Preparation method of high-entropy oxide sodium ion battery positive electrode material
The O3 high-entropy oxide Na(Mn0.2Co0.2Fe0.2Ti0.2)O2 was prepared by co-precipitation method, which solved the problem of volume change and structural damage during the embedding/detachment of electrode materials in sodium ion batteries, and achieved sodium ion The battery's high-rate performance and long cycle stability improve the overall performance of the battery.
Patent Information
- Application Number
- CN202310642349.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-01
- Publication Date
- 2024-12-03
AI Technical Summary
The large radius of sodium ions in sodium ion batteries leads to volume changes and structural damage during the embedding/detachment of electrode materials, limiting the performance and cycle life of sodium ion batteries. The existing high-entropy oxide materials have relatively more particles in solid-phase sintering methods. Large, poor performance, and performance needs to be improved.
O3 high-entropy oxide Na(Mn0.2Co0.2Fe0.2Ti0.2)O2 was synthesized by co-precipitation method, and a high-entropy oxide sodium ion battery with fine particle size was prepared by sintering equal proportions of transition metal elements in an air atmosphere. The positive electrode material broadens the sodium ion channel and improves the ion transfer speed and cycling stability.
The excellent rate performance and excellent cycle stability of the positive electrode material of high-entropy oxide sodium ion battery are achieved, with a reversible specific capacity of 78.4mAh g-1 at 3Ag-1 current density and a voltage range of 2-4.25V at 50mAg-1 current density. 141.6mAh g-1 has a reversible specific capacity in the first week, and the capacity retention rate of 100 weeks of circulation is 80.14%, and the average Coulombic efficiency is as high as 99.91%.
Smart Images

Figure CN119059576A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sodium ion batteries and relates to a method for preparing a high entropy oxide sodium ion battery positive electrode material. Background Art
[0002] As a new energy storage technology, sodium-ion batteries have high energy density and low cost, making them a potential alternative to lithium-ion batteries. However, since the radius of sodium ions in sodium-ion batteries is larger than that of lithium ions, their insertion / extraction process in electrode materials easily leads to volume changes, structural damage of electrode materials, and ion diffusion problems, thus limiting the performance and cycle life of sodium-ion batteries. In order to solve these problems, researchers have been looking for new electrode materials to achieve high-performance sodium-ion batteries.
[0003] As an emerging material, high entropy oxide has unique structure and properties. Unlike traditional oxides, high entropy oxides are composed of multiple metal elements to form a highly complex lattice structure. This structure gives high entropy oxides excellent physical and chemical properties, such as high temperature stability, ion conductivity and electrochemical activity. Therefore, high entropy oxides are considered to be a potential material that can be used in the field of energy storage.
[0004] At present, the most common method for synthesizing high entropy oxides is solid phase sintering. Reference 1 successfully prepared layered O3-type NaNi by solid phase sintering. 0.12 Cu 0.12 Mg 0.12 Fe 0.15 Co 0.15 Mn 0.1 Ti 0.1 Sn 0.1 Sb 0.04 O2 materials are used for the positive electrode of sodium ion batteries (Chenglong Zhao, High-entropy chemistry stabilizing layered O3-type structure in Na-ion cathode, 2019). Due to its extremely complex composition, the high entropy oxide material has good cycle stability, showing a capacity retention rate of 90% after 200 cycles at a current density of 0.5C; the rate capability is also improved, with the capacity retention reaching 80% at a rate of 5C. During the charge and discharge process, a highly reversible phase change behavior is exhibited between the O3 and P3 structures, and this behavior is effectively delayed, with more than 60% of the total capacity stored in the O3 region. Literature 2 also uses a solid phase sintering method to synthesize a single-phase O3-Na(Mn 0.2 Co 0.2 Fe 0.2 Ti 0.2 Ni0.2 )O2 high entropy oxide (Katarzyna Walczak, NaMn 0.2 Co 0.2 Fe 0.2 Ti 0.2 Ni 0.2 O2 high-entropy layered oxide–experimental and theoretical evidence of high electrochemical performance in sodium batteries, 2022) and applied it to the positive electrode material of sodium-ion batteries, which has a high current density of 180 mAh g at a wide voltage window C / 10 of 1.5-4.2 V. -1 The discharge capacity of the 2000 mAh g-1 cell is 200 mAh / g, but the voltage window is low and the particles synthesized by solid phase synthesis are large, resulting in poor rate performance, with a current density of only 60 mAh g-1 at 5 C. -1 The reversible specific capacity of the battery needs to be further improved. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing a high entropy oxide positive electrode material for sodium ion batteries. The general chemical formula of the high entropy oxide of the present invention is Na(Mn 0.2 Co 0.2 Fe 0.2 Ti 0.2 Ni 0.2 )O2, the cathode material prepared by this method has a fine particle size and a broadened sodium ion channel, and exhibits excellent rate performance and excellent cycle stability in sodium ion batteries.
[0006] The technical solution for achieving the purpose of the present invention is as follows:
[0007] The preparation method of the positive electrode material of the high entropy oxide sodium ion battery adopts the co-precipitation method to mix equal proportions of transition metal elements and sinter them, comprising the following steps:
[0008] (1) MnSO4, FeSO4, CoSO4, Ti(SO4)2 and NiSO4 are dissolved in water in an equal molar ratio, a small amount of H2SO4 solution is added dropwise to prevent hydrolysis, and then a NaOH solution is added dropwise to completely precipitate the metal elements in the form of hydroxides, centrifuged, washed with water until the supernatant is neutral, and dried to obtain hydroxide powder;
[0009] (2) Grind and mix the hydroxide powder and Na2CO3 according to the Na content being 1.05 to 1.08 times the total molar amount of the five transition metal elements, and then place the mixture in a muffle furnace under an air atmosphere and heat it to 400°C to 500°C, keep it warm for 2 to 5 hours, then heat it to 850°C to 950°C, keep it warm for 15 to 20 hours, and naturally cool it to room temperature to obtain a high entropy oxide sodium ion battery positive electrode material.
[0010] Preferably, in step (1), the concentration of the NaOH solution is 1 to 3 mol / L.
[0011] Preferably, in step (1), the drying temperature is 50 to 60° C. and the drying time is 12 to 24 hours.
[0012] Preferably, in step (2), the heating rate is 2 to 5°C / min.
[0013] Preferably, in step (2), the temperature is raised to 450° C. and kept at this temperature for 4 hours, and then raised to 900° C. and kept at this temperature for 15 to 20 hours.
[0014] Compared with the prior art, the present invention has the following advantages:
[0015] The present invention adopts the coprecipitation method to synthesize the O3 type high entropy oxide Na (Mn 0.2 Co 0.2 Fe 0.2 Ti 0.2 Ni 0.2 )O2, with a smaller particle size and a broadened sodium ion channel. The P3 phase produced after the charge-discharge phase transition replaces the O3 phase and takes the dominant position, with a faster ion transmission speed. After the transition, the high configuration entropy extends the P3 phase region, and has a better rate performance and good cycle stability than other O3 phase materials. -1 At a high current density of 78.4 mAh g -1 The reversible specific capacity at 50mAg -1 The reversible specific capacity in the first cycle in the high voltage range of 2-4.25V under the current density is 141.6mAh g -1 The capacity retention rate after 100 cycles is 80.14%, and the average coulombic efficiency is as high as 99.91%. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 The Na(Mn) prepared in Example 1 0.2 Co 0.2 Fe 0.2 Ti 0.2 Ni 0.2 )XRD pattern of O2;
[0017] Figure 2 The Na(Mn) prepared in Example 1 0.2 Co 0.2 Fe 0.2 Ti 0.2 Ni 0.2 ) SEM image of O2;
[0018] Figure 3 The Na(Mn) prepared in Example 1, Example 4 and Comparative Example 2 0.2 Co 0.2 Fe 0.2 Ti 0.2 Ni 0.2 ) XRD comparison of O2;
[0019] Figure 4 A comparison chart of the charge and discharge curves of the sodium ion batteries prepared in Example 1 and Comparative Example 1 at 2-4.25V;
[0020] Figure 5 This is a comparison chart of the cycle performance of the sodium ion batteries prepared in Example 1 and Comparative Example 1 at 2-4.25V;
[0021] Figure 6 This is a comparison chart of the rate performance of the sodium ion batteries prepared in Example 1 and Comparative Example 1 at 2-4.25V. DETAILED DESCRIPTION
[0022] The present invention is further described in detail below in conjunction with the embodiments and drawings, but is not intended to limit the protection scope of the present invention.
[0023] Example 1
[0024] (1) Preparation of precursor: Add 0.01 mol MnSO4, 0.01 mol FeSO4, 0.01 mol CoSO4, 0.01 mol Ti(SO4)2 and 0.01 mol NiSO4 to 200 mL of deionized water, and add 5 mL of concentrated H2SO4 solution dropwise to prevent hydrolysis; add 200 mL of 3 mol / L NaOH solution dropwise to the above mixed solution to completely precipitate the metal elements in the form of hydroxides; centrifuge the suspension, and wash and separate with deionized water until the supernatant is neutral; place the precipitate in an oven at 60°C and dry it for 24 h; manually grind and mix the dried hydroxide powder with Na2CO3, wherein the Na content is 1.05 times the total molar number of the five transition metal elements after precipitation.
[0025] (2) Mixed sintering: The mixed powder was placed in a corundum porcelain boat, placed in an air muffle furnace and heated to 450°C at a rate of 5°C / min, kept at this temperature for 4 hours, and then heated to 900°C at a rate of 5°C / min, kept at this temperature for 15 hours; cooled naturally to room temperature and then taken out to obtain high entropy oxide Na(Mn 0.2 Co 0.2 Fe 0.2 Ti 0.2 Ni 0.2 )O2, its XRD spectrum is shown in Figure 1 , Figure 2 This is a scanning electron microscope (SEM) image.
[0026] (3) Electrode preparation: The high entropy oxide Na(Mn 0.2 Co 0.2 Fe 0.2 Ti 0.2 Ni 0.2 )O2 is used as the active material of the battery positive electrode material for the preparation of sodium ion batteries. The specific steps are: prepare Na(Mn 0.2 Co 0.2 Fe 0.2 Ti 0.2 Ni 0.2 )O2 powder is mixed with Super P and binder polyvinylidene fluoride (PVDF) in a mass ratio of 80:10:10, and an appropriate amount of N-methylpyrrolidone (NMP) solution is added. The slurry is ground in a dry environment at room temperature to form a slurry, and then the slurry is evenly coated on the current collector aluminum foil, and after drying in a vacuum oven at 80°C, it is cut into pole pieces with a diameter of 12mm. The pole pieces are dried at 80°C for 12 hours under vacuum conditions and then transferred to a glove box for use.
[0027] (4) Half-cell assembly test: The battery was assembled in a glove box filled with Ar atmosphere, using metallic sodium as the counter electrode and 1M NaClO4 solution as the electrolyte to assemble into a CR2032 button cell. Constant current charge and discharge mode was used to perform constant current charge and discharge tests at a current density of 0.5C. Under the conditions of a discharge cut-off voltage of 2V and a charge cut-off voltage of 4.25V, the first-week discharge specific capacity can reach 141.mAh / g.
[0028] Example 2
[0029] This embodiment is basically the same as embodiment 1, except that the temperature is raised to 850°C for the second time in step (2) and kept for 15 hours. 0.2 Co 0.2 Fe 0.2 Ti 0.2 Ni 0.2)The XRD spectrum of O2 is the same as that of Example 1.
[0030] Example 3
[0031] This embodiment is basically the same as embodiment 1, except that the temperature is raised to 950°C for the second time in step (2) and kept at this temperature for 15 hours. 0.2 Co 0.2 Fe 0.2 Ti 0.2 Ni 0.2 )The XRD spectrum of O2 is the same as that of Example 1.
[0032] Example 4
[0033] This embodiment is basically the same as embodiment 1, except that the temperature is raised to 900°C for the second time in step (2) and kept at this temperature for 20 hours. 0.2 Co 0.2 Fe 0.2 Ti 0.2 Ni 0.2 )The XRD spectrum of O2 is the same as that of Example 1.
[0034] Comparative Example 1
[0035] (1) Preparation of precursor: Add 0.01 mol MnSO4, 0.01 mol FeSO4 and 0.01 mol NiSO4 to 200 mL of deionized water, and add 5 mL of concentrated H2SO4 solution to prevent hydrolysis; add 200 mL of 3 mol / L NaOH solution dropwise to the above mixed solution to completely precipitate the metal elements in the form of hydroxides; centrifuge the suspension and wash and separate it with deionized water until the supernatant is neutral; place the precipitate in an oven at 60°C and dry it for 24 h; manually grind and mix the dried hydroxide powder with Na2CO3, wherein the Na content is 1.05 times the total molar number of the three transition metal elements after precipitation.
[0036] (2) Mixed sintering: The mixed powder was placed in a corundum porcelain boat, placed in an air muffle furnace and heated to 450°C at a rate of 5°C / min, kept at this temperature for 4 hours, and then heated to 900°C at a rate of 5°C / min, kept at this temperature for 15 hours; cooled naturally to room temperature and then taken out to obtain the medium entropy oxide Na(Mn 0.33 Fe 0.33 Ni 0.33 )O2.
[0037] (3) Electrode preparation: The intermediate entropy oxide Na(Mn 0.33 Fe 0.33 Ni 0.33)O2 is used as the active material of the battery positive electrode material for the preparation of sodium ion batteries. The specific steps are: prepare Na(Mn 0.33 Fe 0.33 Ni 0.33 )O2 powder is mixed with Super P and binder polyvinylidene fluoride (PVDF) in a mass ratio of 80:10:10, and an appropriate amount of N-methylpyrrolidone (NMP) solution is added. The slurry is ground in a dry environment at room temperature, and then the slurry is evenly coated on the current collector aluminum foil, and after drying under an infrared lamp, it is cut into pole pieces with a diameter of 12mm. The pole pieces are dried at 80℃ for 12 hours under vacuum conditions and then transferred to a glove box for use.
[0038] (4) Half-cell assembly test: The battery was assembled in a glove box filled with Ar atmosphere, using metallic sodium as the counter electrode and 1 M NaClO4 solution as the electrolyte to form a CR2032 button cell.
[0039] Comparative Example 2
[0040] This comparative example is basically the same as Example 1, except that in step (2), the temperature is raised to 900° C. for the second time and kept at this temperature for 10 h.
[0041] Figure 1 The high entropy oxide Na(Mn) prepared in Example 1 0.2 Co 0.2 Fe 0.2 Ti 0.2 Ni 0.2 ) From the XRD spectrum of O2, it can be seen that the material synthesized by the co-precipitation method is a pure O3 phase material without any extra diffraction peaks. Figure 2 The high entropy oxide Na(Mn) prepared in Example 1 0.2 Co 0.2 Fe 0.2 Ti 0.2 Ni 0.2 )SEM image of O2, the material particles are concentrated around 2 microns and the particle size is uniform. Figure 3 The high entropy oxide Na(Mn) prepared in Example 1, Example 4 and Comparative Example 2 0.2 Co 0.2 Fe 0.2 Ti 0.2 Ni 0.2 )O2 XRD comparison spectrum, in comparative example 2, due to the short sintering time, there are still impurities generated, and redundant diffraction peaks appear; the high entropy oxide Na(Mn 0.2 Co 0.2 Fe 0.2 Ti 0.2 Ni 0.2)O2 and the intermediate entropy oxide Na(Mn 0.33 Fe 0.33 Ni 0.33 Comparison of the charge and discharge curves of sodium ion batteries assembled with )O2 at 2-4.25V Figure 4 As shown in Figure 3, the high configurational entropy makes the P3 phase region longer than other materials after phase transition, and more capacity can be provided in the P3 phase region. Figure 5 In order to use the constant current charge and discharge mode, the constant current charge and discharge test of Example 1 and the long cycle capacity comparison of Comparative Example 1 were carried out at a current density of 0.5C. The first cycle reversible specific capacity of Example 1 can reach 141.6 mAh g -1 The reversible specific capacity of comparative example 1 in the first week is 124 mAh g -1 , and it can be seen that high entropy oxides have a higher cycle retention rate. Figure 6 The high entropy oxide Na(Mn) prepared in Example 1 0.2 Co 0.2 Fe 0.2 Ti 0.2 Ni 0.2 )O2 and the intermediate entropy oxide Na(Mn 0.33 Fe 0.33 Ni 0.33 )O2 rate performance comparison, high entropy oxide in 3Ag -1 At a high current density of 78.4 mAh g -1 The reversible specific capacity of the intermediate entropy oxide in comparative example 1 is only 19 mAh g -1 The above results show that the high entropy oxide Na(Mn) prepared by the coprecipitation method in the present invention has a reversible specific capacity of 0.2 Co 0.2 Fe 0.2 Ti 0.2 Ni 0.2 )O2 has the characteristics of long cycle stability and high rate.
[0042] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. Preparation method of high entropy oxide sodium ion battery positive electrode material, It is characterized in that The following steps are involved: (1) MnSO 4 、FeSO 4 、CoSO 4 、Ti(SO 4 ) 2 and NiSO 4 Dissolve in water in an equal molar ratio and add a small amount of H 2 SO 4 solution to prevent hydrolysis, then add NaOH solution drop by drop to completely precipitate the metal element in the form of hydroxide, centrifuge, wash with water until the supernatant is neutral, and dry to obtain hydroxide powder; (2) The content of Na is 1.05 to 1.08 times the total molar amount of the five transition metal elements. 2 CO 3 The mixture is ground and mixed, and then placed in a muffle furnace under an air atmosphere and heated to 400°C~500°C, kept warm for 2~5 hours, then heated to 850°C~950°C, kept warm for 15~20 hours, and naturally cooled to room temperature to obtain a high entropy oxide sodium ion battery positive electrode material.
2. The preparation method according to claim 1, It is characterized in that In step (1), the concentration of the NaOH solution is 1-3 mol / L.
3. The preparation method according to claim 1, It is characterized in that In step (1), the drying temperature is 50-60°C and the drying time is 12-24 h.
4. The preparation method according to claim 1, It is characterized in that In step (2), the heating rate is 2-5 °C / min.
5. The preparation method according to claim 1, It is characterized in that In step (2), the temperature is raised to 450°C and kept at this temperature for 4 hours, and then the temperature is raised to 900°C and kept at this temperature for 15 to 20 hours.
Citation Information
Cited By
O3-phase sodium-ion battery positive electrode material suitable for high voltage and preparation method of O3-phase sodium-ion battery positive electrode material
CN119361679A
Sodium-ion battery positive electrode based on high-entropy oxide and preparation method of sodium-ion battery positive electrode
CN120383342A