Preparation method of high-capacity lithium iron phosphate positive electrode material and lithium battery
Through ultrasonic and mechanical force processing of raw materials, combined with copper oxide plasma spray coating, the problems of poor dispersion uniformity of raw materials and iron phosphide generation in the production process are solved, the electrochemical performance and production efficiency are improved, and high Preparation of cathode material for capacity lithium iron phosphate.
Patent Information
- Application Number
- CN202411167785.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-26
AI Technical Summary
During the production process, lithium iron phosphate positive electrode material is insufficient in electrochemical performance due to poor dispersion uniformity of raw materials and excessive iron phosphide generation, and high process manufacturing cost, making it difficult to effectively apply in some fields.
Using ultrasonic pretreatment, ball milling, ultrasonic secondary treatment, sand milling and spray drying, combined with copper oxide plasma spray coating during the sintering process, the raw material components are fully mixed and dispersed through ultrasonic and mechanical forces to reduce the particle size. Inhibit the production of iron phosphide and improve electrochemical properties.
It effectively improves the electrochemical performance of lithium iron phosphate positive electrode material, enhances the generation of active components, reduces the agglomeration of fine particles, and improves the electrochemical performance and production efficiency of the material.
Smart Images

Figure BDA0005008338000000081 
Figure BDA0005008338000000091
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium battery production, and in particular relates to a method for preparing a high-capacity lithium iron phosphate positive electrode material and a lithium battery. Background Art
[0002] As a secondary chemical energy storage system, lithium-ion batteries are widely used in electric vehicles, aerospace, military weapons and other fields due to their good stability, high conversion efficiency, high specific capacity, low cost and environmental protection. Lithium iron phosphate (LiFePO4) has unique advantages such as high reversible specific capacity, stable charge and discharge platform, high safety, long cycle life, abundant resources and low price. In recent years, with the in-depth study of the structure, synthesis, charge and discharge mechanism of LiFePO4, it has been widely used in energy storage systems and electric vehicles, becoming one of the most promising lithium-ion battery positive electrode materials. However, the inherent limitations of LiFePO4 positive electrode materials, its low conductivity and low Li + The diffusion rate limits its application in certain fields.
[0003] The main LiFePO4 production processes currently include high-temperature solid-phase reaction, carbothermal reduction, hydrothermal synthesis, sol / gel method, liquid-phase coprecipitation, and microwave synthesis. Each process has its own advantages and disadvantages, but the first three are currently the most widely used after improvements. Carbothermal reduction, also a solid-phase reaction, utilizes the binding ability of carbon and oxygen to reduce the oxide at high temperature. Compared to high-temperature solid-phase methods, it uses a relatively inexpensive and readily available trivalent iron source as a raw material, resulting in a simpler process and ease of industrialization. Furthermore, the residual carbon in the raw material acts as a dispersant and conductive agent, preventing LiFePO4 particle agglomeration and facilitating the production of smaller particles. Furthermore, the residual carbon itself has excellent electrical conductivity, reducing the contact resistance and bulk resistance of LiFePO4 and improving the material's high-current flow dynamics. This method primarily uses two iron sources: red iron oxide and iron phosphate. The iron phosphate process is relatively simple and easily automated. The resulting lithium iron phosphate material has a high specific capacity, nearly round grains, excellent processing properties, and easy batch quality assurance. However, the lithium iron phosphate material prepared by this process is heavily dependent on the quality of the iron phosphate raw materials and cannot be adjusted accordingly. The raw material mixing process requires high uniformity, and the high requirement for uniform dispersion causes a significant increase in process manufacturing costs. In addition, during the sintering process when preparing lithium iron phosphate, there is a possibility that iron phosphate and lithium iron phosphate will be reduced to iron phosphide in a high-temperature reducing atmosphere. Excessive generation of Fe2P will consume some LiFePO4, resulting in a reduction in active materials and a low released capacity. The content of this impurity must be controlled in actual production. Therefore, improving the preparation process is of great significance to improving the electrochemical performance of lithium iron phosphate positive electrode materials. Summary of the Invention
[0004] The purpose of the present invention is to provide a method for preparing a high-capacity lithium iron phosphate positive electrode material and a lithium battery, thereby improving the electrochemical performance of lithium iron phosphate by improving the dispersion uniformity of the raw materials and inhibiting the formation of iron phosphide.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] The present invention provides a method for preparing a high-capacity lithium iron phosphate positive electrode material, comprising the following steps:
[0007] (1) Ultrasonic pretreatment: Weigh iron phosphate, lithium carbonate, glucose, graphite, and deionized water according to the ratio and put them into an ultrasonic machine for ultrasonic dispersion;
[0008] (2) Ball milling: Add the dispersed liquid into a stirred mill and perform ball milling;
[0009] (3) Secondary ultrasonic treatment: the milled liquid is transferred to an ultrasonic machine for secondary ultrasonic treatment;
[0010] (4) Sand milling: the liquid after the second ultrasonic treatment is transferred into a sand mill for sand milling;
[0011] (5) Spray drying: The sand-milled liquid is passed through a high-speed centrifugal atomizer to form mist droplets that enter the drying chamber and are dried in contact with hot air;
[0012] (6) Primary air flow milling: The dried raw materials are transported to a fluidized bed air flow mill for primary milling;
[0013] (7) Sintering: The crushed raw materials are placed into a copper oxide / graphite sagger and transported to a sealed roller kiln for sintering at high temperature under a nitrogen atmosphere;
[0014] (8) Secondary air flow milling: the sintered material is transferred to a fluidized bed air flow mill for secondary milling;
[0015] (9) Vacuum drying: the material crushed in (8) is transferred to a vacuum tray dryer for drying;
[0016] (10) Screening and iron removal: The dried material is passed through a screening machine and an iron remover to remove impurities and obtain lithium iron phosphate positive electrode material.
[0017] Preferably, the molar ratio of iron phosphate and lithium carbonate in the ultrasonic pretreatment is 1:1:1, the amount of glucose added is 45-55% of the mass of iron phosphate and lithium carbonate, the amount of graphite added is 4-10% of the total mass of iron phosphate, lithium carbonate and glucose, and the amount of deionized water added is 5-10 times the total mass of iron phosphate, lithium carbonate, glucose and graphite.
[0018] Preferably, the ultrasonic frequency in the ultrasonic pretreatment is 50-60 KHz and the ultrasonic dispersion time is 45-60 min.
[0019] Preferably, the ball milling speed of the ball milling mixing is 100-200 r / min, and the ball milling time is 8-10 h.
[0020] Preferably, the particle size of the particles in the ball-milled liquid is ≤1.4 mm.
[0021] Preferably, the ultrasonic frequency in the secondary ultrasonic treatment is 20-30 KHz, and the secondary ultrasonic treatment time is 5-10 min.
[0022] Preferably, the sand mill speed in the sand milling is 1000-1500 r / min, and the sand milling time is 1-2 h.
[0023] Preferably, the particle size of the particles in the sand-milled material is ≤150 μm.
[0024] Preferably, the temperature of the drying chamber during the spray drying is 300-350°C.
[0025] Preferably, the copper oxide / graphite sagger used in sintering is a graphite sagger with a copper oxide coating plasma sprayed on the inner surface.
[0026] Preferably, the high-temperature sintering temperature is 600-750° C., and the sintering time is 16-24 hours.
[0027] The present invention also provides a lithium battery, wherein the lithium battery uses the lithium iron phosphate positive electrode material prepared by the above preparation method.
[0028] Beneficial effects of the present invention:
[0029] (1) The raw materials for preparing lithium iron phosphate are sequentially subjected to ultrasonic pretreatment, ball milling, ultrasonic secondary treatment and sand milling, and the ultrasonic effect is used to achieve full mixing and dispersion of the various raw material components in deionized water. The mechanical force of the ball milling is then used to reduce the particle size. The ultrasonic secondary treatment destroys the homogeneous particle agglomeration generated during the long ball milling process by acoustic cavitation. Finally, the particle size is further reduced by short-time sand milling. The ultrasonic acoustic cavitation and the shear and friction forces generated by ball milling (or sand milling) are alternately applied to the particle surface to achieve the reduction of particle size while reducing the agglomeration of fine particles, so that the reaction during the sintering process is more complete, the effective active components are increased, and the electrochemical performance is enhanced.
[0030] (2) A plasma-sprayed copper oxide-coated graphite crucible is used to load the material for sintering. During the sintering process of lithium iron phosphate, a large amount of carbon monoxide gas is generated. The reaction between copper oxide and carbon monoxide consumes the reducing gas, inhibits the production of iron phosphide, and improves the electrochemical performance of the positive electrode material. DETAILED DESCRIPTION
[0031] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative efforts shall fall within the scope of protection of the present invention.
[0032] Example 1
[0033] (1) Ultrasonic pretreatment: Weigh iron phosphate and lithium carbonate in a molar ratio of 1:1, weigh glucose that is 50% of the total mass of iron phosphate and lithium carbonate, and graphite that is 6% of the total mass of iron phosphate, lithium carbonate, and glucose. Put the above solid materials and deionized water (5 times the total mass of the solid materials) into an ultrasonic machine, set the ultrasonic frequency to 50 kHz, and ultrasonically disperse for 60 minutes;
[0034] (2) Ball milling: Add the dispersed liquid into a stirred mill, set the ball milling speed to 150 r / min, and perform ball milling for 9 hours. The particle size of the particles in the liquid after ball milling is ≤1.4 mm;
[0035] (3) Secondary ultrasonic treatment: The milled liquid was transferred into an ultrasonic machine, the ultrasonic frequency was set to 30 kHz, and the secondary ultrasonic treatment was performed for 5 min.
[0036] (4) Sand milling: The liquid after the second ultrasonic treatment was transferred to a sand mill, the speed of the sand mill was set to 1200 r / min, and the sand milling was performed for 1.5 h. The particle size of the particles in the liquid after sand milling was ≤150 μm;
[0037] (5) Spray drying: The milled liquid is passed through a high-speed centrifugal atomizer to form mist droplets that enter the drying chamber and are dried in contact with 300°C hot air in the drying chamber;
[0038] (6) Primary air flow milling: The dried raw materials are transported to a fluidized bed air flow mill for primary milling;
[0039] (7) Sintering: The crushed raw materials are placed into a graphite sagger coated with copper oxide, transported to a sealed roller kiln for sintering, and sintered at a high temperature of 600-750°C for 16 hours under a nitrogen atmosphere;
[0040] (8) Secondary air flow milling: the sintered material is transferred to a fluidized bed air flow mill for secondary milling;
[0041] (9) Vacuum drying: the material crushed in (8) is transferred to a vacuum tray dryer for drying;
[0042] (10) Screening and iron removal: The dried material is passed through a screening machine and an iron remover to remove impurities and obtain lithium iron phosphate positive electrode material.
[0043] The lithium iron phosphate cathode material prepared above is used to make a lithium battery.
[0044] Example 2
[0045] The difference from Example 1 is that the ultrasonic frequency of the ultrasonic pretreatment is set to 55 KHz, the ultrasonic time is 55 min, and the other steps are the same as Example 1.
[0046] Example 3
[0047] The difference from Example 1 is that the ultrasonic frequency of the ultrasonic pretreatment is set to 60 KHz, the ultrasonic time is 45 minutes, and the other steps are the same as Example 1.
[0048] Example 4
[0049] The difference from Example 1 is that the ultrasonic frequency of the secondary ultrasonic treatment is set to 25 KHz and the ultrasonic time is 8 minutes.
[0050] Example 5
[0051] The difference from Example 1 is that the ultrasonic frequency of the secondary ultrasonic treatment is set to 20 KHz, the ultrasonic time is 10 minutes, and the other steps are the same as Example 1.
[0052] Example 6
[0053] The difference from Example 1 is that the rotation speeds of the ball mill and the sand mill are reduced. The specific steps are as follows:
[0054] (1) Ultrasonic pretreatment: Weigh iron phosphate and lithium carbonate in a molar ratio of 1:1, weigh glucose that is 50% of the total mass of iron phosphate and lithium carbonate, and weigh graphite that is 6% of the total mass of iron phosphate, lithium carbonate, and glucose. Put the above solid materials and deionized water (8 times the total mass of the solid materials) into an ultrasonic machine, set the ultrasonic frequency to 50 kHz, and ultrasonically disperse for 60 minutes;
[0055] (2) Ball milling: Add the dispersed liquid into a stirred mill, set the ball milling speed to 100 r / min, and perform ball milling for 10 h. The particle size of the particles in the liquid after ball milling is ≤1.4 mm;
[0056] (3) Secondary ultrasonic treatment: The milled liquid was transferred into an ultrasonic machine, the ultrasonic frequency was set to 30 kHz, and the secondary ultrasonic treatment was performed for 5 min.
[0057] (4) Sand milling: The liquid after the second ultrasonic treatment was transferred to a sand mill, the speed of the sand mill was set to 1000 r / min, and the sand milling was performed for 2 h. The particle size of the particles in the liquid after sand milling was ≤150 μm;
[0058] (5) Spray drying: The milled liquid is passed through a high-speed centrifugal atomizer to form mist droplets that enter the drying chamber and are dried in contact with 300°C hot air in the drying chamber;
[0059] (6) Primary air flow milling: The dried raw materials are transported to a fluidized bed air flow mill for primary milling;
[0060] (7) Sintering: The crushed raw materials are placed into a graphite crucible with a copper oxide inner coating, transported to a sealed roller kiln for sintering, and sintered at a high temperature of 600-750°C for 20 hours under a nitrogen atmosphere;
[0061] (8) Secondary air flow milling: the sintered material is transferred to a fluidized bed air flow mill for secondary milling;
[0062] (9) Vacuum drying: the material crushed in (8) is transferred to a vacuum tray dryer for drying;
[0063] (10) Screening and iron removal: The dried material is passed through a screening machine and an iron remover to remove impurities and obtain lithium iron phosphate positive electrode material.
[0064] The lithium iron phosphate cathode material prepared above is used to make a lithium battery.
[0065] Example 7
[0066] The difference from Example 1 is that the rotation speed of the ball mill and the sand mill is increased. The specific steps are as follows:
[0067] (1) Ultrasonic pretreatment: Weigh iron phosphate and lithium carbonate in a molar ratio of 1:1, weigh glucose that is 50% of the total mass of iron phosphate and lithium carbonate, and weigh graphite that is 6% of the total mass of iron phosphate, lithium carbonate, and glucose. Put the above solid materials and deionized water (8 times the total mass of the solid materials) into an ultrasonic machine, set the ultrasonic frequency to 50 kHz, and ultrasonically disperse for 60 minutes;
[0068] (2) Ball milling: Add the dispersed liquid into a stirred mill, set the ball milling speed to 200 r / min, and perform ball milling for 8 hours. The particle size of the particles in the liquid after ball milling is ≤1.4 mm;
[0069] (3) Secondary ultrasonic treatment: The milled liquid was transferred into an ultrasonic machine, the ultrasonic frequency was set to 30 kHz, and the secondary ultrasonic treatment was performed for 5 min.
[0070] (4) Sand milling: The liquid after the second ultrasonic treatment was transferred to a sand mill, the speed of the sand mill was set to 1500 r / min, and the sand milling was performed for 1 h. The particle size of the particles in the liquid after sand milling was ≤150 μm;
[0071] (5) Spray drying: The milled liquid is passed through a high-speed centrifugal atomizer to form mist droplets that enter the drying chamber and are dried in contact with 300°C hot air in the drying chamber;
[0072] (6) Primary air flow milling: The dried raw materials are transported to a fluidized bed air flow mill for primary milling;
[0073] (7) Sintering: The crushed raw materials are placed into a graphite crucible with a copper oxide inner coating, transported to a sealed roller kiln for sintering, and sintered at a high temperature of 600-750°C for 20 hours under a nitrogen atmosphere;
[0074] (8) Secondary air flow milling: the sintered material is transferred to a fluidized bed air flow mill for secondary milling;
[0075] (9) Vacuum drying: the material crushed in (8) is transferred to a vacuum tray dryer for drying;
[0076] (10) Screening and iron removal: The dried material is passed through a screening machine and an iron remover to remove impurities and obtain lithium iron phosphate positive electrode material.
[0077] The lithium iron phosphate cathode material prepared above is used to make a lithium battery.
[0078] Comparative Example 1
[0079] Compared with Example 1, the raw materials of this comparative example were not subjected to ultrasonic pretreatment and ultrasonic secondary treatment, and the specific steps were as follows:
[0080] (1) Ball milling: Weigh ferric phosphate and lithium carbonate in a molar ratio of 1:1, weigh glucose that is 50% of the total mass of ferric phosphate and lithium carbonate, and weigh graphite that is 6% of the total mass of ferric phosphate, lithium carbonate, and glucose. Add the above solid materials and deionized water (5 times the total mass of the solid materials) into a stirred mill. Set the ball milling speed to 150 r / min and perform ball milling for 9 hours. The particle size of the particles in the milled liquid is ≤1.4 mm.
[0081] (2) Sand milling: The slurry after the second ball milling was transferred to a sand mill, the sand mill speed was set to 1200 r / min, and the sand milling was performed for 1.5 h. The particle size of the particles in the slurry after sand milling was ≤150 μm;
[0082] (3) Spray drying: The sand-milled liquid is formed into mist droplets by a high-speed centrifugal atomizer and enters the drying chamber, where it comes into contact with 300°C hot air to dry.
[0083] (4) Primary air flow milling: The dried raw materials are transported to a fluidized bed air flow mill for primary milling;
[0084] (5) Sintering: The crushed raw materials are placed into a graphite sagger coated with copper oxide, transported to a sealed roller kiln for sintering, and sintered at a high temperature of 600-750°C for 16 hours under a nitrogen atmosphere;
[0085] (6) Secondary air flow milling: the sintered material is transferred to a fluidized bed air flow mill for secondary milling;
[0086] (7) Vacuum drying: the crushed material in (7) is transferred to a vacuum tray dryer for drying;
[0087] (8) Screening and iron removal: The dried material is passed through a screening machine and an iron remover to remove impurities and obtain lithium iron phosphate positive electrode material.
[0088] The lithium iron phosphate cathode material prepared above is used to make a lithium battery.
[0089] Comparative Example 2
[0090] Compared with Example 1, the charging sagger used in the sintering of this comparative example is a graphite sagger, the inner surface is not plasma-sprayed with a copper oxide coating, and the other steps are the same as in Example 1.
[0091] The performance tests were conducted on the lithium iron phosphate cathode materials and lithium batteries prepared in Examples 1 to 7, Comparative Example 1, and Comparative Example 2. The results are shown in Table 1:
[0092] Table 1
[0093]
[0094]
[0095] As can be seen from Table 1, the preparation method in Comparative Example 1 does not use ultrasonic pretreatment and ultrasonic secondary treatment. Compared with the products in Examples 1-7, due to the interaction force during the raw material grinding and mixing process, the refined homogeneous particles will agglomerate, resulting in insufficient contact between the different raw material components, reducing the active components in the sintered product and its electrochemical performance is correspondingly poor. Unlike Example 1, Comparative Example 2 uses a graphite crucible commonly used in the prior art. Based on the removal of carbon monoxide by the copper oxide coating in Example 1 under high temperature conditions, it can effectively reduce the production of iron phosphide.
[0096] In Examples 1 to 3, the ultrasonic frequency of ultrasonic pretreatment gradually increases and the ultrasonic time gradually shortens. The higher the ultrasonic frequency, the better the dispersion effect between different particles, which is conducive to uniform mixing of components. However, too high a frequency will increase the heat generated, causing homogeneous particles to agglomerate under the thermal effect, which is not conducive to particle dispersion.
[0097] Compared with Example 1, the ultrasonic frequency of the ultrasonic secondary treatment in Example 4 and Example 5 is lower. The lower the ultrasound, the stronger its penetration, and the higher the destructive force on the agglomerated particles, which can promote the dispersion of homogeneous particle agglomerates during long-term grinding. However, if the frequency is too low, the original structure and morphology of the particles will be destroyed, resulting in an increase in irregular-shaped particles, a decrease in the compaction density after sintering, and a decrease in electrochemical performance.
[0098] In Examples 6 and 7, the ball milling and sand milling parameters were adjusted. Too high or too low a rotation speed was not conducive to particle dispersion, and the battery capacity was slightly reduced compared with Example 1.
[0099] It should be noted that, in this document, relational terms such as first and second, etc., are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations. Moreover, the terms "comprises," "comprising," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a list of elements includes not only those elements but also other elements not explicitly listed, or elements inherent to such process, method, article, or apparatus.
[0100] While embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions, and variations may be made to these embodiments without departing from the principles and spirit of the invention, and that the scope of the invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a high-capacity lithium iron phosphate positive electrode material, characterized in that: The following steps are involved: (1) Ultrasonic pretreatment: Weigh iron phosphate, lithium carbonate, glucose, graphite and deionized water according to the ratio, and put them into an ultrasonic machine for ultrasonic dispersion; (2) Ball milling: Add the dispersed liquid into a stirred mill for ball milling; (3) Secondary ultrasonic treatment: The ball-milled liquid is transferred into an ultrasonic machine for secondary ultrasonic treatment; (4) Sand milling: the liquid material after the second ultrasonic treatment is transferred into a sand mill for sand milling; (5) Spray drying: The sand-ground liquid is passed through a high-speed centrifugal atomizer to form mist liquid beads that enter the drying chamber and are dried in contact with hot air; (6) Primary air flow pulverization: the dried raw material is transported to a fluidized bed air flow pulverizer for primary pulverization; (7) Sintering: The crushed raw materials are loaded into a copper oxide / graphite sagger and transported to a sealed roller kiln for sintering at high temperature under a nitrogen atmosphere; (8) Secondary air flow milling: the sintered material is transferred to a fluidized bed air flow mill for secondary milling; (9) Vacuum drying: the crushed material in (8) is transferred into a vacuum tray dryer for drying; (10) Screening and iron removal: The dried material is passed through a screener and an iron remover to remove impurities to obtain lithium iron phosphate positive electrode material.
2. The method for preparing a high-capacity lithium iron phosphate positive electrode material according to claim 1, characterized in that: In the ultrasonic pretreatment, the molar ratio of iron phosphate to lithium carbonate is 1:1, the amount of glucose added is 45-55% of the mass of iron phosphate and lithium carbonate, the amount of graphite added is 4-10% of the total mass of iron phosphate, lithium carbonate and glucose, and the amount of deionized water added is 5-10 times the total mass of iron phosphate, lithium carbonate, glucose and graphite.
3. The method for preparing a high-capacity lithium iron phosphate positive electrode material according to claim 1, characterized in that: The ultrasonic pretreatment has an ultrasonic frequency of 50-560 KHz and an ultrasonic dispersion time of 45-60 min.
4. The method for preparing a high-capacity lithium iron phosphate positive electrode material according to claim 1, characterized in that: The ball milling speed of the ball milling mixing is 100-200 r / min, and the ball milling time is 8-10 h; The particle size of the particles in the ball-milled liquid is ≤1.4 mm.
5. The method for preparing a high-capacity lithium iron phosphate positive electrode material according to claim 1, characterized in that: The ultrasonic frequency in the secondary ultrasonic treatment is 20-30 KHz, and the secondary ultrasonic treatment time is 5-10 min.
6. The method for preparing a high-capacity lithium iron phosphate positive electrode material according to claim 1, characterized in that: The sand mill speed in the sand mill is 1000-1500r / min, and the sand milling time is 1-2h; The particle size of the particles in the sand-milled material is ≤150 μm.
7. The method for preparing a high-capacity lithium iron phosphate positive electrode material according to claim 1, characterized in that: The temperature of the drying chamber in the spray drying is 300-350°C.
8. The method for preparing a high-capacity lithium iron phosphate positive electrode material according to claim 1, characterized in that: The copper oxide / graphite sagger is a graphite sagger with a copper oxide coating plasma sprayed on the inner surface.
9. The method for preparing a high-capacity lithium iron phosphate positive electrode material according to claim 1, characterized in that: The high temperature sintering temperature is 600-700° C., and the sintering time is 16-24 hours.
10. A lithium battery, characterized in that: The lithium battery adopts the lithium iron phosphate positive electrode material prepared by the preparation method of the high-capacity lithium iron phosphate positive electrode material according to any one of claims 1-9.
Citation Information
Cited By
Preparation method of lithium iron phosphate positive electrode material
CN121974320A
Dry-method electrode film and preparation method therefor, electrode and battery
WO2025195536A1