Anti-bonding production process for cold-rolled thin-gauge strip steel

By adjusting the parameters of the emulsion, hood annealing and skin-pass mill, the production process of cold-rolled thin-gauge strip was optimized, the problem of interlayer adhesion of the strip was solved, and product quality and production efficiency were improved.

CN120619052APending Publication Date: 2025-09-12XINJIANG BAYI IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511015043.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-23
Publication Date
2025-09-12

AI Technical Summary

Technical Problem

During the production process of cold-rolled thin strip steel, improper rolling process parameters and insufficient lubrication performance of the emulsion cause interlayer adhesion of the strip steel, which affects product quality and production efficiency.

Method used

Adjust emulsion parameters, hood annealing parameters and skin-pass mill elongation parameters, including emulsion composition and concentration, cooling rate, tension control, etc., to optimize lubrication and cooling effects, reduce friction and thermal stress, and improve strip surface and plate shape.

Benefits of technology

Effectively reduce strip adhesion, improve product qualification rate, reduce energy consumption, ensure dimensional accuracy and plate shape stability, and reduce equipment damage and unplanned downtime.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 5HKWFZLZKVV34XVIL1EQL67RLYUGEZW7LNYHHEOV
    Figure 5HKWFZLZKVV34XVIL1EQL67RLYUGEZW7LNYHHEOV
  • Figure YBRMN7QJROCZEFEY3B48UYIVWM6NI34MNS53EFVL
    Figure YBRMN7QJROCZEFEY3B48UYIVWM6NI34MNS53EFVL
Patent Text Reader

Abstract

The invention belongs to the technical field of cold-rolled thin-gauge strip steel production, and particularly discloses a cold-rolled thin-gauge strip steel anti-bonding production process which comprises the following steps: adjusting emulsion parameters: controlling the emulsion concentration to be 1.5-2.2%, the saponification value to be 120-170mgKOH / g, the iron content to be less than or equal to 380ppm and the chloride ion content to be 0.5-28mg / l; cover annealing parameters are adjusted, specifically, the cooling rate is controlled in different temperature zones in a stepped slow cooling mode, and the heating time, the heat preservation time and the cooling time of the strip steel are adjusted according to the actual charging amount; the annealing cold blowing flow is controlled to be 80-120 m / h, the oxygen content is smaller than 0.1%, the hot blowing flow is controlled to be 120-150 m / h, and the hydrogen concentration is larger than or equal to 98%; the tension weight is adjusted in real time according to the thickness of the strip steel and the target elongation; when thin-specification strip steel is produced, adhesion between the strip steel is reduced by adjusting emulsion parameters, cover annealing parameters and temper mill elongation parameters; the problem that in an existing cold-rolled thin-gauge strip steel production process, strip steel interlayer bonding is caused by improper rolling process parameters and insufficient emulsion lubricating performance is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cold-rolled thin-gauge strip steel production, and in particular to an anti-sticking production process for cold-rolled thin-gauge strip steel. Background Art

[0002] The cold-rolled thin-gauge strip process includes: hot rolling and coiling - pickling - lubricated cold rolling - hood annealing - annealing and purging - temper rolling - surface treatment - slitting and coiling. Prior to cold rolling, the raw material is pickled and then gradually thinned to the target thickness through multiple cold rolling passes. Cold rolling utilizes high-precision rolling force and tension control, along with emulsion lubrication and cooling. Intermediate annealing then eliminates work hardening, and surface cleaning and temper rolling improve performance. Finally, the strip is slit and oiled for delivery as coils. Strip sticking refers to the partial or complete adhesion of adjacent strip layers during cold rolling or annealing due to factors such as excessive coiling tension, high annealing temperatures, or residual rolling oil or impurities on the surface. This can manifest as surface damage, flaking, or abnormal mechanical properties during separation, severely impacting product quality and subsequent processing.

[0003] When the strip steel sticks, it will cause sudden breakage during the uncoiling or rolling process, which may damage key equipment components such as rollers and guide devices, increase the frequency of unplanned maintenance shutdowns, and seriously affect production efficiency; the sticky strip steel will cause uneven thickness and plate shape defects of the strip steel, interfere with the automatic control system of the rolling mill, cause tension fluctuations and deviation, and cause the finished product size tolerance to exceed the standard, which cannot meet the requirements of high-end applications; dealing with bonding defects requires additional processes such as manual coiling and surface grinding, while the scrap rate and energy loss increase, which directly pushes up production costs and weakens the product's market competitiveness.

[0004] The main causes of strip sticking during production include: improper rolling process parameters leading to localized temperature rise and lubricant film breakdown; emulsion lubrication failure or contamination leading to metal-to-metal friction; low material hardness and surface defects exacerbating the sticking effect; and excessive interlayer pressure during coiling, causing microscopic adhesion. Improper rolling process parameters include excessively fast annealing cooling rates and excessive fluctuations in flattening elongation. Summary of the Invention

[0005] The purpose of the present invention is to provide a production process for preventing adhesion of cold-rolled thin-gauge strip steel, so as to solve the problem of interlayer adhesion of strip steel caused by improper rolling process parameters and insufficient lubrication performance of emulsion in the existing cold-rolled thin-gauge strip steel production process.

[0006] To achieve the above objectives, the present invention provides a basic solution: a production process for preventing adhesion of cold-rolled thin-gauge steel strip, including adjusting emulsion parameters, bell annealing parameters, and skin-pass mill elongation parameters. The specific contents are as follows: Adjust the emulsion parameters: the emulsion concentration should be 1.5-2.2%, the saponification value should be 120-170 mgKOH / g, the iron content should be ≤380 ppm, and the chloride ion content should be 0.5-28 mg / l. Adjust the bell annealing parameters: Use the step-by-step slow cooling method to control the cooling rate in different temperature zones, and adjust the strip heating, insulation and cooling time according to the actual furnace load; during annealing purge, control the cold blow flow rate to 80-120m 3 / h, oxygen content <0.1%, control hot blowing flow rate 120-150m 3 / h, hydrogen concentration ≥98%; Adjust skin-pass mill elongation parameters: Adjust tension weights in real time based on strip thickness and target elongation.

[0007] The principles and beneficial effects of the present invention are as follows: adjusting the emulsion parameters will affect the rolling lubrication and cooling effects, reduce the friction between the rollers and the strip, and also reduce uneven deformation and defects such as edge waves and middle waves during the rolling process; controlling the hood annealing parameters can control surface oxidation and decarburization, ensure that the surface of the strip is bright and clean after annealing, eliminate cold rolling hardening, and improve deep drawing performance; adjusting the elongation parameters of the leveling mill can improve the plate shape of the strip, eliminate the yield platform, improve dimensional accuracy and surface finish, control residual stress, reduce the risk of deformation or cracking during subsequent processing, and can also adjust the mechanical properties to meet the needs of different uses. When producing thin-gauge strip, the adhesion between the strips can be reduced by adjusting the three process parameters of emulsion parameters, hood annealing parameters and leveling mill elongation parameters.

[0008] Option 2 is the preferred option of the basic option. The emulsion composition is: 42-55% synthetic ester, 22-38% natural oil, 15-21% lubricating additive, 8-9.5% emulsifier, 7-7.5% stabilizer, 2-4.5% anti-rust additive, 1-2% annealing cleaning agent and 1-2.7% others. The pH value is 8.5-9.06, and the temperature and particle size of the emulsion are adjusted. The optimized emulsion composition can improve the lubrication and cooling efficiency of the rolling process, reduce the friction between the rollers and the strip, avoid surface scratches and thermal stress deformation, thereby ensuring the dimensional accuracy and plate shape stability of the strip. By precisely controlling the concentration, pH value and additive ratio of the emulsion, it can adapt to the needs of different steel grades and rolling processes. Good emulsion stability can effectively prevent oil film rupture or impurity deposition, reduce surface residue after rolling, provide a clean substrate for subsequent annealing process, and reduce the risk of adhesion.

[0009] Option 3 is the preferred option of Option 2. The temperature of the emulsion is controlled at 55-60°C, and the proportion of particles with a size of <1μm is 90%. By precisely controlling the temperature of the emulsion within the range of 55-60°C, its lubrication performance can be optimized, promoting the rolling oil film to evenly cover the surface of the strip, effectively reducing post-rolling residue, and avoiding the carbonization of residual oil stains during annealing to form a bonding medium. Refining the emulsion particle size to below 1μm can reduce the mechanical pressure of coarse particles on the strip surface, prevent direct metal contact caused by local oil film rupture, eliminate the inducing conditions of interlayer micro-welding from the source, reduce bonding caused by surface contamination or microscopic unevenness, and improve product qualification rate.

[0010] Option 4 is the preferred option of the basic option. The stepped slow cooling is divided into temperature intervals of 600℃. When the temperature zone is above 600℃, the cooling rate is controlled to be ≤‌25℃ / h; when the temperature zone is below 600℃, the cooling rate is controlled to be ≥80℃ / h. The heating time, holding time, cooling time before hood and furnace discharge temperature are adjusted according to the actual furnace load. A slower cooling rate is adopted in the high-temperature zone to promote the uniform release of residual stress on the strip surface and avoid local deformation differences caused by rapid cooling. The cooling is slowed down again in the low-temperature zone to reduce phase transformation stress concentration. This segmented control strategy can improve the contact state between strip layers and avoid microscopic adhesion caused by uneven shrinkage or thermal stress concentration. At the same time, with the cooperation of the protective atmosphere, oxidation and carbon deposition can be further reduced, thereby reducing strip adhesion.

[0011] Scheme 5 is the preferred option of Scheme 4. When the initial charge is 55-65t, the heating temperature is controlled to be 690℃, the heating time is 9h, the holding temperature is 620℃, the holding time is 2h, the cooling time before hood is 3h, and the discharge temperature is 95℃. For every 10t increase in charge, the holding time increases by 0.5h, and the heating and discharge temperatures increase by 5℃. For 55-75t, the heating time is 9h, and the cooling time before hood is 3h. For 75-90t, the heating time is 10h, and for every 10t increase in charge, the cooling time before hood is increased by 0.5h. Different charging capacities correspond to different heating temperatures, heating times, holding temperatures, holding times, cooling times before hood and discharge temperatures. When the charging capacity is large, the heating rate is reduced to avoid excessive temperature difference between the surface and the core. The rolling stress is fully eliminated and the structure is uniform during the holding stage. Step-by-step cooling reduces thermal stress concentration. The final discharge temperature is controlled to avoid carbonization of residual oil stains. This differentiated process design can not only ensure the recrystallization effect and mechanical property consistency of the strip under different furnace loadings, but also reduce the micro-diffusion and oxidation adhesion of the interlayer contact surface through precise thermodynamic control, thereby significantly reducing the bonding defect rate.

[0012] Option 6 is the preferred basic option. When the thickness is 0.28-0.33mm, the tension weight is 0.057-0.767, and the target elongation is 0.45-0.55%. The rolling tension is dynamically adjusted according to the thickness of the strip. Lower tension can avoid microscopic surface tearing caused by excessive stretching of ultra-thin strips and reduce mechanical bite between layers. At the same time, precise tension control can ensure stable transmission of the strip between the rolls, eliminate local wrinkles or stress concentration caused by tension fluctuations, and thus maintain the surface integrity of the strip. It not only prevents surface damage caused by uneven tension during rolling, but also provides a uniform substrate state for the subsequent annealing process, reducing interlayer bonding caused by surface defects or residual stress.

[0013] Option 7, which is the preferred option of the basic option, adjusts the tension weight according to the strip thickness as follows: , where K T is the tension weight, and H is the strip thickness. Through actual production, the relationship between the thickness and tension weight of thin-gauge strip steel is obtained, which can ensure the stable transmission of the strip steel between the rolls, reduce the surface damage caused by uneven tension during rolling, and reduce the interlayer bonding induced by residual stress. DETAILED DESCRIPTION

[0014] The present invention will be further described in detail below through specific embodiments: Example A production process for preventing cold-rolled thin-gauge steel strip from sticking includes adjusting emulsion parameters, bell annealing parameters, and skin-pass mill elongation parameters. The specific contents are as follows: Adjust emulsion parameters: emulsion composition: 42-55% synthetic ester, 22-38% natural oil, 15-21% lubricating additive, 8-9.5% emulsifier, 7-7.5% stabilizer, 2-4.5% anti-rust additive, 1-2% annealing cleaning agent, and 1-2.7% others; pH value: 8.5-9.06; emulsion concentration: 1.5-2.2%; saponification value: 120-170 mgKOH / g; iron content: ≤380 ppm; chloride ion content: 0.5-28 mg / l; adjust emulsion temperature and particle size; emulsion temperature: 55-60°C; particle size: <1 μm: 90%; Adjust the bell annealing parameters: Use the step-by-step cooling method to control the cooling rate in different temperature zones. The step-by-step cooling is divided into temperature intervals of 600℃. When the temperature zone is above 600℃, the cooling rate is controlled to be ≤25℃ / h; when the temperature zone is below 600℃, the cooling rate is controlled to be ≥80℃ / h. Adjust the heating time, holding time, bell cooling time and furnace discharge temperature according to the actual furnace load. When the initial furnace load is 55-65t, control the heating temperature to 690℃, the heating time to 9h, and the holding time to 9h. The temperature is 620℃, the holding time is 2h, the cooling time before hood is 3h, the furnace discharge temperature is 95℃, and for every 10t increase in furnace load, the holding time increases by 0.5h, and the heating temperature and furnace discharge temperature increase by 5℃; for a furnace load of 55-75t, the heating time is 9h, and the cooling time before hood is 3h; for a furnace load of 75-90t, the heating time is 10h, and for every 10t increase in furnace load, the cooling time before hood is increased by 0.5h; during annealing purge, control the cold blow flow rate to 80-120m 3 / h, oxygen content <0.1%, control hot blowing flow rate 120-150m 3 / h, hydrogen concentration ≥98%; Adjust the elongation parameters of the skin-pass mill: adjust the tension weight in real time according to the strip thickness and target elongation. When the thickness is 0.28-0.33mm, the tension weight is 0.057-0.767, and the target elongation is 0.45-0.55%. The formula for adjusting the tension weight according to the strip thickness is: , where K T is the tension weight, and H is the strip thickness.

[0015] The implementation method of this embodiment is as follows: before rolling, the emulsion components are first prepared, and the emulsion components are: 42-55% synthetic ester, 22-38% natural oil, 15-21% lubricating additive, 8-9.5% emulsifier, 7-7.5% stabilizer, 2-4.5% rust inhibitor, 1-2% annealing cleaning agent and 1-2.7% others. The pH value of the emulsion is controlled to be 8.5-9.06, the concentration is 1.5-2.2%, the saponification value is 120-170 mgKOH / g, the iron content is ‌≤380 ppm, the chloride ion content is 0.5-28 mg / l, the temperature of the emulsion is controlled to be 55-60°C, and the proportion of particle size <1μm is 90%.

[0016] Cold rolling adopts multiple rolling passes to reduce the thickness of the strip. After cold rolling, hood annealing is used. During annealing, the cooling rate is controlled in different temperature zones by step-by-step slow cooling. The step-by-step slow cooling uses 600℃ as the temperature interval. When the temperature zone is above 600℃, the cooling rate is controlled to be ≤25℃ / h; when the temperature zone is below 600℃, the cooling rate is controlled to be ≥80℃ / h. The heating time, holding time, hood cooling time and furnace discharge temperature are adjusted according to the actual furnace load. When the initial furnace load is 55-65t, the heating temperature is controlled to be 690℃, the heating time is 9h, and the holding temperature is 62 0℃, holding time is 2h, cooling time before hood is 3h, and the discharge temperature is 95℃. For every 10t increase in the load, the holding time increases by 0.5h, and the heating temperature and discharge temperature increase by 5℃; for a load of 55-75t, the heating time is 9h, and the cooling time before hood is 3h; for a load of 75-90t, the heating time is 10h, and for every 10t increase in the load, the cooling time before hood increases by 0.5h; the specific heating temperature, heating time, holding temperature, holding time, cooling time before hood and discharge temperature corresponding to different loads are shown in Table 1 below: Table 1 Different annealing parameters corresponding to different furnace loadings During annealing and purging of the bell-type annealing furnace entrance section and the protective gas circulation system in the furnace, control the cold blowing flow rate to 80-120m 3 / h, oxygen content <0.1%, control hot blowing flow rate 120-150m 3 / h, hydrogen concentration ≥98%.

[0017] After annealing, temper rolling is performed. The target elongation during rolling is 0.45-0.55%. When the thickness is 0.28-0.33 mm, the tension weight is 0.057-0.767. The formula for adjusting the tension weight according to the strip thickness is: , where K T is the tension weight, and H is the strip thickness. The conventional process and the optimized process are compared in terms of the incidence of strip adhesion, energy consumption per ton of steel, rolling accuracy, and finished product qualification rate. The comparison results are shown in Table 2 below: Table 2 Comparison of traditional process and optimized process The above is only an embodiment of the present invention, and the common knowledge such as the specific structure and characteristics of the scheme is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the structure of the present invention, several variations and improvements can be made, which should also be regarded as the scope of protection of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A production process for preventing adhesion of cold-rolled thin-gauge steel strip, characterized in that: Including adjusting the emulsion parameters, hood annealing parameters and skin pass mill elongation parameters, the specific contents are as follows: Adjust the emulsion parameters: the emulsion concentration should be 1.5-2.2%, the saponification value should be 120-170 mgKOH / g, the iron content should be ≤380 ppm, and the chloride ion content should be 0.5-28 mg / l. Adjust the bell annealing parameters: Use the step-by-step slow cooling method to control the cooling rate in different temperature zones, and adjust the strip heating, insulation and cooling time according to the actual furnace load; during annealing purge, control the cold blow flow rate to 80-120m 3 / h, oxygen content <0.1%, control hot blowing flow rate 120-150m 3 / h, hydrogen concentration ≥98%; Adjust skin-pass mill elongation parameters: Adjust tension weights in real time based on strip thickness and target elongation.

2. The anti-sticking production process for cold-rolled thin-gauge steel strip according to claim 1, characterized in that: The emulsion composition is: 42-55% synthetic ester, 22-38% natural oil, 15-21% lubricating additive, 8-9.5% emulsifier, 7-7.5% stabilizer, 2-4.5% anti-rust additive, 1-2% annealing cleaning agent and 1-2.7% others. The pH value is 8.5-9.

06. The temperature and particle size of the emulsion are adjusted.

3. The anti-sticking production process for cold-rolled thin-gauge steel strip according to claim 2, characterized in that: The temperature of the emulsion is controlled at 55-60°C, and the proportion of particle size <1μm is 90%.

4. The anti-sticking production process for cold-rolled thin-gauge steel strip according to claim 1, characterized in that: Step slow cooling uses 600℃ as the temperature interval. When the temperature is above 600℃, the cooling rate is controlled to be ≤25℃ / h. When the temperature is below 600℃, control the cooling rate to ≥80℃ / h, and adjust the heating time, holding time, cooling time before hood and furnace temperature according to the actual furnace load.

5. The anti-sticking production process for cold-rolled thin-gauge steel strip according to claim 4, characterized in that: When the initial load is 55-65t, the heating temperature is controlled at 690℃, the heating time is 9h, the holding temperature is 620℃, the holding time is 2h, the cooling time is 3h, and the discharge temperature is 95℃. For every 10t increase in load, the holding time increases by 0.5h, and the heating and discharge temperatures increase by 5℃. The furnace capacity is 55-75t, the heating time is 9h, and the cooling time before hood is 3h; The loading capacity is 75-90t, the heating time is 10h, and the hood cooling time increases by 0.5h for every 10t increase in loading capacity.

6. The anti-sticking production process for cold-rolled thin-gauge steel strip according to claim 1, characterized in that: When the thickness is 0.28-0.33mm, the tension weight is 0.057-0.767 and the target elongation is 0.45-0.55%.

7. The anti-sticking production process for cold-rolled thin-gauge steel strip according to claim 6, characterized in that: The formula for adjusting the tension weight according to the strip thickness is: , where K T is the tension weight, and H is the strip thickness.