ITO (Indium Tin Oxide) etching solution as well as preparation method and application thereof

By using an ITO etching solution containing organic acid, surfactant, polymer additive and ultrapure water, the problems of ITO layer residue and particle precipitation when etching ITO-Ag-ITO structure with traditional ITO etching solution are solved, achieving efficient and stable ITO layer etching, and improving process yield and product performance.

CN120665600APending Publication Date: 2025-09-19ZHEJIANG AUFIRST MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510742996.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-06-05
Publication Date
2025-09-19

AI Technical Summary

Technical Problem

Traditional ITO etching solutions have problems such as residual ITO layer, long etching time and severe granular precipitation when etching ITO-Ag-ITO structures, especially during the etching process of high-thickness ITO layers.

Method used

An ITO etchant containing an organic acid, surfactant, polymer additive, and ultrapure water is used to achieve stable etching of ITO-Ag-ITO by optimizing the component ratios and process parameters. This etchant is particularly suitable for etching the ITO layer in the third step of the three-step ITO-Ag-ITO etching process, effectively eliminating residual ITO layers.

Benefits of technology

It significantly improves the etching efficiency and product performance of the ITO layer, reduces the etching time, avoids the residue and precipitation of ITO particles, and improves the process yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120665600A_ABST
    Figure CN120665600A_ABST
Patent Text Reader

Abstract

The invention provides an ITO (Indium Tin Oxide) etching solution as well as a preparation method and application thereof. The ITO etching solution comprises the following components in parts by weight: 1-8 parts of organic acid; 0.1 to 2 parts of a surfactant; 0.6-8 parts of a polymer additive; 50 to 100 parts of ultrapure water; the polymer additive is a mixture of a multi-carboxyl polymer and a multi-nitrogen polymer, and the mass ratio of the multi-carboxyl polymer to the multi-nitrogen polymer is (0.1-5): (0.5-3). The invention further discloses a preparation method and application of the ITO etching solution. The ITO etching solution provided by the invention has a stable etching rate for ITO-Ag-ITO, and has no damage to an insulating layer and a photoresist. The ITO etching liquid is particularly suitable for an OLED pixel electrode manufacturing process, and is used for third-step ITO etching of three-step ITO-Ag-ITO etching, so that residues of an ITO layer can be effectively eliminated, and the process yield and the product performance can be remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to etching liquid technology, in particular to an ITO etching liquid, a preparation method and application thereof. Background Art

[0002] ITO-Ag-ITO etching solutions are commonly used to etch pixel electrodes in the manufacturing of liquid crystal displays (TFT-LCDs) and organic light-emitting diodes (OLEDs). Currently, commercial ITO-Ag-ITO etching methods can be categorized into one-step, two-step, and three-step methods based on their process steps.

[0003] The currently common three-step ITO-Ag-ITO etching process divides the etching process into three steps: the upper and lower ITO layers are etched with ITO etchant, and the middle Ag layer (the very small amount of residual ITO) is etched with Ag etchant. This three-layer etching process allows for individual adjustment of process parameters in each step, enabling more precise morphology control.

[0004] In the three-step etching process, aqueous oxalic acid is often used to achieve the first / third step of ITO etching. Its advantage is that oxalic acid is a weak acid that can react with ITO to form metal oxalate and water, and it is difficult to react with Ag.

[0005] Studies have shown that In2O3 dissolves faster in oxalic acid because it forms soluble complexes such as [In(C2O4)2] - The specific reactions are as follows:

[0006] In2O3+3H2C2O4→In2(C2O4)3+3H2O

[0007] In contrast, the dissolution rate of SnO2 is significantly slower. In theory, SnO2 may react to form tin oxalate (Sn(C2O4)2), but studies have shown that this compound has low solubility and poor reaction kinetics, making it difficult for SnO2 to completely dissolve. Residual SnO2 may also become a nucleation site / electron donor for the precipitation of In ions, so ITO particles are likely to remain when treated with oxalic acid aqueous solution. Summary of the Invention

[0008] The present invention aims to address the problems of ITO-Ag-ITO etching with conventional ITO etching solutions, such as residual ITO layer, long etching times for thick ITO layers, and severe granular precipitation. The invention proposes an ITO etching solution that exhibits a stable etching rate for ITO-Ag-ITO and does not damage either the insulating layer or the photoresist. The ITO etching solution is particularly suitable for use in the third step of a three-step ITO-Ag-ITO etching process, effectively eliminating residual ITO layer and significantly improving process yield and product performance.

[0009] It should be noted that, in the present invention, unless otherwise specified, the specific meaning of "including" in relation to composition limitations and descriptions includes both open-ended "including", "comprising", etc. and similar meanings, as well as closed-ended "composed of", "composed of", etc. and similar meanings.

[0010] To achieve the above object, the technical solution adopted by the present invention is: an ITO etching solution comprising the following components in the following weight proportions:

[0011] 1-8 parts of organic acid;

[0012] 0.1-2 parts of surfactant;

[0013] 0.6-8 parts of polymer additives;

[0014] 50-100 parts of ultrapure water;

[0015] The polymer additive is a mixture of a polycarboxyl polymer and a polynitrogen polymer.

[0016] Furthermore, the organic acid is one or more of acetic acid, citric acid, tartaric acid, oxalic acid, glycolic acid, ascorbic acid, nitrosulfuric acid, trichloroacetic acid and trinitrobenzenesulfonic acid.

[0017] Furthermore, the organic acid is preferably a mixture of oxalic acid and tartaric acid.

[0018] Furthermore, the mass ratio of the oxalic acid to the tartaric acid is 0.5-5:0.5-3.

[0019] Furthermore, the preferred mass ratio of the oxalic acid to the tartaric acid is 2:1.

[0020] Furthermore, the organic acid is 3-5 parts.

[0021] Furthermore, the surfactant is one or more of sodium lauryl sulfate, sodium α-olefin sulfonate, alkyl polyglucoside, sodium cocoamphoacetate and polyethylene glycol.

[0022] Furthermore, the surfactant is preferably polyethylene glycol.

[0023] Furthermore, the surfactant is more preferably polyethylene glycol 400.

[0024] Furthermore, the surfactant is 0.3-0.8 parts.

[0025] Furthermore, the mass ratio of the polycarboxyl polymer to the polynitrogen polymer is 0.1-5:0.5-3.

[0026] Furthermore, the preferred mass ratio of the polycarboxyl polymer to the polynitrogen polymer is 1-2:0.5-1.

[0027] Furthermore, the molecular weight of the polycarboxyl polymer is less than or equal to 30,000. Too large a molecular weight may easily cause solubility problems.

[0028] Furthermore, the molecular weight of the polynitrogen polymer is less than or equal to 30,000. Too large a molecular weight may easily cause solubility problems.

[0029] Furthermore, the polycarboxyl polymer is one or more of polymethacrylic acid (PMAA), polyepoxysuccinic acid (PESA), and polyaspartic acid.

[0030] Furthermore, the polycarboxyl polymer is preferably polymethacrylic acid (PMAA).

[0031] PMAA is mostly random in configuration, and its spatial structure is in the shape of a random coil, with the carboxyl group located next to the methyl group and distributed along the main chain. Due to the repulsive effect of the methyl group, the distance and orientation between the carboxyl groups are more dispersed, which can maximize the stretching on the ITO surface and increase the effective coordination area. In addition, the steric effect of the methyl group makes PMAA form a looser coordination unit during coordination, which is more suitable for metals with larger ionic radius such as In. 3+ or Sn 4+ , which promotes the dissolution of ITO grains and chelates In dissolved in the solution 3+ or Sn 4+ effect.

[0032] Furthermore, the polynitrogen polymer is one or more of polyamidoamine (PAMAM), polydiallyldimethylammonium chloride (PDADMAC) and polyhexamethylene biguanide (PHMB).

[0033] Furthermore, the polynitrogen polymer is preferably polyamidoamine (PAMAM).

[0034] The spherical structure and high density of functional groups inside PAMAM allow metal ions to be "wrapped" in its internal cavity. 3+or Sn 4+ It can destroy the stability of the ITO lattice and promote the dissolution of metal ions. PMAA increases the etching rate through surface coordination adsorption and stabilizes chelation to prevent the occurrence of residues and precipitates.

[0035] Furthermore, the polymer additive is 1.5-3 parts.

[0036] Furthermore, the ultrapure water is deionized water with a resistance of at least 18 MΩ.

[0037] Furthermore, the ultrapure water is 80-90 parts.

[0038] Another object of the present invention is to disclose a method for preparing an ITO etching solution, comprising the following steps:

[0039] Step 1: Weigh each component separately;

[0040] Step 2: Add all components into a container and stir until all components are completely dissolved to prepare an ITO etching solution.

[0041] Another object of the present invention is to disclose an application of an ITO etching solution in the field of ITO-Ag-ITO etching.

[0042] Furthermore, the ITO etching solution is particularly suitable for the third step etching of the three-step ITO-Ag-ITO etching method.

[0043] Furthermore, the method of etching ITO-Ag-ITO using the ITO etching solution is as follows:

[0044] In the first etching step, the substrate coated with the ITO-Ag-ITO composite layer is immersed in an ITO etching solution containing oxalic acid;

[0045] In the second etching step, the substrate is immersed in Ag etching solution;

[0046] The third step is etching, immersing the substrate in the ITO etching solution.

[0047] Furthermore, in the first etching step, the concentration of oxalic acid in the ITO etching solution containing oxalic acid is 3.4 wt %.

[0048] Furthermore, in the first etching step, the etching time is 40-80 seconds.

[0049] Furthermore, in the first etching step, the etching time is preferably 50-70 seconds.

[0050] Furthermore, in the first etching step, the etching temperature is 45°C.

[0051] Furthermore, in the second etching step, the etching time is 50-150s.

[0052] Furthermore, in the second etching step, the etching time is preferably 80-110 s.

[0053] Furthermore, in the second etching step, the etching temperature is 25°C.

[0054] Furthermore, in the third etching step, the etching time is 40-80s.

[0055] Furthermore, in the third etching step, the etching time is preferably 50-70s.

[0056] Furthermore, in the third etching step, the etching temperature is 45°C.

[0057] Furthermore, after the third etching step, the substrate is rinsed in ultrapure water and blown dry using nitrogen.

[0058] The ITO etching solution of the present invention, its preparation method and application have the following advantages compared with the prior art:

[0059] 1) The ITO etching solution of the present invention comprises a combination of a polycarboxyl polymer and a polynitrogen polymer. The polycarboxyl / polynitrogen polymer can adsorb In through the lone pair electrons of the carboxyl oxygen / nitrogen atoms in its structure. 3+ or Sn 4+ , improving chelation performance and promoting corrosion. As a preferred combination of the rigid linear chain of PMAA and the dendritic structure of PAMAM, the frontier orbital HOMO energy of PMAA and PAMAM is more compatible with the ITO conduction band, enhancing electron transfer; and the two maintain efficient coordination in an acidic environment, promoting the dissolution of In2O3 and SnO2, and achieving a higher etching rate than aqueous oxalic acid solution; in terms of chelation effect, the dispersed long-chain PMAA provides more chelation sites, and the more compact spatial structure of PAMAM provides stronger chelation performance. The two produce a synergistic effect and reinforce each other, which has the effect of improving the etching rate and stabilizing the dissolution of metal ions.

[0060] 2) The ITO etching solution of the present invention contains a surfactant, which can further promote the dissolution of the polymer additive and eliminate bubbles at the same time to prevent uneven etching caused by bubbles.

[0061] 3) The ITO etching solution of the present invention has a stable etching rate for ITO. For example, the ITO etching rate at 45°C is:

[0062] In summary, the ITO etching solution of the present invention has very good application prospects and large-scale industrial promotion potential in the field of display panels. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] Attachment Figure 1This is a SEM image of the cross section of the ITO layer etched with the etching solution of Comparative Example 7, magnified 20,000 times.

[0064] Attachment Figure 2 This is a SEM image of a cross section of an ITO layer etched with the etching solution of Example 1, magnified 20,000 times.

[0065] Attachment Figure 3 This is a SEM image of the surface of the ITO layer etched with the etching solution of Comparative Example 7, magnified 1000 times.

[0066] Attachment Figure 4 The EDS element analysis results of etching the ITO layer using the etching solution of Comparative Example 7 are shown.

[0067] Attachment Figure 5 This is a SEM image of the surface of the ITO layer etched with the etching solution of Example 1, magnified 1000 times.

[0068] Attachment Figure 6 The EDS element analysis results of etching the ITO layer using the etching solution of Example 1 are shown. DETAILED DESCRIPTION

[0069] The present invention will be further described below with reference to the following examples. The following description of the technical features is based on representative embodiments and specific examples of the present invention, but the present invention is not limited to these embodiments and specific examples. It should be noted that:

[0070] Unless otherwise stated, the units used in this specification are international standard units, and the numerical values ​​and numerical ranges appearing in the present invention should be understood to include the inevitable systematic errors in industrial production.

[0071] In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints A and B.

[0072] In this specification, the numerical range expressed using "above" or "below" means a numerical range including the number.

[0073] In this specification, the use of "may" includes both the meaning of performing a certain process and the meaning of not performing a certain process.

[0074] In this specification, the use of "optional" or "optional" indicates that certain substances, components, execution steps, application conditions and other factors are used or not used.

[0075] In this specification, when "normal temperature" or "room temperature" is used, the temperature may be 15-25°C.

[0076] In this manual, the reagents or instruments used without indicating the manufacturer are all conventional products that can be obtained through commercial purchase.

[0077] Examples 1-8

[0078] Examples 1-8 disclose a variety of ITO etching solutions, the components and weight ratios of which are shown in Table 1. The preparation methods thereof are as follows:

[0079] Step 1: Weigh each component separately;

[0080] Step 2: Add all components into a container and stir until all materials are completely dissolved to prepare an ITO etching solution.

[0081] Table 1 Components and ratios of etching solutions of Examples 1-8

[0082]

[0083]

[0084] Comparative Examples 1-7

[0085] Comparative Examples 1-7 disclose a variety of etching solutions, the components and weight ratios of which are shown in Table 2, and the preparation methods thereof are the same as those of Example 1.

[0086] Table 2 Components and ratios of etching solutions of Comparative Examples 1-7

[0087]

[0088]

[0089] The ITO etching solutions of Examples 1-8 and Comparative Examples 1-7 were tested, and the test methods and results are as follows:

[0090] Table 3 Test results

[0091]

[0092] Based on the performance indicators in Table 3, it can be seen that the ITO etching rate of the ITO etching solution of the present invention is high, and the ITO etching solutions of Examples 1-8 have no residue or particle precipitation. However, Comparative Example 1 lacks polymethacrylic acid, resulting in a reduced etching rate, particle precipitation, and a large amount of residue. Comparative Example 2 lacks polyamide-amine, resulting in residue / precipitation. Comparative Example 3 uses polyacrylic acid instead of polymethacrylic acid. Since polyacrylic acid does not contain a methyl group, the long chain ductility is poor, resulting in particle precipitation. Comparative Example 4 uses polyallyl sulfonic acid instead of polymethacrylic acid, resulting in a reduced etching rate. Comparative Example 5 uses polyvinyl alcohol instead of polyamide-amine, which has a weak chelating effect, resulting in a reduced etching rate and a large amount of residue. Comparative Example 6 does not add a surfactant, resulting in particle precipitation. Comparative Example 7 uses a conventional ITO etching solution containing oxalic acid, resulting in a large amount of residue and particle precipitation.

[0093] Attachment Figure 1 This is a SEM effect of a cross section of the ITO layer etched with the etching solution of Comparative Example 7 at a magnification of 20,000 times. The white layer at the bottom is the ITO that has not been completely etched. Figure 2 This is a SEM effect of a cross section of the ITO layer etched with the etching solution of Example 1 at a magnification of 20,000 times, showing that the bottom white layer is completely etched.

[0094] Attachment Figure 3 The SEM effect of etching the surface of the ITO layer with the etching solution of Comparative Example 7 at a magnification of 1000 times is shown. Figure 4 This is the EDS elemental analysis result of etching the ITO layer using the etching solution of Comparative Example 7. Combined with the elemental analysis results, it can be seen that there is an In element signal, indicating that the ITO layer is residual, and granular precipitates appear in the morphology image.

[0095] Attachment Figure 5 The SEM effect of etching the surface of the ITO layer with the etching solution of Example 1 at a magnification of 1000 times is shown. Figure 6 The EDS elemental analysis results of etching the ITO layer using the etching solution of Example 1. Combined with the elemental analysis results, it shows that there are no particles remaining on the surface after etching, and the pattern is not damaged or defective.

[0096] The performance 1CD-loss test method is:

[0097] The ITO-Ag-ITO samples were etched using the etching solutions of the above embodiments and comparative examples of the present invention, and then cleaned after etching. The specific steps are as follows:

[0098] Step 1: Immerse the substrate coated with the ITO-Ag-ITO composite layer in a 3.4 wt % oxalic acid ITO etching solution for the first etching step; the etching time is 65 s and the etching temperature is 45° C.

[0099] Step 2: Immerse the substrate after the first step of etching in an Ag etching solution for the second step of etching; the etching time is 100 s, and the etching temperature is 25°C; the Ag etching solution is an aqueous solution containing phosphoric acid, nitric acid, and acetic acid, and the mass ratio of phosphoric acid, nitric acid, and acetic acid in the aqueous solution is 40:10:8.

[0100] Step 3: Immerse the substrate after the second step of etching in the ITO etching solution of the corresponding example and perform the third step of etching; the etching time is 65s and the etching temperature is 45°C.

[0101] Step 4: Rinse the ITO-Ag-ITO substrate in ultrapure water at least twice and blow dry with nitrogen.

[0102] Step 5: After FIB ion beam cutting, observe the sample morphology under SEM and measure CD-loss.

[0103] The ultrapure water used in the above steps is deionized water with a resistance of at least 18 MΩ.

[0104] The test method for performance 2 etching rate is:

[0105] Etching was performed using the ITO etching solution of the embodiment and the comparative example, and cleaning was performed after etching. The specific steps were as follows:

[0106] Step 1: Prepare the etching solution according to the proportions in the embodiment, heat the water bath to 45°C, immerse the sample in the etching solution and shake it in a gradient of 10 seconds until the metal on the surface of the sample is completely etched;

[0107] Step 2: Rinse the sample in ultrapure water at least twice and blow dry with nitrogen.

[0108] Step 3: Measure the thickness of the sample under SEM and calculate the average etching rate.

[0109] The test method for performance 3 post-etching morphology is:

[0110] The ITO-Ag-ITO samples were etched using the etching solutions of the above embodiments and comparative examples of the present invention, and then cleaned after etching. The specific steps are as follows:

[0111] Step 1: Immerse the substrate coated with the ITO-Ag-ITO composite layer in a 3.4 wt% oxalic acid ITO etching solution for the first etching step; the etching time is 65 s and the etching temperature is 45°C.

[0112] Step 2: Immerse the substrate after the first step of etching in an Ag etching solution for the second step of etching; the etching time is 100 s, and the etching temperature is 25°C; the Ag etching solution is an aqueous solution containing phosphoric acid, nitric acid, and acetic acid, and the mass ratio of phosphoric acid, nitric acid, and acetic acid in the aqueous solution is 40:10:8.

[0113] Step 3: Immerse the substrate after the second step of etching in the ITO etching solution of the corresponding example and perform the third step of etching; the etching time is 65s and the etching temperature is 45°C.

[0114] Step 4: Observe the sample morphology under SEM and scan the elemental composition.

[0115] The ultrapure water used in the above steps is deionized water with a resistance of at least 18 MΩ.

[0116] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the above embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. An ITO etching solution, characterized in that, The composition comprises the following components in the following weight ratios: 1-8 parts of organic acid; 0.1-2 parts of surfactant; 0.6-8 parts of polymer additives; 50-100 parts of ultrapure water; The polymer additive is a mixture of a polycarboxyl polymer and a polynitrogen polymer.

2. The ITO etching solution according to claim 1, wherein The organic acid is one or more of acetic acid, citric acid, tartaric acid, oxalic acid, glycolic acid, ascorbic acid, nitrosulfuric acid, trichloroacetic acid and trinitrobenzenesulfonic acid.

3. ITO etching solution according to claim 1, characterized in that, The surfactant is one or more of sodium lauryl sulfate, sodium α-olefin sulfonate, alkyl polyglucoside, sodium cocoamphoacetate and polyethylene glycol.

4. The ITO etching solution according to claim 1, wherein The mass ratio of the polycarboxyl polymer to the polynitrogen polymer is 0.1-5:0.5-3.

5. The ITO etching solution according to claim 1 or 4, wherein The polycarboxyl polymer is one or more of polymethacrylic acid, polyepoxysuccinic acid, and polyaspartic acid; And / or, the molecular weight of the polycarboxyl polymer is less than or equal to 30,000.

6. The ITO etching solution according to claim 1 or 4, wherein The polynitrogen polymer is one or more of polyamidoamine, polydiallyldimethylammonium chloride and polyhexamethylene biguanide; And / or, the molecular weight of the polynitrogen polymer is less than or equal to 30,000.

7. A method for preparing an ITO etching solution according to any one of claims 1 to 6, characterized in that: The following steps are involved: Step 1: Weigh each component separately; Step 2: Add all components into a container and stir until all components are completely dissolved to prepare an ITO etching solution.

8. Application of the ITO etching solution according to any one of claims 1 to 6 in the field of ITO-Ag-ITO etching.

9. The application according to claim 8, characterized in that: The ITO etching solution is particularly suitable for the third step etching of the three-step ITO-Ag-ITO etching method.

10. The use according to claim 9, characterized in that: The method for etching ITO-Ag-ITO using ITO etching solution is as follows: In the first etching step, the substrate coated with the ITO-Ag-ITO composite layer is immersed in an ITO etching solution containing oxalic acid; In the second etching step, the substrate is immersed in Ag etching solution; The third step is etching, immersing the substrate in the ITO etching solution.