A high-durability Pt fuel cell cathode catalyst and its preparation method
By introducing rhodium into platinum and performing reduction etching, a high-durability Pt fuel cell cathode catalyst was prepared, which solved the problems of low activity, poor stability and insufficient durability of existing catalysts, and achieved high durability and high performance of the catalyst.
Patent Information
- Application Number
- CN202510915229.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-07-03
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-07-03
AI Technical Summary
In existing commercial PEMFC stacks, carbon-supported platinum catalysts suffer from low activity, insufficient stability, lack of anti-reverse polarity performance, and high cost, resulting in insufficient fuel cell durability and easy damage to the catalyst layer structure.
By introducing a small amount of the precious metal rhodium into platinum, and selectively etching unstable metal particles on the catalyst surface using a reduction etching method, the electronic structure is optimized and alloying is enhanced, thus preparing a high-durability Pt fuel cell cathode catalyst.
It significantly improves the durability and stability of the catalyst, improves the metal loading on the catalyst surface, reduces the dissolution of Pt in oxidizing environments, delays the overall corrosion of the catalyst, and improves the activity of the catalyst and the performance of the fuel cell.
Smart Images

Figure CN120809848B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a high-durability Pt fuel cell cathode catalyst and its preparation method, belonging to the field of fuel cells. Background Technology
[0002] Currently, commercial PEMFC stacks mainly rely on carbon-supported platinum (Pt / C) or platinum-cobalt (PtCo) alloy catalysts. Among these, carbon-supported platinum catalysts remain the most widely used, but they suffer from low activity, insufficient stability, lack of anti-reverse polarity, and high cost. Using platinum-based catalysts with high platinum loading can thin the catalyst layer, effectively reducing gas mass transfer resistance, which is crucial for improving fuel cell output performance. Furthermore, in actual operating conditions, uneven gas distribution, instantaneous start-up or shutdown can lead to reverse polarity, severely damaging the catalyst layer structure and causing irreversible damage. Moreover, the durability of current fuel cells falls far short of expectations. Therefore, developing high-performance catalysts with high platinum loading and high stability (high durability) is of paramount importance for the development and large-scale commercial application of fuel cells. Summary of the Invention
[0003] The purpose of this invention is to overcome the shortcomings of existing technologies and provide a high-durability Pt fuel cell cathode catalyst and its preparation method. The catalyst of this invention is prepared by introducing a small amount of the precious metal rhodium into metallic platinum to prepare a platinum-rhodium catalyst, which optimizes the electronic structure of metallic platinum, significantly improving catalyst durability. Furthermore, a special reduction etching method is used to selectively etch metal particles that are not tightly bound to the support during the metal reduction loading process on the catalyst surface, and the alloying process on the catalyst surface is enhanced, further improving catalyst durability.
[0004] To achieve the above technical objectives, the technical solution adopted in the embodiments of the present invention is as follows: In a first aspect, embodiments of the present invention provide a method for preparing a high-durability Pt fuel cell cathode catalyst, comprising the following steps: (1) Preparation of catalyst precursor: Disperse 2-10g of carbon powder in 2-10L of ultrapure water, homogenize and emulsify for 5-15min, add 5.3-26.3g of platinum source and 0.02-0.1g of rhodium source, sonicate for 10-20min to form a homogeneous solution; add alkaline substance to adjust the pH of the solution to 9-11.5, stir further for 30-60min, after stirring, filter and wash and dry at 60-90℃ to obtain catalyst precursor; (2) Reduction etching treatment: After grinding and mixing 2-10g of catalyst precursor and 2-10g of ammonium salt obtained in step (1) evenly, the mixture is placed in a tube furnace and calcined at 400-650℃ for 1-4h under an inert atmosphere with a flow rate of 400-700sccm to obtain a high-durability Pt fuel cell cathode catalyst.
[0005] Further, in step (1), the platinum source includes one or more of potassium chloroplatinate, chloroplatinic acid, platinum nitrate, sodium chloroplatinate, and ammonium chloroplatinate, with a purity ≥98%; The rhodium source includes one or more of rhodium phosphate, rhodium chloride, rhodium nitrate, rhodium acetate, and rhodium tribromide.
[0006] Further, in step (1), the alkaline substance is one or more of potassium hydroxide, potassium carbonate, sodium carbonate, sodium hydroxide, ammonia, and sodium bicarbonate.
[0007] Furthermore, in step (2), the ammonium salt is one or more of ammonium iodide, ammonium chloride and ammonium fluoride, with a purity ≥99%.
[0008] Furthermore, in step (2), the inert atmosphere is one or more of helium, argon and nitrogen, with a purity ≥99.999%.
[0009] In a second aspect, embodiments of the present invention provide a high-durability Pt fuel cell cathode catalyst, which is prepared using the preparation method described in the first aspect.
[0010] The beneficial effects of the technical solution provided by the embodiments of the present invention are as follows: 1. The preparation method of the present invention introduces a small amount of the noble metal rhodium. The introduction of Rh reduces the d-band center of Pt, weakens the adsorption energy of Pt with oxygen-containing intermediates (such as OH*, O*), and reduces the dissolution of Pt in an oxidizing environment. At the same time, Rh atoms inhibit the surface migration and shedding of Pt atoms through strong interaction with Pt. Meanwhile, the corrosion resistance of Rh itself also delays the overall corrosion of the catalyst surface metal.
[0011] 2. The preparation method of the present invention can selectively etch the metal on the catalyst surface while reducing and strengthening the metal alloying of the catalyst surface, thereby removing unstable metal particles on the surface. It can improve the metal loading on the catalyst surface while strengthening the metal alloying of the catalyst surface, thus significantly improving the catalyst durability. The method is novel and the steps are simple. Attached Figure Description
[0012] Figure 1 These are XRD comparison diagrams of the catalysts prepared in Example 1 and Comparative Examples 1-2 of this invention.
[0013] Figure 2a , Figure 2b These are transmission electron microscopy (TEM) images comparing the surface metal dispersion of the catalysts prepared in Example 1 and Comparative Example 2.
[0014] Figure 3 These are the linear volt-ampere curves of the half-cells in Embodiment 2, Comparative Example 1, and Comparative Example 2 of the present invention.
[0015] Figure 4a , Figure 4b , Figure 4c The figures are the half-cell durability curves before and after preparation of the catalysts prepared in Example 3, Comparative Example 2 and Comparative Example 1 of this invention.
[0016] Figure 5 This is a comparison graph of the polarization curves of fuel cell single cells prepared by the catalysts in Example 4, Comparative Example 1 and Comparative Example 2 of the present invention.
[0017] Figure 6a , Figure 6b , Figure 6c These are comparison graphs of the polarization curves of fuel cell single cells prepared by the catalysts in Example 5, Comparative Example 2, and Comparative Example 1 of this invention before and after accelerated durability testing. Detailed Implementation
[0018] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0019] Example 1 A method for preparing a high-durability Pt fuel cell cathode catalyst includes the following steps: (1) Preparation of catalyst precursor: 2g of XC-72R carbon powder was dispersed in 2L of ultrapure water, homogenized and emulsified for 5min, 5.3g of platinum nitrate (China National Pharmaceutical Group Co., Ltd., analytical grade 99.8%) and 0.02g of rhodium chloride (China National Pharmaceutical Group Co., Ltd., analytical grade 99.8%) were added, and the mixture was sonicated for 10min to form a homogeneous solution; ammonia water (China National Pharmaceutical Group Co., Ltd., 25~28wt%) was added to adjust the pH of the solution to 9, and the mixture was stirred for 30min. After stirring, the solution was filtered, washed, and dried at 60℃ to obtain the catalyst precursor. (2) Reduction etching treatment: 2g of catalyst precursor obtained in step (1) and 2g of ammonium iodide (Chinese medicine, analytical grade 99.8%) are ground and mixed evenly and placed in a tube furnace. The mixture is calcined at 400℃ for 1h under a nitrogen atmosphere (purity 99.999%) with a flow rate of 400sccm to obtain a high-durability Pt fuel cell cathode catalyst. (3) Single-cell fuel cell test: Accurately weigh 200 mg of the platinum-rhodium catalyst prepared above; measure 20 mL of pure water, 15 mL of isopropanol and 1.5 mL of 5 wt% perfluorosulfonic acid resin solution (DuPont D520), add them to the catalyst, and pulverize the cells for 30 min to form a uniform catalyst ink. Coat the ink evenly on the cut proton exchange membrane and mark it as the cathode; weigh the platinum-carbon catalyst in the same way and coat it on the other side of the proton exchange membrane as the anode, forming the CCM; the gas diffusion layer uses SGL 28BC model GDL. Disassemble the balticFuelCells QCF25 quick assembly test fixture, and place the thickness limit sheet, the first GDL, the CCM and the second GDL in sequence. After fixing, rotate the pneumatic button to complete the clamping. After connecting the gas pipeline, perform a gas tightness test. After passing the test, conduct a single-cell test.
[0020] Single cell test conditions: Single cell area 25cm² 2 The stoichiometric ratio of anode to cathode is 1.5:2.5, the anode dew point is set at 64℃, the cathode dew point is set at 64℃, the anode feed pressure is 1.1 bar, the cathode feed pressure is 1.0 bar, and the battery test temperature is 80℃.
[0021] Example 2 A method for preparing a high-durability Pt fuel cell cathode catalyst includes the following steps: (1) Preparation of catalyst precursor: 10g of XC-72R carbon powder was dispersed in 10L of ultrapure water, homogenized and emulsified for 15min, 26.3g of chloroplatinic acid (China National Pharmaceutical Group Co., Ltd., analytical grade 99.8%) and 0.1g of rhodium acetate (China National Pharmaceutical Group Co., Ltd., analytical grade 99.8%) were added, and the mixture was sonicated for 20min to form a homogeneous solution; sodium hydroxide (China National Pharmaceutical Group Co., Ltd., analytical grade 99.8%) was added to adjust the pH of the solution to 11.5, and the mixture was stirred for 60min. After stirring, the mixture was filtered, washed, and dried at 90℃ to obtain the catalyst precursor. (2) Reduction etching treatment: 10g of catalyst precursor obtained in step (1) and 10g of ammonium chloride (Chinese medicine, analytical grade 99.8%) are ground and mixed evenly and placed in a tube furnace. The mixture is calcined at 650℃ for 4h under an argon atmosphere with a flow rate of 700sccm (purity 99.999%) to obtain a high-durability Pt fuel cell cathode catalyst.
[0022] (3) The single cell test of the fuel cell using the high-durability Pt fuel cell cathode catalyst prepared in this embodiment is the same as in Example 1.
[0023] Example 3 The difference between this embodiment and Example 1 is that potassium hydroxide is added as the alkaline substance in step (1) to adjust the pH of the solution to 9.5. The other steps are the same as in Example 1. The single-cell fuel cell test using the high-durability Pt fuel cell cathode catalyst prepared in this embodiment is the same as in Example 1.
[0024] Example 4 The difference between this embodiment and Embodiment 2 is that the inert atmosphere strength in step (2) is 450 sccm and the calcination temperature is 500℃, while the other steps are the same as in Embodiment 2. The single-cell test of the fuel cell using the high-durability Pt fuel cell cathode catalyst prepared in this embodiment is the same as in Embodiment 1.
[0025] Example 5 The difference between this embodiment and Example 1 is that in step (1), the pH of the solution is adjusted to 10.5 and the calcination temperature is 600℃. All other steps are the same as in Example 1. The single-cell fuel cell test using the high-durability Pt fuel cell cathode catalyst prepared in this embodiment is the same as in Example 1.
[0026] Comparative Example 1 This comparative example provides a platinum-carbon catalyst. The difference between this comparative example and Example 1 is that only platinum nitrate is added in step (1), and rhodium chloride is not added. Ammonium salt is not added in step (2). Other ratios and conditions are the same as in Example 1.
[0027] Comparative Example 2 This comparative example provides a platinum-rhodium carbon catalyst that has not been reduced and etched. The difference between this comparative example and Example 1 is that no ammonium salt is added in step (2), while the other proportions and conditions are the same as in Example 1.
[0028] from Figure 1 It can be seen that Example 1, Comparative Example 1, and Comparative Example 2 all exhibited four standard platinum peaks between 40° and 90°, with essentially consistent intensity. Compared to Comparative Example 1, the platinum peaks in Example 1 and Comparative Example 2 showed varying degrees of rightward shift, with Example 1 showing the largest shift. This rightward shift indicates platinum lattice compression and a higher degree of alloying. The shifts in Example 1 and Comparative Example 2 are attributed to the addition of rhodium, while the larger shift in Example 1 compared to Comparative Example 2 is due to the further reduction caused by the high-temperature decomposition of ammonium iodide into ammonia during the reduction etching process. Better lattice compression and alloying results in better catalyst activity and durability.
[0029] Figure 2b shows the surface metal distribution of the catalyst prepared in Comparative Example 2. It can be seen from the figure that there are obvious large metal agglomerates on the surface. These agglomerates often have weak bonding with the support and are easily corroded during the fuel cell reaction, resulting in poor catalyst durability. In contrast, Figure 2a shows the surface metal distribution of the catalyst prepared in Example 1. It can be seen that there are no large metal agglomerates on the surface and the surface metal is uniformly dispersed. This indicates that the reduction etching treatment can etch away the large metal agglomerates with weak bonding with the support, thereby improving the surface metal durability of the catalyst.
[0030] from Figure 3 The linear voltammetry curves show that the mass activity of Example 2 is 0.2020 A / mgPt, that of Comparative Example 2 is 0.2002 A / mgPt, and that of Comparative Example 1 is 0.0968 A / mgPt. The activity of Example 2 is slightly higher than that of Comparative Example 2, and the mass activities of both Example 2 and Comparative Example 2 are much greater than those of Comparative Example 1, indicating that the addition of Rh has a certain effect on improving the catalyst activity.
[0031] Depend on Figure 4a From the curves of the 30,000-cycle half-cell durability test before and after, it can be calculated that the mass activity of the catalyst prepared in Example 3 before and after the durability test is 0.2056 A / mgPt and 0.2020 A / mgPt, respectively, showing almost no change before and after the durability test, thus exhibiting excellent catalyst durability; Figure 4b It can be seen that the mass activities of the catalyst prepared in Comparative Example 2 before and after durability were 0.2002 A / mgPt and 0.1826 A / mgPt, respectively, with a decay rate of 8.79%; Figure 4c It can be seen that the mass activity of the catalyst prepared in Comparative Example 1 before and after durability improvement is 0.0968 A / mgPt and 0.0499 A / mgPt, respectively, with a decay rate of 48.45%. Compared with the other two examples, the catalyst prepared in Example 3 with rhodium addition and reduction etching treatment has better durability than Comparative Example 2 without reduction etching treatment, and is far better than Comparative Example 1 without rhodium addition and reduction etching treatment, indicating that the addition of rhodium and reduction etching treatment can significantly improve catalyst durability.
[0032] Depend on Figure 5 The polarization performance curves of the single fuel cell show that the single fuel cell performance of the catalyst prepared in Example 4 is 2 A / cm. 2 @0.668V, the performance of Comparative Example 2 is 2A / cm. 2 @0.653V, the performance of Comparative Example 1 is 2A / cm 2@0.611V. Compared with the other two, the fuel cell in Example 4 has the best single-cell performance. This is due to the addition of rhodium and the reduction etching treatment, which makes the noble metal platinum on the surface more uniformly dispersed and causes a lattice compression effect, which optimizes the adsorption of reaction intermediates by active sites, thereby significantly improving the performance of the catalyst cell.
[0033] from Figure 6a The accelerated durability test curves of the fuel cell single cell show that the performance of Example 5 showed almost no degradation before and after the accelerated durability test; Figure 6b It can be seen that the durability performance before and after Comparative Example 2 is 2A / cm. 2 @0.653V and 2A / cm 2 @0.621V, the potential decayed by 32mV; by Figure 6c It can be seen that the durability performance before and after Comparative Example 1 is 2A / cm. 2 @0.611V and 2A / cm 2 At 0.567V, the potential decayed by 44mV. Compared to the other two, Example 5 exhibited the best durability, indicating that the addition of rhodium and the reduction etching treatment significantly improve the durability of the fuel cell under actual operating conditions.
[0034] Finally, it should be noted that the above specific embodiments are only used to illustrate the technical solutions of the present invention and not to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A method for preparing a high-durability Pt fuel cell cathode catalyst, characterized in that, Includes the following steps: (1) Preparation of catalyst precursor: Disperse 2-10g of carbon powder in 2-10L of ultrapure water, homogenize and emulsify for 5-15min, add 5.3-26.3g of platinum source and 0.02-0.1g of rhodium source, sonicate for 10-20min to form a homogeneous solution; add alkaline substance to adjust the pH of the solution to 9-11.5, stir further for 30-60min, after stirring, filter and wash and dry at 60-90℃ to obtain catalyst precursor; (2) Reduction etching treatment: 2-10g of catalyst precursor and 2-10g of ammonium salt obtained in step (1) are ground and mixed evenly and then placed in a tube furnace and calcined at 400-650℃ for 1-4h under an inert atmosphere with a flow rate of 400-700sccm to obtain a high-durability Pt fuel cell cathode catalyst. In step (2), the ammonium salt is one or more of ammonium iodide, ammonium chloride and ammonium fluoride.
2. The method for preparing the high-durability Pt fuel cell cathode catalyst according to claim 1, characterized in that, In step (1), the platinum source includes one or more of potassium chloroplatinate, chloroplatinic acid, platinum nitrate, sodium chloroplatinate, and ammonium chloroplatinate, with a purity ≥98%; The rhodium source includes one or more of rhodium phosphate, rhodium chloride, rhodium nitrate, rhodium acetate, and rhodium tribromide.
3. The method for preparing the high-durability Pt fuel cell cathode catalyst according to claim 1, characterized in that, In step (1), the alkaline substance is one or more of potassium hydroxide, potassium carbonate, sodium carbonate, sodium hydroxide, ammonia, and sodium bicarbonate.
4. The method for preparing the high-durability Pt fuel cell cathode catalyst according to claim 1, characterized in that, In step (2), the purity of the ammonium salt is ≥99%.
5. The method for preparing the high-durability Pt fuel cell cathode catalyst according to claim 1, characterized in that, In step (2), the inert atmosphere is one or more of helium, argon and nitrogen, with a purity ≥99.999%.
6. A high-durability Pt fuel cell cathode catalyst, characterized in that, It is prepared by the preparation method according to any one of claims 1-5.
Citation Information
Patent Citations
Preparation and application of PtCo / C ordered alloy catalyst
CN118315602A
Method for preparing fuel cell catalyst using sulfide precipitation process
CN1814349A