Preheat treatment process for carburizing bearing steel
Through a four-step preparatory heat treatment process, the grain and structure of the carburized bearing steel are refined, solving the problems of uneven structure and stress concentration in the existing technology, and improving the fatigue performance and service life of the bearing.
Patent Information
- Application Number
- CN202510702006.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-28
- Publication Date
- 2025-10-03
AI Technical Summary
The existing preparatory heat treatment process for carburizing bearing steel cannot effectively control the core structure and grain size of the steel, resulting in limited improvement in the fatigue performance of the bearings and insufficient service life.
A four-step preparatory heat treatment process is adopted, including high-temperature normalizing, tempering, spheroidizing annealing and stress relief annealing. Through multi-stage heat preservation and cooling treatment, the grains are refined, the tissue heredity and stress concentration are eliminated, and a uniform preparatory tissue is provided.
It significantly improves the bearing's fatigue resistance and core impact toughness, reduces the difficulty of machining, and extends the bearing's service life.
Smart Images

Figure CN120738432A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of heat treatment of bearing materials, in particular to a preliminary heat treatment process for carburized bearing steel. Background Art
[0002] Carburized bearing steel is a common type of bearing steel. Its combination of high surface hardness and excellent fatigue resistance with high core toughness allows it to be used in complex operating conditions. Carburized bearing steel requires multiple heat treatment steps to achieve the desired performance, including preliminary heat treatment, carburizing, quenching, and tempering.
[0003] Existing research focuses primarily on carburizing and quenching / tempering processes, with limited research on preparatory heat treatment. Existing preparatory heat treatment solutions are limited to eliminating the structural inheritance of metals after thermoplastic deformation, and lack specific heat treatment solutions tailored to the specific requirements of bearings.
[0004] In fact, regulating the core structure and grain size of steel through preliminary heat treatment can affect the fatigue performance of bearings. The appropriate combination of structure and grain size can help extend the service life of bearings. However, the core structure of steel produced by existing preliminary heat treatment processes is not ideal, and there is still room for further improvement. Summary of the Invention
[0005] The purpose of the present invention is to provide a preliminary heat treatment process for carburizing bearing steel. By improving the preliminary heat treatment process, the grain size of the treated carburized steel is made finer and the structure is made more uniform, thereby improving the service life of the bearing.
[0006] In order to achieve the above-mentioned purpose, the present invention adopts the following technical solutions.
[0007] A preparatory heat treatment process for carburizing bearing steel comprises the following steps: Step 1: Heat the steel piece to be processed to 1100-1200°C and keep it warm. After the heat preservation is completed, naturally cool it to 900-850°C, and then cool it to 500-300°C in a cooling medium before taking it out; Step 2: Heat the steel piece to be processed to 680-720°C, keep it warm, and then air-cool it to room temperature; Step 3: Heat the steel to be processed to 780-800°C, keep it warm and then cool it to 500-450°C. Step 4: Heat the steel part to be processed to 680-700°C, keep it warm and then cool it to room temperature in the furnace.
[0008] Furthermore, in step 1, the insulation time is 1 to 2 hours.
[0009] Furthermore, in step 2, the holding time is 1 to 2 min / mm, depending on the effective size of the steel part to be processed.
[0010] Furthermore, in step 3, the holding time is 1 to 2 hours. Furthermore, in step 4, the insulation time is 10 to 12 hours.
[0011] After adopting the above technical solution, the present invention has the following beneficial effects: 1. The present invention improves the overall performance of the material through the synergistic effect of high-temperature normalizing and tempering in steps one and two, and can effectively enhance the fatigue resistance of the bearing under complex loads; 2. The present invention promotes the conversion of lamellar pearlite into uniformly distributed spherical pearlite through spheroidizing annealing and stress relief annealing in steps 3 and 4, thereby achieving metal grain refinement, eliminating microscopic stress concentration areas, and improving the impact toughness of the core of the material. Combined with the long-term heat preservation of stress relief annealing, the spheroidal carbides are further homogenized, further refining the grains while reducing the material hardness and reducing the difficulty of mechanical processing; 3. The present invention pays attention to the optimization of adjacent process compatibility during design. In step 1, the natural cooling stage can be simultaneously performed with forging, which fully utilizes the waiting time and eliminates defects in the steel part through forging, achieving mutual promotion. In steps 3 and 4, the hereditary structure of the original austenite coarse grains is completely eliminated through the synergistic effect of multi-stage annealing, providing a uniform preparatory structure for subsequent carburizing and quenching. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 Schematic diagram of the microstructure of the material before treatment in an embodiment of the present invention.
[0013] Figure 2 Schematic diagram of the microstructure of the material after treatment in an embodiment of the present invention.
[0014] Figure 3 Schematic diagram of the grain size of the material before treatment in an embodiment of the present invention.
[0015] Figure 4 Schematic diagram of the grain size of the material after treatment in an embodiment of the present invention. DETAILED DESCRIPTION
[0016] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the characteristics and performance of a preliminary heat treatment process for carburizing bearing steel in the present invention are further described in detail below with reference to the accompanying drawings and embodiments.
[0017] A preparatory heat treatment process for carburized bearing steel includes the following steps.
[0018] Step 1: Heat the steel part to be processed to 1100-1200°C and keep it warm for 1-2 hours. After the insulation is completed, naturally cool it to 900-850°C, and then cool it to 500-300°C in a quenching cooling medium before taking it out.
[0019] During the natural cooling process to 900-850°C, the steel parts to be processed can be forged, which makes rational use of time and facilitates subsequent further finishing.
[0020] Step one is high-temperature normalizing. When heated to 1100-1200°C, the steel becomes fully austenitized. Holding the steel at this temperature for 1-2 hours prevents excessive grain growth. This allows for forging of the steel. Forging not only gives the steel a preliminary shape, but also eliminates defects, increases its density, and improves its overall mechanical properties.
[0021] After the steel part has cooled to 900-850°C, a cooling medium is used to rapidly cool it to 500-300°C, transforming the austenite into fine pearlite or bainite while retaining some undissolved carbides. Rapid cooling also inhibits carbide coarsening, forming a more uniform microstructure and providing a uniform matrix for subsequent process steps.
[0022] Step 2: Heat the steel part to be processed to 680-720°C and keep it warm for 1-2 min / mm, depending on the effective size of the steel part to be processed. After the insulation is completed, air cool it to room temperature and the structure is transformed from austenite to pearlite.
[0023] The second step is high-temperature tempering (quenching and tempering). The steel is heated to 680-720°C and held at this temperature. This allows the small amount of martensite or bainite that may form during the actual process to decompose during high-temperature tempering, precipitating fine, dispersed carbides (such as cementite) to form tempered troostite or tempered troostite. This process aims to reduce internal stress, reduce hard phases, and disperse the alloy carbides, preparing for subsequent spheroidizing annealing.
[0024] After the holding time is over, the steel parts are slowly air-cooled to room temperature to avoid the generation of secondary stress.
[0025] Step three: heat the steel to be processed to 780-800°C, keep it warm for 1-2 hours, and then cool it to 500-450°C. This step does not require cooling to room temperature, which improves processing efficiency.
[0026] Step three is spheroidizing annealing, heating the steel to 780-800°C. This temperature is in the coexistence zone of austenite, ferrite, and carbides (incomplete austenitization), allowing some austenite grains to nucleate and grow within the original coarse grains. The holding time is controlled to 1-2 hours to prevent further grain growth and achieve grain refinement.
[0027] During the heat preservation process, the untransformed lamellar pearlite gradually spheroidizes and transforms into granular pearlite, further refining the grains and providing a uniform matrix structure for subsequent machining.
[0028] Step 4: Heat the steel piece to be processed to 680-700°C, keep it warm for 10-12 hours, and then cool it to room temperature with the furnace.
[0029] Step four is stress relief annealing, where the steel is held at a temperature below Ac1 for an extended period of time. This prevents microstructural changes while promoting further homogenization of the spheroidal carbides and eliminating microsegregation. Slow cooling prevents carbide aggregation and coarsening, stabilizing the ferrite matrix and spheroidal structure.
[0030] Stress relief annealing reduces stress concentration in steel parts, lowers their hardness, improves cutting performance, and prepares them for machining. It also provides a uniform preparatory structure for subsequent carburizing and quenching, avoiding uneven carburized layers.
[0031] In the specific implementation, this embodiment takes a carburized bearing steel sample made of G20Cr2Ni4 and with an outer size of φ40 mm as an example to illustrate the steps of this solution.
[0032] Step 1: Heat the sample to 1150°C, burn it through for 1 hour, and then perform initial forging. When the final forging temperature reaches 900°C, cool it to 450°C in a quenching cooling medium and take out the sample.
[0033] Step 2: The sample removed from the cooling medium is heated to 700°C again for tempering, kept at this temperature for 1 hour, and then removed from the furnace and air-cooled to room temperature.
[0034] Step 3: Heat the sample to 790℃ for annealing, keep it at this temperature for 1h, and then cool it down to 500℃.
[0035] Step 4: Heat the sample to 680°C, keep it at this temperature for 10 hours, and then cool it to room temperature in the furnace.
[0036] After the above treatment, the hardness of the sample is 210-230 HBW, and the microstructure of the sample is granular alloy carbides evenly distributed on the ferrite matrix.
[0037] The microstructure of the sample before and after treatment with the present invention is compared. Figures 1-2 As shown in the figure, there is a relatively obvious lamellar structure before treatment, and after treatment, granular pearlite is evenly distributed on the ferrite matrix.
[0038] The grain size comparison of the sample before and after treatment with the present invention is as follows: Figures 3-4 As shown, the grain size level before treatment is level 5, and the grain size level after treatment is level 9.
[0039] The samples that had undergone the preliminary heat treatment were carburized, quenched and tempered simultaneously with the samples processed by the conventional process, and 6 groups of impact tests were carried out. The impact energy was 24% higher than that of the conventional process, as shown in Table 1.
[0040] It should be noted that the parts not described in detail in this solution are all prior art, and the above embodiments are only used to illustrate the present invention, but the present invention is not limited to the above embodiments. Any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention fall within the scope of protection of the present invention.
Claims
1. A preparatory heat treatment process for carburizing bearing steel, characterized by: The following steps are included: Step 1: Heat the steel to be processed to 1100-1200℃ and keep it warm. After the heat preservation is completed, it is naturally cooled to 900-850℃. Then it is cooled to 500-300℃ in the cooling medium and then taken out. Step 2: Heat the steel to be processed to 680-720℃ and keep it warm. After the heat preservation is completed, air cool it to room temperature. Step 3: Heat the steel to be processed to 780-800℃, keep it warm and then cool it to 500-450℃. Step 4: Heat the steel part to be processed to 680-700°C, keep it warm and then cool it to room temperature in the furnace.
2. A preparatory heat treatment process for carburized bearing steel according to claim 1, characterized in that: In step 1, the insulation time is 1 to 2 hours.
3. A preparatory heat treatment process for carburizing bearing steel according to claim 1, characterized in that: In step 2, the holding time is 1 to 2 min / mm, depending on the effective size of the steel part to be processed.
4. A preparatory heat treatment process for carburizing bearing steel according to claim 1, characterized in that: In step 3, the insulation time is 1 to 2 hours.
5. A preparatory heat treatment process for carburizing bearing steel according to claim 1, characterized in that: In step 4, the insulation time is 10 to 12 hours.