Method for preparing carbon nano tube by rapidly decomposing waste high-molecular polymer

The Joule thermal method and metal catalysts work together to quickly raise and lower the temperature to prepare carbon nanotubes, which solves the problems of long reaction time and high energy consumption in traditional methods, and achieves efficient and low-cost carbon nanotube production, improving the purity and diameter uniformity of the product.

CN120440884APending Publication Date: 2025-08-08PEKING UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202510627272.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-15
Publication Date
2025-08-08

AI Technical Summary

Technical Problem

The preparation method of carbon nanotubes in the prior art has problems such as long reaction time, high energy consumption, and uneven product quality. Especially when solid polymers are used as carbon sources, the mass transfer efficiency is low and the catalyst is prone to agglomeration, resulting in high production costs and low yields.

Method used

The Joule thermal method is used to synergize with the metal catalyst through instantaneous high temperature, and mix waste polymer with conductive carbon materials. The power is turned on to produce a Joule thermal effect, which quickly heats up to 600-2500℃, and the reaction time is shortened to second level, inhibiting catalyst agglomeration, promoting the selective decomposition of carbon sources into C1-C3 small molecules, and generating high-purity and high-graphitization carbon nanotubes.

Benefits of technology

It realizes efficient and low-cost preparation of carbon nanotubes, with a yield of more than 80%, and a uniform diameter distribution, which is suitable for industrial-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120440884A_ABST
    Figure CN120440884A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a carbon nano tube by rapidly decomposing a waste high-molecular polymer, and belongs to the technical field of nano material preparation. The method comprises the following steps: mixing a waste high-molecular polymer (such as polyethylene, rubber and the like) serving as a carbon source with a metal-based catalyst and a conductive carbon material, sealing the mixture in a reaction container, connecting an external power supply, instantaneously heating to 600-2500 DEG C under the action of current through the Joule heating effect of the conductive carbon material, and reacting for 5-60 seconds to realize the efficient growth of the carbon nanotube. According to the method, the agglomeration of the catalyst is inhibited through the rapid heating and cooling characteristics of Joule heat, the carbon source is promoted to be selectively decomposed into C1-C3 small molecules, and the graphitization degree and diameter uniformity of the carbon nanotubes are remarkably improved. Compared with the traditional method, the method has the advantages of short reaction time (second level), low energy consumption, high product purity, capability of macroscopic preparation and the like, and is suitable for industrial large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of nanomaterial preparation, and specifically relates to a method for preparing carbon nanotubes by rapidly decomposing waste high-molecular polymers using Joule heat method, which is suitable for large-scale production of high-performance carbon nanotubes. Background Art

[0002] Since their discovery in 1991, carbon nanotubes (CNTs) have become a research hotspot in materials science due to their unique tubular structure, exceptional mechanical properties (such as ultrahigh strength and high elastic modulus), and superior electrical and thermal conductivity. They hold enormous potential for applications in composite materials, energy storage (such as supercapacitors and lithium-ion batteries), electronic devices (such as field-effect transistors and sensors), and biomedicine. However, the practical application of CNTs has long been limited by the lack of efficient, controllable, and economical preparation methods.

[0003] Traditional carbon nanotube production technologies primarily include chemical vapor deposition (CVD), arc discharge, and laser ablation. CVD is the most widely used method due to its mature equipment and scalable production. CVD uses a gaseous carbon source (such as methane, ethylene, etc.) as raw material and produces carbon nanotubes through a cracking reaction at high temperatures (usually above 500°C). This method has a long reaction cycle, typically taking several hours, resulting in high energy consumption. Furthermore, its low growth efficiency further increases the production cost of carbon nanotubes.

[0004] In recent years, research on the preparation of carbon nanotubes using solid polymers (such as polyethylene and polypropylene) as carbon sources has gradually gained momentum. The low cost and high carbon content (e.g., low-density polyethylene has a carbon content of >85%) of these waste materials make them ideal solid carbon sources. However, existing electric furnace pyrolysis technology faces the following bottlenecks: the pyrolysis of polymers easily generates tar and large molecular fragments, resulting in complex products; the high temperature environment causes metal catalyst particles to agglomerate, reducing catalytic activity; the inefficient mass transfer of solid carbon sources leads to reaction times of several hours and low yields; and the carbon nanotubes in the product have a low degree of graphitization and a wide diameter distribution. These issues seriously restrict practical production applications.

[0005] Therefore, developing a method that is simple to operate, low in cost, low in energy consumption, high in product quality, and has the potential to achieve large-scale preparation is of great significance for the production and application of carbon nanotubes. Summary of the Invention

[0006] The purpose of this invention is to provide a rapid, efficient, and environmentally friendly method for producing carbon nanotubes from waste polymers, addressing the high energy consumption and uneven product quality of conventional electric furnace polymer pyrolysis processes. By leveraging the ultrafast heating and cooling characteristics of Joule heating and the catalytic action of a metal catalyst, this method achieves high-value-added conversion of waste polymers and significantly improves the yield, purity, and structural uniformity of carbon nanotubes.

[0007] The technical solutions of the present invention are as follows:

[0008] A method for rapidly decomposing waste high molecular polymers to prepare carbon nanotubes comprises the following steps:

[0009] 1) mixing waste polymer powder with a catalyst to prepare a reaction precursor, wherein the catalyst is a metal-based catalyst containing iron, cobalt, nickel and / or molybdenum;

[0010] 2) Compounding the reaction precursor with the conductive carbon material and sealing it in a reaction container, with both ends connected to the positive and negative electrodes of a power supply;

[0011] 3) A current of 20 to 100 A is passed through the reaction system, and the Joule heating effect of the conductive carbon material is used to heat the reaction system to 600 to 2500° C. at a rate of >1000° C. / s, and the reaction is carried out for 5 to 60 seconds to generate carbon nanotubes.

[0012] In the above step 1), a reaction precursor is provided: waste polymer is used as the main carbon source, preferably a powder with a particle size of less than 1 mm to improve the reaction efficiency; a metal catalyst is used, and the activity and stability of the metal catalyst can be further improved by loading the metal catalyst on an oxide or hydrotalcite carrier.

[0013] The choice of reaction precursors is widely applicable. Waste polymers can be selected from one or more combinations of polyethylene (PE), polypropylene (PP), polyvinyl chloride (PVC), polystyrene (PS), and rubber waste. Catalysts can be selected from one or more of iron powder, nickel powder, cobalt powder, molybdate, and iron, cobalt, and nickel nitrates, sulfates, chlorides, and acetates. Depending on the catalyst's state, the polymer and catalyst can be mixed using either wet deposition or dry mixing. The catalyst can be directly mixed with the polymer powder or wet-deposited onto an oxide or hydrotalcite support before mixing with the polymer powder. The oxide support can be a single compound or a mixture of magnesium oxide, silicon oxide, or aluminum oxide. For metal powder catalysts or oxide or hydrotalcite-supported metal composite catalysts, the catalyst is directly mixed with the polymer powder and then thoroughly ground. For metal salt catalysts, the catalyst is dissolved in water, thoroughly ultrasonically stirred with the polymer powder, and then dried. Preferably, the catalyst in the reaction precursor accounts for 0.5%-20% of the total mass of the reaction precursor.

[0014] The above step 2) constructs a conductive network: the reaction precursor is compounded with a conductive carbon material to construct a conductive network to ensure that the reaction precursor uniformly generates Joule heat under the action of electric current. The conductive carbon material can be selected from carbon black, carbon nanotubes, graphite powder, carbon paper, carbon cloth, graphite paper, carbon fiber film, etc. Depending on the form of the carbon material, the compounding of the reaction precursor and the carbon material can be carried out in two ways: wrapping and mixing. For film-like materials such as carbon paper, carbon cloth, graphite paper, and carbon fiber film, the reaction precursor can be wrapped with a carbon material film, sealed in a quartz tube reactor, and connected to graphite electrodes at both ends. For powder materials such as carbon black, carbon nanotubes, and graphite powder, the carbon material is directly mixed with the reaction precursor and then fully ground, pressed into a certain shape or granulated and loaded into a quartz tube reactor, and connected to graphite electrodes at both ends. For powdered conductive carbon materials, the amount added is 5% to 50% of the mass of the reaction precursor.

[0015] In step 3) Joule heating, the raw materials are energized by a DC power supply to achieve Joule heating, which instantly decomposes the polymer into C1-C3 small molecular carbon sources, and grows carbon nanotubes under the action of a metal catalyst. Heat generation follows the Joule heat law: Q = I 2 Rt, where Q represents heat, I represents current, R represents resistance, and t represents time. Joule heating parameters include a current range of 40 to 120 A (preferably 60 to 100 A), a heating rate greater than 1000°C / s, an instantaneous temperature of 600 to 2500°C, and a reaction time of 5 to 60 seconds (preferably 10 to 30 seconds).

[0016] In the above step 3), the heating method is to apply a constant current to the reactants through an external power supply, so that the conductive carbon material generates Joule heat to heat the reaction precursor, and the reaction temperature is monitored in real time by an infrared temperature detector.

[0017] In the above step 3), the reaction is carried out in an oxygen-free or oxygen-deficient environment (oxygen content <3 vol%), using an inert gas such as argon, nitrogen, or an argon-hydrogen mixture as protection, and the atmosphere pressure P ranges from 0 < P < 101 kPa.

[0018] The carbon nanotubes prepared by the method of the present invention are multi-walled carbon nanotubes or single-walled carbon nanotubes with a diameter ranging from 1 to 50 nm. In some embodiments of the present invention, the diameter of the prepared multi-walled carbon nanotubes is 2 to 14 nm, and the diameter of the single-walled carbon nanotubes is 1.2 to 2.4 nm.

[0019] Beneficial effects of the present invention:

[0020] 1. This invention overcomes the long reaction time and high energy consumption of traditional electric furnace processes, shortening reaction time to seconds and reducing energy consumption by over 80%. A single unit can achieve a carbon nanotube yield of 0.8 to 1.2 g / min, offering significant advantages for industrial applications.

[0021] 2. The equipment of the present invention is simple (only a DC power supply and a reaction chamber are required), and continuous production can be easily realized. The raw material purity requirement is low, the source is wide, and the price is low, which can significantly reduce the production cost of carbon nanotubes.

[0022] 3. This invention utilizes the rapid heating and cooling properties of Joule heat to inhibit catalyst agglomeration, promote the selective decomposition of the carbon source into small C1-C3 molecules, and significantly improve the degree of graphitization and diameter uniformity of carbon nanotubes. This carbon nanotube preparation, based on a Joule heat non-equilibrium reaction process, features high purity, a high degree of graphitization, and uniform diameter distribution. Multi-walled carbon nanotubes have diameters of 2 to 14 nm, while single-walled carbon nanotubes have diameters of 1.2 to 2.4 nm.

[0023] The core innovation of this invention lies in the synergistic system of Joule heat and catalyst: through the synergistic effect of instantaneous high temperature and metal catalyst, the limitations of low carbon source decomposition selectivity and catalyst deactivation are broken through; by adjusting the type and concentration of catalyst precursors, the diameter of carbon nanotubes can be controlled to grow; and the Joule heat method is used to open up a new path of "waste → high-value carbon nanomaterials". BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A schematic diagram of the reaction apparatus of the present invention is shown.

[0025] Figure 2 A typical reaction temperature rise and fall curve of the present invention is shown.

[0026] Figure 3The Raman spectrum (a), scanning electron microscope (SEM) image (b) and transmission electron microscope (TEM) image (c) of the multi-walled carbon nanotubes prepared in Example 1 of the present invention are shown.

[0027] Figure 4 The Raman spectrum (a) and TEM image (b) of the single-walled carbon nanotubes prepared in Example 2 of the present invention are shown.

[0028] Figure 5 The Raman spectrum (a), SEM image (b) and TEM image (c) of the multi-walled carbon nanotubes prepared in Example 3 of the present invention are shown.

[0029] Figure 6 The Raman spectrum (a) and SEM image (b) of the multi-walled carbon nanotubes prepared in Example 4 of the present invention are shown. DETAILED DESCRIPTION

[0030] The present invention will be further described below with reference to the embodiments, through which the features and advantages of the present invention will become more clearly understood.

[0031] Example 1 - Rapid Joule Thermal Catalytic Growth of Multi-Walled Carbon Nanotubes

[0032] Polyethylene powder is used as a carbon source, and a cobalt-molybdenum metal (CoMo / MgAl-LDH) catalyst supported by magnesium-aluminum hydrotalcite is mixed as a reaction precursor for preparing multi-walled carbon nanotubes. Among them, the CoMo / MgAl-LDH catalyst is synthesized by a sol-gel method. According to a preferred embodiment of the present invention, 0.582g Co(NO3)2·6H2O, 2.564g Mg(NO3)2·6H2O and 1.875g Al(NO3)3·9H2O are dissolved in 120mL deionized water and stirred evenly. Subsequently, 1.800g urea and 0.082g (NH4)6Mo7O are added to the solution. 24 4H2O. The homogeneous mixture was transferred to a round-bottom flask and refluxed in an oil bath at 100°C with continuous stirring for 12 hours. The solution was then aged at the same temperature for another 12 hours. The resulting precipitate was collected by filtration and freeze-dried to obtain the CoMo / MgAl-LDH catalyst.

[0033] 1.00g of polyethylene and 0.10g of CoMo / MgAl-LDH catalyst were ground and mixed to obtain a reaction precursor for preparing multi-walled carbon nanotubes. The reaction precursor was then mixed with 0.40g of carbon black and further ground and mixed to obtain a cylindrical precursor. 0.5g of the mixed sample was pressed at a pressure of 20MPa on a tablet press for 20 minutes to obtain a cylindrical precursor. The precursor rod was then placed in a quartz tube lined with graphite paper, with two graphite rod electrodes used as spacers at both ends to connect the copper electrode and the precursor rod ( Figure 1The resistance across the copper electrode was measured to be between 0.5 and 1.5 Ω. According to Joule's law, the precursor will generate Joule heat and heat up rapidly after being energized. The entire reaction was carried out under N2 protection. The reaction current was controlled by a constant current power supply. Under this reaction volume, a current of 29A was passed. The infrared temperature detector measured that the temperature of the reactants rose to about 1150°C ( Figure 2 After 30 seconds of reaction, carbon nanotube products were obtained.

[0034] The carbon nanotubes obtained in Example 1 were characterized by Raman spectroscopy and electron microscopy. Figure 3 The Raman spectrum and electron microscopy characterization results show that the product contains a large amount of graphitized multi-walled carbon nanotubes with a diameter of about 10nm.

[0035] Example 2 - Rapid Joule Thermal Catalytic Growth of Single-Walled Carbon Nanotubes

[0036] This example uses the same synthesis method as Example 1, except that the catalyst in this example is replaced with a CoMo / Al2O3 catalyst prepared by a sol-gel method. According to a preferred embodiment of the present invention, 4.2 mL of sec-butoxyaluminum is dissolved in 35 mL of ethanol at 70°C. Subsequently, 23 mL of ethanol, 200 μL of water, and 60 μL of 65% nitric acid are added under reflux conditions. Next, a solution of 0.485 g of CoAc2·4H2O and 0.053 g of MoO2(acac)2 dispersed in 15 mL of ethanol is added to the sol, refluxed for 0.5 hours, and cooled to room temperature. 1 mL of concentrated aqueous ammonia, 1 mL of water, and 5 mL of ethanol are quickly added and stirred vigorously. After standing for a while, a uniform gel is formed, which is allowed to stand for 12 hours and then supercritically dried to obtain the CoMo / Al2O3 catalyst.

[0037] 1.00 g of polyethylene and 0.10 g of CoMo / Al₂O₃ were ground and mixed to obtain a reaction precursor for preparing single-walled carbon nanotubes. The reaction precursor was then mixed with 0.40 g of carbon black and further ground and mixed to obtain a reaction precursor for preparing single-walled carbon nanotubes. The subsequent process was the same as in Example 1. Carbon nanotubes were obtained after a reaction at approximately 1100°C for 30 seconds at a current of 55 A.

[0038] The carbon nanotubes obtained in Example 2 were characterized by Raman spectroscopy and electron microscopy. Figure 4 The Raman spectrum and electron microscopy characterization results show that the product contains a large number of single-walled carbon nanotubes with a diameter ranging from 1.2 to 2.4 nm.

[0039] Example 3 - Rapid Joule Thermal Catalytic Growth of Multi-Walled Carbon Nanotubes

[0040] The synthesis method of this example is the same as that of Example 1, except that the catalyst in this example is replaced with cobalt and nickel metal salts. According to a preferred embodiment of the present invention, 0.58g of Co(NO3)2·6H2O and 0.58g of Ni(NO3)2·6H2O are dissolved in 100mL of water, 2.8g of polyethylene is added, and ultrasonic dispersion treatment is performed to promote uniform contact between the metal salt solution and the polyethylene surface. Thereafter, mechanical stirring is performed at room temperature for 10h, and the catalyst-loaded dry polymer is obtained after drying in an 80°C oven as a reaction precursor for preparing multi-walled carbon nanotubes. After the above reaction precursor is thoroughly ground and mixed with 1.12g of conductive carbon black, the subsequent process is the same as in Example 1. After reacting at about 1000°C for 30s under a current of 36A, a carbon nanotube product is obtained.

[0041] The carbon nanotubes obtained in Example 3 were characterized by Raman spectroscopy and electron microscopy. Figure 5 The Raman spectrum and electron microscopy characterization results show that the product is graphitized multi-walled carbon nanotubes with a diameter of about 40nm.

[0042] Example 4 - Rapid Joule Heating Catalytic Growth of Carbon Nanotubes Using Rubber as a Carbon Source

[0043] This example follows the same synthesis method as Example 3, except that the polymer carbon source in this example is waste rubber. The waste rubber is immersed in a CoNi nitrate solution to form a CoNi-catalyzed rubber polymer, which serves as a precursor for preparing multi-walled carbon nanotubes. This precursor is thoroughly ground and mixed with 1.12g of conductive carbon black. The subsequent process is the same as in Example 1. The carbon nanotube product is obtained after a reaction at approximately 1450°C for 30 seconds at a current of 40A.

[0044] The carbon nanotubes obtained in Example 4 were characterized by Raman spectroscopy and scanning electron microscopy. Figure 6 The characterization results show that the product contains a large amount of carbon nanotubes.

[0045] The above embodiments merely illustrate several preferred embodiments of the present invention and are not to be construed as limiting the scope of the present invention. Any modifications and improvements made without departing from the spirit of the present invention are within the scope of protection of the present invention. Therefore, the scope of protection of the present invention shall be determined by the appended claims.

Claims

1. A method for rapidly decomposing waste polymers to prepare carbon nanotubes, comprising the following steps: 1) mixing waste polymer powder with a catalyst to prepare a reaction precursor, wherein the catalyst is a metal-based catalyst containing iron, cobalt, nickel and / or molybdenum; 2) Compounding the reaction precursor with the conductive carbon material and sealing it in a reaction container, with both ends connected to the positive and negative electrodes of a power supply; 3) A current of 20 to 100 A is passed through the reaction system, and the Joule heating effect of the conductive carbon material is used to heat the reaction system to 600 to 2500° C. at a rate of >1000° C. / s, and the reaction is carried out for 5 to 60 seconds to generate carbon nanotubes.

2. The method according to claim 1, characterized in that The waste high molecular polymer in step 1) is selected from one or more combinations of polyethylene, polypropylene, polyvinyl chloride, polystyrene, and rubber waste.

3. The method according to claim 1, characterized in that The catalyst in step 1) is selected from one or more of iron powder, nickel powder, cobalt powder, molybdate, and nitrate, sulfate, chloride, and acetate of iron, cobalt, and nickel.

4. The method according to claim 3, characterized in that In step 1), the catalyst is directly mixed with the polymer powder; alternatively, the catalyst is wet-deposited on an oxide support or a hydrotalcite support and then mixed with the polymer powder; alternatively, the catalyst is dissolved in water, fully mixed with the polymer powder and then dried.

5. The method according to claim 4, characterized in that The oxide carrier is a single compound or a mixture of magnesium oxide, silicon oxide or aluminum oxide; the catalyst accounts for 0.5%-20% of the total mass of the reaction precursor.

6. The method according to claim 1, characterized in that The conductive carbon material in step 2) is selected from carbon black, carbon nanotubes, graphite powder, carbon paper, carbon cloth, graphite paper, and carbon fiber film, and the reaction precursor and the conductive carbon material are compounded by wrapping and / or mixing.

7. The method according to claim 1, characterized in that In step 2), for film-like conductive carbon materials, the reaction precursor is wrapped with it, sealed in a quartz tube reactor, and graphite electrodes are connected at both ends; for powdered conductive carbon materials, it is directly mixed with the reaction precursor and then fully ground, pressed into a certain shape or granulated and loaded into a quartz tube reactor, and graphite electrodes are connected at both ends.

8. The method according to claim 7, characterized in that The added amount of the powdered conductive carbon material is 5% to 50% of the mass of the reaction precursor.

9. The method according to claim 1, characterized in that Step 3) The reaction is carried out in an oxygen-free or oxygen-deficient atmosphere with an oxygen content of <3 vol%. The reaction atmosphere is nitrogen, argon or an argon-hydrogen mixture, and the atmosphere pressure P is 0 < P < 101 kPa.

10. The carbon nanotube prepared by the method according to any one of claims 1 to 9, wherein the carbon nanotube is a multi-walled carbon nanotube or a single-walled carbon nanotube, and has a diameter ranging from 1 to 50 nm.

Citation Information

Cited By

  • Single-walled carbon nanotube and preparation method thereof

    CN121063523A

  • Efficient carbon nanotube preparation system and method based on floating catalytic reactor coupling

    CN122273411A