A high-strength ceramic and its blank preparation method

By optimizing the ceramic body clay formula, glaze composition, and gradient glaze firing process, the problems of insufficient strength and poor thermal shock resistance of traditional ceramics have been solved, enabling the preparation of high-strength ceramics. This also reduces costs by utilizing waste materials and improves applicability in multiple scenarios.

CN120864866BActive Publication Date: 2026-11-17JIANGXI YINUO CERAMICS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202511012595.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-07-22
Publication Date
2026-11-17
Estimated Expiration
2045-07-22

AI Technical Summary

Technical Problem

Traditional daily-use ceramics suffer from insufficient strength and poor thermal shock resistance, and there is a shortage of high-quality mineral raw materials and difficulties in waste disposal, resulting in high costs and making it difficult to meet the needs of multiple usage scenarios.

Method used

The clay body formula is made by mixing ceramic kiln slag, red clay, lepidolite, copper-based alloy powder and aluminum borate fiber, and is combined with specific glazes and gradient glaze firing process. Ceramic kiln slag is used as a functional filler and mineralizer, red clay improves the binding, lepidolite reduces volume expansion, copper-based alloy powder improves strength, and aluminum borate fiber enhances mechanical strength.

Benefits of technology

High-strength ceramics with excellent thermal shock resistance are produced, effectively utilizing waste materials to reduce costs. The process has low energy consumption and meets the needs of multiple application scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses a high-strength ceramic and its clay preparation method, belonging to the field of daily-use ceramics technology. The invention provides a clay for preparing high-strength ceramics, with the following raw materials: 28-34 parts quartz sand, 26-32 parts kaolin, 12-18 parts ceramic kiln slag, 5-8 parts red clay, 3-6 parts lepidolite, 2-3.2 parts copper-based alloy powder, and 1-1.5 parts aluminum borate fiber. Simultaneously, a matching glaze is also provided: 16-24 parts ceramic kiln slag, 8-15 parts potassium feldspar, 4-8 parts leucite, 5-7 parts zircon, 3-6 parts calcite, and 0.2-0.8 parts aluminum titanate. This invention not only effectively utilizes ceramic waste to replace some of the mineral raw materials, but also produces ceramics with excellent strength, hardness, and thermal shock resistance, reducing processing costs while meeting the application needs of most daily-use scenarios.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of daily-use ceramics technology, specifically relating to a high-strength ceramic and its clay preparation method. Background Technology

[0002] As a basic material for people's livelihood, daily-use ceramics have a global annual output of over 30 billion pieces. However, their performance has long been limited by the traditional silicate system (kaolin-quartz-feldspar ternary component). This system relies on natural mineral raw materials and has three major advantages: low cost, low energy consumption, and easy processing. However, it has defects such as insufficient strength and poor thermal shock resistance. On the other hand, introducing special advanced ceramics would significantly increase the cost of raw materials and processing, which is not in line with the economics of daily-use ceramics.

[0003] As the foundation and matrix of ceramic products, the composition and properties of the clay directly affect the key performance characteristics of the final ceramic product. During high-temperature firing after drying, clay minerals gradually decompose, a glassy phase begins to form, and solid-phase reactions occur between particles, causing them to bond together. This series of complex physicochemical changes causes the clay to shrink and densify, transforming it from a loose, porous, and brittle clay-like structure into a ceramic body with a certain strength but still retaining porosity. Currently, the mainstream approach to pursuing high-performance ceramics is to use high-quality natural minerals as raw materials for the clay body; however, this strategy faces a dual challenge: on the one hand, the consumption of daily-use ceramics is enormous, and high-quality mineral raw materials cannot meet the demand; on the other hand, the amount of waste generated from daily-use ceramics is increasing daily, urgently requiring effective treatment.

[0004] To further improve the strength and heat resistance of traditional ceramics while ensuring their economic viability and expanding their application range, it is necessary to conduct further research and improvement on the raw materials and firing process of traditional ceramic body clay. Summary of the Invention

[0005] In view of the above-mentioned content, the purpose of this invention is to provide a high-strength ceramic and its preparation method. This invention addresses the shortcomings of traditional kaolin-quartz-feldspar ternary ceramic systems by adjusting and optimizing the raw material composition of the clay and glaze, resulting in ceramic products with a certain proportion of kiln slag waste exhibiting good strength, hardness, and thermal shock resistance, thus meeting the needs of more application scenarios.

[0006] To achieve the above objectives, the present invention specifically adopts the following technical solution: This invention provides a clay blank for preparing high-strength ceramics, wherein the clay blank comprises the following raw materials by weight: 28-34 parts quartz sand, 26-32 parts kaolin, 12-18 parts ceramic kiln slag, 5-8 parts red clay, 3-6 parts lepidolite, 2-3.2 parts copper-based alloy powder, and 1-1.5 parts aluminum borate fiber.

[0007] Furthermore, the clay is prepared by weight from the following raw materials: 32 parts quartz sand, 28 parts kaolin, 15 parts ceramic kiln slag, 6 parts red clay, 5 parts lepidolite, 2.6 parts copper-based alloy powder, and 1.3 parts aluminum borate fiber.

[0008] Furthermore, the copper-based alloy powder has the following composition by mass percentage: Cr 5.5%-6.5%, Si 3.0%-4.8%, Mn 2.4%-3.5%, Co 0.8%-1.6%, with the balance being Cu.

[0009] Furthermore, the main chemical composition of the ceramic kiln slag is: SiO2 62.0%-65.2%, Al2O3 15.4%-18.0%, MgO 6.8%-7.6%.

[0010] The present invention also provides a method for preparing high-strength ceramics using the above-mentioned clay, comprising the following steps: Step 1: Mix and wet grind the raw materials for the clay, pour the resulting slurry into the clay body to form a clay body, bisque-fired and cooled to obtain a bisque-fired clay body; Step 2: Weigh and mix the raw materials of the glaze, then wet grind them. Apply the resulting glaze slurry to the surface of the bisque-fired body to obtain a glazed body. Step 3: Transfer the glazed blank into the kiln for gradient glazing and cooling to obtain the finished ceramic product.

[0011] Furthermore, the process parameters for bisque firing in step one are as follows: under an air atmosphere, the temperature is first raised from room temperature to 595-610℃ at a rate of 4-6℃ / min, and then raised to 950-980℃ at a rate of 2-3℃ / min and held for 30-45 minutes for bisque firing. After the holding period, the temperature is naturally cooled to room temperature.

[0012] Furthermore, the glaze described in step two comprises the following raw materials by weight: 16-24 parts ceramic kiln slag, 8-15 parts potassium feldspar, 4-8 parts leucite, 5-7 parts zircon, 3-6 parts calcite, and 0.2-0.8 parts aluminum titanate.

[0013] Furthermore, in step two, the glaze thickness is 0.4-0.8 mm.

[0014] Furthermore, the process parameters for gradient glaze firing in step three are as follows: Under an air atmosphere, the temperature is first raised from room temperature to 980-1040℃ at a rate of 5-6℃ / min, and then raised to 1120-1180℃ at a rate of 0.5-1.5℃ / min and held for 25-35 min. After the holding period, the temperature is first cooled to 800-820℃ at a rate of 4-5℃ / min, and then the cooling rate is reduced to 1-1.5℃ / min and the temperature is further cooled to room temperature.

[0015] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention improves and optimizes the clay formula: it incorporates a certain proportion of ceramic kiln slag while using red clay, lepidolite, copper-based alloy powder, and aluminum borate fiber. Ceramic kiln slag can serve as a functional filler to replace ore raw materials, reducing costs and effectively utilizing waste materials. Furthermore, the glassy phase contained in the pre-fired clay can act as a mineralizer to accelerate the densification process. Red clay has strong plasticity, which is beneficial for improving bonding and promoting the forming of the green body. Lepidolite can effectively reduce the volume expansion of the green body and significantly improve its resistance to rapid thermal changes. The selected copper-based alloy powder improves strength and wear resistance while providing a good foundation for the stable bonding of the multi-component green body and subsequent glaze layer. Aluminum borate fiber, as a reinforcing additive, can further improve mechanical strength and crack resistance.

[0016] 2. Based on the selected clay body, the present invention also provides a matching glaze: the addition of ceramic kiln slag to replace flux and quartz accelerates the densification of the glaze to form a uniform glaze melt, reduces pinholes, and the use of the same ceramic kiln slag as the clay body brings about synergy in composition and process, which is beneficial to the matching of thermal expansion coefficients; leucite helps to form a good chemical bond and physical compressive stress at the clay body-glaze interface, greatly reducing the risk of glaze cracking.

[0017] 3. In response to the selected clay and glaze, this invention also adjusts the bisque firing and glaze firing processes accordingly, ultimately producing a high-strength daily-use ceramic. This overcomes the shortcomings of traditional ceramics, eliminates the need for high-cost raw materials such as yttrium oxide-stabilized zirconium oxide, ensures low energy consumption in the firing process, effectively utilizes ceramic waste, and significantly improves the strength and thermal shock resistance of the produced ceramic, thus possessing good market competitiveness. Detailed Implementation

[0018] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below in conjunction with embodiments. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0019] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. The terminology used in this specification is for the purpose of describing particular embodiments only and is not intended to limit the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0020] Example 1 A method for preparing high-strength ceramics, comprising the following steps: 1. Weigh the clay and glaze raw materials according to the following proportions by weight: Clay: 32 parts quartz sand, 28 parts kaolin, 15 parts ceramic kiln slag (commercially available, main chemical composition: SiO2 63.4%, Al2O3 16.7%, MgO 7.2%, K2O 3.9%, Na2O 4.5%, ZnO 1.8%, the same below), 6 parts red clay, 5 parts lepidolite, 2.6 parts copper-based alloy powder (Cr 5.9%, Si 4.2%, Mn 2.8%, Co 1.3%, balance Cu), 1.3 parts aluminum borate fiber. Glaze: 20 parts ceramic kiln slag, 12 parts potassium feldspar, 6 parts leucite, 6 parts zircon, 4.5 parts calcite, 0.5 parts aluminum titanate.

[0021] 2. Crush and mix the raw clay, then add zirconia balls and wet grind for 24 hours (material to ball ratio of 1:9). Then, sieve the resulting slurry, knead the clay, and age it (adjust the moisture content to 18%). Take the resulting slurry, pour it into molds, and after the clay blanks are dried, transfer them into the furnace. Under an air atmosphere, heat the clay from room temperature to 605℃ at 5℃ / min, and then continue to heat it to 960℃ at 2℃ / min and hold it for 40 minutes for bisque firing. After natural cooling, the bisque fired blanks are obtained.

[0022] 3. Crush and mix the glaze raw materials, then wet-mill with zirconia balls for 72 hours (material-to-ball ratio of 1:4). The resulting glaze slurry is then sieved and aged (adjusting the specific gravity to 1.7 g / cm³). 3 (Flow rate 42 s); the glaze slurry is dipped onto the surface of the bisque-fired body (thickness 0.6 mm), and after drying, a glazed body is obtained; the glazed body is placed in a furnace and heated from room temperature to 1010℃ at 5℃ / min in an air atmosphere, and then heated to 1140℃ at 1℃ / min and held for 30 min; after the holding period, it is first cooled to 800℃ at 4℃ / min, and then the cooling rate is reduced to 1.5℃ / min and cooled to room temperature to obtain the ceramic product.

[0023] Example 2 A method for preparing high-strength ceramics, comprising the following steps: 1. Weigh the clay and glaze raw materials according to the specified weight proportions. The raw materials are as follows: Clay: 28 parts quartz sand, 26 parts kaolin, 12 parts ceramic kiln slag (commercially available, main chemical composition: SiO2 63.4%, Al2O3 16.7%, MgO 7.2%, K2O 3.9%, Na2O 4.5%, ZnO 1.8%, the same below), 5 parts red clay, 3 parts lepidolite, 2 parts copper-based alloy powder (Cr 6.2%, Si 3.3%, Mn 3.1%, Co 0.8%, balance Cu), 1 part aluminum borate fiber. Glaze: 16 parts ceramic kiln slag, 8 parts potassium feldspar, 4 parts leucite, 5 parts zircon, 3 parts calcite, 0.2 parts aluminum titanate.

[0024] 2. Crush and mix the raw clay, then add zirconia balls and wet grind for 24 hours (material to ball ratio of 1:9). Then, sieve the resulting slurry, knead the clay, and age it (adjust the moisture content to 18%). Take the resulting slurry, pour it into molds, and after the clay blanks are dried, transfer them into the furnace. Under an air atmosphere, heat the clay from room temperature to 595℃ at 4℃ / min, and then continue to heat it to 950℃ at 2℃ / min and hold it for 45 minutes for bisque firing. After natural cooling, the bisque fired blanks are obtained.

[0025] 3. Crush and mix the glaze raw materials, then wet-mill with zirconia balls for 72 hours (material-to-ball ratio of 1:4). The resulting glaze slurry is then sieved and aged (adjusting the specific gravity to 1.7 g / cm³). 3 (Flow rate 42 s); the glaze slurry is dipped onto the surface of the bisque-fired body (thickness 0.6 mm), and after drying, a glazed body is obtained; the glazed body is placed in a furnace and heated from room temperature to 1040℃ at 6℃ / min in an air atmosphere, and then heated to 1180℃ at 0.5℃ / min and held for 25 min; after the holding period, it is first cooled to 800℃ at 5℃ / min, and then the cooling rate is reduced to 1℃ / min and cooled to room temperature to obtain the ceramic product.

[0026] Example 3 A method for preparing high-strength ceramics, comprising the following steps: 1. Weigh the clay and glaze raw materials according to the following proportions by weight: Clay: 34 parts quartz sand, 32 parts kaolin, 18 parts ceramic kiln slag (commercially available, main chemical composition: SiO2 64.9%, Al2O3 17.1%, MgO 6.9%, K2O 3.8%, Na2O 4.4%, ZnO 1.9%, the same below), 8 parts red clay, 6 parts lepidolite, 3.2 parts copper-based alloy powder (Cr 5.9%, Si 4.2%, Mn 2.8%, Co 1.3%, balance Cu), 1.5 parts aluminum borate fiber. Glaze: 24 parts ceramic kiln slag, 15 parts potassium feldspar, 8 parts leucite, 7 parts zircon, 6 parts calcite, 0.8 parts aluminum titanate.

[0027] 2. Crush and mix the raw clay, then add zirconia balls and wet grind for 24 hours (material to ball ratio of 1:9). Then, sieve the resulting slurry, knead the clay, and age it (adjust the moisture content to 18%). Take the resulting slurry, pour it into molds, and after the clay blanks are dried, transfer them into the furnace. Under an air atmosphere, heat the clay from room temperature to 610℃ at 6℃ / min, and then continue to heat it to 980℃ at 3℃ / min and hold it for 30 minutes for bisque firing. After natural cooling, the bisque fired blanks are obtained.

[0028] 3. Crush and mix the glaze raw materials, then wet-mill with zirconia balls for 72 hours (material-to-ball ratio of 1:4). The resulting glaze slurry is then sieved and aged (adjusting the specific gravity to 1.7 g / cm³). 3(Flow rate 42 s); the glaze slurry is dipped onto the surface of the bisque-fired body (thickness 0.6 mm), and after drying, a glazed body is obtained; the glazed body is placed in a furnace and heated from room temperature to 980℃ at 5℃ / min in an air atmosphere, and then heated to 1160℃ at 1.5℃ / min and held for 30 min; after the holding period, it is first cooled to 820℃ at 4℃ / min, and then the cooling rate is reduced to 1.5℃ / min and cooled to room temperature to obtain the ceramic product.

[0029] Comparative Example 1 Referring to the steps and parameters of Example 1 of this application, the only difference is that ceramic kiln slag is not added to the raw material of the clay. The specific formula is: 40 parts of quartz sand, 35 parts of kaolin, 6 parts of red clay, 5 parts of lepidolite, 2.6 parts of copper-based alloy powder, and 1.3 parts of aluminum borate fiber.

[0030] Comparative Example 2 Referring to the steps and parameters of Example 1 of this application, the only difference is that copper-based alloy powder is not added to the raw material of the clay.

[0031] Comparative Example 3 Referring to the steps and parameters of Example 1 of this application, the only difference is that lepidolite is not added to the raw material of the clay.

[0032] Comparative Example 4 Referring to the step parameters of Embodiment 1 of this application, the only difference is that the bisque firing adopts a one-stage heating method: heating from room temperature to 960°C at a rate of 3.2°C / min and holding for 40 min.

[0033] Comparative Example 5 Referring to the steps and parameters of Example 1 of this application, the only difference is that the gradient glazing is adjusted as follows: the temperature is raised from room temperature to 1140°C at 3.5°C / min in an air atmosphere and held for 30 min; after the holding period, the temperature is cooled to room temperature at 3°C / min.

[0034] Test case The ceramic samples prepared in Examples 1-3 and Comparative Examples 1-5 were subjected to performance tests, and the results are shown in Table 1 (the bending strength was tested using the three-point bending method, the water absorption rate was tested according to GB / T 3299-2011, the thermal shock resistance was tested according to GB / T 3298-2022, and the wear resistance was tested using the Taber abrasion tester).

[0035] Table 1. Test results of ceramic sample performance

[0036] The test results above show that the ceramic samples prepared in this invention possess high strength, high hardness, and high wear resistance, especially excellent thermal shock resistance, meeting the performance requirements of a wider range of applications. This invention not only effectively utilizes ceramic waste to partially replace ore raw materials, but also rationally combines other raw materials with corresponding firing processes to achieve a stable bond between the body and glaze layers. It eliminates the need for high-cost raw materials such as yttrium oxide-stabilized zirconium oxide, ensuring low energy consumption in the firing process and giving it strong market competitiveness.

[0037] The embodiments described above are merely preferred embodiments of the present invention, and while the descriptions are specific and detailed, they are not intended to limit the present invention. It should be noted that various changes and modifications can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the concept and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for preparing high-strength ceramics, characterized in that, Includes the following steps: Step 1: Mix and wet grind the raw materials for the clay, pour the resulting slurry into the clay body to form a clay body, bisque-fired and cooled to obtain a bisque-fired clay body; Step 2: Weigh and mix the raw materials of the glaze, then wet grind them. Apply the resulting glaze slurry to the surface of the bisque-fired body to obtain a glazed body. Step 3: Transfer the glazed blank into the kiln for gradient glazing and cooling to obtain the finished ceramic product; The clay, by weight, comprises the following raw materials: 28-34 parts quartz sand, 26-32 parts kaolin, 12-18 parts ceramic kiln slag, 5-8 parts red clay, 3-6 parts lepidolite, 2-3.2 parts copper-based alloy powder, and 1-1.5 parts aluminum borate fiber; the glaze, by weight, comprises the following raw materials: 16-24 parts ceramic kiln slag, 8-15 parts potassium feldspar, 4-8 parts leucite, 5-7 parts zircon, 3-6 parts calcite, and 0.2-0.8 parts aluminum titanate; the copper-based alloy powder, by weight percentage, comprises: Cr 5.5%-6.5%, Si 3.0%-4.8%, Mn 2.4%-3.5%, Co 0.8%-1.6%, balance being Cu; the main chemical composition of the ceramic kiln slag is: SiO2 62.0%-65.2%, Al2O3 15.4%-18.0%, MgO 6.8%-7.6%, K2O 3.7%-4.4%, Na2O 4.0%-4.7%, ZnO 1.6%-1.9%; The bisque firing process parameters are as follows: under an air atmosphere, the temperature is first raised from room temperature to 595-610℃ at a rate of 4-6℃ / min, and then raised to 950-980℃ at a rate of 2-3℃ / min and held for 30-45 minutes for bisque firing. After holding, the temperature is naturally cooled to room temperature. The gradient glaze firing process parameters are as follows: under an air atmosphere, the temperature is first raised from room temperature to 980-1040℃ at a rate of 5-6℃ / min, and then raised to 1120-1180℃ at a rate of 0.5-1.5℃ / min and held for 25-35 minutes. After holding, the temperature is first cooled to 800-820℃ at a rate of 4-5℃ / min, and then the cooling rate is reduced to 1-1.5℃ / min and the temperature is further cooled to room temperature.

2. The method of claim 1, wherein, The clay is prepared by weight of the following raw materials: 32 parts quartz sand, 28 parts kaolin, 15 parts ceramic kiln slag, 6 parts red clay, 5 parts lepidolite, 2.6 parts copper-based alloy powder, and 1.3 parts aluminum borate fiber.

3. The preparation method according to claim 1, characterized in that, Step two: Apply glaze to a thickness of 0.4-0.8 mm.

Citation Information

Patent Citations

  • High-strength multi-purpose ceramic production technique

    CN104961439A

  • High-plasticity daily heat-resistant ceramic and preparation method thereof

    CN106380176A

  • High-hardness domestic ceramic and production process thereof