A method for preparing uniformly coated silicon-carbon anode material

By preparing a porous carbon material and uniformly coating it with nano-silicon, the problems of volume expansion and poor conductivity of silicon-based anode materials during charge and discharge processes were solved, thereby improving the cycle performance and electrochemical performance of the material.

CN120809808BActive Publication Date: 2026-11-17SICHUAN CHANGHONG NEW MATERIAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202511014670.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-07-23
Publication Date
2026-11-17
Estimated Expiration
2045-07-23

AI Technical Summary

Technical Problem

Existing silicon-based anode materials suffer from large volume expansion and poor conductivity during charge and discharge, leading to material pulverization and unstable SEI film, which affects the material's first efficiency and cycle life, thus hindering its commercialization.

Method used

Porous carbon materials are prepared by dispersing carbon source, template agent, tannic acid, carbon nanotubes and porous catalyst in solvent and then sintering them. These materials are then coated with nano-silicon through coupling agent and pitch to form a uniform silicon-carbon anode material.

Benefits of technology

By preparing and degassing large-pore porous carbon, the wetting effect of nano-silicon is improved, the coating uniformity is achieved, the volume expansion is reduced, and the cycling performance and electrochemical performance of the material are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120809808B_ABST
    Figure CN120809808B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a uniformly coated silicon-carbon anode material, belonging to the field of lithium battery anode material technology. The preparation method of this invention includes the following steps: (1) preparation of large-pore porous carbon; (2) synthesis of silicon-carbon anode material. By preparing large-pore porous carbon and combining it with degassing, it is easier for small-particle-size milled nano-silicon particles to enter the pores, thereby improving the uniformity of material coating and thus improving the cycle performance of the material. An amine-based catalytic structure is selected, and tannic acid is used to construct polymerization channels, which is conducive to the entry of small-particle nano-silicon into the channels; the hydrogen bonds of the solvent and raw materials enhance the interfacial interaction, thereby achieving the control of the multi-level pore structure. At the same time, a coupling agent is introduced to realize the reaction between carboxyl groups and hydroxyl groups on the surface of nano-silicon, while long-chain alkyl groups enhance the compatibility with porous carbon; epoxy groups can react with hydroxyl groups on the surface of porous carbon or silanol groups on the surface of nano-silicon, which is suitable for improving the dispersibility of fillers and realizing the effective combination of porous carbon and nano-silicon.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium battery anode material technology, specifically to a method for preparing a uniformly coated silicon-carbon anode material. Background Technology

[0002] Lithium-ion batteries have garnered significant attention due to their advantages such as low self-discharge rate, rapid charge and discharge, and long cycle life. According to the "China Lithium-ion Battery Industry Development White Paper (2025)," global lithium-ion battery shipments reached 1545.1 GWh in 2024, a year-on-year increase of 28.5%. In the power battery market, the large-scale production of 4680 cylindrical batteries and long-range fast-charging vehicles will drive high-capacity anode materials into a period of explosive growth. Currently, China is the world's largest producer and consumer of lithium-ion battery anode materials. While graphite remains the dominant anode material, its energy density is nearing its development limit. Silicon anodes, on the other hand, boast a theoretical specific capacity of up to 4200 mAh / g, more than 10 times that of traditional graphite materials, and are abundant in silicon raw materials, making them considered the most competitive next-generation anode material. While silicon-based anode materials offer significant advantages, their large volume expansion (up to 300%) and poor conductivity lead to problems such as material pulverization, electrode integrity degradation, and SEI film instability during charge and discharge processes. These issues negatively impact electrochemical performance, including initial efficiency and cycle life, hindering commercialization. Therefore, it is essential to develop a preparation method that can effectively improve the coating uniformity of silicon-based anode materials. Summary of the Invention

[0003] In order to overcome the above-mentioned shortcomings of the existing technology, the purpose of this invention is to provide a method for preparing a uniformly coated silicon-carbon anode material, so as to improve the coating uniformity of the silicon-carbon anode material.

[0004] The technical solution of the present invention to solve the above-mentioned technical problems is as follows: A method for preparing a uniformly coated silicon-carbon anode material is provided, comprising the following steps: (1) The carbon source, template agent, tannic acid, carbon nanotubes and porous catalyst are dispersed in a solvent, and then the resulting product is dried. (2) The product obtained in step (1) is sintered in a nitrogen atmosphere and cooled to obtain a carbon skeleton structure containing a template agent; (3) The product obtained in step (2) is soaked in hydrofluoric acid, washed with water and dried to obtain porous carbon material; (4) Dissolve micron-sized silicon and surfactant in ethanol solvent, and then disperse by ball milling to obtain monodisperse nano-silicon; (5) After adding the porous carbon material and coupling agent from step (3) to the product obtained in step (4), continue ball milling, mix well, and then dry the product. (6) Add pitch to the product obtained in step (5), and then sinter it in a nitrogen atmosphere to obtain a uniformly coated silicon-carbon anode material.

[0005] Furthermore, the carbon source is at least one of wood, coconut shell and sugarcane bagasse; the porous catalyst is at least one of ethylenediamine, N-methylethylenediamine and diethylenetriamine; the template agent is a mixture of silica nanoparticles and small-sized microspheres; wherein the diameter of the silica nanoparticles is <50nm; the diameter of the small-sized microspheres is ≤1μm; and the solvent is a mixture of ethanol and water.

[0006] Furthermore, the mass ratio of the carbon source, the template agent, tannic acid, carbon nanotubes, and porous catalyst is 1:2:0.3-0.9:0.02-0.06:0.0003-0.001.

[0007] Furthermore, in step (2), the sintering temperature is 600-1000℃ and the sintering time is 1-5h.

[0008] Furthermore, the mass ratio of micron-sized silicon to surfactant is 1:0.1-0.2; the surfactant is at least one of polyvinylpyrrolidone, polyethylene glycol, and hexadecyltrimethylammonium bromide.

[0009] Furthermore, the D50 of monodisperse nano-silicon is ≤50nm.

[0010] Furthermore, the mass ratio of porous carbon material to coupling agent is 1:0.005-0.02; the coupling agent is γ-glycidoxypropyltrimethoxysilane or stearic acid.

[0011] Furthermore, in step (6), the sintering temperature is 1000-1200℃ and the sintering time is 10-12h.

[0012] The present invention has the following beneficial effects: (1) The present invention uses the preparation of large-pore porous carbon and degassing to facilitate the entry of small-diameter sand-milled nano-silicon particles into the pores, thereby improving the uniformity of material coating and thus improving the material's cycle performance. (2) In the preparation of this invention, an amine catalytic structure is selected and tannic acid is combined to construct polymerization channels, which facilitates the wetting of nano-silicon slurry in the later stage and is conducive to the entry of small nano-silicon particles into the channels; combined with the hydrogen bond of solvent and raw materials, the interfacial interaction is enhanced to achieve multi-level pore structure control. (3) In the preparation of this invention, a coupling agent is introduced to realize the reaction between the carboxyl group (-COOH) and the hydroxyl group on the surface of nano-silicon. At the same time, the long-chain alkyl group enhances the compatibility with porous carbon. The epoxy group (-CH2OCH-) can react with the hydroxyl group on the surface of porous carbon or the silanol group on the surface of nano-silicon, which is suitable for improving the dispersibility of the filler and realizing the effective combination of porous carbon and nano-silicon. Attached Figure Description

[0013] Figure 1 SEM image of the silicon-carbon anode material prepared in Example 1; Figure 2 The image shows the SEM image of the silicon-carbon anode material prepared in Comparative Example 1. Detailed Implementation

[0014] The examples given below are for illustrative purposes only and are not intended to limit the scope of the invention. Unless otherwise specified, conditions in the examples are performed under standard conditions or as recommended by the manufacturer. Reagents or instruments whose manufacturers are not specified are all commercially available products.

[0015] Example 1: A method for preparing a uniformly coated silicon-carbon anode material includes the following steps: (1) 100g coconut shell, 50g template agent (containing 40g & 30nm nano SiO2 and 10g & 1μm small SiO2 microspheres), 15g tannic acid, 1g carbon nanotubes and 0.015g ethylenediamine were mechanically stirred in a mixed solvent of ethanol and water for 2h. After mixing evenly, the slurry was dried at 80℃. (2) The product obtained in step (1) is sintered in a nitrogen atmosphere at 800°C for 3 hours. After cooling to room temperature, it is taken out for use to obtain a carbon skeleton structure containing template agent. (3) The above materials were soaked in 10wt% HF for 24h to remove the SiO2 template agent. After repeated washing with water, surface impurities were removed and the materials were dried to achieve the preparation of mesoporous-macroporous multi-level porous carbon materials. (4) Dissolve 20g of micron-sized silicon and 2g of polyvinylpyrrolidone in ethanol solvent and disperse by ball milling to achieve D50≤50nm of nano-silicon particles and obtain monodisperse nano-silicon. (5) Weigh 20g of the mesoporous-macroporous multi-level porous carbon material obtained in step (3) and 0.1g of γ-glycidyl etheroxypropyltrimethoxysilane and mix them into the product obtained in step (4). Degassing is carried out simultaneously during ball milling. After mixing evenly, the product is spray-dried. (6) Add asphalt (the mass of asphalt is 25% of the mass of the product obtained in step (5)) to the product obtained in step (5), mix well, and sinter in a nitrogen atmosphere at 1000℃ for 10 hours to finally obtain silicon-carbon anode material.

[0016] Example 2: A method for preparing a uniformly coated silicon-carbon anode material includes the following steps: (1) 100g coconut shell, 50g template agent (containing 40g & 30nm nano SiO2 and 10g & 1μm small SiO2 microspheres), 45g tannic acid, 3g carbon nanotubes and 0.05g N-methylethylenediamine were mechanically stirred in a mixed solvent of ethanol and water for 2h. After mixing evenly, the slurry was dried at 100℃. (2) The product obtained in step (1) is sintered in a nitrogen atmosphere at 850°C for 3 hours. After cooling to room temperature, it is taken out for use to obtain a carbon skeleton structure containing template agent. (3) The above materials were soaked in 10wt% HF for 24h to remove the SiO2 template agent. After repeated washing with water, surface impurities were removed and the materials were dried to achieve the preparation of mesoporous-macroporous multi-level porous carbon materials. (4) Dissolve 20g of micron-sized silicon and 4g of polyethylene glycol in ethanol solvent and disperse by ball milling to achieve D50≤50nm of nano-silicon particles and obtain monodisperse nano-silicon; (5) Weigh 20g of the mesoporous-macroporous multi-level porous carbon material obtained in step (3) and 0.1g of γ-glycidyl etheroxypropyltrimethoxysilane and mix them into the product obtained in step (4). Degassing is carried out simultaneously during ball milling. After mixing evenly, the product is spray-dried. (6) Add asphalt (the mass of asphalt is 25% of the mass of the product obtained in step (5)) to the product obtained in step (5), mix well, and sinter in a nitrogen atmosphere at 1000℃ for 10 hours to finally obtain silicon-carbon anode material.

[0017] Example 3: A method for preparing a uniformly coated silicon-carbon anode material includes the following steps: (1) 100g of bamboo, 50g of template agent (containing 40g of 30nm nano SiO2 and 10g of 1μm small SiO2 microspheres), 22g of tannic acid, 2g of carbon nanotubes and 0.03g of diethylenetriamine were mechanically stirred in a mixed solvent of ethanol and water for 2 hours. After mixing evenly, the slurry was dried at 100℃. (2) The product obtained in step (1) is sintered in a nitrogen atmosphere at 900°C for 3 hours. After cooling to room temperature, it is taken out for use to obtain a carbon skeleton structure containing template agent. (3) The above materials were soaked in 10wt% HF for 24h to remove the SiO2 template agent. After repeated washing with water, surface impurities were removed and the materials were dried to achieve the preparation of mesoporous-macroporous multi-level porous carbon materials. (4) Dissolve 20g of micron-sized silicon and 3g of hexadecyltrimethylammonium bromide in ethanol solvent and disperse by ball milling to achieve D50≤50nm of nano-silicon particles, thus obtaining monodisperse nano-silicon; (5) Weigh 20g of the mesoporous-macroporous multi-level porous carbon material obtained in step (3) and 0.4g of stearic acid and mix them into the product obtained in step (4). Degas the mixture during ball milling. After mixing evenly, spray dry the product. (6) Add asphalt (the mass of asphalt is 25% of the mass of the product obtained in step (5)) to the product obtained in step (5), mix well, and sinter in a nitrogen atmosphere at 1000℃ for 10 hours to finally obtain silicon-carbon anode material.

[0018] Example 4: A method for preparing a uniformly coated silicon-carbon anode material includes the following steps: (1) 100g of bamboo, 50g of template agent (containing 40g of 30nm nano SiO2 and 10g of 1μm small SiO2 microspheres), 30g of tannic acid, 1.5g of carbon nanotubes and 0.04g of diethylenetriamine were mechanically stirred in a mixed solvent of ethanol and water for 2 hours. After mixing evenly, the slurry was dried at 100℃. (2) The product obtained in step (1) is sintered in a nitrogen atmosphere at 950°C for 3 hours. After cooling to room temperature, it is taken out for use to obtain a carbon skeleton structure containing template agent. (3) The above materials were soaked in 10wt% HF for 24h to remove the SiO2 template agent. After repeated washing with water, surface impurities were removed and the materials were dried to achieve the preparation of mesoporous-macroporous multi-level porous carbon materials. (4) Dissolve 20g of micron-sized silicon and 3g of polyethylene glycol in ethanol solvent and disperse by ball milling to achieve D50≤50nm of nano-silicon particles, and obtain monodisperse nano-silicon; (5) Weigh 20g of the mesoporous-macroporous multi-level porous carbon material obtained in step (3) and 0.1g of γ-glycidyl etheroxypropyltrimethoxysilane and mix them into the product obtained in step (4). Degassing is carried out simultaneously during ball milling. After mixing evenly, the product is spray-dried. (6) Add asphalt (the mass of asphalt is 25% of the mass of the product obtained in step (5)) to the product obtained in step (5), mix well, and sinter in a nitrogen atmosphere at 1000℃ for 10 hours to finally obtain silicon-carbon anode material.

[0019] Example 5: A method for preparing a uniformly coated silicon-carbon anode material includes the following steps: (1) 100g of pine wood, 50g of template agent (containing 40g of 30nm nano SiO2 and 10g of 1μm small SiO2 microspheres), 38g of tannic acid, 1.5g of carbon nanotubes and 0.04g of diethylenetriamine were mechanically stirred in a mixed solvent of ethanol and water for 2 hours. After mixing evenly, the slurry was dried at 100℃. (2) The product obtained in step (1) is sintered in a nitrogen atmosphere at 1000℃ for 3 hours. After cooling to room temperature, it is taken out for use to obtain a carbon skeleton structure containing template agent. (3) The above materials were soaked in 10wt% HF for 24h to remove the SiO2 template agent. After repeated washing with water, surface impurities were removed and the materials were dried to achieve the preparation of mesoporous-macroporous multi-level porous carbon materials. (4) Dissolve 20g of micron-sized silicon and 4g of polyethylene glycol in ethanol solvent and disperse by ball milling to achieve D50≤50nm of nano-silicon particles and obtain monodisperse nano-silicon; (5) Weigh 20g of the mesoporous-macroporous multi-level porous carbon material obtained in step (3) and 0.1g of stearic acid and mix them into the product obtained in step (4). Degas the mixture during ball milling. After mixing evenly, spray dry the product. (6) Add asphalt (the mass of asphalt is 25% of the mass of the product obtained in step (5)) to the product obtained in step (5), mix well, and sinter in a nitrogen atmosphere at 1000℃ for 11 hours to finally obtain silicon-carbon anode material.

[0020] Example 6: A method for preparing a uniformly coated silicon-carbon anode material includes the following steps: (1) 100g of pine wood, 50g of template agent (containing 40g of 30nm nano SiO2 and 10g of 1μm small SiO2 microspheres), 45g of tannic acid, 1.5g of carbon nanotubes and 0.04g of diethylenetriamine were mechanically stirred in a mixed solvent of ethanol and water for 2 hours. After mixing evenly, the slurry was dried at 100℃. (2) The product obtained in step (1) is sintered in a nitrogen atmosphere at 1000℃ for 3 hours. After cooling to room temperature, it is taken out for use to obtain a carbon skeleton structure containing template agent. (3) The above materials were soaked in 10wt% HF for 24h to remove the SiO2 template agent. After repeated washing with water, surface impurities were removed and the materials were dried to achieve the preparation of mesoporous-macroporous multi-level porous carbon materials. (4) Dissolve 20g of micron-sized silicon and 4g of polyethylene glycol in ethanol solvent and disperse by ball milling to achieve D50≤50nm of nano-silicon particles and obtain monodisperse nano-silicon; (5) Weigh 20g of the mesoporous-macroporous multi-level porous carbon material obtained in step (3) and 0.1g of γ-glycidyl etheroxypropyltrimethoxysilane and mix them into the product obtained in step (4). Degassing is carried out simultaneously during ball milling. After mixing evenly, the product is spray-dried. (6) Add asphalt (the mass of asphalt is 25% of the mass of the product obtained in step (5)) to the product obtained in step (5), mix well, and sinter in a nitrogen atmosphere at 1000℃ for 12 hours to finally obtain silicon-carbon anode material.

[0021] Comparative Example 1: A method for preparing a silicon-carbon anode material includes the following steps: (1) 100g coconut shell and 50g template agent (containing 40g & 30nm nano SiO2 and 10g & 1μm small SiO2 microspheres) were mechanically stirred in a mixed solvent of ethanol and water for 2h. After the mixture was evenly mixed, the slurry was dried at 80℃. (2) The product obtained in step (1) is sintered in a nitrogen atmosphere at 800°C for 3 hours. After cooling to room temperature, it is taken out for use to obtain a carbon skeleton structure containing template agent. (3) The above materials were soaked in 10wt% HF for 24h to remove the SiO2 template agent. After repeated washing with water, surface impurities were removed and the materials were dried to achieve the preparation of mesoporous-macroporous multi-level porous carbon materials. (4) Dissolve 20g of micron-sized silicon and 2g of polyvinylpyrrolidone in ethanol solvent and disperse by ball milling to achieve D50≤50nm of nano-silicon particles; (5) Weigh 20g of the mesoporous-macroporous multi-level porous carbon material obtained in step (3) and 0.1g of γ-glycidyl etheroxypropyltrimethoxysilane and mix them into the product obtained in step (4). After ball milling, spray dry the product. (6) Add asphalt (the mass of asphalt is 25% of the mass of the product obtained in step (5)) to the product obtained in step (5), mix well, and sinter in a nitrogen atmosphere at 1000℃ for 10 hours to finally obtain silicon-carbon anode material.

[0022] Comparative Example 2: A method for preparing a silicon-carbon anode material includes the following steps: (1) 100g coconut shell and 50g template agent (containing 40g & 30nm nano SiO2 and 10g & 1μm small SiO2 microspheres) were mechanically stirred in a mixed solvent of ethanol and water for 2h. After the mixture was evenly mixed, the slurry was dried at 80℃. (2) The product obtained in step (1) is sintered in a nitrogen atmosphere at 800°C for 3 hours. After cooling to room temperature, it is taken out for use to obtain a carbon skeleton structure containing template agent. (3) The above materials were soaked in 10wt% HF for 24h to remove the SiO2 template agent. After repeated washing with water, surface impurities were removed and the materials were dried to achieve the preparation of mesoporous-macroporous multi-level porous carbon materials. (4) Dissolve 20g of micron-sized silicon and 2g of polyvinylpyrrolidone in ethanol solvent and disperse by ball milling to achieve D50≤50nm of nano-silicon particles; (5) Weigh 20g of the mesoporous-macroporous multi-level porous carbon material obtained in step (3) and mix it into the product obtained in step (4). After ball milling, spray dry the product. (6) Add asphalt (the mass of asphalt is 25% of the mass of the product obtained in step (5)) to the product obtained in step (5), mix well, and sinter in a nitrogen atmosphere at 1000℃ for 10 hours to finally obtain silicon-carbon anode material.

[0023] The materials prepared in Examples 1-6 and Comparative Examples 1-2 were subjected to electrochemical performance testing. Firstly, they were assembled into coin cell materials to test their specific capacity. Secondly, the materials were compounded with graphite to a concentration of 500 mAh / g and then paired with ternary cathode materials for full-cell performance testing. The performance is shown in Table 1 below.

[0024] Table 1 Electrochemical performance tests of materials prepared in Examples 1-6 and comparative examples Table 1 shows that the preparation of large-pore porous carbon, combined with degassing treatment, can effectively improve the wetting effect of nano-silicon. Small nano-silicon particles successfully enter the pores, achieving uniform silicon coating, improving material properties, and reducing material volume expansion. Figure 1-2 It can be seen that the sample surface of Example 1 is covered with a continuous, dense and uniform coating layer with a narrow particle size distribution and regular morphology; while the coating layer of the material surface of Comparative Example 1 has obvious roughness. Generally, a uniform and dense coating layer can better buffer the volume change stress of the active material during the lithiation / delithiation process, reduce particle breakage and pulverization, and therefore the examples have better electrochemical performance.

[0025] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing a uniformly coated silicon-carbon anode material, characterized in that, Includes the following steps: (1) The carbon source, template agent, tannic acid, carbon nanotubes and porous catalyst are dispersed in a solvent, and then the resulting product is dried. (2) The product obtained in step (1) is sintered in a nitrogen atmosphere and cooled to obtain a carbon skeleton structure containing a template agent; (3) The product obtained in step (2) is soaked in hydrofluoric acid, washed with water and dried to obtain porous carbon material; (4) Dissolve micron-sized silicon and surfactant in ethanol solvent, and then disperse by ball milling to obtain monodisperse nano-silicon; (5) After adding the porous carbon material and coupling agent from step (3) to the product obtained in step (4), continue ball milling. During the ball milling process, degassing is carried out simultaneously. After mixing, the product is dried. (6) Add asphalt to the product obtained in step (5), and then sinter it in a nitrogen atmosphere to obtain a uniformly coated silicon-carbon anode material. The carbon source is at least one of wood, coconut shell, and sugarcane bagasse; the porous catalyst is at least one of ethylenediamine, N-methylethylenediamine, and diethylenetriamine; the template agent is a mixture of silica nanoparticles and small-sized microspheres; wherein the diameter of the silica nanoparticles is <50 nm; the diameter of the small-sized microspheres is ≤1 μm; and the solvent is a mixture of ethanol and water.

2. The production method according to claim 1, characterized by, The mass ratio of the carbon source, the template agent, the tannic acid, the carbon nanotubes, and the porous catalyst is 1:2:0.3-0.9:0.02-0.06:0.0003-0.

001.

3. The preparation method according to claim 1, characterized in that, The sintering temperature in step (2) is 600-1000℃ and the sintering time is 1-5h.

4. The production method according to claim 1, characterized by, The mass ratio of the micron-sized silicon to the surfactant is 1:0.1-0.2; the surfactant is at least one selected from polyvinylpyrrolidone, polyethylene glycol, and hexadecyltrimethylammonium bromide.

5. The preparation method according to claim 1, characterized in that, The D50 of the monodisperse nano-silicon is ≤50nm.

6. The method of claim 1, wherein, The mass ratio of the porous carbon material to the coupling agent is 1:0.005-0.02; the coupling agent is γ-glycidoxypropyltrimethoxysilane or stearic acid.

7. The preparation method according to claim 1, characterized in that, The sintering temperature in step (6) is 1000-1200℃; the sintering time is 10-12h.

Citation Information

Patent Citations

  • Porous core-shell structure silicon-carbon negative electrode material for lithium ion battery and preparation method thereof

    CN111146430A

  • Porous carbon, preparation method thereof and silicon-carbon material with high silicon content

    CN119430142A