Copper powder and its preparation methods, conductive copper paste and its applications

By connecting copper oxides between copper particles and treating them with an organic coating layer, copper powder with high conductivity and stability was prepared, which solved the problem of high cost of grid electrodes in solar cells and enabled copper electrodes to efficiently replace silver electrodes.

CN120460719BActive Publication Date: 2026-11-17LONGI GREEN ENERGY TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510474827.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-04-15
Publication Date
2026-11-17
Estimated Expiration
2045-04-15

AI Technical Summary

Technical Problem

The grid electrodes of existing solar cells are mainly made of silver, which is expensive. It is difficult to effectively reduce costs while maintaining high conductivity by replacing them with copper.

Method used

Composite copper particles are used, and a stable conductive path is formed through the connection of copper oxide between the copper particles, which reduces the interfacial contact resistance. An organic coating layer is used to isolate oxidation, and the preparation method of copper powder is optimized to improve conductivity and stability.

Benefits of technology

This technology achieves high conductivity and stability in copper electrodes, reducing the cost of solar cells while maintaining conductivity characteristics close to those of silver electrodes, providing a base metal alternative to silver for photovoltaic cell grid line materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120460719B_ABST
    Figure CN120460719B_ABST
Patent Text Reader

Abstract

This application provides a copper powder and its preparation method, a conductive copper paste, and its application, belonging to the field of conductive materials technology. The copper powder includes composite copper particles, wherein the composite copper particles comprise copper particles at least partially interconnected by copper oxides.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of conductive materials technology. Specifically, this application relates to a copper powder and its preparation method, a conductive copper paste and its application. More specifically, this application relates to a copper powder and its preparation method, a conductive copper paste, a copper electrode and a solar cell. Background Technology

[0002] Building a new energy system dominated by clean energy, especially developing renewable energy technologies with the potential for large-scale application, has become an important strategic direction for breaking through energy bottlenecks. Among them, solar energy is one of the most important renewable energy sources, characterized by being pollution-free, renewable, and having huge reserves.

[0003] Photovoltaic power generation is a clean energy technology that uses photovoltaic cell modules to directly convert solar energy into electrical energy. In the manufacturing process of photovoltaic cells, in order to reduce costs, other metals have been tried to replace silver. Copper has similar conductivity to silver, but copper itself is highly reactive, and its conductivity gradually deteriorates when stored in conductive copper paste at room temperature, making it difficult to widely use in photovoltaic cells. Summary of the Invention

[0004] In view of this, in order to at least partially solve the aforementioned technical problems, this application provides a copper powder and its preparation method, a conductive copper paste and its application.

[0005] According to one embodiment of this application, a copper powder is provided, comprising: composite copper particles, the composite copper particles comprising: copper particles at least partially connected by copper oxide.

[0006] According to another embodiment of this application, a method for preparing copper powder is provided, comprising: acid washing of copper particles to obtain acid-washed copper particles; washing the acid-washed copper particles with water and centrifuging them in air to obtain composite copper particles formed by copper particles at least partially connected to each other by copper oxides, thereby obtaining copper powder.

[0007] According to another embodiment of this application, a conductive copper paste is provided, comprising copper powder and a dispersion medium. The copper powder is copper powder as described above or copper powder prepared by the preparation method described above. Preferably, the conductive copper paste comprises 80-92% copper powder and 8-20% dispersion medium by weight.

[0008] According to another embodiment of this application, a copper electrode is provided, which is formed from the above-described conductive copper paste.

[0009] According to another embodiment of this application, a solar cell is provided, comprising a copper electrode as described above.

[0010] According to embodiments of this application, the composite copper particles consist of copper particles at least partially connected by copper oxide, enabling dense connections. While maintaining high continuity of the conductive path, this effectively reduces the interfacial contact resistance between copper particles, significantly improving the overall current-carrying capacity of the composite copper particles. Through performance optimization of the copper powder, it is ensured that, in subsequent applications, the copper electrode exhibits conductivity and stability similar to that of a silver electrode, providing an effective solution for the base metal substitution of silver in photovoltaic cell grid materials. Attached Figure Description

[0011] The above and other objects, features and advantages of this application will become clearer from the following description of embodiments with reference to the accompanying drawings, in which:

[0012] Figure 1 A schematic diagram of the structure of composite copper particles according to an embodiment of this application is shown;

[0013] Figure 2 A schematic diagram of the structure of composite copper particles according to another embodiment of this application is shown;

[0014] Figure 3 A flowchart illustrating a method for preparing copper powder according to an embodiment of this application is shown;

[0015] Figure 4 A transmission electron microscope (TEM) image of copper powder from Embodiment 1 of this application is shown;

[0016] Figure 5 It shows Figure 4 A magnified view of a portion of the copper powder at point A;

[0017] Figure 6 It shows Figure 4 A magnified view of a portion of the copper powder at point B;

[0018] Figure 7 It shows Figure 6 The images show magnified views of copper powder, where a shows a magnified view of point E; b shows a magnified view of point F; c shows a magnified view of point G; d shows a magnified view of point H; and e shows a magnified view of point I.

[0019] In the accompanying drawings, the meanings of the reference numerals are as follows:

[0020] 1-Copper powder;

[0021] 11-Copper oxide;

[0022] 12-Copper particles;

[0023] 13-Organic coating layer;

[0024] The thickness of M-copper oxide. Detailed Implementation

[0025] The embodiments of this application will now be described with reference to the accompanying drawings. However, it should be understood that these descriptions are exemplary only and are not intended to limit the scope of this application. In the following detailed description, numerous specific details are set forth to provide a thorough understanding of the embodiments of this application for ease of explanation. However, it will be apparent that one or more embodiments may be implemented without these specific details. Furthermore, descriptions of well-known structures and technologies are omitted in the following description to avoid unnecessarily obscuring the concepts of this application.

[0026] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the scope of this application. The term "comprising" as used herein indicates the presence of features, steps, or operations, but does not exclude the presence or addition of one or more other features.

[0027] When using expressions such as "at least one of A, B, and C," the expression should generally be interpreted in accordance with the meaning commonly understood by a person skilled in the art (e.g., "a system having at least one of A, B, and C" should include, but is not limited to, systems having A alone, having B alone, having C alone, having A and B, having A and C, having B and C, and / or having A, B, and C, etc.). When using expressions such as "at least one of A, B, or C," the expression should generally be interpreted in accordance with the meaning commonly understood by a person skilled in the art (e.g., "a system having at least one of A, B, or C" should include, but is not limited to, systems having A alone, having B alone, having C alone, having A and B, having A and C, having B and C, and / or having A, B, and C, etc.).

[0028] Solar energy, with its widespread distribution and superior energy density, demonstrates significant technological advantages in photovoltaic power generation. Achieving efficient utilization of solar energy through the photoelectric conversion effect of photovoltaic modules has become a crucial technological path for driving energy structure transformation.

[0029] However, the main reason limiting the widespread use of solar cells is their high cost. Currently, the grid electrodes of solar cells are mainly made of silver or silver-plated copper. Although silver-plated copper uses copper to replace some of the silver, which can reduce costs to some extent, the cost reduction is limited because the main material is silver. Therefore, it is necessary to find a way to reduce the cost of solar cells while ensuring their high conductivity.

[0030] In realizing the concept of this application, it was discovered that by using copper particles to form copper oxide in a relatively weak oxidizing environment and connecting the copper particles with copper oxide, the copper oxide at the connection point reduces the interfacial barrier height in the conductive path when forming a conductive path after the subsequent fabrication of the copper electrode, thus giving the copper electrode higher conductivity.

[0031] Specifically, according to one aspect of this application, a copper powder is provided, comprising composite copper particles. Figure 1 A schematic diagram of the structure of the composite copper particles according to an embodiment of this application is shown, as follows: Figure 1 As shown, copper powder 1 includes composite copper particles. The composite copper particles include copper oxide 11 and copper particles 12. At least a portion of the copper particles 12 are connected to each other by copper oxide 11.

[0032] According to the embodiments of this application, but not wanting to be bound by theory, by utilizing the oxidation environment provided during the washing and centrifugal separation process in the air, the copper particles 12 adsorb each other under centrifugal action and form copper oxide 11 at the adsorption interface between the copper particles 12. Through the in-situ bonding of copper oxide 11, a relatively stable interconnection structure between the copper particles 12 is formed, and a conductive path with low contact resistance is constructed.

[0033] In this embodiment, it can be understood at least partially that there are at least two copper particles 12 in the composite copper particles, which can be connected to each other entirely through copper oxide 11, or partially through copper oxide 11.

[0034] For example, two copper particles 12 can be connected to each other via copper oxide 11 to form composite copper particles. Alternatively, three copper particles 12 can be interconnected, with two copper particles 12 connected to each other via copper oxide 11, and the third copper particle 12 connected to at least one of the aforementioned two copper particles 12 through mutual adsorption between copper particles, i.e., through elemental copper. Furthermore, all three copper particles 12 can be interconnected via copper oxide 11.

[0035] It should be noted that copper particles 12 refers to particles whose main component is zero-valent copper.

[0036] It is understood that this application does not require all particles in the copper powder to be the aforementioned composite copper particles; the copper powder may also contain other copper particles (e.g., discrete copper particles not connected to other copper particles via oxides). In actual testing, several particles can be randomly selected and examined using an electron microscope to determine whether they contain the aforementioned particle composite.

[0037] Because copper particles and copper oxides have different crystal states, interplanar spacings, and positional distributions, they can be distinguished using an electron microscope.

[0038] In some embodiments, the composite copper particles are further coated with an organic coating layer 13, which covers the exposed surface of the composite copper particles, the exposed surface being the surface of the composite copper particles excluding the copper oxide bonding region.

[0039] In some embodiments, the organic coating layer 13 is amorphous and can be detected by an electron microscope. Of course, it is not limited to electron microscopy. Other methods known in the art can also be used to distinguish it, or a combination of multiple detection and testing methods can be used to distinguish it, such as XPS, infrared spectroscopy, XES, etc.

[0040] Figure 2 A schematic diagram of the structure of composite copper particles according to another embodiment of this application is shown. For example, two copper particles 12 are connected to each other by copper oxide 11. Figure 2 As shown, the junction between the two copper particles 12 forms a connection region. An organic coating layer 13 is applied to the exposed surface of the copper particles 12 outside the connection region. Compared with the traditional full-surface coating passivation process, this reduces the interface between the two organic coating layers (which can be understood as the copper oxide 11 at the connection replacing the traditional double organic coating layer structure), significantly reducing the interface barrier height in the conductive path and resulting in higher conductivity compared to the traditional organic coating layer.

[0041] Furthermore, this application forms an organic coating layer 13 on the exposed surface of the composite copper particles, which can prevent external oxygen from entering, improve antioxidant performance, and extend storage time.

[0042] In some embodiments, the copper oxide 11 comprises copper oxide or cuprous oxide. The copper oxide 11 forms a conductive interface for a copper-copper oxide heterojunction at the junction of the copper particles 12. The copper oxide or cuprous oxide has a band structure that matches that of metallic copper, reducing the barrier height when forming a copper-copper oxide heterojunction at the junction of the copper particles 12. The presence of copper oxide or cuprous oxide at the interface junction region facilitates carrier tunneling and thermionic emission, reduces the contact resistance at the interface junction region, and further improves conductivity. Furthermore, copper oxide exhibits better thermodynamic stability in high-temperature oxidation environments, maintaining a good passivation effect, which is beneficial for the long-term stable use of the copper powder 1 formed by subsequent copper oxide connections as a copper electrode.

[0043] In some implementations, such as Figure 1As shown, the thickness M of the copper oxide 11 is 0.1~10 nm, for example, it can be 0.1 nm, 0.2 nm, 0.3 nm, 0.4 nm, 0.5 nm, 0.6 nm, 0.7 nm, 0.8 nm, 0.9 nm, 1.0 nm, 1.5 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 10 nm, or a range consisting of any two of the above values. Preferably, it is 0.2-8 nm, more preferably 0.2-1 nm. When the thickness is too thin, it is difficult to form a continuous coverage, making the connection area between the copper particles 12 more prone to oxidation, resulting in decreased stability; when the thickness is too thick, it reduces the tunneling probability of charge carriers, increases the interface resistance between adjacent copper particles 12, and thus degrades the conductivity. When the thickness M of the copper oxide 11 is set within the above range, charge carriers can pass through the connection area of ​​the thinner copper oxide 11 to form a conductive path between adjacent copper particles 12, thereby reducing the hindering effect of the copper oxide 11 on conductivity.

[0044] It should be noted that the thickness M of the copper oxide 11 can be understood as the length in any tangential direction perpendicular to the connection area of ​​adjacent copper particles 12. Here, "any tangential" can be understood as the tangent of any one of the adjacent copper particles 12. For example, such as... Figure 6 As shown, for example, a tangent line (dashed line) can be drawn from point P on the surface of a copper particle 12, with point P as the starting point; similarly, a tangent line (dashed line) can be drawn from point Q on the surface of an adjacent copper particle 12, with point Q as the starting point. The thickness direction of the copper oxide 11 is as follows. Figure 6 As shown, the length of the copper oxide 11 connection area extending perpendicular to the direction of the dashed line (which can be understood as the normal direction of the dashed line) is the thickness M of the copper oxide 11.

[0045] In some embodiments, the copper oxide can be crystalline or amorphous (e.g., its structure does not show a lattice in transmission electron microscopy (TEM) analysis). In some embodiments, the copper oxide 11 is copper oxide with a (002) crystal orientation. Copper oxide has a monoclinic crystal phase, and oxygen atoms are densely packed in layers on the (002) crystal plane. The low surface energy of copper oxide on the (002) crystal plane allows for stable exposure and lattice matching with the (111) crystal plane of elemental copper. The regular layered arrangement of oxygen atoms on the (002) crystal plane promotes relatively stable bonding with the surfaces of adjacent copper particles 12, further enhancing the stability and conductivity of the composite copper particles.

[0046] In some embodiments, the copper particles 12 are flake-shaped copper particles or spherical copper particles.

[0047] Flaky copper particles can be understood as having a two-dimensional planar structure, exhibiting a two-dimensional planar extension morphology. Flaky copper particles have a relatively small thickness and a large aspect ratio, which can be understood as the ratio between the shortest diameter and the thickness along the two-dimensional planar extension direction. Specifically, flaky copper particles can be understood as copper particles with an aspect ratio greater than or equal to 2 12. Because flaky copper particles form a relatively flat surface and achieve surface-to-surface contact, their effective contact area is high, significantly reducing contact resistance. Furthermore, the organic coating layer 13 provides a relatively continuous and uniform coverage, resulting in good oxidation resistance for the flaky copper particles. Spherical copper particles have better fluidity and are more densely packed than flaky copper particles, contributing to higher mechanical stability during subsequent copper electrode formation. Specifically, spherical copper particles can be understood as copper particles with an aspect ratio less than 2 12. During the preparation of copper powder 1 or during the subsequent mixing to form copper slurry, flake copper particles and spherical copper particles can be compounded as needed. The spherical copper particles provide a supporting framework, while the flake copper particles dispersed between the spherical copper particles construct a lower resistance path. The compounding ratio of the two can be adjusted according to actual needs, and this application does not impose any special limitations on this.

[0048] It is understandable that when copper particles 12 are flake-shaped copper particles, the D of copper powder 1... 50 Particle size can be understood as the cumulative particle size by volume, which is the median particle size (D) in the volume-based particle size distribution measured by a laser diffraction / scattering particle size distribution measuring device for copper powder 1. 50 The cumulative particle size is used as the volumetric particle size. Similarly, when copper particles 12 are spherical copper particles, the D of copper powder 1 is... 50 Particle size can be understood as the cumulative particle size by volume, which is the median particle size (D) in the volume-based particle size distribution measured by a laser diffraction / scattering particle size distribution measuring device for copper powder 1. 50 ) is used as the cumulative particle size.

[0049] It should be noted that copper powder 1 was mixed into ethanol and dispersed by ultrasonic irradiation, and the resulting product was used as the test sample.

[0050] Considering the need for better oxidation resistance and good adhesion to the substrate during subsequent preparation of conductive metal pastes, when copper particles 12 are flake-shaped copper particles, the D of copper powder 1 is... 50 The particle size is 1~10μm, for example, it can be 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm, 5μm, 5.5μm, 6μm, 6.5μm, 7μm, 7.5μm, 8μm, 8.5μm, 9μm, 9.5μm or 10μm, or a range composed of any two of these values; when the copper particles 12 are spherical copper particles, the D of the copper powder 150 The particle size is 0.1~1μm, for example, it can be 0.1μm, 0.2μm, 0.3μm, 0.4μm, 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm or 1μm, or a range consisting of any two of these values.

[0051] Optionally, when the copper particles 12 are spherical copper particles, the D of the copper powder 1 50 The particle size is 100~800nm, for example, it can be 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm, 450nm, 500nm, 550nm, 600nm, 650nm, 700nm, 750nm or 800nm, or a range consisting of any two of these values. This setting further maintains the good stability and low resistivity of copper powder 1.

[0052] In some implementations, the median thickness of the sheet-like copper particles is 100–500 nm. The median thickness can be understood as the midpoint of the distribution of sheet-like copper particles in the thickness dimension. For example, a median thickness of 100 nm indicates that 50% of the sheet-like copper particles have a thickness of 100 nm or less, and 50% have a thickness greater than 100 nm. The median thickness can be obtained by directly observing and statistically analyzing scanning electron microscopy images, generating a cumulative distribution curve, and then extracting the median thickness.

[0053] The median thickness of the sheet-like copper particles is 100–500 nm, for example, it can be 100 nm, 120 nm, 150 nm, 180 nm, 200 nm, 220 nm, 250 nm, 280 nm, 300 nm, 320 nm, 350 nm, 380 nm, 400 nm, 420 nm, 450 nm, 480 nm, or 500 nm, or a range consisting of any two of these values. This setting makes it easier to form a surface-to-surface contact network structure during the formation of composite copper particles, thereby reducing contact resistance. If the median thickness is too high, the aspect ratio (the ratio between diameter and thickness) of the sheet-like copper particles decreases, resulting in a reduced contact area and increased resistivity; if the median thickness is too low, the mechanical strength of the sheet-like copper particles decreases, making them prone to breakage during processing and compromising the continuity of the conductive path.

[0054] Optionally, the ratio of the longest diameter to the shortest diameter of the sheet-like copper particles along the two-dimensional plane extension direction is 1 to 10, for example, it can be 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10, etc.

[0055] In some embodiments, the tap density of copper powder 1 is 4.3~4.7 g / mL, for example, it can be 4.3 g / mL, 4.4 g / mL, 4.5 g / mL, 4.6 g / mL or 4.7 g / mL. With this setting, because the tap density of copper powder 1 is relatively high, when subsequently used in conductive paste, the volume of the same mass of copper particles 12 is significantly reduced, thereby lowering the viscosity of the conductive paste and thus reducing the occurrence of possible incomplete or broken copper grid lines.

[0056] In some embodiments, when the copper particles 12 are flake-shaped copper particles, the specific surface area of ​​the copper powder 1 is 0.1~0.9 m². 2 / g, when copper particles 12 are spherical copper particles, the specific surface area of ​​copper powder 1 is 1~9m². 2 / g. Specific surface area can be understood as the surface area per unit mass of copper powder 1, and can be measured by conventional methods, such as the determination of specific surface area of ​​metal powders according to GB / T 13390-2008. This setting allows the flake-shaped copper particles and / or spherical copper particles to have good oxidation resistance. If the specific surface area is too large, the surface activity of copper particles 12 is higher, making them easier to oxidize; if the specific surface area is too small, the particle size of copper particles 12 is larger, affecting the low-temperature sintering performance of the copper conductive paste prepared by copper particles 12, resulting in difficulty in fully sintering at low temperatures, or poor contact between the copper particles 12 and the substrate after sintering.

[0057] For example, when the copper particles 12 are flake-shaped copper particles, the specific surface area of ​​the copper powder 1 can be, for example, 0.1 m². 2 / g, 0.2m 2 / g, 0.3m 2 / g, 0.4m 2 / g, 0.5m 2 / g, 0.6m 2 / g, 0.7m 2 / g, 0.8m 2 / g or 0.9m 2 / g, or a range consisting of any two of these values. When the copper particles 12 are spherical copper particles, the specific surface area of ​​the copper powder 1 can be, for example, 1m². 2 / g、2m 2 / g、3m 2 / g、4m 2 / g、5m 2 / g、6m 2 / g、7m 2 / g or 8m 2 / g, or a range consisting of any two of these values.

[0058] In some embodiments, the organic coating layer 13 includes at least one of organic amine compounds, organic acid compounds, and thiol compounds. This configuration helps to isolate the composite copper particles from external oxygen and moisture, thereby inhibiting oxidation reactions and improving the stability of the copper powder 1 in humid and hot environments. The organic coating layer 13 forms a dense molecular layer through chemisorption, reducing the resistivity of the conductive pathway.

[0059] It should be noted that the organic amine compounds, organic acid compounds, and thiol compounds used here can be long-chain organic coating agents. The steric hindrance effect of long carbon chains helps reduce the agglomeration between composite copper particles, maintaining good rheological properties during subsequent copper paste preparation. Simultaneously, long-chain organic coating agents can withstand the effects of high-temperature sintering during subsequent processing, avoiding performance degradation caused by thermal decomposition. The amine groups in the organic amine compounds and the carboxyl groups in the organic acid compounds form a chemisorbed organic coating layer 13 with the copper surface through coordination bonds, significantly increasing the bonding strength between the organic coating layer 13 and the composite copper particles. The thiol groups in the thiol compounds form covalent bonds with the copper surface, and the empty orbitals of sulfur atoms undergo charge transfer with the d electrons of copper, which helps inhibit chemical corrosion and optimize electrochemical performance.

[0060] Optionally, the organic coating layer 13 includes C6~C 22 Aliphatic amine compounds, C6~C 22 Fatty acid compounds, C6~C 22 At least one of aliphatic thiols. Long carbon chain, C6-C6. 22 Aliphatic amine compounds self-assemble into molecular membranes via van der Waals forces, further blocking the permeation of water molecules. With this configuration, C6~C 22 Aliphatic amines and C6~C 22 Fatty acid compounds help to further enhance the adhesion between the organic coating layer 13 and the composite copper particles, C6~C 22 Aliphatic thiols were used to further optimize electrochemical performance.

[0061] Further optionally, C6~C 22 The aliphatic amine compound is selected from at least one of n-octylamine, n-hexylamine, dodecylamine, tetradecylamine, hexadecylamine, stearylamine, and oleylamine, wherein C6~C 12 Short-chain amines, such as n-hexylamine and n-octylamine, have lower molecular weights and suitable high-temperature volatility, making them more suitable for low-temperature slurry curing processes. Among them, C... 14 ~C 22 Long-chain amines, such as hexadecylamine and stearylamine, have longer carbon chains, which help provide stronger steric hindrance and inhibit the agglomeration of composite copper particles during sintering. (C6~C) 22The fatty acid compound is oleic acid, which can form a denser monolayer film structure on the copper surface and has lower contact resistance. (C6~C) 22 The aliphatic thiol compound is selected from at least one of hexathiol, octethiol, and dodecyl mercaptan. Among them, short-chain thiols such as hexathiol or octethiol have a faster molecular diffusion rate, which can achieve the formation of the organic coating layer 13 in a shorter time and improve the passivation efficiency. Among them, long-chain thiols such as dodecyl mercaptan form an organic coating layer 13 with a thicker thickness and higher wear resistance, which helps to provide effective passivation protection for the composite copper particles.

[0062] It is understood that the organic coating layer 13 can be a single-layer membrane structure of the above-mentioned materials, or a multilayer membrane structure of different above-mentioned materials, without any particular limitation.

[0063] In some embodiments, the thickness of the organic coating layer 13 is 1~15nm, for example, it can be 1nm, 2nm, 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm, 10nm, 11nm, 12nm, 13nm, 14nm, or 15nm. If the thickness is too thin, it is difficult to form a continuous coverage of the composite copper particle surface by the organic coating layer 13, and pores or gaps may appear on the surface of the organic coating layer 13, making the composite copper particles more susceptible to oxidation and reducing stability. If the thickness is too thick, it may cause cracking under stress, making it difficult to maintain long-term stability in humid and hot environments. Furthermore, excessive thickness can result in high resistance when used as a copper electrode, thus reducing conductivity. Setting the thickness of the organic coating layer 13 within the above-mentioned range ensures continuous coverage of the composite copper particle surface by the organic coating layer 13, provides high conductivity when used as a copper electrode, and also ensures long-term stability during use.

[0064] The thickness of the organic coating layer 13 can be obtained by image analysis using transmission electron microscopy.

[0065] According to another embodiment of this application, a method for preparing copper powder is provided. Figure 3 A flowchart illustrating the preparation method of copper powder 1 according to an embodiment of this application is shown, as follows: Figure 3 As shown, the preparation method includes operations S301 to S302.

[0066] In operation S301, the copper particles 12 are acid-washed to obtain acid-washed copper particles 12.

[0067] In this embodiment, acid washing of the initial copper particles 12 helps to remove the original oxides and impurities attached to the copper particles 12, thereby improving the surface activity of the copper particles 12 in subsequent processing. It can be understood that acid washing here can be interpreted as removing all or part of the original oxides attached to the surface of the copper particles 12, preferably removing all of the original oxides.

[0068] In operation S302, the acid-washed copper particles 12 are washed with water and centrifuged in air to obtain composite copper particles formed by copper particles 12 that are at least partially connected to each other by copper oxide 11, thereby obtaining copper powder 1.

[0069] In this embodiment, the water washing step helps to remove all or part of the copper ions generated during the pickling process of the copper particles 12, thereby avoiding the interaction between free copper ions and the dispersion medium during the rolling process when the copper particles 12 are used in the conductive slurry. This ensures the stability of the conductive slurry and improves its shelf life. Simultaneously, water washing in the air helps to create a weakly oxidizing environment on the surface of the copper particles 12. Centrifugal separation provides a greater centrifugal force to the copper particles 12, allowing at least some of the copper particles 12 to adsorb onto each other under centrifugal force in low-oxygen conditions. This results in the formation of a copper oxide 11 connecting layer between at least some of the copper particles 12, linking two or more copper particles 12 together to form composite copper particles with copper oxide 11 as the connecting medium.

[0070] According to the embodiments of this application, the surface of copper particles 12 is controlled to oxidize by a combination of air washing and centrifugal separation, and the reaction process is shown in the following formula (I):

[0071] 4Cu+O2+2H2O→2Cu(OH)2→CuO / Cu2O formula (I).

[0072] Through the synergistic effect of dissolved oxygen in the water washing environment and centrifugal mechanical energy, selective growth of copper oxide at the contact sites between copper particles 12 is achieved. Two or more copper particles 12 are connected by copper oxide 11. When subsequently applied to copper electrodes, the traditional passivation structure is avoided at the copper oxide 11 site, which significantly reduces the interface barrier height in the conductive path, resulting in higher conductivity and lower resistance.

[0073] It is understood that the material of copper oxide 11, the shape of copper particles 12, the particle size and tap density of copper powder 1 are the same as those mentioned above, and will not be repeated here.

[0074] In some embodiments, the preparation method further includes: coating the composite copper particles with an organic coating agent solution to obtain copper powder 1 with an organic coating layer 13 on the surface.

[0075] The organic coating layer 13 is applied to the surface outside the connection area of ​​the composite copper particles (i.e., the exposed surface), which helps to isolate oxygen and moisture from the environment and maintain the efficient transmission of the conductive path. Furthermore, since the organic coating layer 13 covers the exposed surface of the composite copper particles but not the connection area of ​​the copper oxide 11, the interfacial barrier height in the conductive path is further reduced when a conductive path is formed in the connection area of ​​the copper oxide 11, resulting in lower resistance.

[0076] In some embodiments, the centrifugal speed is 3000~15000 rpm, and the centrifugation time is 20~200 s. This setting helps to maintain a certain amount of copper oxide 11 formation, allowing the copper oxide 11 to provide suitable bonding without affecting the overall conductivity of the copper particles 12. It can be understood that the higher the speed and the longer the centrifugation time, the greater the centrifugal force experienced by the copper particles 12, resulting in more connections of copper oxide 11. If the centrifugation speed and time are too high, too much copper oxide 11 will be formed, leading to increased resistance of the copper powder 1 and lower conductivity. If the centrifugation speed and time are too low, it is difficult to form sufficient copper oxide 11 connections, thus making it difficult to achieve high conductivity.

[0077] For example, the centrifugal speed for centrifugation can be 3000r, 4000r, 5000r, 6000r, 7000r, 8000r, 9000r, 10000r, 11000r, 12000r, 13000r, 14000r, 15000r, or a range of any two of these values. The centrifugation time can be 20s, 30s, 40s, 50s, 70s, 90s, 100s, 120s, 140s, 160s, 180s, 200s, or a range of any two of these values.

[0078] In some embodiments, the organic coating agent solution includes at least one of an organic amine solution, an organic acid solution, and a thiol solution. The organic coating agent solution can be understood as a solution formed by dissolving an organic coating agent in an organic solvent. The type of organic coating agent is the same as the material of the aforementioned organic coating layer 13, and will not be described again here. The organic solvent can be an alcohol solvent, such as methanol or ethanol. The addition of the organic solvent helps to fully dissolve the organic coating agent.

[0079] In some embodiments, pickling includes adding copper particles 12 to an acid solution and stirring. Pickling further removes the oxide layer and organic contaminants present on the copper particles 12, while retaining some active sites to promote subsequent oxidative bonding. The acid solution includes at least one of hydrochloric acid, hydrobromic acid, hydroiodic acid, sulfuric acid, nitric acid, perchloric acid, sulfurous acid, phosphoric acid, hydrofluoric acid, acetic acid, carbonic acid, hydrosulfuric acid, and hypochlorous acid. It is understood that a lower concentration of acid solution can be used as needed, for example, mixing concentrated sulfuric acid with water in a certain proportion to obtain a dilute sulfuric acid solution of a certain concentration. The concentration of the acid solution can be adjusted according to the thickness of the oxide layer.

[0080] Optionally, the stirring temperature is 25~35℃, for example, 25℃, 30℃ or 35℃, and the pickling time is 40~60min, for example, 40min, 45min, 50min, 55min or 60min. This setting helps to fully remove impurities and native oxide layers attached to the surface of copper particles 12.

[0081] According to another aspect of this application, a conductive copper paste is provided, comprising: copper powder 1 as described above or copper powder 1 prepared by the preparation method described above, and a dispersion medium.

[0082] According to an embodiment of this application, copper powder 1 provides composite copper particles, which are formed by copper particles 12 connected by at least a portion of copper oxide 11. The connection of copper oxide 11 forms a low-barrier conductive path, thereby reducing the volume resistivity of the conductive paste.

[0083] Optionally, the copper powder 1 also includes an organic coating layer 13 covering the surface other than the copper oxide 11. The organic coating layer 13 blocks moisture and oxygen in the environment and provides better antioxidant stability.

[0084] Optionally, the conductive copper paste comprises 80-92% copper powder 1 and 8-20% dispersion medium by mass. If the mass content of copper powder 1 is too high, although it can provide more conductive particles, it may result in poor dispersion, affecting the uniformity of conductivity. If the mass content of copper powder 1 is too low, it is difficult to provide sufficient conductivity, resulting in higher resistance and lower conductivity efficiency. Adjusting the mass content of copper powder 1 within the above range helps to form a sufficient conductive network, reducing resistance while ensuring the uniformity of the conductive network. If the mass content of the dispersion medium is too high, the copper powder 1 content is low, resulting in higher resistance. If the mass content of the dispersion medium is too low, the conductive copper paste becomes too viscous, making subsequent printing or coating processes difficult. Adjusting the mass content of the dispersion medium within the above range helps to balance the fluidity and conductivity of the conductive copper paste.

[0085] In some embodiments, the dispersion medium includes a resin, a curing agent, a dispersant, and a solvent. The addition of the resin and curing agent provides better low-temperature curing, while the addition of the dispersant and solvent reduces the viscosity of the conductive copper paste, making it suitable for finer copper grid line printing processes.

[0086] From the perspective of obtaining better low-temperature curing effect, the resin is selected from at least one of epoxy resin, phenolic resin, phenoxy resin, acrylic resin, aldehyde-ketone resin, polyurethane, and polyester.

[0087] Optionally, the epoxy resin can be a thermosetting resin, specifically selected from one or more of the following: bisphenol A type epoxy resin, bisphenol F type epoxy resin, hydrogenated bisphenol A type epoxy resin, polyurethane modified epoxy resin, dimer acid modified epoxy resin, siloxane modified epoxy resin, phenolic type epoxy resin, polyol glycidyl ether type epoxy resin, and polyacid glycidyl ester type epoxy resin. Of course, other resins known in the art that can be used in this application may also be selected, but since this is not the focus of this application, further limitations are not made here.

[0088] The curing agent is selected from at least one of dicyandiamide curing agents, tertiary amine curing agents, isocyanate curing agents, blocked isocyanate curing agents, imidazole curing agents, and acid anhydride curing agents.

[0089] Optionally, the curing agent may be selected from one or more of the following: triethanolamine, blocked isocyanate, 1-butyl-3-methylimidazolium dibutyl phosphate, Baxington 7982, Trixene BI 7982 (blocked isocyanate based on HDI), MF-K60X (blocked polyisocyanate HDI curing agent), ketoxime-terminated isocyanate, hexamethylene hexamethylene diisocyanate-terminated, and dodecyl mercaptan-terminated diphenyl diisocyanate. Of course, other curing agents known in the art that can be used in this application may also be selected, but since this is not the focus of this application, further limitations are not made here.

[0090] From the perspective of reducing the viscosity of conductive copper paste, the dispersant is selected from C. 16 ~C 22 Ether dispersants, C 16 ~C 22 Amine dispersants, C 16 ~C 22 At least one of carboxylic acid dispersants, wherein the end group of the dispersant is a polar group such as an amino group or a hydroxyl group.

[0091] Optionally, the dispersant may be selected from at least one of Tween-type dispersants, oleic acid, and Span-type dispersants. Of course, other dispersants known in the art that can be used in this application may also be selected, but since this is not the focus of this application, no further limitation is made here.

[0092] From the perspective of improving the solubility of various dispersion media, the solvent can be selected from at least one of ester solvents, ether solvents, ketone solvents or alcohol solvents.

[0093] Optionally, the solvent may be selected from sec-amyl acetate, cyclohexanone, amyl propionate, isopropyl lactate, divalent esters, amyl acetate, diethylene glycol acetate, diethylene glycol butyl ether acetate, ethylene glycol carbonate, propylene glycol carbonate, tributyl borate, triphenyl phosphate, tricresyl phosphate, butyl acetate, diethyl carbonate, ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, γ-butyrolactone, butyl carbitol acetate, ethyl carbitol acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate. The following are included in the list of esters, ethylene glycol monoethyl ether, ethylene glycol monomethyl ether, ethylene glycol butyl ether, ethylene glycol diethyl ether, diethylene glycol butyl ether, ethylene glycol monoisopropyl ether, dipropylene glycol methyl ether, dipropylene glycol ethyl ether, dipropylene glycol propyl ether, dipropylene glycol butyl ether, dipropylene glycol ether, ethylene glycol dimethyl ether, tripropylene glycol methyl ether, tripropylene glycol dimethyl ether, diethylene glycol monobutyl ether, 4-heptanone, sec-pentanol, ethylene glycol, propylene glycol, pentanol, hexanol, heptanol, octanol, methylpentanol, butyl carbitol, terpineol, and dihydroterpineol.

[0094] It is understandable that conductive copper paste may also include other additives such as accelerators as needed, which will not be elaborated here.

[0095] According to another aspect of this application, a copper electrode is provided, which is formed from the above-described conductive copper paste.

[0096] According to the embodiments of this application, as described above, since the copper particles 12 connected at least partially through the copper oxide 11 form a conductive copper paste, a low-barrier conductive path is formed through the connection region of the copper oxide 11, thereby reducing the volume resistivity of the copper electrode.

[0097] Optionally, since the copper powder 1 also has an organic coating layer 13, and the organic coating layer 13 covers the exposed area, it helps to isolate moisture and oxygen in the copper electrode's operating environment, further improving the stability of the copper electrode in use.

[0098] According to another embodiment of this application, a solar cell is provided, including the copper electrode described above.

[0099] According to the embodiments of this application, as described above, the copper electrode thus configured provides a conductive path with low contact resistance, and when applied to solar cells, it provides an effective approach and solution for the base metallization of grid line materials.

[0100] In some embodiments, the solar cell is selected from any one of a back contact cell, a heterojunction cell, or a perovskite-crystalline silicon tandem cell.

[0101] It is understood that the electrodes of the back contact battery are located on the back side of the battery. The copper electrodes mentioned above are applied to the electrode material of the back grid line. For example, the electrodes can be formed by screen printing. The copper powder 1 formed based on the copper particles 12 connected by copper oxide 11 helps to provide better current collection and transmission efficiency of the back contact battery. Since it replaces the silver electrode, it helps to reduce costs.

[0102] It is understood that heterojunction solar cells are bifacial cells. Copper electrodes are formed on the substrate surface, for example, grid electrodes can be fabricated using screen printing. A transparent conductive layer can be prepared using the copper powder 1 of this application via electrochemical deposition, as needed. Similarly, by replacing the silver electrode, better current collection and transmission efficiency can be provided while reducing costs.

[0103] It is understandable that in perovskite-crystalline silicon tandem solar cells, copper electrodes can be used as the intermediate connecting layer to replace the traditional ITO / Ag, or as the electrode of the top cell. Since it replaces silver, similar to the above, it can provide better current collection and transmission efficiency while reducing costs.

[0104] The present application is further illustrated below through embodiments, accompanying drawings, and related test experiments and results. In the following detailed description, numerous specific details are set forth for ease of explanation to provide a comprehensive understanding of the embodiments of the present application. However, it is apparent that one or more embodiments may be implemented without these specific details. Moreover, the details in the following embodiments can be arbitrarily combined to form other feasible embodiments without conflict.

[0105] It should be noted that the specific embodiments described below are merely illustrative examples, and the scope of protection of this application is not limited thereto. The chemicals and raw materials used in the following embodiments are all commercially available or prepared using recognized processing methods.

[0106] Example 1:

[0107] Take 100g of raw copper powder particles (spherical, D50=200nm), add 200ml of pre-diluted 3mol / L dilute sulfuric acid, stir at 30℃ for 50min to finish acid washing, remove the antioxidant layer, oxides and impurities on the surface of the raw copper powder particles, and obtain a mixed solution.

[0108] The mixture was poured into a centrifuge tank and centrifuged at 5000 rpm for 60 seconds to separate the solid and liquid phases, yielding acid-washed copper particles. The acid-washed copper particles were then washed multiple times with pure water to remove all or part of the copper ions. The copper particles were then centrifuged at 5000 rpm for 30 seconds to allow oxide bonding, resulting in composite copper particles, which were then washed clean and set aside.

[0109] A passivation solution was prepared by mixing 40 mL of dodecyl mercaptan and 200 mL of ethanol. The composite copper particles were then placed into the passivation solution and stirred at room temperature until the reaction was complete to obtain copper powder. The passivated copper powder was washed with ethanol and dried in a displacement gas oven to obtain copper powder.

[0110] Figure 4 A transmission electron microscope (TEM) image of copper powder from Embodiment 1 of this application is shown. Figure 5 It shows Figure 4 A magnified view of a portion of the copper powder at point A; Figure 6 It shows Figure 4 A magnified view of a portion of the copper powder at point B; Figure 7 It shows Figure 6 The images show magnified views of copper powder, where a shows a magnified view of point E; b shows a magnified view of point F; c shows a magnified view of point G; d shows a magnified view of point H; and e shows a magnified view of point I. Figures 4-7 It can be seen, especially through magnified local areas at the powder junctions, that there are two types of connection structures between the powder particles: one is the connection between the original powder particles, i.e. Figure 5 Point C in the middle (which can be understood as) Figure 4 The connection pattern shown in the magnified view at point A in the image originates during the original powder production process, where elemental copper particles are linked together. Another type occurs during copper powder processing, where copper particles connect with copper oxides. In a low-oxygen environment, copper oxides form on the surface of the copper particles, causing them to connect and form composite copper particles. The centrifugal force provided by the high-speed centrifugation further tightens the powder connections. After passivation treatment, the composite copper particles completely encapsulate the linked powder particles. Lattice calculations from the transmission electron microscopy image show... Figure 4 Point A in the figure represents the powder connection of copper particles, mainly the copper (111) crystal plane. Figure 4 Point B in the diagram represents the connection of copper oxide, primarily the CuO (002) crystal plane. Detailed analysis follows... Figure 7 As shown in a~e in the figure, the interplanar spacing of the crystal planes in the area within the dashed box is measured. The interplanar spacings at positions E, F, G, and I are all between 1.83 and 1.88 angstroms, which are copper (200) crystal planes; the interplanar spacing at position H is 2.53 angstroms, which is CuO (002) crystal plane.

[0111] Examples 2-10:

[0112] Except for adjusting the rotation speed and centrifugation time according to Table 1, the process was the same as in Example 1. Transmission electron microscopy (TEM) images of the prepared copper powder confirmed the presence of copper oxide between the copper particles.

[0113] Comparative Example 1:

[0114] Take 100g of raw copper powder particles (spherical, D50=200nm), add 200ml of pre-diluted 3mol / L dilute sulfuric acid, stir at 30℃ for 50min to finish acid washing, remove the surface antioxidant layer, oxides and impurities, and obtain a mixed solution.

[0115] The mixture was subjected to solid-liquid separation using a vacuum filter to obtain acid-washed copper particles. The copper particles were then washed multiple times with pure water to remove residual substances, either partially or completely, of the copper ions. Once the powder was thoroughly washed, copper particles were obtained.

[0116] A passivation solution was prepared by mixing 40 mL of dodecyl mercaptan and 200 mL of ethanol. Copper particles were then placed into the passivation solution and stirred at room temperature until the reaction was complete. The passivated copper particles were washed with ethanol and dried in a displacement oven to obtain copper powder.

[0117] Table 1

[0118]

[0119] The copper powders prepared in Examples 1, 4-5, and Comparative Example 1 were subjected to electrical performance tests. As shown in Table 1 above, it can be seen that the weak oxidizing environment provided by centrifugation in Examples 1-5 resulted in copper oxide at the joints of the prepared copper powders. However, in Comparative Example 1, which used a conventional filtration method, copper oxide joints could not be formed.

[0120] The copper powders obtained after passivation in Examples 1, 4-5, and Comparative Example 1 were respectively formulated into conductive copper pastes. Specifically, 0.4g of hydrogenated bisphenol A epoxy resin, 0.15g of blocked isocyanate as curing agent, 0.2g of 2-propylimidazolium as curing accelerator, 0.05g of oleylamine as dispersant, and 0.3g of diethylene glycol acetate as solvent were mixed and stirred evenly to obtain a slurry mother liquor. 8g of the copper powder obtained after passivation in Examples 1, 4-5, or Comparative Example 1 was poured into the slurry mother liquor, stirred, and then poured into a three-roll mill for rolling and grinding to obtain a homogeneous conductive copper paste.

[0121] The copper grid lines are screen-printed onto the solar cell with a width of 70μm. They are then heated and cured in a nitrogen oven at a temperature of 100~200℃ for 30 minutes to form copper electrode blocks and copper grid lines. The electrical properties of the paste can be obtained through a series of tests.

[0122] The copper electrode block and copper grid lines were tested. The copper electrode block was tested using a low-resistance tester, and the grid line contact resistance was tested using transmission line mode (TLM). DH5 represents the contact resistance of the cured battery after being placed at 85% humidity and 85°C for 5 hours. Table 2 below shows the relevant performance parameters of the copper electrodes of Examples 1, 4-5, and Comparative Example 1.

[0123] Table 2 Performance parameters of copper electrodes in Examples 1, 4-5, and Comparative Example 1

[0124]

[0125] As shown in Table 2, it can be seen that in Examples 1 and 4-5, the washing and centrifugal separation processes in the air provided a weak oxidizing environment, and the centrifugal force generated an interaction interface between copper particles, promoting the connection between copper particles through copper oxide. After subsequent coating with an organic coating layer, the connection between the two organic coating layers was reduced, thus reducing the interface barrier height when forming a conductive path, significantly lowering the resistivity in the conductive path, and improving the conductivity efficiency. Examples 1, 4-5, and Comparative Example 1 all showed good initial contact at the start of the electrochemical reaction. Furthermore, the copper electrodes of Examples 1 and 4-5 maintained low contact resistance even under high temperature and high humidity conditions. DH5 testing confirmed that Examples 1 and 4-5 of this application still exhibited good stability after multiple cycles. Further comparison between Examples 1 and 4-5 showed that Example 1 had better stability than Examples 4-5.

[0126] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of this application. It should be understood that the above descriptions are merely specific embodiments of this application and are not intended to limit this application. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A copper powder, comprising: Composite copper particles, the composite copper particles comprising: copper particles at least partially connected to each other by copper oxide; The thickness of the copper oxide is 0.1~10 nm; The copper particles are either flake-shaped or spherical; when the copper particles are flake-shaped, the D of the copper powder is... 50 The particle size is 1~10μm; when the copper particles are spherical copper particles, the D of the copper powder is... 50 The particle size is 0.1~1μm.

2. The copper powder according to claim 1, wherein, The composite copper particles are also coated with an organic coating layer, which covers the exposed surface of the composite copper particles. The exposed surface is the surface of the composite copper particle excluding the copper oxide bonding area.

3. The copper powder according to claim 1 or 2, wherein, The copper oxide includes copper oxide or cuprous oxide.

4. The copper powder according to claim 1 or 2, wherein, The copper oxide is copper oxide, and the crystal orientation of copper oxide is (002).

5. The copper powder according to claim 1, wherein, The median thickness of the sheet-like copper particles is 100~500 nm.

6. The copper powder according to claim 1, wherein, When the copper particles are flaky copper particles, the specific surface area of ​​the copper powder is 0.1~0.9 m². 2 / g; when the copper particles are spherical copper particles, the specific surface area of ​​the copper powder is 1~9m². 2 / g.

7. The copper powder according to claim 1 or 2, wherein, The tap density of the copper powder is 4.3~4.7 g / mL.

8. The copper powder according to claim 2, wherein, The organic coating layer includes at least one of organic amine compounds, organic acid compounds, and thiol compounds.

9. The copper powder according to claim 2, wherein, The organic coating layer comprises C6~C 22 Aliphatic amine compounds, C6~C 22 Fatty acid compounds, C6~C 22 At least one of aliphatic thiols.

10. The copper powder according to claim 9, wherein, The C6~C 22 The aliphatic amine compound is selected from at least one of n-octylamine, n-hexylamine, dodecylamine, tetradecylamine, hexadecylamine, stearylamine, and oleylamine, wherein C6~C 22 The fatty acid compound is oleic acid, wherein the C6~C 22 The aliphatic thiol compound is selected from at least one of the following: thiothiol, octethiol, and dodecanethiol.

11. The copper powder according to claim 2, wherein, The thickness of the organic coating layer is 1~15nm.

12. A method for preparing copper powder, comprising: The copper particles are acid-washed to obtain acid-washed copper particles; The acid-washed copper particles are washed with water and centrifuged in air to obtain composite copper particles formed by copper particles that are at least partially connected to each other by copper oxides, thereby obtaining the copper powder. The thickness of the copper oxide is 0.1~10 nm; The copper particles are either flake-shaped or spherical; when the copper particles are flake-shaped, the D of the copper powder is... 50 The particle size is 1~10μm; when the copper particles are spherical copper particles, the D of the copper powder is... 50 The particle size is 0.1~1μm.

13. The preparation method according to claim 12, further comprising: The composite copper particles are coated with an organic coating agent solution to obtain copper powder with an organic coating layer on the surface.

14. The preparation method according to claim 12 or 13, wherein, The centrifugation speed is 3000~15000r, and the centrifugation time is 20~200s.

15. The preparation method according to claim 13, wherein, The organic coating agent solution includes at least one of the following: organic amine solution, organic acid solution, and thiol solution.

16. The preparation method according to claim 12, wherein, The pickling process includes adding the copper particles to an acid solution and stirring. The acid solution includes at least one of hydrochloric acid, hydrobromic acid, hydroiodic acid, sulfuric acid, nitric acid, perchloric acid, sulfurous acid, phosphoric acid, hydrofluoric acid, acetic acid, carbonic acid, hydrosulfuric acid, and hypochlorous acid.

17. The preparation method according to claim 16, wherein, The stirring temperature is 25~35℃, and the pickling time is 40~60min.

18. A conductive copper paste, comprising: Copper powder and dispersion medium, wherein the copper powder is the copper powder as described in any one of claims 1 to 11 or the copper powder prepared by any one of claims 12 to 17.

19. The conductive copper paste according to claim 18, wherein, The conductive copper paste comprises 80-92% copper powder and 8-20% dispersion medium by weight.

20. The conductive copper paste according to claim 19, wherein, The dispersion medium includes: resin, curing agent, dispersant and solvent.

21. A copper electrode, formed from any one of the conductive copper pastes according to claims 18-20.

22. A solar cell comprising the copper electrode as claimed in claim 21.

23. The solar cell according to claim 22, wherein, The solar cell is selected from any one of back contact cells, heterojunction cells, and perovskite-crystalline silicon tandem cells.

Citation Information

Patent Citations

  • photoelectric element and process for its manufacture.

    CH161683A

  • Composite copper powder and preparation method and application thereof

    CN119098583A