A UV-curable adhesive, its preparation method and its application

By introducing a silicon-substituted bisphenol fluorene structure and a compounded UV-curable adhesive composition into a UV-curable adhesive, the problem of increasing the refractive index of UV-curable adhesives in the prior art has been solved, achieving the preparation of adhesives with high refractive index, low curing shrinkage and cost-effectiveness, suitable for LCD brightness enhancement films.

CN120484732BActive Publication Date: 2026-11-10NANJING BREADY ELECTRONICS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510773226.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-06-11
Publication Date
2026-11-10
Estimated Expiration
2045-06-11

AI Technical Summary

Technical Problem

Existing UV-curable adhesives suffer from poor process compatibility, increased curing shrinkage, or high costs in terms of improving refractive index, making it difficult to meet the development needs of LCDs.

Method used

A UV-curable adhesive formulation was developed by incorporating a silicon-substituted bisphenol fluorene structure. By compounding a UV-curable adhesive composition, including compound A, acrylate oligomers, polyurethane-modified acrylates, diluent monomers, antioxidants, and photoinitiators, a UV-curable adhesive with a refractive index greater than 1.58 was prepared.

Benefits of technology

This invention achieves a high refractive index UV-curable adhesive with good process compatibility, low curing shrinkage, and cost-effectiveness, making it suitable for formulations of high refractive index brightening films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120484732B_ABST
    Figure CN120484732B_ABST
Patent Text Reader

Abstract

This invention provides a UV-curable adhesive, its preparation method, and its application. The UV-curable adhesive of this invention has the following composition: Compound A: 25-35 parts, acrylate oligomer: 30-45 parts, polyurethane-modified acrylate: 10-15 parts, diluent monomer: 10-15 parts, antioxidant: 0.1-2 parts, photoinitiator: 2-5 parts, coupling agent: 0.1-2 parts. The acrylate oligomer is prepared from the following components in parts by weight: trimethylolpropane triacrylate: 30-40 parts, epoxy acrylate: 20-30 parts, butyl acrylate: 20-30 parts, and 2-hydroxyethyl acrylate: 10-15 parts. The structural formula of Compound A is [formula missing], where R is [formula missing], and n is an integer selected from 1 to 5. Testing showed that the UV-curable adhesive prepared by this invention further improved the refractive index and brightness of the brightening film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of adhesive technology, and in particular to a UV-curable adhesive for LCDs, its preparation method, and its application. Background Technology

[0002] The statements herein provide only background information in relation to this invention and do not necessarily constitute prior art.

[0003] LCDs are among the most dynamic electronic products of the early 21st century. Their development and advancements have broadened the application range of displays, making electronic display devices more convenient and widely adopted. In the manufacturing process of LCD modules, optical adhesives (such as UV-curable adhesives and LOCA liquid optical adhesives) are widely used in key processes such as panel bonding, brightness enhancement film adhesion, and polarizer fixation. Without altering the microscopic prism structure of the brightness enhancement film, the higher the refractive index of the film itself, the greater the brightness gain, thus enabling the LCD to produce higher brightness with the same energy consumption.

[0004] Currently, the industry mainly improves the refractive index by optimizing the resin matrix (such as introducing benzene rings, bisphenol A, or thiolated structures) or by doping with nanoparticles (such as TiO2 and ZrO2). However, challenges remain, including poor process compatibility (such as particle sedimentation), increased curing shrinkage, and high costs. Osaka Gas Co., Ltd. of Japan has proposed a method to synthesize multifunctional (meth)acrylate oligomers or their epoxide adducts by performing a polyphenol substitution reaction at the 9-position of fluorene. These oligomers exhibit high crosslinking density, significantly improving the hardness, heat resistance, and mechanical strength of optical materials. Further research revealed that the acrylate oligomers incorporating the fluorene backbone not only possess high refractive index (RI>1.50) but also maintain low curing shrinkage and high light transmittance, demonstrating significant application potential in the field of optical adhesives.

[0005] Building upon existing research and development experience, the applicant surprisingly discovered that introducing silicon-substituted bisphenol fluorene structures into UV-curable adhesive formulations can increase the refractive index of the UV-curable adhesive, thereby better meeting the development needs of LCDs. Currently, there are few reports on this method in domestic and international literature. Summary of the Invention

[0006] To address the shortcomings of existing technologies and improve the refractive index of UV-curable adhesives, this invention provides a UV-curable adhesive for LCDs, its preparation method, and its application.

[0007] To achieve the above objectives, the present invention is implemented through the following technical solution:

[0008] In a first aspect, the present invention provides a UV-curable adhesive that can be used in LCD brightness enhancement films, the UV-curable adhesive having a refractive index greater than 1.58.

[0009] Furthermore, the refractive index of the UV-curable adhesive is greater than 1.60.

[0010] Furthermore, the UV-curable adhesive includes compound A, which has the general formula shown in formula (I): (Equation I), where R is n is an integer selected from 1 to 5, specifically 1, 2, 3, 4 or 5.

[0011] Specifically, compound A can be compound A1 or A2.

[0012] The structural formula of compound A1 is:

[0013] ;

[0014] The structural formula of compound A2 is: ;

[0015] The UV-curable adhesive also includes acrylate oligomers, which are composed of trimethylolpropane triacrylate, epoxy acrylate, butyl acrylate, and 2-hydroxyethyl acrylate.

[0016] The UV-curable adhesive also includes polyurethane-modified acrylate. Because the polyurethane-modified acrylate molecular chain contains urethane groups, the polyurethane-modified acrylate resin has a low glass transition temperature, thereby improving fluidity and exhibiting high adhesion, improving curing performance, and enhancing abrasion resistance and flexibility.

[0017] The preparation method of the polyurethane-modified acrylate includes the following steps:

[0018] (1) Add diol dropwise to diisocyanate, heat to 60℃ and react. After the reaction is complete, product 1 is obtained.

[0019] (2) Under light-protected conditions, ethanolamine was slowly added dropwise to the acrylate monomer, and the temperature was increased to react. After the reaction was complete, product 2 was obtained.

[0020] (3) Under argon protection and light-proof conditions, product 1 is added dropwise to product 2 and the temperature is raised to 60°C to react. After the reaction, the polyurethane modified acrylate resin is obtained.

[0021] Preferably, the diisocyanate is selected from toluene diisocyanate, dimethyl biphenyl diisocyanate, and diphenylmethane diisocyanate; the diol is polyethylene glycol and / or polypropylene glycol, with a number average molecular weight of 1000 to 2000.

[0022] The molar ratio of diol to diisocyanate is 1:(1.8-2.2); the molar ratio of acrylate monomer to ethanolamine is (1.95-2.1):1.

[0023] The UV-curable adhesive also includes antioxidants and photoinitiators;

[0024] The antioxidant is selected from commonly used antioxidants in the prior art, such as tris(2,4-di-tert-butylphenyl) phosphite and dodecanol thiodipropionate.

[0025] The photoinitiator is selected from one or a combination of two of diphenyl(2,4,6-trimethoxybenzoyl)-phosphine oxide, 1-hydroxycyclohexylphenyl ketone, or 2,2-azobis(2-methylpropionitrile).

[0026] The UV-curable adhesive also includes a coupling agent, which is an isocyanate coupling agent, preferably selected from one or more of 3-propyl isocyanatetriethoxysilane, 3-isocyanatepropyltrimethoxysilane, and 3-isocyanatepropylmethyldimethoxysilane.

[0027] The UV-curable adhesive also includes a diluent monomer, which is a sulfur-containing acrylate; the sulfur-containing acrylate is selected from: bisphenol S methacrylate, bisphenol S epoxy methacrylate, bisphenol S bifunctional methacrylate, 4,4'-dimercaptodiphenyl sulfide dimethacrylate or 4,4'-dimethacryloyloxydiphenyl sulfone.

[0028] Furthermore, the UV-curable adhesive of the present invention has the following composition:

[0029] Compound A: 25-35 parts

[0030] Acrylic ester oligomers: 30-45 parts

[0031] Polyurethane modified acrylate: 10-15 parts

[0032] Diluent monomer: 10-15 parts

[0033] Antioxidant: 0.1-2 parts

[0034] Photoinitiator: 2-5 parts

[0035] Coupling agent: 0.1-2 parts

[0036] The acrylate oligomers are prepared from the following components in parts by weight:

[0037] Trimethylolpropane triacrylate: 30-40 parts;

[0038] Epoxy acrylate: 20-30 parts;

[0039] Butyl acrylate: 20-30 parts;

[0040] 2-Hydroxyethyl acrylate: 10-15 parts.

[0041] A second aspect of the present invention provides a method for preparing a UV-curable adhesive that can be used in LCD brightness enhancement films.

[0042] S1, add the following parts by weight of trimethylolpropane triacrylate (30-40 parts), epoxy acrylate (20-30 parts), butyl acrylate (20-30 parts), and 2-hydroxyethyl acrylate (10-15 parts) to a reaction vessel in sequence, stir under inert gas protection, and after stirring evenly, subject to UV irradiation to obtain the target acrylate oligomer.

[0043] S2, the preparation of polyurethane modified acrylate is as follows: (1) add diol to diisocyanate, heat to 60℃ and react for 3-4 hours. After the reaction is complete, product 1 is obtained; (2) under light-protected conditions, slowly add ethanolamine to acrylate monomer, heat and react for 20-30 hours. After the reaction is complete, product 2 is obtained; (3) under argon protection and light-protected conditions, add product 1 to product 2, heat to 60℃ and react for 3-4 hours. After the reaction, the polyurethane modified acrylate resin is obtained.

[0044] S3. First, add the photoinitiator (2-5 parts) to the reactor. Then, add the following components in the following proportions: Compound A: 25-35 parts, acrylate oligomer: 30-45 parts, polyurethane modified acrylate: 10-15 parts, diluent monomer: 10-15 parts, antioxidant: 0.1-2 parts, coupling agent: 0.1-2 parts. Stir thoroughly in the dark at room temperature until homogeneous. After standing, the UV-curable adhesive can be obtained.

[0045] In a third aspect of the invention, the UV-curable adhesive is used in the preparation of an LCD brightness enhancement film.

[0046] The beneficial effects of this invention are as follows:

[0047] Compared with existing technologies, the UV-curable adhesive composition prepared according to the present invention, through the compounding of UV-curable adhesive composition raw materials, results in a UV-curable adhesive composition with a high refractive index. The use of compound A imparts the high refractive index characteristic to the product, and the preparation method is simple and low-cost. Testing has shown that the UV-curable adhesive prepared according to the present invention can be used in the formulation of high refractive index brightening films. Detailed Implementation

[0048] Although the specification concludes with specifically pointing out and clearly claiming the invention, it is believed that the invention will be better understood from the following description. Unless otherwise specified, all percentages and ratios used herein are by weight of the entire composition, and all measurements were performed at 25°C and normal pressure. Unless otherwise stated, all temperatures are expressed in degrees Celsius. The invention may comprise (open-ended) the components of the invention as well as other ingredients or elements described herein, or may consist substantially of the components of the invention as well as other ingredients or elements described herein. As used herein, “comprising” means the stated ingredients, or their structural or functional equivalents, plus any other ingredients not stated. Unless the context otherwise implies, the terms “having” and “comprising” are also interpreted as open-ended. Compounds in the invention can be prepared according to methods for preparing compounds with the same or similar structures in the prior art; for example, compound B2 can also be prepared according to methods for synthesizing compound B1 in the prior art. As used herein, “consistently of” means that, in addition to those recited in the claims, the invention may include ingredients, but only if the addition of ingredients does not substantially alter the essential and novel characteristics of the claimed invention. Preferably, such additives will be absent or present only in trace amounts. However, it may include up to about 10% by weight of materials that can substantially alter the essential and novel characteristics of the claimed invention, provided that the utility (rather than the extent of utility) of the compound is maintained.

[0049] All ranges described herein include endpoints, including those describing ranges "between" two values. Terms such as "approximately," "usually," "substantially," etc., will be interpreted as modifying a term or value so that it is not absolute and does not relate to prior art. Such terms will be defined by the circumstances they modify and the terms themselves, when understood by one of ordinary skill in the art. This includes, at least, expected experimental, technical, and instrumental errors for a given technique used to measure the value.

[0050] Next, the structure and function of the present invention will be explained in more detail with reference to the following embodiments. These embodiments are provided for illustrative purposes only and are not to be construed as limiting the present invention in any way. The present invention will be further described below with reference to the embodiments.

[0051] Preparation Example 1

[0052] The reaction route for preparing compound A1 from raw material B1 is shown below:

[0053]

[0054] In a four-necked flask reactor equipped with a stirrer, oil-water separator, and thermometer, 0.25 mol (18.02 g) of acrylic acid, 0.1 mol (45.42 g) of raw material B1, and 200 ml of toluene were added, along with 0.01 mol (1.72 g) of PTS (p-toluenesulfonic acid) catalyst. The mixture was stirred thoroughly and heated. As the reaction proceeded, the azeotropic gases of toluene and water entered the oil-water separator, where the toluene was recovered for later use. The acid value was measured periodically as the reaction continued, and the reaction was stopped when the acid value dropped to 128 mg KOH / g. The reaction product was allowed to stand, separated, washed with water, and then added to a four-necked flask. A small amount of THQ (o-methylhydroquinone) was added, and the mixture was subjected to vacuum distillation to obtain the target product A1.

[0055] Preparation Example 2

[0056] The reaction route for preparing compound A2 from raw material B2 is shown below:

[0057]

[0058] In a four-necked flask reactor equipped with a stirrer, oil-water separator, and thermometer, 0.25 mol (18.02 g) of acrylic acid, 0.1 mol (54.22 g) of raw material B2, and 200 ml of toluene were added, along with 0.01 mol (1.72 g) of PTS (p-toluenesulfonic acid) catalyst. The mixture was stirred thoroughly and heated. As the reaction proceeded, the azeotropic gases of toluene and water entered the oil-water separator, where the toluene was recovered for later use. The acid value was measured periodically as the reaction continued, and the reaction was stopped when the acid value dropped to 128 mg KOH / g. The reaction product was allowed to stand, separated, washed with water, and then added to a four-necked flask. A small amount of THQ was added, and the mixture was subjected to vacuum distillation to obtain the target product A2.

[0059] Preparation Example 3

[0060] Preparation of polyurethane-modified acrylate

[0061] (1) Under argon protection, 300g of toluene diisocyanate was added to the reaction flask, the temperature was raised to 60℃, stirred, and 1000g of polypropylene glycol-1000 was added dropwise. After the addition was completed, the reaction was kept at the temperature for 3h, the reaction was stopped, and the temperature was lowered to obtain product 1.

[0062] (2) Under light-protected conditions, 600g of tripropylene glycol diacrylate was added to the reaction flask, heated to 50°C, stirred, and then 61g of ethanolamine was slowly added dropwise. After the addition was completed, the reaction was kept at the temperature for 25h, the reaction was stopped, and the temperature was lowered to obtain product 2.

[0063] (3) Under argon protection and light-proof conditions, product 2 was added to the reaction flask, heated to 60°C, stirred, and product 1 was added dropwise. The mass ratio of product 2 to product 1 was 1:1.1. After the addition was completed, the reaction was kept at the temperature for 4 hours. No -NCO groups were found. The reaction was stopped and the temperature was lowered to obtain the polyurethane modified acrylate.

[0064] Preparation Example 4

[0065] Preparation of product C

[0066] In a four-necked flask reactor equipped with a stirrer, oil-water separator, and thermometer, 0.25 mol (18.02 g) of acrylic acid, 0.1 mol (43.81 g) of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene, and 200 ml of toluene were added, along with 0.01 mol (1.72 g) of PTS (p-toluenesulfonic acid) catalyst. The mixture was stirred thoroughly and heated. As the reaction proceeded, the azeotropic gases of toluene and water entered the oil-water separator, where the toluene was recovered for later use. The acid value was measured periodically as the reaction continued, and the reaction was stopped when the acid value dropped to 128 mg KOH / g. The reaction product was allowed to stand, separated, washed with water, and then added to a four-necked flask. A small amount of THQ was added, and the mixture was subjected to vacuum distillation to obtain product C.

[0067] Example 1

[0068] The UV-curable adhesive of this invention has the following composition:

[0069] Compound A1: 35 parts

[0070] Acrylic ester oligomers: 30 parts

[0071] Polyurethane modified acrylate: 15 parts

[0072] Diluent monomer bisphenol S methacrylate: 12 parts

[0073] Antioxidant: 1 part

[0074] Photoinitiator: 5 parts

[0075] Coupling agent: 2 parts

[0076] The acrylate oligomers are prepared from the following components in parts by weight:

[0077] Trimethylolpropane triacrylate: 40 parts;

[0078] Epoxy acrylate: 25 parts;

[0079] Butyl acrylate: 25 parts;

[0080] 2-Hydroxyethyl acrylate: 10 parts.

[0081] The antioxidant is tris(2,4-di-tert-butylphenyl) phosphite.

[0082] The photoinitiator is diphenyl(2,4,6-trimethoxybenzoyl)-phosphine oxide.

[0083] The coupling agent is propyltriethoxysilane 3-isocyanate.

[0084] The specific preparation method is as follows:

[0085] The following parts by weight of trimethylolpropane triacrylate (40 parts), epoxy acrylate (25 parts), butyl acrylate (25 parts), and 2-hydroxyethyl acrylate (10 parts) were added sequentially to a reaction vessel and stirred under inert gas protection. After stirring until homogeneous, UV irradiation was performed to obtain the target acrylate oligomer.

[0086] First, add the photoinitiator (5 parts) to the reactor. Then, add the following components in the following proportions: compound A1 prepared in Preparation Example 1: 35 parts, acrylate oligomer: 30 parts, polyurethane modified acrylate prepared in Preparation Example 2: 15 parts, diluent monomer bisphenol S methacrylate: 12 parts, antioxidant: 1 part, coupling agent: 2 parts. Stir thoroughly in the dark at room temperature until homogeneous, and then let stand to obtain UV-curable adhesive.

[0087] Example 2

[0088] The difference from Example 1 is that compound A1 is replaced with A2.

[0089] Comparative Example 1

[0090] The UV-curable adhesive of this invention has the following composition:

[0091] Compound C: 35 parts

[0092] Acrylic ester oligomers: 30 parts

[0093] Polyurethane modified acrylate: 15 parts

[0094] Diluent monomer: 12 parts

[0095] Antioxidant: 1 part

[0096] Photoinitiator: 5 parts

[0097] Coupling agent: 2 parts

[0098] The acrylate oligomers are prepared from the following components in parts by weight:

[0099] Trimethylolpropane triacrylate: 40 parts;

[0100] Epoxy acrylate: 25 parts;

[0101] Butyl acrylate: 25 parts;

[0102] 2-Hydroxyethyl acrylate: 10 parts.

[0103] The antioxidant is tris(2,4-di-tert-butylphenyl) phosphite.

[0104] The photoinitiator is diphenyl(2,4,6-trimethoxybenzoyl)-phosphine oxide.

[0105] The coupling agent is propyltriethoxysilane 3-isocyanate.

[0106] The diluent monomer is bisphenol S methacrylate.

[0107] The specific preparation method is as follows:

[0108] The following parts by weight of trimethylolpropane triacrylate (40 parts), epoxy acrylate (25 parts), butyl acrylate (25 parts), and 2-hydroxyethyl acrylate (10 parts) were added sequentially to a reaction vessel and stirred under inert gas protection. After stirring until homogeneous, UV irradiation was performed to obtain the target acrylate oligomer.

[0109] First, add the photoinitiator (5 parts) to the reaction vessel, and then add the following components in the following proportions: compound C obtained in Preparation Example 4: 35 parts, acrylate oligomer: 30 parts, polyurethane modified acrylate obtained in Preparation Example 2: 15 parts, diluent monomer bisphenol S methacrylate: 12 parts, antioxidant: 1 part, coupling agent: 2 parts. Then, stir thoroughly in the dark at room temperature until uniform, and let stand to obtain UV-curable adhesive.

[0110] Comparative Example 2

[0111] The UV-curable adhesive of this invention has the following composition:

[0112] Compound A1: 35 parts

[0113] Acrylic ester oligomers: 30 parts

[0114] Acrylate: 15 parts

[0115] Diluent monomer: 12 parts

[0116] Antioxidant: 1 part

[0117] Photoinitiator: 5 parts

[0118] Coupling agent: 2 parts

[0119] The acrylate oligomers are prepared from the following components in parts by weight:

[0120] Trimethylolpropane triacrylate: 40 parts;

[0121] Epoxy acrylate: 25 parts;

[0122] Butyl acrylate: 25 parts;

[0123] 2-Hydroxyethyl acrylate: 10 parts.

[0124] The antioxidant is tris(2,4-di-tert-butylphenyl) phosphite.

[0125] The photoinitiator is diphenyl(2,4,6-trimethoxybenzoyl)-phosphine oxide.

[0126] The coupling agent is propyltriethoxysilane 3-isocyanate.

[0127] The diluent monomer is bisphenol S methacrylate.

[0128] The specific preparation method is as follows:

[0129] The following parts by weight of trimethylolpropane triacrylate (40 parts), epoxy acrylate (25 parts), butyl acrylate (25 parts), and 2-hydroxyethyl acrylate (10 parts) were added sequentially to a reaction vessel and stirred under inert gas protection. After stirring until homogeneous, UV irradiation was performed to obtain the target acrylate oligomer.

[0130] First, add the photoinitiator (5 parts in proportion) to the reaction vessel. Then, add the following components in the following proportions: compound A1 prepared in Preparation Example 1: 35 parts, acrylate oligomer: 30 parts, acrylate: 15 parts, diluent monomer bisphenol S methacrylate: 12 parts, antioxidant: 1 part, coupling agent: 2 parts. Stir thoroughly in the dark at room temperature until homogeneous, and then let stand to obtain UV-curable adhesive.

[0131] Comparative Example 3

[0132] The UV-curable adhesive of this invention has the following composition:

[0133] Compound A1: 35 parts

[0134] Polyurethane modified acrylate: 45 parts

[0135] Diluent monomer: 12 parts

[0136] Antioxidant: 1 part

[0137] Photoinitiator: 5 parts

[0138] Coupling agent: 2 parts

[0139] in,

[0140] The antioxidant is tris(2,4-di-tert-butylphenyl) phosphite.

[0141] The photoinitiator is diphenyl(2,4,6-trimethoxybenzoyl)-phosphine oxide.

[0142] The coupling agent is propyltriethoxysilane 3-isocyanate.

[0143] The diluent monomer is bisphenol S methacrylate.

[0144] The specific preparation method is as follows:

[0145] First, add the photoinitiator (5 parts in proportion) to the reactor. Then, add the following components in the following proportions: compound A1 obtained in Preparation Example 1: 35 parts; polyurethane modified acrylate obtained in Preparation Example 2: 45 parts; diluent monomer bisphenol S methacrylate: 12 parts; antioxidant: 1 part; coupling agent: 2 parts. Stir thoroughly in the dark at room temperature until homogeneous, and then let stand to obtain UV-curable adhesive.

[0146] Performance Evaluation

[0147] Preparation of Brightening Film

[0148] The molding process is mainly divided into two steps: coating and curing. First, as the PET substrate moves forward, UV adhesive is evenly applied to the surface of the PET substrate by the coating rod. Second, under the irradiation of the UV lamp, the roller with the microprism structure cures the microstructure on the PET substrate coated with adhesive and forms it on the surface of the film. After demolding, the target structure brightening film can be obtained.

[0149] Performance testing of brightening film

[0150] The refractive index of the adhesive was measured at 25°C using an ATAGO NAR-1T solid refractometer.

[0151] Brightness (Cd / m) 2 Each prism film was fixed on the backlight unit of the 17-inch LCD screen, and then the brightness was measured at 25 points and 9 points on the LCD screen using a luminance photometer (model: BM-7, Topcon, Japan) to calculate the average value.

[0152] The quality of the film's formation can be judged primarily by observing whether there are any abnormal sounds during demolding;

[0153] The cross-cut test involves using a cross-cutting tool to evenly cut squares of a specific size on the film surface. The degree of adhesion of the coating to the substrate is rated based on the integrity of the coating within the squares, with 5B being the highest grade, indicating that the edges of the cuts are completely smooth and there is no peeling at the edges of the squares. Grades from 4B to 0B follow the same pattern.

[0154] Abrasion resistance (g): Each composition was coated onto a clear PET base film and cured. The cured prismatic layer was then flipped over to contact the opposite glass surface. A counterweight of up to 500g was placed on it and moved back and forth 10 times at a distance of 10cm. The weight of the counterweight was then measured at the point where the prismatic layer began to be damaged.

[0155] Release properties: The processability of each UV-cured resin composition when placed between a prism-shaped metal mold and a polyester base film to form a laminate, and then the base film is peeled off from the metal mold, is expressed as a releasing sound on a scale of 0 to 10. Here, 10 is defined as excellent release performance.

[0156] The performance parameters of the brightening films in the examples and comparative examples are shown in Table 1:

[0157] Table 1

[0158]

[0159] As shown in Table 1, the brightness enhancement films prepared according to Examples 1 and 2 have significantly higher refractive indices and improved brightness compared to the brightness enhancement films prepared in Comparative Examples 1-3. Furthermore, while the refractive index and brightness are improved, other properties also exhibit better performance. Moreover, a comparison between Examples 1 and 2 shows that the length of n also affects the refractive index and brightness.

[0160] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A light-curing adhesive, characterized in that, The UV-curable adhesive comprises the following components by weight: Compound A: 25-35 parts Acrylic ester oligomers: 30-45 parts Polyurethane modified acrylate: 10-15 parts Diluent monomer: 10-15 parts Antioxidant: 0.1-2 parts Photoinitiator: 2-5 parts Coupling agent: 0.1-2 parts The structural formula of compound A is as follows: The structural formula of compound A is as follows: (Formula I), Where R is n is an integer selected from 1 to 5.

2. The light-curing adhesive according to claim 1, characterized in that, The acrylate oligomers are prepared from the following components in parts by weight: Trimethylolpropane triacrylate: 30-40 parts; Epoxy acrylate: 20-30 parts; Butyl acrylate: 20-30 parts; 2-Hydroxyethyl acrylate: 10-15 parts.

3. The light-curing adhesive according to claim 1, characterized in that, The antioxidant is selected from tris(2,4-di-tert-butylphenyl) phosphite and / or dodecayl thiodipropionate.

4. The light-curing adhesive according to claim 1, characterized in that, The photoinitiator is selected from one or a combination of two of diphenyl(2,4,6-trimethoxybenzoyl)-phosphine oxide or 1-hydroxycyclohexylphenyl ketone.

5. The light-curing adhesive according to claim 1, characterized in that, The coupling agent is an isocyanate coupling agent, selected from one or more of 3-propyl isocyanatetriethoxysilane, 3-isocyanatepropyltrimethoxysilane, and 3-isocyanatepropylmethyldimethoxysilane.

6. The light-curing adhesive according to claim 1, characterized in that, The diluent monomer is a sulfur-containing acrylate, which is selected from: bisphenol S methacrylate, bisphenol S epoxy methacrylate, bisphenol S bifunctional methacrylate, 4,4'-dimercaptodiphenyl sulfide dimethacrylate or 4,4'-dimethacryloyloxydiphenyl sulfone.

7. A method for preparing the light-curing adhesive according to any one of claims 1-6, characterized in that, Add the photoinitiator to the reaction vessel, and then add compound A, acrylate oligomer, polyurethane modified acrylate, diluent monomer, antioxidant, and coupling agent in the following proportions. Stir thoroughly in the dark at room temperature until homogeneous, and then let stand to obtain the light-curing adhesive.

8. The method according to claim 7, characterized in that, The method for preparing the acrylate oligomer is as follows: Trimethylolpropane triacrylate, epoxy acrylate, butyl acrylate, and 2-hydroxyethyl acrylate are added sequentially to a reaction vessel, stirred under inert gas protection, and after being stirred evenly, subjected to ultraviolet light irradiation to obtain the target acrylate oligomer.

9. The method according to claim 7, characterized in that, The preparation of the polyurethane-modified acrylate includes the following steps: (1) Add diol dropwise to diisocyanate, heat to 60℃ and react. After the reaction is complete, product 1 is obtained. (2) Under light-protected conditions, ethanolamine was slowly added dropwise to the acrylate monomer, and the temperature was increased to react. After the reaction was complete, product 2 was obtained. (3) Under argon protection and light-proof conditions, product 1 is added dropwise to product 2 and the temperature is raised to 60°C to react. After the reaction, the polyurethane modified acrylate resin is obtained.

10. A brightness enhancement film, characterized in that, It is prepared from the light-curing adhesive according to any one of claims 1-6 or the light-curing adhesive prepared by any one of claims 7-9.

Citation Information

Patent Citations

  • Bisphenol having fluorene skeleton and production method thereof, polyarylate resin derived from said bisphenol, (METH)acrylate compound and epoxy resin

    CN108602744A

  • Glue for brightening film

    CN109722198A