogen atoms on the triazole ring in benzotriazole-6-sulfonic acid can coordinate with the metal surface to form stable chemical bonds. By introducing a sulfonic acid group on the triazole ring, the adhesion between the material and the metal surface can be further enhanced. The triazole functional group and pyridine functional group in 7-methyl-(1,2,4)triazolo(1,5-a)pyridin-2(3H)-imine can chemically adsorb with the active sites on the metal surface to form stable coordination bonds, thereby adsorbing on the metal surface and forming a dense protective film to ensure the wear resistance and stability of the material, effectively isolating external corrosive media, and reducing the oxidation and corrosion of the metal. At the same time, the imine group modifies the alloy particles, improving the characteristic that the self-repairing material is difficult to disperse and suspend in the lubricating oil, and further enhancing the ability of friction damage self-repair. The polymer containing semicarbazide amine can form a dense uneven surface on the metal surface and maintain the stability of the material at the same time.

[0021] The various raw materials of the present invention cooperate with each other and play a synergistic role. When the lubricating oil using the high-hardness anti-wear composite material of the present invention is used in the friction of mechanical equipment, a metal ceramic protective layer with excellent anti-friction performance is generated on the metal friction surface, improving the hardness and smoothness of the friction surface, significantly reducing the friction coefficient, and restoring the worn parts to their original dimensions, completing the self-repair of the metal worn parts, greatly extending the service life of the equipment, and saving energy consumption. Therefore, it can not only reduce the friction coefficient of the surface of the machine parts themselves, reduce friction and wear caused by friction, but also reduce the wear of the machine parts surface by abrasive particles generated by wear, and can reduce the working temperature of the lubricating oil. Detailed Embodiment

[0022] The following further illustrates the present invention with specific embodiments, but does not limit the present invention in any way.

[0023] Example 1

[0024] The high-hardness anti-wear composite material of this embodiment includes an iron-based alloy (average particle size < 1 μm), alkyl dimethyl ammonium chloride, and an additive; the additive includes 7-methyl-(1,2,4)-triazolo(1,5-a)pyridin-2(3H)-imine and benzotriazole-6-sulfonic acid with a mass ratio of 1:0.25; the iron-based alloy is composed of Mn, Mo, Co, Cr, Fe, and Ni, where the atomic percentage of Fe is 30%, the atomic percentage of Mn is 10%, the atomic percentage of Mo is 15%, the atomic percentage of Co is 20%, the atomic percentage of Cr is 15%, and the atomic percentage of Ni is 10%;

[0025] By mass, the mass fraction of the iron-based alloy is 100 parts, the mass fraction of the polymer containing semicarbazide is 3 parts, and the mass fraction of the additive is 24 parts.

[0026] The preparation method of the high-hardness anti-wear composite material of this embodiment includes the following steps:

[0027] (1) Prepare the metal raw materials by formulating the raw materials of Mn, Mo, Co, Cr, Fe, and Ni according to the atomic percentage;

[0028] (2) Coarsely grind the metal raw materials for 8 hours and then finely grind for 10 hours to obtain an iron-based alloy with an average particle size less than 1 μm;

[0029] (3) Add the iron-based alloy and the polymer containing semicarbazide into an aqueous solution containing the additive for homogeneous dispersion, and then obtain a solid by centrifugal separation and dry it to prepare the high-hardness anti-wear composite material.

[0030] Example 2

[0031] The high-hardness anti-wear composite material of this embodiment includes an iron-based alloy (average particle size < 1 μm), alkyl dimethyl ammonium chloride, and an additive; the additive includes 7-methyl-(1,2,4)-triazolo(1,5-a)pyridin-2(3H)-imine and benzotriazole-6-sulfonic acid with a mass ratio of 1:0.1; the iron-based alloy is composed of Mn, Mo, Co, Cr, Fe, and Ni, where the atomic percentage of Fe is 40%, the atomic percentage of Mn is 5%, the atomic percentage of Mo is 25%, the atomic percentage of Co is 10%, the atomic percentage of Cr is 15%, and the atomic percentage of Ni is 5%;

[0032] By mass, the mass fraction of the iron-based alloy is 100 parts, the mass fraction of the polymer containing semicarbazide is 1 part, and the mass fraction of the additive is 15 parts.

[0033] The preparation method of the high-hardness anti-wear composite material of this embodiment includes the following steps:

[0034] (1) Prepare metal raw materials by formulating Mn, Mo, Co, Cr, Fe, and Ni raw materials according to atomic percentages;

[0035] (2) Coarsely grind the metal raw materials for 7 h and then finely grind them for 15 h to obtain an iron-based alloy with an average particle size of less than 1 μm;

[0036] (3) Add the iron-based alloy and the polymer containing semicarbazide to an aqueous solution containing additives for homogeneous dispersion, and then obtain a solid by centrifugal separation and dry it to prepare a high-hardness anti-wear composite material.

[0037] Example 3

[0038] The high-hardness anti-wear composite material of this example includes an iron-based alloy (average particle size < 1 μm), alkyl dimethyl ammonium chloride, and additives; the additives include 7-methyl-(1,2,4)-triazolo(1,5-a)pyridin-2(3H)-imine and benzotriazole-6-sulfonic acid with a mass ratio of 1:0.5; the iron-based alloy is composed of Mn, Mo, Co, Cr, Fe, and Ni, where the atomic percentage of Fe is 20%, the atomic percentage of Mn is 10%, the atomic percentage of Mo is 30%, the atomic percentage of Co is 15%, the atomic percentage of Cr is 15%, and the atomic percentage of Ni is 10%;

[0039] By mass, the mass fraction of the iron-based alloy is 100 parts, the mass fraction of the polymer containing semicarbazide is 3 parts, and the mass fraction of the additives is 15 parts.

[0040] The preparation method of the high-hardness anti-wear composite material of this example includes the following steps:

[0041] (1) Prepare metal raw materials by formulating Mn, Mo, Co, Cr, Fe, and Ni raw materials according to atomic percentages;

[0042] (2) Coarsely grind the metal raw materials for 8 h and then finely grind them for 10 h to obtain an iron-based alloy with an average particle size of less than 1 μm;

[0043] (3) Add the iron-based alloy and the polymer containing semicarbazide to an aqueous solution containing additives for homogeneous dispersion, and then obtain a solid by centrifugal separation and dry it to prepare a high-hardness anti-wear composite material.

[0044] Example 4

[0045] The difference between this example and Example 1 is only that: the mass ratio of 7-methyl-(1,2,4)-triazolo(1,5-a)pyridin-2(3H)-imine and benzotriazole-6-sulfonic acid is 1:0.1.

[0046] Example 5

[0047] The only difference between this embodiment and embodiment 1 is that the mass ratio of 7-methyl-(1,2,4)triazolo(1,5-a)pyridine-2(3H)-imine and benzotriazole-6-sulfonic acid is 1:0.5.

[0048] Example 6

[0049] The only difference between this embodiment and embodiment 1 is that, in parts by mass, the iron-based alloy is 100 parts by mass, the polymer containing aminourea is 1 part by mass, and the additive is 25 parts by mass.

[0050] Example 7

[0051] The only difference between this embodiment and embodiment 1 is that, in parts by mass, the iron-based alloy is 100 parts by mass, the polymer containing aminourea is 3 parts by mass, and the additive is 10 parts by mass.

[0052] Comparative Example 1

[0053] The only difference between this comparative example and Example 1 is that no polymer containing aminourea is added in this comparative example.

[0054] Comparative Example 2

[0055] The only difference between this comparative example and Example 1 is that 7-methyl-(1,2,4)triazolo(1,5-a)pyridine-2(3H)-imine is not added in this comparative example.

[0056] Comparative Example 3

[0057] The only difference between this comparative example and Example 1 is that no benzotriazole-6-sulfonic acid is added in this comparative example.

[0058] Comparative Example 4

[0059] The only difference between this comparative example and Example 1 is that the mass ratio of 7-methyl-(1,2,4)triazolo(1,5-a)pyridine-2(3H)-imine and benzotriazole-6-sulfonic acid is 1:2.

[0060] Comparative Example 5

[0061] The only difference between this comparative example and Example 1 is that the mass ratio of 7-methyl-(1,2,4)triazolo(1,5-a)pyridine-2(3H)-imine and benzotriazole-6-sulfonic acid is 10:0.1.

[0062] Comparative Example 6

[0063] The only difference between this comparative example and Example 1 is that, in parts by mass, the iron-based alloy is 100 parts by mass, the polymer containing aminourea is 5 parts by mass, and the additive is 5 parts by mass.

[0064] Comparative Example 7

[0065] The only difference between this comparative example and Example 1 is that, in parts by mass, the iron-based alloy is 100 parts by mass, the polymer containing aminourea is 5 parts by mass, and the additive is 30 parts by mass.

[0066] Application Example 1

[0067] A lubricating oil, comprising the composite material provided in Examples 1-7 and Comparative Examples 1-7 and a base oil (Class II base oil, model XHH-150N); a method for preparing the lubricating oil comprising: mixing the composite material provided in Examples 1-7 and Comparative Examples 1-7 and the base oil, and performing stirring premixing, shear infiltration, ultrasonic dispersion, and homogenization treatment, to obtain the lubricating oil. The volume ratio of the high-hardness anti-wear composite material to the base lubricating oil is 0.5:100, the stirring rate in the stirring premixing is 5000 r / min, and the stirring time is 10 min; strong mechanical dispersion is performed in a shear disperser, the shear speed is 4000 rpm, the shear time is 40 min, and the cycle temperature is controlled at 10-35°C; the ultrasonic dispersion power is 800 W, the frequency is 20 kHz, the ultrasonic temperature is controlled at no more than 35°C, and the ultrasonic time is 40 min; the homogenization pressure is 1000 bar, the homogenization temperature is 10-35°C, and the homogenization is performed 150 times.

[0068] Comparative Application Example 1

[0069] A lubricating base oil (category II base oil, model XHH-150N) is provided without adding any composite materials.

[0070] Performance Testing

[0071] 1. An SRV micro-friction tester was used to measure the changes in the anti-friction and anti-wear properties of the lubricating base oil provided in Application Example 1 compared to that in Comparative Application Example 1. The test conditions were: load 200 N, frequency 50 Hz, temperature 50°C, and stroke 1 mm. The friction coefficient and wear spot diameter were recorded. The percentage decrease in the friction coefficient and wear spot diameter of Application Example 1, which contains the lubricating oil with the composite material, compared to the lubricating base oil was calculated. The smaller the friction coefficient and wear spot diameter, the better the anti-friction and anti-friction properties.

[0072] Friction coefficient reduction percentage = (lubricating base oil friction coefficient - lubricating oil friction coefficient) / lubricating base oil friction coefficient * 100%;

[0073] Wear spot diameter reduction percentage = (lubricating base oil wear spot diameter - lubricating oil wear spot diameter) / lubricating base oil wear spot diameter * 100%.

[0074] 2. The low-temperature corrosion performance and high-temperature corrosion performance including those of Application Example 1 were determined using GB / T 5096. Low-temperature corrosion: Detection was carried out according to GB / T 5096. The test temperature was set at 50 °C and detection was carried out after 3 h. High-temperature corrosion: Detection was carried out according to GB / T 5096. The starting temperature was 120 °C and the test temperature was increased at a rate of 1 °C / min. Detection was carried out after 3 h.

[0075] 3. The change in the self-healing performance including that of Application Example 1 was determined using an MRH-3 high-speed ring-block wear testing machine. The test conditions were as follows: On the MRH-3 high-speed ring-block wear testing machine, under the conditions of a load of 200 N, a rotational speed of 100 r / min, and a time of 20 s, a wear scar of 12 mm × 0.6 mm was dry-ground on the surface of the test block. Using the MRH-3 high-speed ring-block wear testing machine under 200 N, the self-healing effect of the above Application Example 1 was investigated. The speed was 0.257 m / s and the time was 4 h. Self-healing performance evaluation: The self-healing effect was investigated by comparing the wear amounts before and after repair.

[0076] Table 1 Performance test results

[0077] Coefficient of friction Wear scar diameter (mm) Low-temperature corrosion resistance High-temperature corrosion resistance Example 1 0.108 0.208 2b 1b Example 2 0.114 0.223 2b 1b Example 3 0.129 0.215 2b 1b Example 4 0.133 0.237 2b 1b Example 5 0.141 0.241 2b 1b Example 6 0.127 0.219 2b 1b Example 7 0.147 0.246 2b 1b Comparative Example 1 0.249 0.349 3a 3b Comparative Example 2 0.245 0.341 3a 3a Comparative Example 3 0.244 0.336 3a 3b Comparative Example 4 0.236 0.324 3a 3b Comparative Example 5 0.242 0.318 3a 3b Comparative Example 6 0.211 0.313 3a 3b Comparative Example 7 0.203 0.302 3a 3b Comparative Application Example 1 0.218 0.45 / /

[0078] Table 2 Self-healing performance test results

[0079] 200N Example 1 0.48 mg Example 2 0.41 mg Example 3 0.47 mg Example 4 0.27 mg Example 5 0.22 mg Example 6 0.23 mg Example 7 0.30 mg Comparative Example 1 0.023 mg Comparative Example 2 0.029 mg Comparative Example 3 0.041 mg Comparative Example 4 0.037 mg Comparative Example 5 0.046 mg Comparative Example 6 0.052 mg Comparative Example 7 0.049 mg

[0080] As can be seen from Tables 1-3, compared with Comparative Examples 1-7, the materials provided by Examples 1-7 of the present invention have a significantly reduced friction coefficient, a significantly reduced wear scar diameter, an improved level of both low-temperature corrosion performance and high-temperature corrosion performance test results, and good self-healing properties. Therefore, the addition of the composite material can improve the anti-wear and friction-reducing performance, corrosion resistance, and self-healing performance to varying degrees. In addition, the addition ratio between the components has a significant impact on the friction-reducing and anti-wear as well as self-healing performance.

[0081] The above-described embodiments merely represent several implementation manners of the present invention. The description is relatively specific and detailed, but it should not be construed as a limitation to the scope of the patent application. It should be noted that for those of ordinary skill in the art, without departing from the concept of the present invention, several modifications and improvements can still be made, and these all fall within the protection scope of the present invention. Therefore, the protection scope of the present invention patent shall be subject to the appended claims.

Claims

1. A high-hardness anti-wear composite material, characterized in that, The high-hardness anti-wear composite material comprises an iron-based alloy, a polymer containing semicarbazide, and an additive; The additive comprises 7-methyl-(1,2,4)-triazolo(1,5-a)pyridin-2(3H)-imine and benzotriazole-6-sulfonic acid with a mass ratio of 1:(0.1-0.5); The iron-based alloy is composed of Mn, Mo, Co, Cr, Fe, and Ni, wherein the atomic percentage of Fe is 20%-40%, the atomic percentage of Mn is 5%-10%, the atomic percentage of Mo is 15%-30%, the atomic percentage of Co is 5%-20%, the atomic percentage of Cr is 5%-15%, and the atomic percentage of Ni is 5%-10%; By mass, the mass of the iron-based alloy is 100 parts, the mass of the polymer containing semicarbazide is 1-3 parts, and the mass of the additive is 10-25 parts.

2. The high-hardness anti-wear composite material according to claim 1, characterized in that The polymer containing semicarbazide is alkyl dimethyl ammonium chloride.

3. The high-hardness anti-wear composite material according to claim 1, wherein The Mn, Mo, Co, Cr, Fe, and Ni are pure metal powders with a purity ≥99.5%.

4. The high-hardness anti-wear composite material according to claim 1, wherein The average particle size of the iron-based alloy is <1 μm.

5. A method for preparing a high-hardness anti-wear composite material according to any one of claims 1-4, characterized in that, It includes the following steps: (1) Prepare metal raw materials by formulating Mn, Mo, Co, Cr, Fe, and Ni raw materials according to the atomic percentage; (2) Coarsely grind and then finely grind the metal raw materials to obtain the iron-based alloy with an average particle size less than 1 μm; (3) Add the iron-based alloy and the polymer containing semicarbazide into an aqueous solution containing the additive for homogeneous dispersion, then obtain a solid by centrifugal separation and dry it to prepare the high-hardness anti-wear composite material.

6. The preparation method according to claim 5, characterized in that, In step (2), the time for coarse grinding is 5 h - 8 h; The time for fine grinding is 10 h - 15 h.

7. The preparation method according to claim 5, characterized in that, In step (2), the liquid medium for fine grinding is alcohol.

8. Use of a high-hardness anti-wear composite material according to any one of claims 1-7 in a lubricating oil, characterized in that, The lubricating oil comprises a base lubricating oil and the high-hardness anti-wear composite material.

9. The application according to claim 8, characterized in that, The volume ratio of the high-hardness anti-wear composite material to the base lubricating oil is (0.1 - 0.5):100.

Citation Information

Patent Citations

  • Composite lithium-base grease and method for making same

    CN101200670A

  • Lubricant additive with ultra-lubrication antifriction function

    CN101402895A

  • Preparation method of lubricating oil composition containing ionic liquid, modified nano-zinc powder and graphene

    CN104830404A

  • Preparation method of anti-oxidation and abrasion-resistant self-repairing lubricating oil

    CN106281603A

  • Preparation method of nano lubricating oil for internal combustion engine

    CN108531276A