Processing method of antenna shell

Through the method of one-piece shell material oxidation treatment and hot pressing molding, the problems of color difference and complex process in antenna shell manufacturing are solved, and the appearance consistency and cost reduction are achieved.

CN120734671AInactive Publication Date: 2025-10-03SHENZHEN FUTAIXIN TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202511157464.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-08-19
Publication Date
2025-10-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing antenna housing manufacturing process is complex, and uneven oxidation treatment of metal parts leads to color difference, which affects the consistency of appearance and is costly.

Method used

The one-piece shell material is oxidized and combined with fillers to improve electromagnetic performance. It is fixed by hot pressing to simplify the process.

Benefits of technology

It eliminates the color difference of shell materials, improves the appearance consistency and processing efficiency, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120734671A_ABST
    Figure CN120734671A_ABST
Patent Text Reader

Abstract

The invention discloses a processing method of an antenna shell, and relates to the technical field of electronic equipment. Comprising the following steps that S1, primary machining is conducted, specifically, a metal base material is machined and formed into a shell material in a preset shape, a connecting piece is reserved on the shell material to maintain the integrity of the shell material, and a filling area is reserved; s2, oxidation treatment: carrying out oxidation treatment on the shell material; s3, a filling part is prepared, the filling part matched with the filling area is prepared, and the filling part is used for improving the electromagnetic performance of the antenna; s4, surface treatment is conducted, specifically, surface treatment is conducted on the shell material and the filling piece; and S5, forming is conducted, specifically, the connecting piece is removed, and the shell material subjected to oxidation treatment and the filling piece are combined and formed. By adopting the technical scheme, the shell material is subjected to integrated oxidation treatment, and the method has the advantages of eliminating or remarkably reducing the color difference of the shell material, improving the consistency of the appearance, being simple in process and being capable of reducing the cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electronic equipment, and in particular to a processing method of an antenna housing. Background Art

[0002] Nanoinjection molding is a common method for combining metal and plastic in the manufacture of products such as antenna housings. The existing process involves placing multiple independent metal parts in an injection mold and then injecting a plastic melt to achieve an integrated metal-plastic bond. However, this process is complex and cumbersome, limiting efficiency. Furthermore, the metal parts must undergo an oxidation treatment before injection molding, and it's difficult to completely standardize the treatment conditions across multiple metal parts, which can lead to variations in the oxide film's state. This ultimately causes color variations after the housing is molded, severely impacting the consistency of the appearance. Summary of the Invention

[0003] The purpose of the present invention is to provide a processing method for an antenna shell in response to the defects and shortcomings of the existing technology, to solve at least one of the above-mentioned technical problems, to oxidize the shell material as a whole, to eliminate or significantly reduce the color difference of the shell material, to improve the consistency of the appearance, and to simplify the process and reduce costs.

[0004] To achieve the above-mentioned object, the technical solution adopted by the present invention is: a method for processing an antenna housing, characterized in that it includes the following steps: S1. Primary processing: forming the metal substrate into a shell material of a preset shape, retaining connectors on the shell material to maintain its integrity, and reserving a filling area; S2, oxidation treatment, oxidation treatment of the shell material; S3. Prepare a filling piece, preparing a filling piece adapted to the filling area, wherein the filling piece is used to improve the electromagnetic performance of the antenna; S4, surface treatment, performing surface treatment on the shell material and the filling member; S5, molding, removing the connecting piece, combining the oxidized shell material and the filling piece and molding.

[0005] The present invention further provides that, in step S1, the shell material includes: a first shell, a second shell and the connecting member provided between the first shell and the second shell.

[0006] The present invention is further provided with that in step S1, the shell material is processed and formed by stamping, and the shell material is formed in one piece.

[0007] The present invention further provides that, in step S1, the metal substrate is an aluminum alloy or a magnesium alloy.

[0008] The present invention further provides that, in step S1, the connecting members are distributed at intervals along the edge of the filling area.

[0009] The present invention further provides that, in step S2, the oxidation treatment adopts one or more of sulfuric acid anodizing, hard anodizing or chromic acid anodizing.

[0010] The present invention further provides that, in step S3, the filling piece is prepared into a shape matching the filling area, and the filling piece is made of PBT or PPS material.

[0011] The present invention further provides that, in step S4, the surface treatment adopts surface polishing.

[0012] The present invention further provides that, in step S5, the connecting piece is removed by CNC cutting.

[0013] The present invention further provides that in step S5, the shell material and the filler are formed by hot pressing, and a pushing action is applied during the forming process; the temperature of the hot pressing forming is 80°C-120°C.

[0014] After adopting the above technical solution, the beneficial effects of the present invention are as follows: in the present invention, by processing the metal substrate into a shell material of a preset shape, and retaining connecting parts on the shell material to maintain the integrity of the shell material, and then oxidizing the integrated shell material, the color difference of the shell material can be eliminated or significantly reduced, and the oxidation quality and consistency of the appearance can be improved; and it is formed by hot pressing and splicing, and compared with the existing process, no injection molding is required, the process flow is simple, and the processing cost can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0016] Figure 1 is a flowchart of the steps of a method for processing an antenna housing; Figure 2 is a schematic structural diagram of the shell material in step S1; Figure 3 is a schematic diagram of the structure without the connector in step S4; Figure 4 is a structural schematic diagram of the antenna housing formed in step S4; Figure 5 1 is a schematic diagram of the cross-sectional structure of the AA portion of the antenna housing; Figure 6 It corresponds to Figure 5 An enlarged schematic diagram of part B in FIG.

[0017] Explanation of the accompanying reference numerals: 1. Shell material; 11. First shell; 12. Second shell; 13. Connecting piece; 2. Filling piece; 21. Limiting groove. DETAILED DESCRIPTION

[0018] The present invention will be further described in detail below with reference to the accompanying drawings.

[0019] This specific embodiment is merely an explanation of the present invention and is not a limitation of the present invention. After reading this specification, those skilled in the art may make non-creative modifications to this embodiment as needed, but as long as they are within the scope of the claims of the present invention, they are protected by patent law.

[0020] This embodiment relates to a method for processing an antenna housing. Figures 1-4 , including the following steps: S1, primary processing, forming the metal substrate into a shell material 1 of a preset shape, retaining the connecting piece 13 on the shell material 1 to maintain its integrity, and reserving a filling area; S2, oxidation treatment, oxidation treatment of the shell material 1; S3. Prepare a filling piece, preparing a filling piece 2 adapted to the filling area, the filling piece 2 being used to improve the electromagnetic performance of the antenna; S4, surface treatment, performing surface treatment on the shell material 1 and the filler 2; S5, molding, removing the connecting piece 13, combining the oxidized shell material 1 and the filling piece 2 and molding.

[0021] In step S1, a metal substrate is stamped into a shell material 1 of a predetermined shape. The shell material 1 is integrally formed to form the preliminary antenna housing outline. This integral forming ensures structural stability during processing. In some embodiments, the shell material 1 can also be processed using hydraulic or other integral forming methods. Specifically, in this embodiment, the metal substrate is cut to the desired size of the shell material 1 by shearing before stamping. In other embodiments, other methods can be used to prepare the metal substrate to the desired size of the shell material 1. The retaining of connectors 13 in the shell material 1 temporarily maintains the integrity of the shell material 1, facilitating subsequent oxidation treatment of the integral shell material 1 and facilitating processing. Specifically, in this embodiment, the connectors 13 are connecting strips. In some embodiments, the connectors 13 can also be connecting ribs or bridges. Furthermore, a reserved filling area provides space for the subsequent installation of the filler 2, ensuring a precise fit. Specifically, in this embodiment, the metal substrate is an aluminum alloy or a magnesium alloy. In other embodiments, the metal substrate can also be a copper alloy, stainless steel, or a titanium alloy.

[0022] Further, refer to Figure 2The shell material 1 includes: a first shell 11, a second shell 12 and a connector 13 arranged between the first shell 11 and the second shell 12. Specifically, the first shell 11 and the second shell 12 are in the same horizontal plane, and the two constitute the main structure of the antenna shell. The connector 13 serves as a temporary rigid connection between the first shell 11 and the second shell 12 to ensure that the integrity of the shell material 1 is maintained during transportation or oxidation treatment. Preferably, the connectors 13 are distributed at intervals along the edge of the filling area, and can form multi-point dispersed supports at the edge of the filling area, dispersing the connection force between the first shell 11 and the second shell 12 to multiple points, thereby avoiding local deformation of the shell material 1 due to excessive force at a single point.

[0023] In step S2, the surface of the integral metal shell material 1 is oxidized to form a dense oxide film, which can eliminate or significantly reduce the color difference of the shell material 1, improve the oxidation quality and consistency of the appearance, and the integral shell material 1 is oxidized. Compared with the existing piecewise oxidation treatment, the oxidation treatment improves the processing efficiency and reduces the processing cost. The oxidation treatment significantly improves the surface hardness, wear resistance, corrosion resistance and insulation of the shell material 1. At the same time, the oxide film can serve as a base for subsequent surface treatment, enhance the adhesion of the surface coating, and extend the service life of the shell. Specifically in this embodiment, the oxidation treatment adopts sulfuric acid anodizing. In other embodiments, the oxidation treatment can also adopt hard anodizing or chromic acid anodizing.

[0024] In step S3, a filler 2 is prepared with a shape that matches the filler area, based on the dimensions of the filler area and the antenna's electromagnetic performance requirements. This filler 2 specifically improves the antenna's electromagnetic performance, compensating for the electromagnetic parameter deficiencies of the metal housing and ensuring that antenna performance meets the required standards. Specifically, the filler material is cut into filler pieces 2 that are compatible with the filler area. In other embodiments, other methods for preparing the filler 2 may also be used.

[0025] Specifically in this embodiment, the filler 2 is made of PBT material. In some embodiments, the filler 2 can also be made of PPS material.

[0026] In step S5, the shell material and filler are surface treated. Specifically, the surface treatment is performed by surface polishing. Surface polishing processes the shell surface through grinding, cloth wheel polishing, etc., eliminating microscopic defects and surface flaws generated during the processing process, improving the surface finish and aesthetics, and further enhancing the protective performance of the shell.

[0027] In step S5, refer to Figure 3-Figure 4The temporary connector 13 from the initial processing is removed, and the oxidized shell material 1 and filler 2 are fixed together through hot pressing to form a complete antenna housing structure. The temporary connector 13 is removed to allow the filler 2 to be spliced ​​between the first housing 11 and the second housing 12. Specifically, in this embodiment, CNC cutting is used to remove the connector 13. In some embodiments, laser cutting can also be used to remove the connector 13.

[0028] Furthermore, the shell material 1 and the filler 2 are combined by hot pressing. During the forming process, a pushing action needs to be applied, that is, directional pressure needs to be applied, so that the shell material 1 and the filler 2 are fully tightened and connected, the interface gap is eliminated, the bonding strength is enhanced, the process flow is simple, and the processing efficiency is high. Specifically in this embodiment, it is also necessary to maintain pressure during the pushing action, and the pressure holding time is maintained at about 25 seconds. It should be noted that the pressure holding time can also be adjusted according to the specific product, and there is no need to specify it here. In some embodiments, the shell material 1 and the filler 2 can also be combined by insert injection molding or laser welding.

[0029] Reference Figure 5-Figure 6 Specifically, in this embodiment, before the shell material 1 and filler 2 are hot-pressed, the outer surface of the filler 2 is sprayed with varnish to enhance its aesthetics. A paste-like glue is applied to the joint of the filler 2 facing the shell material 1. This secures the filler 2 to a fixture (not shown). The shell material 1 is then snapped onto the filler 2, with one end of the filler 2 embedded within the filling area. The hot-pressing process is then heated to 100°C, causing the glue at the joint of the filler 2 to liquidize. This push action ensures that the filler 2 conforms to the fine contours of the filling area, preventing any interfacial gaps. The holding period allows the glue to cool and solidify naturally, completing the hot-pressing of the shell material 1 and filler 2 into the antenna housing. In other embodiments, the hot-pressing temperature can be 80°C, 90°C, 110°C, 120°C, or other temperatures. As long as the hot-pressing temperature is within the 80°C-120°C range, this is not a specific limitation. Specifically in this embodiment, a limiting groove is provided on the side of the filling piece facing the shell material to limit the overflow of the glue that is heated to a liquid state.

[0030] The above is only used to illustrate the technical solution of the present invention and is not intended to limit it. Other modifications or equivalent substitutions made to the technical solution of the present invention by ordinary technicians in this field should be included in the scope of the claims of the present invention as long as they do not depart from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for processing an antenna housing, characterized in that: The following steps are involved: S1, preliminary processing, processing the metal substrate into a shell material (1) of a preset shape, retaining a connecting piece (13) on the shell material (1) to maintain its integrity, and reserving a filling area; S2, oxidation treatment, performing oxidation treatment on the shell material (1); S3, preparing a filling piece, preparing a filling piece (2) adapted to the filling area, wherein the filling piece (2) is used to improve the electromagnetic performance of the antenna; S4, surface treatment, performing surface treatment on the shell material (1) and the filler (2); S5, molding, removing the connecting piece (13), combining the oxidized shell material (1) and the filling piece (2) and molding.

2. The method for processing an antenna housing according to claim 1, wherein: In step S1, the shell material (1) includes: a first shell (11), a second shell (12) and the connecting member (13) arranged between the first shell (11) and the second shell (12).

3. The method for processing an antenna housing according to claim 2, wherein: In step S1, the shell material (1) is processed and formed by stamping, and the shell material (1) is formed in one piece.

4. The method for processing an antenna housing according to claim 1, wherein: In step S1 , the metal substrate is an aluminum alloy or a magnesium alloy.

5. The method for processing an antenna housing according to claim 1, wherein: In step S1, the connecting members (13) are distributed at intervals along the edge of the filling area.

6. The method for processing an antenna housing according to claim 1, wherein: In step S2 , the oxidation treatment adopts one or more of sulfuric acid anodizing, hard anodizing or chromic acid anodizing.

7. The method for processing an antenna housing according to claim 1, wherein: In step S3, the filling piece (2) is prepared into a shape matching the filling area, and the filling piece (2) is made of PBT or PPS material.

8. The method for processing an antenna housing according to claim 1, wherein: In step S4, surface polishing is used for surface treatment.

9. The method for processing an antenna housing according to claim 1, wherein: In step S5, the connector (13) is removed by CNC cutting.

10. The method for processing an antenna housing according to claim 1, wherein: In step S5, the shell material (1) and the filler (2) are formed by hot pressing, and a pushing action is applied during the forming process; the temperature of the hot pressing forming is 80°C-120°C.

Citation Information

Patent Citations

  • Electronic device shell and manufacturing method thereof

    CN101573009A

  • Back shell of mobile terminal and preparation method of back shell of mobile terminal

    CN105847495A

  • Shell machining method, shell and mobile terminal

    CN107443021A

  • Preparation method of metal-plastic mixed structural part based on secondary anodic oxidation method

    CN112721352A

  • Antenna mast

    WO2013098281A1