Resin composition and method for producing connected structure

By using a resin composition containing thermosetting components, flux, and solder particles, the problem of inaccurate semiconductor chip positioning in laser transfer printing was solved, achieving efficient inter-electrode connection and reliable insulation.

CN121002591APending Publication Date: 2025-11-21SEKISUI CHEMICAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202480011775.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-06-26
Filing Date
2024-06-24
Publication Date
2025-11-21

AI Technical Summary

Technical Problem

When using laser transfer to configure semiconductor chips, it is difficult to accurately position the semiconductor chips at the specified locations on the circuit board, resulting in failure of conductive connections between electrodes.

Method used

A resin composition containing thermosetting components, flux, solder particles, and rubber particles is used to accurately capture and connect semiconductor chips to a circuit board via laser transfer. The connection between electrodes is achieved by heating the flux and solder particles above their melting points.

Benefits of technology

It improves the capture and positioning accuracy of semiconductor chips, reduces damage to circuit boards, and ensures the reliability of conductive connections and insulation between electrodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121002591A_ABST
    Figure CN121002591A_ABST
Patent Text Reader

Abstract

The invention provides a resin composition capable of improving trapping performance of a semiconductor chip (3) flying at a high speed. This resin composition (11) contains a thermosetting component (11B), a flux (11D), solder particles (11A), and rubber particles (11C), wherein the flux has an average particle diameter of 10 [mu] m or less.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to a resin composition containing solder particles. In addition, the present application relates to a manufacturing method of a connection structure using the resin composition. BACKGROUND

[0002] Anisotropic conductive paste and anisotropic conductive film and the like anisotropic conductive materials are well known. In the anisotropic conductive material, conductive particles are dispersed in an adhesive. As the conductive particles, solder particles are widely used.

[0003] The anisotropic conductive material is used for obtaining various connection structures. As the connection of the anisotropic conductive material, for example, a connection of a flexible printed board and a glass board (FOG (Film on Glass)), a connection of a semiconductor chip and a flexible printed board (COF (Chip on Film)), a connection of a semiconductor chip and a glass board (COG (Chip on Glass)), and a connection of a flexible printed board and a glass epoxy board (FOB (Film on Board)) and the like can be cited.

[0004] In recent years, miniaturization and weight reduction of devices using a connection structure are progressing. Along with this, development of a connection structure using a fine semiconductor chip such as a micro-light emitting diode chip is required. As a method of disposing a fine semiconductor chip such as a micro-light emitting diode chip on a circuit board, a laser transfer method is attracting attention.

[0005] A laser transfer device is disclosed in Patent Literature 1 described below. In the laser transfer device, a transfer source substrate on which a plurality of elements are formed is disposed above a transfer destination substrate. By irradiating laser light from above to the transfer source substrate, a plurality of transfer target elements which are a plurality of elements of the plurality of elements as a transfer target are moved downward, and the transfer target elements are transferred to the transfer destination substrate.

[0006] A transfer method of transferring a chip component held to a transfer substrate via an adhesive layer of light curability to a transfer destination substrate is disclosed in Patent Literature 2 described below. The transfer method comprises: an exposure step of performing pattern exposure of the adhesive layer with light of a wavelength that causes the adhesive layer to cure, to locally reduce the adhesion of the adhesive layer; and a laser lift-off step of transferring the chip component to the transfer destination substrate by a laser lift-off method after the exposure step.

[0007] PRIOR ART DOCUMENTS

[0008] PATENT LITERATURE

[0009] Patent Literature 1: WO 2020 / 188780 A1

[0010] Patent Literature 2: Japanese Patent Application Publication No. 2020-53558 SUMMARY

[0011] PROBLEMS TO BE SOLVED BY THE INVENTION

[0012] In a method of arranging semiconductor chips using a laser transfer method, a plurality of semiconductor chips can be moved and mounted on a circuit substrate (transfer destination substrate) from a wafer substrate (transfer source substrate) at once, and thus the productivity of a connection structure can be improved.

[0013] However, in a method of arranging semiconductor chips using a laser transfer method, the semiconductor chips flying at high speed sometimes cannot be accurately arranged at a prescribed position on a circuit substrate (connection object member) due to an impact when the semiconductor chips land on the circuit substrate (connection object member). If a positional deviation occurs at the time of arrangement of the semiconductor chips, the conductive connection between the electrodes above and below sometimes cannot be made.

[0014] An object of the present application is to provide a resin composition capable of improving the catchability of semiconductor chips flying at high speed. In addition, an object of the present application is to provide a method of manufacturing a connection structure using the resin composition.

[0015] MEANS OF SOLVING THE PROBLEMS

[0016] The present inventors and others have conducted intensive studies, and as a result, have found that by arranging a specific resin composition on the surface of a circuit substrate (connection object member), semiconductor chips flying at high speed by a laser transfer method or the like can be caught well.

[0017] In the present specification, the following resin composition and a method of manufacturing a connection structure using the resin composition are disclosed.

[0018] Item 1. A resin composition comprising a thermosetting component, a flux, solder particles, and rubber particles, the average particle diameter of the flux being 10 μm or less.

[0019] Item 2. A resin composition comprising a thermosetting component, a flux, solder particles, and rubber particles, the tack force of the resin composition at 25°C and 50% RH being 150 N or more.

[0020] Item 3. The resin composition according to item 1 or 2, wherein the glass transition temperature of the rubber particles is 25°C or less.

[0021] Item 4. The resin composition according to any one of items 1 to 3, wherein the average particle diameter of the rubber particles is 1 μm or less.

[0022] Item 5. The resin composition according to any one of items 1 to 4, wherein, in 100% by weight of the resin composition, the content of the rubber particles is 1% by weight or more and 10% by weight or less.

[0023] Item 6. The resin composition according to any one of items 1 to 5, wherein the thermosetting component comprises a thermosetting compound, and the content of the rubber particles is 2 parts by weight or more and 20 parts by weight or less relative to 100 parts by weight of the thermosetting compound.

[0024] Item 7. A method for manufacturing a connecting structure, comprising: a first configuration step in which a resin composition, as described in any one of items 1 to 6, is configured on the surface of a first connecting member having at least one first electrode; a second configuration step in which a second connecting member having at least one second electrode on its surface is moved to a surface of the resin composition opposite to the side of the first connecting member by means of a laser transfer method, and the second connecting member is configured such that the first electrode and the second electrode are opposite to each other; and a connection step in which the resin composition is heated to above the melting point of the solder particles to form a connection portion that connects the first connecting member and the second connecting member, and the first electrode and the second electrode are electrically connected by the solder portion in the connection portion.

[0025] Item 8. The method for manufacturing a connecting structure according to Item 7, wherein, in the second configuration step, the second connecting object component is moved at a speed of 1 cm / s or more to the surface of the resin composition opposite to the side of the first connecting object component by means of laser transfer, and the second connecting object component is configured such that the first electrode and the second electrode are opposite to each other.

[0026] Invention Effects

[0027] The resin composition of the present invention comprises a thermosetting component, a flux, solder particles, and rubber particles, wherein the average particle size of the flux is 10 μm or less. Due to the aforementioned configuration, the resin composition of the present invention can improve the capture performance of semiconductor chips arriving at high speeds.

[0028] Furthermore, the resin composition of the present invention comprises thermosetting components, flux, solder particles, and rubber particles, and the initial tack of the resin composition at 25°C and 50% RH is 150 N or more. In the resin composition of the present invention, due to the aforementioned structure, the capture performance of high-speed incoming semiconductor chips can be improved. Attached Figure Description

[0029] Figure 1is a cross-sectional view schematically showing a connection structure body obtained using the resin composition according to an embodiment of the present application.

[0030] Figure 2 is a cross-sectional view showing a process for explaining a method of manufacturing a connection structure body using the resin composition according to an embodiment of the present application.

[0031] Figure 3 is a cross-sectional view showing a process for explaining a method of manufacturing a connection structure body using the resin composition according to an embodiment of the present application.

[0032] Figure 4 is a cross-sectional view showing a process for explaining a method of manufacturing a connection structure body using the resin composition according to an embodiment of the present application.

[0033] Figure 5 is a cross-sectional view showing a modification of the connection structure body. DETAILED DESCRIPTION

[0034] Hereinafter, the present application will be described in detail.

[0035] (Resin composition)

[0036] The resin composition of the present application contains a thermosetting component, a flux, solder particles, and rubber particles. In the resin composition of the present application, the average particle diameter of the flux is 10 μm or less.

[0037] In addition, the resin composition of the present application contains a thermosetting component, a flux, solder particles, and rubber particles. In the resin composition of the present application, the initial tack of the resin composition at 25°C and 50% RH is 150 N or more.

[0038] In the past, in a method of arranging a semiconductor chip using a laser transfer method, damage has sometimes occurred on the surface of a circuit substrate (connection target member) due to the impact when a high-speed flying semiconductor chip lands on the circuit substrate (connection target member), or the semiconductor chip has sometimes not been accurately arranged at a prescribed site on the circuit substrate (connection target member). If a positional deviation occurs at the time of arrangement of the semiconductor chip, the conductive connection between the upper and lower electrodes has sometimes not been possible.

[0039] In the resin composition of the present application, because of the above-described configuration, the catchability of a high-speed flying semiconductor chip can be improved. In particular, the catchability of a high-speed flying semiconductor chip by a laser transfer method can be improved. As a result, the flying semiconductor chip can be accurately arranged at a prescribed site on a circuit substrate (connection target member) (the positional deviation at the time of arrangement of the semiconductor chip is effectively suppressed).

[0040] Further, in the resin composition of the present application, since the above configuration is provided, it is possible to absorb the impact when the semiconductor chip lands on the circuit substrate (connection target member), and effectively suppress damage to the surface of the circuit substrate (connection target member).

[0041] In the present application, in order to obtain the above effects, the use of a specific resin composition is very contributory.

[0042] In the manufacturing method of the connection structure, the resin composition is used by being disposed on the surface of the connection target member (circuit substrate, substrate to be transferred). In the manufacturing method of the connection structure, the resin composition is preferably used for good capture of the semiconductor chip flying at high speed by the laser transfer method. The resin composition is preferably a resin composition for semiconductor chip capture by the laser transfer method.

[0043] In particular, the resin composition of the present application is suitable for connection of a semiconductor chip by the laser transfer method (use of the resin composition for connection of a semiconductor chip by the laser transfer method). More specifically, the resin composition of the present application is more suitable for connection of a semiconductor chip to a substrate by the laser transfer method (use of the resin composition for connection of a semiconductor chip to a substrate by the laser transfer method).

[0044] The initial tack of the resin composition at 25°C and 50% RH is 150 N or more. The initial tack of the resin composition at 25°C and 50% RH is preferably 200 N or more, more preferably 250 N or more, further preferably 300 N or more, preferably 750 N or less, more preferably 700 N or less, further preferably 650 N or less. If the initial tack of the resin composition at 25°C and 50% RH is the lower limit or more, the capture property of the semiconductor chip flying at high speed by the laser transfer method can be further improved. If the initial tack of the resin composition at 25°C and 50% RH is the upper limit or less, the resin composition can be thinly and favorably coated on the surface of the connection target member, and the cohesiveness of the solder at the time of conductive connection can be effectively improved.

[0045] The initial tack of the resin composition at 25°C and 50% RH can be measured, for example, by the following method. The resin composition is coated on the surface of a glass substrate at a thickness of 250 μm. Using a tack tester (for example, manufactured by RHESCA Corporation), the initial tack is measured at 25°C and 50% RH in an environment, under conditions of a probe diameter of 5.1 mm and a speed of 2.5 mm / minute.

[0046] The initial tack of the resin composition at 25°C and 50% RH can be adjusted by, for example, the following methods. A method of adjusting the particle size of the flux. A method of selecting the kind of rubber particles. A method of adjusting the particle size of the rubber particles.

[0047] The resin composition is preferably in a liquid state at 25°C. The paste is contained in the liquid state. The resin composition is preferably in a paste state at 25°C. The resin composition contains solder particles, and is therefore an electrically conductive material. The resin composition is preferably an electrically conductive paste. The resin composition is preferably an electrically conductive paste at 25°C. In these cases, the resin composition can be thinly and favorably applied to the surface of the connection target member, the catchability of the semiconductor chip flying at high speed by the laser transfer method can be more effectively improved, and the cohesiveness of the solder at the time of electrically conductive connection can be more effectively improved.

[0048] The viscosity of the resin composition at 25°C (η25) is preferably 30 Pa-s or more, more preferably 50 Pa-s or more, and is preferably 250 Pa-s or less, more preferably 200 Pa-s or less. If the viscosity (η25) is the lower limit or more, the catchability of the semiconductor chip flying at high speed by the laser transfer method can be more effectively improved. If the viscosity (η25) is the upper limit or less, the resin composition can be thinly and favorably applied to the surface of the connection target member, and the cohesiveness of the solder at the time of electrically conductive connection can be effectively improved. The viscosity (η25) can be appropriately adjusted depending on the kind and the amount of the blending component.

[0049] The viscosity (η25) can be measured at 25°C and 5 rpm, for example, using an E-type viscometer (TVE-22L manufactured by Tokimec Inc.).

[0050] The viscosity of the resin composition at the melting point of the solder particles (ηmp) is preferably 0.1 Pa-s or more, more preferably 1 Pa-s or more, and is preferably 10 Pa-s or less, more preferably 5 Pa-s or less. The viscosity (ηmp) can be appropriately adjusted depending on the kind and the amount of the blending component. If the viscosity (ηmp) is the lower limit or more and the upper limit or less, the cohesiveness of the solder at the time of electrically conductive connection can be more effectively improved, the void at the connection portion can be more effectively suppressed, and the overflow of the resin composition to the outside of the connection portion can be more effectively suppressed. If the viscosity (ηmp) is the lower limit or more and the upper limit or less, the insulation reliability between the electrodes can be more effectively improved, and the conduction reliability between the electrodes can be more effectively improved.

[0051] The viscosity (ηmp) can be measured, for example, using a viscoelasticity measuring device (HAAKE manufactured by SCIENTIFIC) under conditions of stress control 1 Pa, frequency 1 Hz, temperature increase rate 20°C / min, and measurement temperature range 25°C to 200°C. However, in the case where the melting point of the solder particle exceeds 200°C, the upper limit of the temperature is set to the melting point of the solder particle. In this measurement, the viscosity (ηmp) is calculated by reading the viscosity at the melting point of the solder particle.

[0052] The resin composition can be used as an electrically conductive paste, an electrically conductive film, and the like. The electrically conductive paste is preferably an anisotropic conductive paste, and the electrically conductive film is preferably an anisotropic conductive film. From the viewpoint of more effectively suppressing positional deviation at the time of arranging the connection target member and more effectively improving the cohesiveness of the solder at the time of electrically conductive connection, the resin composition is preferably in a paste form, and is preferably an electrically conductive paste. The resin composition is suitable for use in electrical connection of electrodes. The resin composition is preferably a circuit connecting material.

[0053] Hereinafter, each component contained in the resin composition will be described. In the present specification, the term "(meth)acrylate" means acrylate and methacrylate. The term "(meth)acrylic" means acrylic and methacrylic. The term "(meth)acryloyl" means acryloyl and methacryloyl.

[0054] (Thermosetting Component)

[0055] The resin composition of the present application contains a thermosetting component. The thermosetting component preferably contains a thermosetting compound. The resin composition can contain a thermosetting agent as the thermosetting component, or can not contain a thermosetting agent as the thermosetting component. In the resin composition of the present application, since the constitution described above is provided, even in the case where the resin composition does not contain a thermosetting agent, the catchability of a semiconductor chip flying at high speed by the laser transfer method can be improved. From the viewpoint of more effectively improving the cohesiveness of the solder at the time of electrically conductive connection, the resin composition preferably does not contain a thermosetting agent. In order to more favorably cure the resin composition, the resin composition can contain a curing accelerator as the thermosetting component.

[0056] (Thermosetting Component: Thermosetting Compound)

[0057] The resin composition of the present application preferably contains a thermosetting compound. The thermosetting compound is a compound capable of being cured by heating. The thermosetting compound is not particularly limited. As the thermosetting compound, there can be mentioned oxetane compounds, epoxy compounds, episulfide compounds, (meth)acrylic compounds, phenol compounds, amino compounds, unsaturated polyester compounds, polyurethane compounds, polysiloxane compounds, and polyimide compounds, etc. From the viewpoint of bettering the curability and viscosity of the resin composition, further improving the conduction reliability, as the thermosetting compound, an epoxy compound or an episulfide compound is preferred, and an epoxy compound is more preferred. The resin composition preferably contains an epoxy compound or an episulfide compound, and more preferably contains an epoxy compound. The thermosetting compound can be used singly or in combination of two or more.

[0058] The epoxy compound is a compound having at least one epoxy group. As the epoxy compound, there can be mentioned bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, bisphenol S type epoxy compounds, phenol novolak type epoxy compounds, biphenyl type epoxy compounds, biphenyl novolak type epoxy compounds, biphenol type epoxy compounds, naphthalene type epoxy compounds, fluorene type epoxy compounds, phenol aralkyl type epoxy compounds, naphthol aralkyl type epoxy compounds, dicyclopentadiene type epoxy compounds, anthracene type epoxy compounds, adamantane skeleton-containing epoxy compounds, tricyclodecane skeleton-containing epoxy compounds, naphthalene ether type epoxy compounds, and epoxy compounds having a triazine nucleus in the skeleton, etc. The epoxy compound can be used singly or in combination of two or more.

[0059] The epoxy compound is in a liquid state or is a solid at ordinary temperature (25°C), and in the case where the epoxy compound is a solid at ordinary temperature, the melting temperature of the epoxy compound is preferably below the melting point of the solder particle. By using the preferred epoxy compound, the viscosity is high at the stage of attaching the connection target member, and when acceleration is imparted due to an impact such as conveyance, the positional displacement of the connection target member (circuit board) and the semiconductor chip can be suppressed. Further, by the heat at the time of curing, the viscosity of the resin composition can be greatly reduced, and the aggregation of the solder at the time of conductive connection can be efficiently performed.

[0060] From the viewpoint of more effectively improving the insulation reliability, more effectively improving the conduction reliability, the thermosetting component preferably contains an epoxy compound, and the thermosetting compound preferably contains an epoxy compound.

[0061] From the viewpoint of more effectively disposing the solder on the electrode, the thermosetting compound preferably contains a thermosetting compound having a polyether skeleton.

[0062] As the thermosetting compound having a polyether skeleton, a compound having glycidyl ether groups at both ends of an alkyl chain having 3 to 12 carbon atoms, a polyether-type epoxy compound having a polyether skeleton having 2 to 4 carbon atoms and having 2 to 10 structural units formed by continuous bonding of the polyether skeleton, and the like can be given.

[0063] From the viewpoint of more effectively improving the heat resistance of the cured product, the thermosetting compound preferably contains a thermosetting compound having an isocyanuric acid skeleton.

[0064] As the thermosetting compound having an isocyanuric acid skeleton, a triisocyanurate-type epoxy compound and the like can be given, and the TEPIC series (TEPIC-G, TEPIC-S, TEPIC-SS, TEPIC-HP, TEPIC-L, TEPIC-PAS, TEPIC-VL, and TEPIC-UC) manufactured by Nissan Chemical Industries, Ltd., and the like can be given.

[0065] From the viewpoint of more efficiently disposing the solder on the electrodes, the viewpoint of more effectively improving the conduction reliability between the upper and lower electrodes to be connected, and the viewpoint of more effectively suppressing discoloration of the thermosetting compound, the thermosetting compound preferably has high heat resistance, and more preferably contains a novolac-type epoxy compound. The novolac-type epoxy compound has high heat resistance.

[0066] The content of the thermosetting compound in the resin composition 100% by weight is preferably 5% by weight or more, more preferably 8% by weight or more, further preferably 10% by weight or more, and is preferably 99% by weight or less, more preferably 90% by weight or less, further preferably 80% by weight or less, and particularly preferably 70% by weight or less. When the content of the thermosetting compound is the lower limit or more and the upper limit or less, the catchability of the semiconductor chip flying at high speed by the laser transfer method can be more effectively improved, the solder can be more efficiently disposed on the electrodes, the insulation reliability between the electrodes can be more effectively improved, and the conduction reliability between the electrodes can be more effectively improved. From the viewpoint of more effectively improving the impact resistance of the obtained connected structure, it is preferable that the content of the thermosetting compound be large.

[0067] The content of the epoxy compound in the resin composition is preferably 5% by weight or more, more preferably 8% by weight or more, further preferably 10% by weight or more, and preferably 99% by weight or less, more preferably 90% by weight or less, further preferably 80% by weight or less, and particularly preferably 70% by weight or less. When the content of the epoxy compound is within the above range, the capturing property of a semiconductor chip flying at high speed by the laser transfer method can be more effectively improved, the solder can be more efficiently disposed on the electrode, the insulation reliability between electrodes can be more effectively improved, and the conduction reliability between electrodes can be more effectively improved. From the viewpoint of further improving the impact resistance of the resulting connection structure, it is preferable that the content of the epoxy compound be large.

[0068] The content of the novolac epoxy compound in the resin composition is preferably 1% by weight or more, more preferably 3% by weight or more, further preferably 5% by weight or more, and preferably 99% by weight or less, more preferably 90% by weight or less, further preferably 80% by weight or less, and particularly preferably 70% by weight or less. When the content of the novolac epoxy compound is within the above range, the capturing property of a semiconductor chip flying at high speed by the laser transfer method can be more effectively improved, the solder can be more efficiently disposed on the electrode, the insulation reliability between electrodes can be more effectively improved, and the conduction reliability between electrodes can be more effectively improved. From the viewpoint of further improving the impact resistance of the resulting connection structure, it is preferable that the content of the novolac epoxy compound be large.

[0069] (Soldering flux)

[0070] The resin composition contains a soldering flux. By using a soldering flux, the cohesiveness of the solder at the time of conductive connection can be more effectively improved.

[0071] The soldering flux is not particularly limited. As the soldering flux, for example, a soldering flux generally used in solder joining and the like can be used.

[0072] As the soldering flux, zinc chloride, a mixture of zinc chloride and an inorganic halide, a mixture of zinc chloride and an inorganic acid, a molten salt, phosphoric acid, a derivative of phosphoric acid, an organic acid, an amine salt of an organic acid, an organic halide, a hydrazine compound different from the amine salt of an organic acid, and rosin can be given. The soldering flux can be used alone or in combination with two or more kinds.

[0073] As the molten salt, ammonium chloride and the like can be given.

[0074] As the organic acid, lactic acid, citric acid, stearic acid, glutamic acid, and glutaric acid can be given.

[0075] As the organic acid amine salt, for example, glutaric acid benzylamine salt, adipic acid benzylamine salt, azelaic acid benzylamine salt, glutaric acid stearylamine salt, adipic acid stearylamine salt, and azelaic acid stearylamine salt can be given.

[0076] As the amine compound other than the organic acid amine salt, for example, dicyclohexylamine, benzylamine, benzylmethylamine, imidazole, benzimidazole, phenylimidazole, carboxybenzimidazole, benzotriazole, and carboxybenzotriazole can be given.

[0077] As the rosin, for example, activated rosin and non-activated rosin can be given. The rosin is a rosin acid class in which abietic acid is a main component. As the rosin acid class, for example, abietic acid and acrylic acid-modified rosin can be given.

[0078] From the viewpoint of more efficiently disposing the solder on the electrode, more effectively improving the insulation reliability, and more effectively improving the conduction reliability, the flux preferably contains a salt of an acid compound and a base compound, and preferably contains an organic acid amine salt. From the viewpoint of more efficiently disposing the solder on the electrode, more effectively improving the insulation reliability, and more effectively improving the conduction reliability, the organic acid amine salt is preferably a carboxylic acid amine salt, and more preferably an organic acid amine salt having two or more carboxyl groups.

[0079] As the organic acid in the organic acid amine salt having two or more carboxyl groups, for example, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid can be given.

[0080] The acid compound is preferably an organic compound having a carboxyl group. As the acid compound, for example, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, citric acid, malic acid, cyclohexyl carboxylic acid, 1,4-cyclohexyl dicarboxylic acid, isophthalic acid, terephthalic acid, trimellitic acid, and ethylenediaminetetraacetic acid as aliphatic carboxylic acids, and cyclohexyl carboxylic acid, 1,4-cyclohexyl dicarboxylic acid, isophthalic acid, terephthalic acid, trimellitic acid, and ethylenediaminetetraacetic acid as aromatic carboxylic acids can be given. From the viewpoint of more efficiently disposing the solder on the electrode, more effectively improving the insulation reliability, and more effectively improving the conduction reliability, the acid compound is preferably glutaric acid, cyclohexyl carboxylic acid, or adipic acid.

[0081] The base compound is preferably an organic compound having an amino group. As the base compound, for example, diethanolamine, triethanolamine, methyldiethanolamine, ethyldiethanolamine, cyclohexylamine, dicyclohexylamine, benzylamine, benzylmethylamine, 2-methylbenzylamine, 3-methylbenzylamine, 4-tert-butylbenzylamine, N-methylbenzylamine, N-ethylbenzylamine, N-phenylbenzylamine, N-tert-butylbenzylamine, N-isopropylbenzylamine, N,N-dimethylbenzylamine, imidazole compounds, and triazole compounds can be given. From the viewpoint of more efficiently disposing the solder on the electrode, more effectively improving the insulation reliability, and more effectively improving the conduction reliability, the base compound is preferably benzylamine.

[0082] The flux is preferably solid. The flux can be spherical, can be other than spherical, and can be flat.

[0083] The average particle diameter of the flux is 10 μm or less. The average particle diameter of the flux is preferably 7 μm or less, more preferably 5 μm or less, and further preferably 3 μm or less. When the average particle diameter of the flux is the upper limit or less, the catchability of the semiconductor chip flying at high speed by the laser transfer method can be more effectively improved. The lower limit of the average particle diameter of the flux is not particularly limited. The average particle diameter of the flux can be 0.01 μm or more, can be 0.1 μm or more, can be 0.5 μm or more, and can be 1.0 μm or more. The range of the average particle diameter of the flux can be set by appropriately selecting the lower limit value and the upper limit value. Note that, in the case where the flux contains two or more kinds of fluxes, the average particle diameter of the flux indicates the average particle diameter in the entire flux.

[0084] The average particle diameter of the flux is the number average particle diameter. The average particle diameter of the flux is calculated, for example, by observing any 50 fluxes under an electron microscope or an optical microscope, calculating the average of the particle diameters of the respective fluxes, or by laser diffraction particle size distribution measurement. In the observation under the electron microscope or the optical microscope, the particle diameter of each flux is found as the particle diameter under the equivalent circle diameter. In the observation under the electron microscope or the optical microscope, the average particle diameter under the equivalent circle diameter of any 50 fluxes is approximately equal to the average particle diameter under the equivalent sphere diameter. In the laser diffraction particle size distribution measurement, the particle diameter of each flux is found as the particle diameter under the equivalent sphere diameter. The average particle diameter of the flux is preferably calculated by the laser diffraction particle size distribution measurement.

[0085] The flux having an average particle diameter of 10 μm or less can be a pulverized product of a commercially available flux. As a method of pulverizing a commercially available flux, there are a method of pulverizing with an agate mortar, a method of pulverizing with a jet mill, and a method of pulverizing with a bead mill.

[0086] The coefficient of variation (CV value) of the particle diameter of the flux is preferably 10% or less, and more preferably 5% or less. When the coefficient of variation of the particle diameter of the flux is the upper limit or less, the flux can be more efficiently disposed on the electrode. The lower limit of the coefficient of variation (CV value) of the particle diameter of the flux is not particularly limited. The coefficient of variation (CV value) of the particle diameter of the flux can be 0% or more, can be 1% or more, and can be 5% or more. The range of the coefficient of variation of the particle diameter of the flux can be set by appropriately selecting the lower limit value and the upper limit value.

[0087] The coefficient of variation (CV value) of the particle diameter of the flux can be determined as follows.

[0088] CV (%) = (p / Dn) x 100

[0089] p: standard deviation of particle diameter of the flux

[0090] Dn: average value of particle diameter of the flux

[0091] The active temperature (melting point) of the flux is preferably 50°C or higher, more preferably 70°C or higher, further preferably 80°C or higher, and is preferably 200°C or lower, more preferably 190°C or lower, further preferably 180°C or lower. If the active temperature of the flux is the lower limit or higher and the upper limit or lower, the flux effect is more effectively exerted, and the solder is more efficiently disposed on the electrode. The active temperature (melting point) of the flux is preferably 70°C or higher and 190°C or lower, and particularly preferably 80°C or higher and 180°C or lower.

[0092] The active temperature (melting point) of the flux can be found by differential scanning calorimetry (DSC). As the differential scanning calorimetry (DSC) device, "EXSTAR DSC7020" manufactured by SII Co., Ltd. or the like can be given.

[0093] As the flux having an active temperature (melting point) of 80°C or higher and 180°C or lower, dicarboxylic acids such as glutaric acid (melting point 96°C), glutaric acid benzylamine salt (melting point 108°C), adipic acid (melting point 152°C), adipic acid benzylamine salt (melting point 180°C), pimelic acid (melting point 104°C), and suberic acid (melting point 142°C), benzoic acid (melting point 122°C), and malic acid (melting point 130°C) or the like can be given.

[0094] In addition, the boiling point of the flux is preferably 200°C or lower.

[0095] The flux can be dispersed in the resin composition, or can be attached to the surface of the solder particle.

[0096] The flux is preferably a flux that releases a cation by heating. By using a flux that releases a cation by heating, the solder can be more efficiently disposed on the electrode.

[0097] The content of the flux in the resin composition 100% by weight is preferably 0.5% by weight or more, more preferably 1% by weight or more, further preferably 5% by weight or more, particularly preferably 10% by weight or more, and is preferably 30% by weight or less, more preferably 25% by weight or less. If the content of the flux is the lower limit or more and the upper limit or less, an oxide film is less likely to be formed on the surface of the solder and the electrode, and furthermore, the oxide film formed on the surface of the solder and the electrode can be more effectively removed.

[0098] (Solder particle)

[0099] The resin composition contains solder particles. The central portion and the outer surface of the solder particles are each formed of solder. The solder particles are particles in which the central portion and the outer surface are solder. In a case where the conductive particles having the base particle formed of a material other than solder and the solder portion disposed on the surface of the base particle are used instead of the solder particles, the conductive particles are difficult to be aggregated on the electrode. In addition, in the conductive particles, since the solder joinability between the conductive particles is low, there is a tendency that the conductive particles moved to the electrode easily move outside the electrode.

[0100] The solder is preferably a metal having a melting point of 450°C or lower (low-melting-point metal). The solder particles are preferably metal particles having a melting point of 450°C or lower (low-melting-point metal particles). The low-melting-point metal particles are particles containing a low-melting-point metal. The low-melting-point metal means a metal having a melting point of 450°C or lower. The melting point of the low-melting-point metal is preferably 300°C or lower, more preferably 220°C or lower, and further preferably 190°C or lower.

[0101] The melting point of the solder particles is preferably 100°C or higher, more preferably 105°C or higher, and preferably 250°C or lower, and more preferably 245°C or lower. If the melting point of the solder particles is the lower limit or more and the upper limit or less, the cohesiveness of the solder at the time of conductive connection can be more effectively improved. If the melting point of the solder particles is the lower limit or more and the upper limit or less, in a case where the electrodes are electrically connected, the conduction reliability can be more effectively improved, and the insulation reliability can be more effectively improved.

[0102] The melting point of the solder particles can be found by differential scanning calorimetry (DSC). As the differential scanning calorimetry (DSC) device, "EXSTAR DSC7020" manufactured by SII Co., Ltd., or the like can be given.

[0103] The solder particles preferably contain 90% by weight or more of solder in 100% by weight of the solder particles. In addition, the solder particles preferably contain tin. The content of tin is preferably 30% by weight or more, more preferably 40% by weight or more, further preferably 70% by weight or more, and particularly preferably 90% by weight or more, in 100% by weight of the metal contained in the solder particles. If the content of tin in the solder particles is the lower limit or more, the connection reliability of the solder portion to the electrode can be more effectively improved.

[0104] Note that the content of tin can be measured using a high-frequency inductively coupled plasma emission spectrometry device ("ICP-AES" manufactured by HORIBA, Ltd.), a fluorescent X-ray analysis device ("EDX-800 HS" manufactured by Shimadzu Corporation), or the like.

[0105] By using the solder particles, the solder is melted to be joined with the electrode, and the solder portion makes the electrodes conductive. For example, the solder portion easily makes surface contact with the electrode without making point contact with the electrode, and thus the connection resistance becomes low. In addition, by using the solder particles, the joining strength of the solder portion with the electrode becomes high, and as a result, peeling of the solder portion from the electrode is less likely to occur, and the conduction reliability and the connection reliability can be more effectively improved.

[0106] The low-melting-point metal constituting the solder particles is not particularly limited. The low-melting-point metal is preferably tin or an alloy containing tin. The alloy can include, for example, a tin-silver alloy, a tin-copper alloy, a tin-silver-copper alloy, a tin-bismuth alloy, a tin-zinc alloy, and a tin-indium alloy. Since the wettability with respect to the electrode is excellent, the low-melting-point metal is preferably tin, a tin-silver alloy, a tin-silver-copper alloy, a tin-bismuth alloy, or a tin-indium alloy. The low-melting-point metal is more preferably a tin-bismuth alloy or a tin-indium alloy.

[0107] The solder particles are preferably a filler metal having a liquidus of 450°C or lower based on JIS Z3001: Welding Terms. As the composition of the solder particles, for example, a metal composition containing zinc, gold, silver, lead, copper, tin, bismuth, indium, or the like can be given. The solder particles are preferably lead-free, and preferably contain tin and indium or contain tin and bismuth.

[0108] In order to more effectively improve the joining strength of the solder portion with the electrode, the solder particles can also contain metals such as nickel, copper, antimony, aluminum, zinc, iron, gold, titanium, phosphorus, germanium, tellurium, cobalt, bismuth, manganese, chromium, molybdenum, and palladium. In addition, from the viewpoint of further improving the joining strength of the solder portion with the electrode, the solder particles preferably contain nickel, copper, antimony, aluminum, or zinc. From the viewpoint of more effectively improving the joining strength of the solder portion with the electrode, the content of these metals for improving the joining strength is preferably 0.0001% by weight or more and preferably 1% by weight or less, in 100% by weight of the metals contained in the solder particles.

[0109] The average particle diameter of the solder particles is preferably 0.01 μm or more and more preferably 0.03 μm or more. If the average particle diameter of the solder particles is the lower limit or more, the solder can be more efficiently disposed on the electrode. The average particle diameter of the solder particles can be 5 μm or less or 3 μm or less. The range of the average particle diameter of the solder particles can be set by appropriately selecting the lower limit value and the upper limit value.

[0110] The average particle diameter of the solder particles is a number average particle diameter. The average particle diameter of the solder particles is obtained, for example, by observing any 50 solder particles with an electron microscope or an optical microscope, calculating the average of the particle diameters of the respective solder particles, or performing laser diffraction particle size distribution measurement. In the observation with the electron microscope or the optical microscope, the particle diameter of each solder particle is obtained as the particle diameter under the equivalent circle diameter. In the observation with the electron microscope or the optical microscope, the average particle diameter under the equivalent circle diameter of any 50 solder particles is approximately equal to the average particle diameter under the equivalent sphere diameter. In the laser diffraction particle size distribution measurement, the particle diameter of each solder particle is obtained as the particle diameter under the equivalent sphere diameter. The average particle diameter of the solder particles is preferably calculated by the laser diffraction particle size distribution measurement.

[0111] The coefficient of variation (CV value) of the particle diameters of the solder particles is preferably 5% or more, more preferably 10% or more, and is preferably 40% or less, more preferably 30% or less. If the coefficient of variation of the particle diameters of the solder particles is the lower limit or more and the upper limit or less, the solder can be more efficiently disposed on the electrodes. However, the CV value of the particle diameters of the solder particles can be less than 5%.

[0112] The coefficient of variation (CV value) can be measured as follows.

[0113] CV value (%) = (p / Dn) x 100

[0114] p: standard deviation of the particle diameters of the solder particles

[0115] Dn: average value of the particle diameters of the solder particles

[0116] The shape of the solder particles is not particularly limited. The shape of the solder particles can be spherical, can be a shape other than spherical, or can be flat.

[0117] The content of the solder particles in the resin composition 100% by weight is preferably 1% by weight or more, more preferably 2% by weight or more, further preferably 10% by weight or more, particularly preferably 20% by weight or more, most preferably 30% by weight or more, and is preferably 80% by weight or less, more preferably 60% by weight or less, further preferably 50% by weight or less. If the content of the solder particles is the lower limit or more and the upper limit or less, the solder can be more efficiently disposed on the electrodes, the solder can be easily disposed in a large amount between the electrodes, and the conduction reliability can be more effectively improved. From the viewpoint of more effectively improving the conduction reliability, it is preferable that the content of the solder particles be large.

[0118] (Rubber particles)

[0119] The resin composition contains rubber particles. The rubber particles are preferably insoluble in a solvent such as an organic solvent. The rubber particles are preferably not compatible with the components in the resin composition such as a thermosetting component. In the resin composition, the rubber particles are preferably present in a dispersed state. In electrically conductive joining, the rubber particles preferably do not hinder the coagulation of solder particles. In electrically conductive joining, the rubber particles are preferably not incorporated into a solder portion (a solder solidification formed by the coagulation of molten solder particles after the melting of the solder particles). The rubber particles can be particles having a core-shell structure or particles not having a core-shell structure. The core-shell structure is a structure having a core and a shell disposed on the surface of the core. In the case where the rubber particles are particles having the core-shell structure, it is preferable that, at the interface between the core and the shell, a compound constituting the core and a compound constituting the shell are chemically bonded. The chemical bonding is preferably graft bonding. The rubber particles can be used singly or in combination of two or more kinds.

[0120] The material of the rubber particles is not particularly limited. As the material of the rubber particles, for example, polyolefin resins such as polyethylene, polypropylene, polystyrene, polyvinyl chloride, polyvinylidene chloride, polyisobutylene, and polybutadiene; (meth)acrylic resins such as polymethyl methacrylate and polymethyl acrylate; polycarbonates, polyamides, phenol formaldehyde resins, melamine formaldehyde resins, benzoguanamine formaldehyde resins, urea formaldehyde resins, phenol formaldehyde resins, melamine resins, benzoguanamine resins, urea formaldehyde resins, epoxy resins, unsaturated polyester resins, saturated polyester resins, polyethylene terephthalate, polysulfones, polyphenylene ether, polyacetals, polyimides, polyamide-imides, polyether ether ketone, polyether sulfone, divinylbenzene polymers, and divinylbenzene-based copolymers, and the like can be given. As the divinylbenzene-based copolymers and the like, divinylbenzene-styrene copolymers, divinylbenzene-(meth)acrylate copolymers, and the like can be given. Since the hardness of the rubber particles can be easily controlled in an appropriate range, the rubber particles are preferably polymers in which one or two or more kinds of polymerizable monomers having an ethylenic unsaturated group are polymerized.

[0121] In the case where the rubber particles are obtained by polymerizing a polymerizable monomer having an ethylenic unsaturated group, as the polymerizable monomer having an ethylenic unsaturated group, non-crosslinking monomers and crosslinking monomers can be given.

[0122] As the non-crosslinkable monomer, for example, styrene-based monomers such as styrene, α-methylstyrene, and the like; carboxyl group-containing monomers such as (meth)acrylic acid, maleic acid, maleic anhydride, and the like; (meth)acrylic acid alkyl ester compounds such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, and the like; oxygen atom-containing (meth)acrylate compounds such as 2-hydroxyethyl (meth)acrylate, glyceryl (meth)acrylate, polyoxyethylene (meth)acrylate, glycidyl (meth)acrylate, and the like; nitrile-containing monomers such as (meth)acrylonitrile; vinyl ether compounds such as methyl vinyl ether, ethyl vinyl ether, propyl vinyl ether, and the like; acid vinyl ester compounds such as vinyl acetate, vinyl butyrate, vinyl laurate, vinyl stearate, and the like; unsaturated hydrocarbons such as ethylene, propylene, isoprene, butadiene, and the like; halogen-containing monomers such as trifluoromethyl (meth)acrylate, pentafluoroethyl (meth)acrylate, chlorovinyl, fluorovinyl, chlorostyrene, and the like, and the like can be exemplified.

[0123] As the crosslinkable monomer, for example, multifunctional (meth)acrylate compounds such as tetramethylolmethane tetra(meth)acrylate, tetramethylolmethane tri(meth)acrylate, tetramethylolmethane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate, glycerol tri(meth)acrylate, glycerol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, (poly)tetramethylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, and the like; silane-containing monomers such as triallyl (iso)cyanurate, trimellitic acid triallyl ester, divinylbenzene, diallyl phthalate, diallyl acrylamide, diallyl ether, γ-(meth)acryloxypropyltrimethoxysilane, trimethoxysilylphenylethylene, vinyltrimethoxysilane, and the like; and the like can be exemplified.

[0124] The rubber particles can be obtained by polymerizing the polymerizable monomer having an ethylenic unsaturated group by using a known method. As the method, for example, a method of performing suspension polymerization in the presence of a radical polymerization initiator, a method of swelling a monomer with a radical polymerization initiator using a non-crosslinkable seed particle to perform polymerization, and the like can be exemplified.

[0125] The rubber particles preferably include divinylbenzene-based polymer particles, silicone rubber particles, polybutadiene rubber particles, or acrylic rubber particles, more preferably include divinylbenzene-based polymer particles, polybutadiene rubber particles, or acrylic rubber particles, further preferably include polybutadiene rubber particles or acrylic rubber particles. By using these rubber particles, the catchability of a semiconductor chip flying at high speed by the laser transfer method can be further improved.

[0126] The glass transition temperature of the rubber particles is preferably -90°C or higher, more preferably -75°C or higher, further preferably -60°C or higher, preferably 25°C or lower, more preferably 15°C or lower, further preferably 5°C or lower, particularly preferably -5°C or lower. If the glass transition temperature of the rubber particles is the lower limit or higher, the positional deviation at the arrangement of the connection target member can be more efficiently suppressed. If the glass transition temperature of the rubber particles is the upper limit or lower, the cohesiveness of the solder at the conductive connection can be more efficiently improved, and the rubber particles can be more efficiently prevented from being taken into the solder portion.

[0127] The glass transition temperature of the rubber particles can be measured using dynamic viscoelasticity measurement (ARES-G2 manufactured by TA Instruments, Inc.), or the like.

[0128] The average particle diameter of the rubber particles is preferably 1 μm or lower, more preferably 0.8 μm or lower, further preferably 0.5 μm or lower. The lower limit of the average particle diameter of the rubber particles is not particularly limited. The average particle diameter of the rubber particles can be 0.03 μm or higher, or 0.1 μm or higher. If the average particle diameter of the rubber particles is the upper limit or lower, the positional deviation at the arrangement of the connection target member can be more efficiently suppressed. If the average particle diameter of the rubber particles is the upper limit or lower, the cohesiveness of the solder at the conductive connection can be more efficiently improved, and the rubber particles can be more efficiently prevented from being taken into the solder portion. By efficiently preventing the rubber particles from being taken into the solder portion, the conduction reliability can be more efficiently improved. The range of the particle diameter of the rubber particles can be set by appropriately selecting the lower limit value and the upper limit value.

[0129] The average particle diameter of the rubber particles is a number average particle diameter. The average particle diameter of the rubber particles is, for example, calculated by observing any 50 rubber particles under an electron microscope or an optical microscope, calculating the average of the particle diameters of the respective rubber particles, or performing laser diffraction type particle size distribution measurement. In the observation under the electron microscope or the optical microscope, the particle diameter of each rubber particle is calculated as the particle diameter under the equivalent circle diameter. In the observation under the electron microscope or the optical microscope, the average particle diameter under the equivalent circle diameter of any 50 solder particles is approximately equal to the average particle diameter under the equivalent sphere diameter. In the laser diffraction type particle size distribution measurement, the particle diameter of each rubber particle is calculated as the particle diameter under the equivalent sphere diameter. The average particle diameter of the rubber particles is preferably calculated by the laser diffraction type particle size distribution measurement.

[0130] In the resin composition, the ratio of the average particle diameter of the rubber particles to the average particle diameter of the solder particles (average particle diameter of rubber particles / average particle diameter of solder particles) is preferably 3.0 or less, more preferably 2.0 or less. The lower limit of the ratio (average particle diameter of rubber particles / average particle diameter of solder particles) is not particularly limited. The ratio (average particle diameter of rubber particles / average particle diameter of solder particles) can be 0.001 or more. If the ratio (average particle diameter of rubber particles / average particle diameter of solder particles) is the lower limit or more and the upper limit or less, the positional deviation at the arrangement of the connection target members can be more effectively suppressed. If the ratio (average particle diameter of rubber particles / average particle diameter of solder particles) is the lower limit or more and the upper limit or less, the cohesiveness of the solder at the conductive connection can be more effectively improved, and the rubber particles can be effectively prevented from being taken into the solder portion. By effectively preventing the rubber particles from being taken into the solder portion, the conduction reliability can be more effectively improved. The range of the ratio (average particle diameter of rubber particles / average particle diameter of solder particles) can be set by appropriately selecting the lower limit value and the upper limit value.

[0131] In the particle size distribution of the rubber particles on a volume basis, the D90 of the rubber particles is preferably 3 μm or less, more preferably 2 μm or less, and further preferably 1 μm or less. The lower limit of the D90 of the rubber particles is not particularly limited. The D90 of the rubber particles can be 0.01 μm or more or 0.03 μm or more. In the particle size distribution of the rubber particles on a volume basis, if the D90 of the rubber particles is the upper limit or less, the gap between the connection target members further decreases. The range of the D90 of the rubber particles can be set by appropriately selecting the lower limit value and the upper limit value.

[0132] Note that the D90 of the rubber particles is the particle diameter of the rubber particles at which the cumulative volume of the rubber particles is 90%. The D90 of the rubber particles can be calculated from the particle size distribution on a volume basis.

[0133] The particle size distribution of the rubber particles on a volume basis is measured using a laser diffraction particle size distribution measuring device. As the laser diffraction particle size distribution measuring device, "Mastersizer 3000" manufactured by Malvern Co., Ltd. or the like can be mentioned.

[0134] The content of the rubber particles in 100% by weight of the resin composition is preferably 0.5% by weight or more, more preferably 1% by weight or more, further preferably 1.5% by weight or more, preferably 10% by weight or less, more preferably 8% by weight or less, further preferably 5% by weight or less, particularly preferably 4% by weight or less. If the content of the rubber particles is the lower limit or more, the catchability of the semiconductor chip flying at high speed by the laser transfer method can be further improved. If the content of the rubber particles is the upper limit or less, the resin composition can be thinly and favorably applied to the surface of the connection target member.

[0135] The content of the rubber particles is preferably 1 parts by weight or more, more preferably 2 parts by weight or more, further preferably 3 parts by weight or more, with respect to 100 parts by weight of the thermosetting component, preferably 20 parts by weight or less, more preferably 16 parts by weight or less, further preferably 10 parts by weight or less. If the content of the rubber particles is the lower limit or more, the catchability of the semiconductor chip flying at high speed by the laser transfer method can be further improved. If the content of the rubber particles is the upper limit or less, the resin composition can be thinly and favorably applied to the surface of the connection target member.

[0136] In the case where the thermosetting component contains the thermosetting compound, the content of the rubber particles is preferably 2 parts by weight or more, more preferably 4 parts by weight or more, further preferably 6 parts by weight or more, with respect to 100 parts by weight of the thermosetting compound, preferably 20 parts by weight or less, more preferably 16 parts by weight or less, further preferably 10 parts by weight or less. If the content of the rubber particles is the lower limit or more, the catchability of the semiconductor chip flying at high speed by the laser transfer method can be further improved. If the content of the rubber particles is the upper limit or less, the resin composition can be thinly and favorably applied to the surface of the connection target member.

[0137] (Filler)

[0138] The resin composition can contain a filler. The filler can be an organic filler or an inorganic filler. By adding a filler, the solder can be more uniformly aggregated on all the electrodes of the connection target member.

[0139] The resin composition preferably does not contain the filler, or contains the filler in an amount of 5% by weight or less. In the case where the resin composition contains the thermosetting compound, the less the content of the filler, the more easily the solder particles move to the electrode.

[0140] The content of the filler in the resin composition of 100% by weight is preferably 5% by weight or less, more preferably 2% by weight or less, further preferably 1% by weight or less, and most preferably 0% by weight (not contained). If the content of the filler is the upper limit or less, the solder is more uniformly disposed on the electrode.

[0141] (Other components)

[0142] The resin composition can contain various additives such as extenders, softeners, plasticizers, thickening agents, thixotropic agents, leveling agents, polymerization catalysts, curing catalysts, colorants, antioxidants, heat stabilizers, light stabilizers, ultraviolet absorbers, lubricants, antistatic agents, and flame retardants, as needed.

[0143] (Connected structure and method for manufacturing connected structure)

[0144] The connected structure of the present application includes a first connection target member having a first electrode on a surface thereof, a second connection target member having a second electrode on a surface thereof, and a connection portion connecting the first connection target member and the second connection target member. In the connected structure of the present application, the material of the connection portion is the resin composition. In the connected structure of the present application, the first electrode and the second electrode are electrically connected through a solder portion in the connection portion.

[0145] In the connected structure of the present application, since a specific resin composition is used, the solder easily gathers between the first electrode and the second electrode, and the solder can be efficiently disposed on the electrodes (wires). In addition, a part of the solder is less likely to be disposed in a region (space) where no electrode is formed, and the amount of the solder disposed in the region where no electrode is formed can be made quite small. Therefore, the conduction reliability between the first electrode and the second electrode can be improved. Moreover, the electrical connection between the electrodes adjacent in a direction in which connection is not possible can be prevented, and the insulation reliability can be improved.

[0146] In addition, in order to efficiently dispose the solder on the electrodes and make the amount of the solder disposed in the region where no electrode is formed quite small, the resin composition preferably uses a conductive paste rather than a conductive film.

[0147] In the connected structure, the first connection target member is preferably a circuit substrate. In the connected structure, the second connection target member is preferably a semiconductor chip.

[0148] The manufacturing method of the connection structure of the present application has the following steps. (1) A first arrangement step of arranging the resin composition on the surface of a first connection target member having at least one first electrode on the surface using the resin composition. (2) A second arrangement step of moving a second connection target member having at least one second electrode on the surface to the surface of the resin composition opposite to the first connection target member side by a laser transfer method to arrange the second connection target member in a manner that the first electrode and the second electrode face each other. (3) A connection step of forming a connection portion connecting the first connection target member and the second connection target member by the resin composition by heating the resin composition to a temperature above the melting point of the solder particles, and electrically connecting the first electrode and the second electrode by a solder portion in the connection portion.

[0149] In the manufacturing method of the connection structure of the present application, since the above configuration is provided, the capturing property of the second connection target member (semiconductor chip) flying at high speed by the laser transfer method can be improved.

[0150] Hereinafter, a specific embodiment of the present application will be described with reference to the drawings.

[0151] Figure 1 is a cross-sectional view schematically showing a connection structure obtained using the resin composition of an embodiment of the present application.

[0152] Figure 1 The connection structure 1 shown in the figure has a first connection target member 2, a second connection target member 3, and a connection portion 4 connecting the first connection target member 2 and the second connection target member 3. The connection portion 4 is formed of the resin composition.

[0153] In the present embodiment, the resin composition contains a thermosetting component, a flux, solder particles, and rubber particles. The flux contains a flux having an average particle diameter of 10 μm or less. In the present embodiment, as the resin composition, a conductive paste is used.

[0154] The connection portion 4 has a solder portion 4A in which a plurality of solder particles are aggregated and joined to each other, and a cured product portion 4B in which the thermosetting component is thermally cured.

[0155] The rubber particles are preferably present in the cured product portion 4B. Note that the rubber particles can also be present in the solder portion 4A in a small amount.

[0156] The first connecting member 2 has a plurality of first electrodes 2a on its surface (upper surface). The second connecting member 3 has a plurality of second electrodes 3a on its surface (lower surface). The first electrodes 2a and the second electrodes 3a are electrically connected through a solder section 4A. Therefore, the first connecting member 2 and the second connecting member 3 are electrically connected through the solder section 4A. It should be noted that in the connecting section 4, there is no solder in the area different from the solder section 4A (the cured portion 4B) that is concentrated between the first electrodes 2a and the second electrodes 3a. There is no solder separated from the solder section 4A in the area different from the solder section 4A (the cured portion 4B). It should be noted that, if the amount is small, solder may be present in the area different from the solder section 4A (the cured portion 4B) that is concentrated between the first electrodes 2a and the second electrodes 3a.

[0157] like Figure 1 As shown, in the connection structure 1, multiple solder particles gather between the first electrode 2a and the second electrode 3a. After the solder particles melt, the molten solder particles wet and spread on the surface of the electrodes and then solidify to form a solder portion 4A. Therefore, the connection area between the solder portion 4A and the first electrode 2a, and between the solder portion 4A and the second electrode 3a, becomes larger. That is, by using solder particles, compared to the case where conductive particles with an outer surface portion of a conductive part made of metals such as nickel, gold, or copper are used, the contact area between the solder portion 4A and the first electrode 2a, and between the solder portion 4A and the second electrode 3a, becomes larger. Therefore, the conductivity reliability and connection reliability in the connection structure 1 are higher. It should be noted that the flux contained in the resin composition is usually gradually deactivated by heating.

[0158] It should be noted that, in Figure 1 In the connection structure 1 shown, the solder part 4A is entirely located in the opposing area between the first and second electrodes 2a and 3a. Figure 5 The modified example shown has a connection structure 1X with only the connecting part 4X connected to it. Figure 1 The connection structure 1 shown is different. The connection portion 4X has a solder portion 4XA and a cured portion 4XB. Alternatively, as with the connection structure 1X, most of the solder portion 4XA may be located in the region opposite to the first and second electrodes 2a and 3a, and a portion of the solder portion 4XA may extend laterally from the region opposite to the first and second electrodes 2a and 3a. The solder portion 4XA extending laterally from the region opposite to the first and second electrodes 2a and 3a is part of the solder portion 4XA, not solder separated from the solder portion 4XA. It should be noted that in this embodiment, the amount of solder far from the solder portion can be reduced, but solder far from the solder portion may also exist in the cured portion.

[0159] If the amount of the solder particles is reduced, the connection structure 1 is easily obtained. If the amount of the solder particles is increased, the connection structure 1X is easily obtained.

[0160] The thickness of the solder portion between the first electrode and the second electrode is preferably 10 μm or more, more preferably 20 μm or more, and is preferably 100 μm or less, more preferably 80 μm or less. In the first electrode and the second electrode, the solder wetted area on the surface of the electrode (the area contacted by the solder in 100% of the area exposed by the electrode) is preferably 50% or more, more preferably 60% or more, and further preferably 70% or more, and is preferably 100% or less. By causing the solder portion in the connection portion to satisfy the preferable mode, the on-reliability and the insulation reliability can be more effectively improved.

[0161] In the connection structure 1, 1X, when the mutually opposing portions of the first electrode 2a and the second electrode 3a are observed in the stacking direction of the first electrode 2a and the connection portion 4, 4X and the second electrode 3a, it is preferable that the solder portion 4A, 4XA in the connection portion 4, 4X is disposed in 50% or more of 100% of the area of the mutually opposing portions of the first electrode 2a and the second electrode 3a. By causing the solder portion 4A, 4XA in the connection portion 4, 4X to satisfy the preferable mode, the on-reliability can be further improved.

[0162] When the mutually opposing portions of the first electrode and the second electrode are observed in the stacking direction of the first electrode, the connecting portion, and the second electrode, it is preferable that the solder portion in the connecting portion be provided in 50% or more of the area 100% of the mutually opposing portions of the first electrode and the second electrode. When the mutually opposing portions of the first electrode and the second electrode are observed in the stacking direction of the first electrode, the connecting portion, and the second electrode, it is more preferable that the solder portion in the connecting portion be provided in 60% or more of the area 100% of the mutually opposing portions of the first electrode and the second electrode. When the mutually opposing portions of the first electrode and the second electrode are observed in the stacking direction of the first electrode, the connecting portion, and the second electrode, it is further preferable that the solder portion in the connecting portion be provided in 70% or more of the area 100% of the mutually opposing portions of the first electrode and the second electrode. When the mutually opposing portions of the first electrode and the second electrode are observed in the stacking direction of the first electrode, the connecting portion, and the second electrode, it is particularly preferable that the solder portion in the connecting portion be provided in 80% or more of the area 100% of the mutually opposing portions of the first electrode and the second electrode. When the mutually opposing portions of the first electrode and the second electrode are observed in the stacking direction of the first electrode, the connecting portion, and the second electrode, it is most preferable that the solder portion in the connecting portion be provided in 90% or more of the area 100% of the mutually opposing portions of the first electrode and the second electrode. By causing the solder portion in the connecting portion to satisfy the preferable manner, the conduction reliability can be further improved.

[0163] When the mutually opposing portions of the first electrode and the second electrode are observed in a direction orthogonal to the stacking direction of the first electrode, the connecting portion, and the second electrode, it is preferable that 60% or more of the solder portion in the connecting portion be arranged in the mutually opposing portions of the first electrode and the second electrode. When the mutually opposing portions of the first electrode and the second electrode are observed in a direction orthogonal to the stacking direction of the first electrode, the connecting portion, and the second electrode, it is more preferable that 70% or more of the solder portion in the connecting portion be arranged in the mutually opposing portions of the first electrode and the second electrode. When the mutually opposing portions of the first electrode and the second electrode are observed in a direction orthogonal to the stacking direction of the first electrode, the connecting portion, and the second electrode, it is further preferable that 90% or more of the solder portion in the connecting portion be arranged in the mutually opposing portions of the first electrode and the second electrode. When the mutually opposing portions of the first electrode and the second electrode are observed in a direction orthogonal to the stacking direction of the first electrode, the connecting portion, and the second electrode, it is particularly preferable that 95% or more of the solder portion in the connecting portion be arranged in the mutually opposing portions of the first electrode and the second electrode. When the mutually opposing portions of the first electrode and the second electrode are observed in a direction orthogonal to the stacking direction of the first electrode, the connecting portion, and the second electrode, it is most preferable that 99% or more of the solder portion in the connecting portion be arranged in the mutually opposing portions of the first electrode and the second electrode. By causing the solder portion in the connecting portion to satisfy the preferable manner, the conduction reliability can be further improved.

[0164] Next, referring to Figures 2-4 An example of a method of manufacturing the connection structure 1 using the resin composition according to an embodiment of the present application will be described. Figures 2-4 is a cross-sectional view for explaining each process of an example of a method of manufacturing a connection structure using the resin composition according to an embodiment of the present application.

[0165] First, a first connection target member (circuit board) 2 having a first electrode 2a on a surface (upper surface) is prepared. Next, as shown in Figure 2 A resin composition 11 (first arrangement process) containing a thermosetting component 11B, solder particles 11A, rubber particles 11C, and a flux 11D is arranged on the surface of the first connection target member (circuit board) 2. The thermosetting component 11B contains a thermosetting compound.

[0166] A resin composition 11 is disposed on the surface of the first connection component (circuit board) 2 where the first electrode 2a is provided. After the resin composition 11 is disposed, solder particles 11A, rubber particles 11C, and flux 11D are disposed on both the first electrode 2a (line) and the area (space) where the first electrode 2a is not formed. It should be noted that the resin composition may be disposed only on the surface of the first electrode.

[0167] There are no particular limitations on the preparation method of the resin composition 11. Examples of preparation methods for the resin composition 11 include coating using a dispenser, screen printing, and ejection using an inkjet device.

[0168] Additionally, a second connection target member (semiconductor chip) 3 having a second electrode 3a on its surface (lower surface) is prepared. The second connection target member (semiconductor chip) 3 having a second electrode 3a on its surface (lower surface) is disposed on the surface of the transfer source substrate on the side of the support film 6, which includes the support member 5 and the support film 6. The second connection target member (semiconductor chip) 3 having a second electrode 3a on its surface (lower surface) is disposed on the surface of the support film 6.

[0169] Next, as Figure 3 As shown, in the resin composition 11 on the surface of the first connecting member (circuit substrate) 2, a second connecting member (semiconductor chip) 3 is moved to the surface of the resin composition 11 opposite to the side of the first connecting member (circuit substrate) 2 by laser transfer, and the second connecting member (semiconductor chip) 3 is disposed (second placement step). The second connecting member (semiconductor chip) 3 is disposed on the surface of the resin composition 11 from the side of the second electrode 3a. In the second placement step, by irradiating the support member 5 side of the transfer source substrate with a laser using a laser irradiation device 51, the curing reaction of the curable component (resin component) in the support film 6 proceeds, and the adhesion force on the surface of the support film 6 is significantly reduced. As a result, the second connecting member (semiconductor chip) 3 peels off from the transfer source substrate (especially the support film 6) and moves to the surface of the resin composition 11 opposite to the side of the first connecting member (circuit substrate) 2. The second connecting component (semiconductor chip) 3 moves as a single unit, for example, in a state where its surface is not in contact with other components (not held by other components). At this time, the first electrode 2a is positioned opposite the second electrode 3a.

[0170] In the present embodiment, since the resin composition is used, in the second placement step, the catchability of the second connection target member (semiconductor chip) 3 flying at high speed by the laser transfer method can be improved. As a result, the flying second connection target member (semiconductor chip) can be accurately placed on the prescribed site on the first connection target member (circuit board) (the positional deviation at the time of placement of the semiconductor chip is effectively suppressed).

[0171] In addition, in the present embodiment, since the resin composition is used, the impact at the time when the second connection target member (semiconductor chip) lands on the first connection target member (circuit board) can be absorbed, and the damage to the surface of the first connection target member (circuit board) is effectively suppressed.

[0172] Next, the resin composition 11 is heated to a temperature above the melting point of the solder particles 11A. It is preferable to heat the resin composition 11 to a temperature above the curing temperature of the thermosetting component 11B (thermosetting compound). At this heating, the solder particles 11A present in the region where the electrode is not formed are aggregated between the first electrode 2a and the second electrode 3a (self-aggregation effect). In the case where the conductive paste is used instead of the conductive film, the solder particles 11A are more effectively aggregated between the first electrode 2a and the second electrode 3a. In addition, the solder particles 11A are melted and joined to each other. In addition, the thermosetting component 11B is thermally cured. As a result, as shown in FIG. 4, the connection portion 4 connecting the first connection target member (circuit board) 2 and the second connection target member (semiconductor chip) 3 is formed of the resin composition 11. By the resin composition 11 forming the connection portion 4, the solder portion 4A is formed by the joining of a plurality of solder particles 11A, the cured product portion 4B is formed by the thermal curing of the thermosetting component 11B, and the first electrode 2a and the second electrode 3a are electrically connected by the solder portion 4A in the connection portion 4 (connection step). If the solder particles 11A sufficiently move, the temperature can not be kept constant from the start of the movement of the solder particles 11A not present between the first electrode 2a and the second electrode 3a to the completion of the movement of the solder particles 11A between the first electrode 2a and the second electrode 3a. Figure 4

[0173] In the second placement step and the connection step, it is preferable not to perform pressurization. In this case, the weight of the second connection target member (semiconductor chip) 3 is applied to the resin composition 11. Therefore, at the time of formation of the connection portion 4, the solder particles 11A are more effectively aggregated between the first electrode 2a and the second electrode 3a. Note that, in at least one of the second placement step and the connection step, if pressurization is performed, the tendency of the action that hinders the aggregation of the solder particles 11A between the first electrode 2a and the second electrode 3a becomes higher.

[0174] ​In addition, in the present embodiment, since pressurization is not performed, even in a case where the first connection target member (circuit board) 2 and the second connection target member (semiconductor chip) 3 are overlapped in a state where the alignment of the first electrode 2a and the second electrode 3a is slightly shifted, the slight shift can be corrected to connect the first electrode 2a and the second electrode 3a (self-alignment effect). This is because, in a case where the area of the molten solder that self-aggregates between the first electrode 2a and the second electrode 3a contacts other components of the resin composition becomes the minimum, the molten solder becomes stable in energy, and the force of the aligned connection structure having the connection structure as its minimum area acts. At this time, it is preferable that the resin composition not be cured, and that the viscosity of the components other than the solder particles of the resin composition be sufficiently low at the temperature and time.

[0175] Thus, the connection structure body 1 shown in FIG. 1 is obtained. Figure 1 It should be noted that the second arrangement process and the connection process can also be performed consecutively. In addition, after the second arrangement process is performed, the obtained stack of the first connection target member 2, the resin composition 11, and the second connection target member 3 can be moved to a heating section, and the connection process can be performed. In order to perform the heating, the stack can be arranged on a heating member, or the stack can be arranged in a space after heating.

[0176] In the second arrangement process, it is preferable that the second connection target member be moved onto the surface of the resin composition opposite the first connection target member side at a speed of 1 cm / s or more by the laser transfer method, and the second connection target member be arranged in a manner such that the first electrode and the second electrode face each other. In the second arrangement process, it is preferable that the second connection target member be moved onto the surface of the resin composition opposite the first connection target member side at a speed of 5 cm / s or more, more preferably 10 cm / s or more, and further preferably 50 cm / s or more by the laser transfer method. The upper limit of the speed at which the second connection target member is moved by the laser transfer method is not particularly limited. In the laser transfer method in the second arrangement process, the second connection target member can be moved onto the surface of the resin composition opposite the first connection target member side at a speed of 500 cm / s or less. In the second arrangement process, the speed at which the second connection target member is moved onto the surface of the resin composition opposite the first connection target member side by the laser transfer method can be set by appropriately selecting the lower limit value and the upper limit value.

[0177] The heating temperature in the connecting step is preferably 250°C or higher, more preferably 300°C or higher, preferably 450°C or lower, more preferably 400°C or lower, and further preferably 350°C or lower. If the heating temperature in the connecting step is the lower limit or higher and the upper limit or lower, the solder can be more efficiently disposed on the electrodes, and the conduction reliability between the upper and lower electrodes to be connected can be more effectively improved.

[0178] As the heating method in the connecting step, there are a method of heating the entire connection structure to a temperature above the melting point of the solder and above the curing temperature of the thermosetting component using a reflow furnace or an oven, and a method of locally heating only the connection portion of the connection structure to a temperature above the melting point of the solder and above the curing temperature of the thermosetting component.

[0179] As the tool used in the local heating method, there are a hot plate, a hot air gun that blows hot air, a soldering iron, an infrared heater, and the like.

[0180] In addition, when local heating is performed using a hot plate, the upper surface of the hot plate is preferably formed such that the portion directly below the connection portion is formed of a metal having high thermal conductivity, and the other portions to which heat is not preferably applied are formed of a material having low thermal conductivity such as a fluororesin.

[0181] The first and second connection target members are not particularly limited. As the first and second connection target members, there are electronic components such as semiconductor chips, semiconductor packages, capacitors, diodes, and the like, and circuit boards such as resin films, printed boards, flexible printed boards, flexible flat cables, rigid-flexible combined boards, glass epoxy boards, and glass boards. The semiconductor chip can be an LED chip, and the semiconductor package can be an LED package. The second connection target member is preferably an electronic component. The second connection target member is preferably a semiconductor chip, more preferably an LED chip, and further preferably a micro LED chip.

[0182] At least one of the first connection target member and the second connection target member is preferably a resin film, a flexible printed board, a flexible flat cable, or a rigid-flexible combined board. The first connection target member is preferably a resin film, a flexible printed board, a flexible flat cable, or a rigid-flexible combined board. Resin films, flexible printed boards, flexible flat cables, and rigid-flexible combined boards have the properties of being highly flexible and relatively lightweight. In the case where a conductive film is used in the connection of such connection target members, there is a tendency that the solder is difficult to gather on the electrodes. In contrast, by using a conductive paste, even if a resin film, a flexible printed board, a flexible flat cable, or a rigid-flexible combined board is used, the conduction reliability between the electrodes can be sufficiently improved by efficiently gathering the solder on the electrodes.

[0183] As the electrode provided to the connection target member, a metal electrode such as a gold electrode, a nickel electrode, a tin electrode, an aluminum electrode, a copper electrode, a molybdenum electrode, a silver electrode, a SUS electrode, and a tungsten electrode can be given. In the case where the connection target member is a flexible printed board, the electrode is preferably a gold electrode, a nickel electrode, a tin electrode, a silver electrode, or a copper electrode. In the case where the connection target member is a glass substrate, the electrode is preferably an aluminum electrode, a copper electrode, a molybdenum electrode, a silver electrode, or a tungsten electrode. Note that in the case where the electrode is an aluminum electrode, the electrode can be formed of only aluminum or can be an electrode in which an aluminum layer is stacked on the surface of a metal oxide layer. As the material of the metal oxide layer, indium oxide doped with a trivalent metal element and zinc oxide doped with a trivalent metal element can be given. As the trivalent metal element, Sn, Al, Ga, and the like can be given.

[0184] The support member is not particularly limited. As the support member, a glass substrate, a sapphire substrate, a polysiloxane substrate, a metal substrate, an organic substrate, and the like can be given.

[0185] The support film is not particularly limited. As the support film, a polysiloxane resin film, an acrylic resin film, a polyimide resin film, and the like can be given. The support film preferably has an adhesive layer.

[0186] In the second arrangement step, the cumulative light amount of the irradiated laser light is preferably 100 mJ / cm 2 More preferably, the cumulative light amount is 150 mJ / cm 2 Further preferably, the cumulative light amount is 200 mJ / cm 2 Preferably, the cumulative light amount is 400 mJ / cm 2 More preferably, the cumulative light amount is 350 mJ / cm 2 Further preferably, the cumulative light amount is 300 mJ / cm 2 Further. If the cumulative light amount of the laser light irradiated in the second arrangement step is the lower limit or more and the upper limit or less, the catchability of the high-speed incoming semiconductor chip can be further improved.

[0187] The present application will be specifically described below by citing examples and comparative examples. The present application is not limited to the following examples.

[0188] Thermosetting component (thermosetting compound):

[0189] Phenol novolak type epoxy compound ("JER152" manufactured by Mitsubishi Chemical Corporation)

[0190] Hydrogenated bisphenol A type epoxy compound ("YX8000" manufactured by Mitsubishi Chemical Corporation)

[0191] Bisphenol F type epoxy compound ("830-S" manufactured by DIC Corporation)

[0192] flux:

[0193] adipic acid benzylamine salt 1 (average particle diameter 5 μm, melting point 180°C, produced according to the following Synthesis Example 1)

[0194] adipic acid benzylamine salt 2 (average particle diameter 10 μm, melting point 180°C, produced according to the following Synthesis Example 1)

[0195] adipic acid benzylamine salt 3 (average particle diameter 30 μm, melting point 180°C, produced according to the following Synthesis Example 1)

[0196] glutaric acid benzylamine salt (average particle diameter 10 μm, melting point 108°C, produced according to the following Synthesis Example 2)

[0197] Synthesis Example 1:

[0198] A glass bottle was charged with water 24 g as a reaction solvent and adipic acid (manufactured by Fuji Photo Film Co., Ltd. and Wako Pure Chemical Industries, Ltd.) 14.612 g, and heated at 100°C for 10 minutes to dissolve it. Then, benzylamine (manufactured by Fuji Photo Film Co., Ltd. and Wako Pure Chemical Industries, Ltd.) 10.715 g was added, and stirred for about 5 minutes to obtain a mixed solution. The obtained mixed solution was put in a refrigerator at 5°C to 10°C, and left overnight. The crystals that had precipitated were separated by filtration, washed with water, and vacuum-dried to obtain adipic acid benzylamine salt 3 (average particle diameter 30 μm). The obtained adipic acid benzylamine salt 3 was pulverized by a jet mill pulverization method to obtain adipic acid benzylamine salt 1 (average particle diameter 5 μm) and adipic acid benzylamine salt 2 (average particle diameter 10 μm).

[0199] Synthesis Example 2:

[0200] A glass bottle was charged with water 24 g as a reaction solvent and glutaric acid (manufactured by Fuji Photo Film Co., Ltd. and Wako Pure Chemical Industries, Ltd.) 13.212 g, and dissolved at room temperature until uniform. Then, benzylamine (manufactured by Fuji Photo Film Co., Ltd. and Wako Pure Chemical Industries, Ltd.) 10.715 g was added, and stirred for about 5 minutes to obtain a mixed solution. The obtained mixed solution was put in a refrigerator at 5°C to 10°C, and left overnight. The crystals that had precipitated were separated by filtration, washed with water, and vacuum-dried to obtain glutaric acid benzylamine salt. The obtained glutaric acid benzylamine salt was pulverized by a jet mill pulverization method to obtain glutaric acid benzylamine salt (average particle diameter 10 μm).

[0201] solder particles:

[0202] SnAgCu solder particles (solder particles of "Sn96.5Ag3Cu0.5" manufactured by Mitsui Mining Co., Ltd. with a melting point of 220°C, average particle diameter 3 μm)

[0203] SnBi solder particles (solder particles of "Sn42Bi58" manufactured by Mitsui Mining Co., Ltd. with a melting point of 139°C, average particle diameter 3 μm)

[0204] Rubber particles:

[0205] Polybutadiene rubber particles 1 ("C series" manufactured by Mitsubishi Rayon Co., Ltd., glass transition temperature -60°C, average particle diameter 0.2 μm)

[0206] Acrylic rubber particles 1 ("W series" manufactured by Mitsubishi Rayon Co., Ltd., glass transition temperature 0°C, average particle diameter 0.065 μm)

[0207] Acrylic rubber particles 2 ("W series" manufactured by Mitsubishi Rayon Co., Ltd., glass transition temperature 0°C, average particle diameter 0.1 μm)

[0208] Acrylic rubber particles 3 ("W series" manufactured by Mitsubishi Rayon Co., Ltd., glass transition temperature 0°C, average particle diameter 0.25 μm)

[0209] Acrylic rubber particles 4 ("W series" manufactured by Mitsubishi Rayon Co., Ltd., glass transition temperature 0°C, average particle diameter 0.5 μm)

[0210] Divinylbenzene-based polymer particles 1 ("Micropearl-EL series" manufactured by Sekisui Chemical Co., Ltd., no glass transition temperature, average particle diameter 3 μm): Since a crosslinking agent was added, no glass transition temperature was observed

[0211] (Average particle diameters of the flux, solder particles and rubber particles)

[0212] The average particle diameters of the flux, solder particles and rubber particles were measured using a laser diffraction particle size distribution measuring device ("LA-920" manufactured by Horiba, Ltd.).

[0213] (Melting points of the solder particles and the flux)

[0214] The melting points of the solder particles and the flux were calculated using differential scanning calorimetry (DSC). As the differential scanning calorimetry (DSC) device, "EXSTAR DSC7020" manufactured by SII Co., Ltd. was used.

[0215] (Examples 1 to 11 and Comparative Examples 1 and 2)

[0216] (1) Production of the resin composition (anisotropic conductive paste)

[0217] The components shown in Tables 1 to 4 below were formulated in the formulation amounts shown in Tables 1 to 4 below to obtain the resin composition (anisotropic conductive paste).

[0218] (2) Production of the connection structure

[0219] As the first connection object member (circuit board), a glass substrate (thickness: 0.7 mm) having a plurality of electrodes (first electrodes, copper electrodes of 23 pm in lateral direction x 30 pm in longitudinal direction x 12 pm in thickness, 14 pm of electrode-to-electrode space) on the surface was prepared.

[0220] As the second connection object member (semiconductor chip), a micro LED chip (material: GaN, thickness: 0.01 mm) having a plurality of electrodes (second electrodes, gold electrodes of 20 pm in lateral direction x 20 pm in longitudinal direction x 3 pm in thickness, 10 pm of electrode-to-electrode space) on the surface was prepared.

[0221] On the upper surface of the glass substrate, the resin composition (anisotropic conductive paste) immediately after preparation was applied by screen printing in a manner of 10 pm in thickness, and a resin composition (anisotropic conductive paste) layer was formed. Next, the semiconductor chip was laminated on the upper surface of the resin composition (anisotropic conductive paste) layer in a manner of electrodes facing each other by laser transfer method. From this state, heating was performed in a manner that the temperature of the resin composition (anisotropic conductive paste) layer became the melting point of the solder particle 5 seconds after the start of temperature increase. Further, heating was performed in a manner that the temperature of the resin composition (anisotropic conductive paste) layer became 250°C 10 seconds after the start of temperature increase, and the resin composition (anisotropic conductive paste) layer was cured, and a connection structure was obtained. At the time of heating, no pressure was applied.

[0222] (Evaluation)

[0223] (1) Average particle diameter of flux as a whole

[0224] For the obtained resin composition, a laser diffraction type particle size distribution measuring device (HORIBA, Ltd. "LA-920") was used to measure the average particle diameter of the flux as a whole.

[0225] (2) Initial tack of resin composition at 25°C and 50% RH

[0226] For the obtained resin composition, the initial tack at 25°C and 50% RH was measured by the method.

[0227] (3) Screen printability (coatability)

[0228] For the obtained resin composition (anisotropic conductive paste), screen printing was performed on a glass substrate using a metal mask having a size of 114 μm x 60 μm for each opening portion and a thickness of 10 μm. For 50 of the printed patterns, the printed surface immediately after printing was observed with a laser microscope, and the volume of the resin composition applied to the glass substrate was calculated, and the proportion X (%) of the volume of the resin composition applied to the glass substrate with respect to the volume of each opening portion of the metal mask was calculated. The screen printability was determined according to the following criteria.

[0229] [Criteria for determining screen printability]

[0230] O0: X is 50% or more

[0231] O: X is more than 30% and less than 50%

[0232] X: X is less than 30%

[0233] (4) Agglomeration of solder

[0234] Among the obtained connection structures (20), when the mutually opposing portions of the first electrode and the second electrode in the stacking direction of the first electrode, the connection portion, and the second electrode were observed, the proportion of the area of the solder portion in the connection portion in the area 100% of the mutually opposing portions of the first electrode and the second electrode was evaluated. The proportion of the area Y was obtained by averaging 20 values. According to the proportion of the area Y, the agglomeration of the solder at the time of conductive connection was determined according to the following criteria.

[0235] [Criteria for determining agglomeration of solder]

[0236] O0: Y is 70% or more

[0237] O: Y is more than 60% and less than 70%

[0238] △: Y is more than 50% and less than 60%

[0239] X: Y is less than 50%

[0240] (5) Catchability of semiconductor chip

[0241] In "(3) Screen printability", 20 semiconductor chips were arranged so that the first electrode of the glass substrate and the second electrode of the semiconductor chip were opposed to each other, by moving the semiconductor chips at a speed of 1 cm / s onto the surface of the resin composition applied to the glass substrate by screen printing, using the laser transfer method. The proportion Z of the number of semiconductor chips caught at a position within ±3 μm from a prescribed position among 20 semiconductor chips was calculated. The catchability of the semiconductor chip was determined according to the following criteria.

[0242] [Judgment criteria for catchability of semiconductor chips]

[0243] O: Proportion Z is 70% or more

[0244] O: Proportion Z is 50% or more and less than 70%

[0245] X: Proportion Z is less than 50%

[0246] The results are shown in Tables 1 to 4 below.

[0247] [Table 1]

[0248]

[0249] [Table 2]

[0250]

[0251] [Table 3]

[0252]

[0253] [Table 4]

[0254] BRIEF DESCRIPTION OF DRAWINGS

[0255] 1, 1X… connection structure

[0256] 2… first connection target member (circuit board)

[0257] 2a… first electrode

[0258] 3… second connection target member (semiconductor chip)

[0259] 3a… second electrode

[0260] 4, 4X… connection portion

[0261] 4A, 4XA… solder portion

[0262] 4B… 4XB… cured product portion

[0263] 5… support member

[0264] 6… support film

[0265] 11… resin composition

[0266] 11A… solder particle

[0267] 11B… thermosetting component

[0268] 11C… rubber particle

[0269] 11D… flux

[0270] 51 laser irradiation device

Claims

1. A resin composition comprising: a thermosetting component, a flux, solder particles, and rubber particles, the average particle diameter of the flux being 10 μm or less.

2. A resin composition comprising: a thermosetting component, a flux, solder particles, and rubber particles, the initial tack of the resin composition at 25°C and 50% RH being 150 N or more.

3. The resin composition according to claim 1 or 2, wherein the glass transition temperature of the rubber particles is 25°C or less.

4. The resin composition according to any one of claims 1 to 3, wherein the average particle diameter of the rubber particles is 1 μm or less.

5. The resin composition according to any one of claims 1 to 4, wherein the content of the rubber particles is 1% by weight or more and 10% by weight or less in 100% by weight of the resin composition.

6. The resin composition according to any one of claims 1 to 5, wherein the thermosetting component comprises a thermosetting compound, and the content of the rubber particles is 2 parts by weight or more and 20 parts by weight or less with respect to 100 parts by weight of the thermosetting compound.

7. A manufacturing method of a connection structure body, comprising: a first placement step of placing a resin composition according to any one of claims 1 to 6 on a surface of a first connection target member having at least one first electrode on the surface; a second placement step of moving a second connection target member having at least one second electrode on a surface to a surface of the resin composition opposite to the first connection target member side by a laser transfer method, and placing the second connection target member in a manner that the first electrode and the second electrode face each other; and a connection step of forming a connection portion that connects the first connection target member and the second connection target member by the resin composition by heating the resin composition to a melting point of the solder particles or more, and electrically connecting the first electrode and the second electrode by a solder portion in the connection portion.

8. The manufacturing method of a connection structure body according to claim 7, wherein in the second placement step, the second connection target member is moved to the surface of the resin composition opposite to the first connection target member side by the laser transfer method at a speed of 1 cm / s or more, and the second connection target member is placed in a manner that the first electrode and the second electrode face each other. ​ ​ ​ ​ ​ ​ ​ ​ ​ ​ ​ ​ ​ ​ ​ ​ ​ ​ ​ ​

Citation Information

Patent Citations

  • Transfer method, method of manufacturing image display device using the same, and transfer device

    JP2020053558A