SiOC aerogel-molecular sieve composite material with coating structure for protecting methane gas sensor and preparation method of SiOC aerogel-molecular sieve composite material

By coating molecular sieves with SiOC aerogel, a composite material with a multi-level porous structure was prepared, which solved the problem of uneven pore size during the preparation of SiOC aerogel, improved the selectivity and stability of the methane sensor, and extended its service life.

CN121082240APending Publication Date: 2025-12-09TIANJIN UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410690780.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-30
Publication Date
2025-12-09

AI Technical Summary

Technical Problem

Existing SiOC aerogels have structural defects during the preparation process, resulting in uneven pores, making it difficult to effectively filter and isolate interfering gases, thus affecting the accuracy and lifespan of methane sensors.

Method used

The structure of SiOC aerogel-coated molecular sieve is adopted. Molecular sieves with micron-sized particles and nano-sized pores are used, and SiOC aerogel-molecular sieve composite materials are prepared by sol-gel method to form a multi-level porous structure and enhance gas adsorption and filtration capabilities.

Benefits of technology

This improves the selectivity and anti-poisoning performance of the methane sensor, ensuring the accuracy of methane concentration detection and the stability of the sensor, and extending its service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121082240A_ABST
    Figure CN121082240A_ABST
Patent Text Reader

Abstract

The invention discloses a SiOC aerogel-molecular sieve composite material with a coating structure for protecting a methane gas sensor and a preparation method of the SiOC aerogel-molecular sieve composite material, the SiOC aerogel-molecular sieve composite material adopts a structural design of coating a molecular sieve with SiOC aerogel, and the inner core structure adopts a molecular sieve with micron-scale granularity and nano-scale internal pores; and the SiOC aerogel coated outside is prepared by adopting methyl trimethoxy silane and vinyl triethoxy silane as silicon sources and adopting a sol-gel method. On one hand, defects caused in the preparation process of the aerogel can be reduced as much as possible, on the other hand, interface contact between the aerogel and the molecular sieve can be effectively ensured, the specific surface area and the micropore porosity of the aerogel are further improved while the structural stability of the aerogel is ensured, and the preparation method is simple and convenient. Therefore, the SiOC aerogel and molecular sieve composite material has better gas adsorption and filtration capacity and can be stably applied to a methane gas sensor protection material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to aerogel material preparation technology, and more specifically, to a method for preparing a protective material for methane sensors. Background Technology

[0002] In today's society, natural gas, as a clean and efficient energy source, is widely used in various fields such as chemical production, industrial fuel, and domestic gas supply. Methane is the most abundant gas in natural gas, accounting for approximately 85%. However, methane is a potent greenhouse gas, significantly impacting global climate change. Furthermore, methane is flammable; a concentration of 6% in the air will explode upon contact with an open flame. Methane is colorless and odorless, with a molecular diameter of approximately 0.38 nanometers, making it highly susceptible to leakage. With the increasing use of natural gas, the risk of methane leaks is also gradually increasing, making real-time monitoring of methane leaks crucial. Methane gas sensors can detect the concentration of methane in the environment, but the presence of gases such as ethanol, acetic acid, and carbon monoxide in the air can interfere with these sensors. Especially during daily cooking with condiments such as vinegar and cooking wine, false alarms from methane sensors are easily triggered, causing significant disruption to daily life. Therefore, improving the anti-interference capabilities of methane sensors to ensure the accuracy of methane concentration detection is essential.

[0003] (Resistance to humidity interference, lifespan)

[0004] Methane sensors rely on the physical or chemical interaction between the gas-sensitive material and methane to cause changes in certain properties of the material. However, the gas-sensitive material often interacts with multiple gases simultaneously, making it difficult to guarantee specific concentration monitoring of methane. An external protective layer material for the methane gas sensor can effectively adsorb and filter gas molecules before they reach the surface of the gas-sensitive material, thus avoiding interference from non-methane gases. SiOC aerogels have advantages such as simple and economical preparation, large specific surface area, and high porosity, and are widely used in gas adsorption and filtration. However, the preparation process of SiOC aerogels can introduce structural defects, resulting in some pore inhomogeneity, which makes it difficult to effectively filter and isolate interfering gases in the environment. Therefore, as an external protective layer material for sensors, SiOC aerogel, while leveraging its own advantages, needs to be combined with other porous materials to minimize the uneven pores caused by structural defects. On the other hand, SiOC aerogel composite materials need to be modified to possess functional properties such as gas-specific adsorption and self-degradation and regeneration through loading and grafting organic functional groups and doping with functional components, thereby improving the service life of the protective material.

[0005] To further homogenize and reduce the pore size of SiOC aerogels, porous materials with smaller particle sizes and pore sizes, such as molecular sieves and activated carbon, can be added during the aerogel preparation process to fill the large pores in its structure. Simultaneously, these porous materials themselves possess a certain adsorption capacity, which can further enhance the adsorption and filtration effect of the protective material on interfering gases. However, in the process of filling aerogels with molecular sieves, if the filling amount is too small, the enhancing effect of the molecular sieves cannot be utilized; if the filling amount is too large, it will lead to more interfacial defects between the molecular sieve and the aerogel. Summary of the Invention

[0006] The purpose of this invention is to overcome the shortcomings of existing technologies and obtain a molecular sieve aerogel composite material with high gas adsorption and filtration performance. This invention employs a SiOC aerogel coating molecular sieve scheme to provide a SiOC aerogel-molecular sieve composite material with a coating structure for methane gas sensor protection, along with its preparation method. On the one hand, this minimizes defects caused by the aerogel preparation process itself; on the other hand, it effectively ensures interfacial contact between the aerogel and the molecular sieve, guaranteeing the stability of the aerogel structure while further increasing the specific surface area and micropore porosity of the aerogel. This results in the SiOC aerogel@molecular sieve composite material having better gas adsorption and filtration capabilities, enabling its stable application in methane gas sensor protection materials.

[0007] The technical objective of this invention is achieved through the following technical solution.

[0008] A SiOC aerogel-molecular sieve composite material with a protective coating structure for methane gas sensors and its preparation method are disclosed. The method employs a SiOC aerogel-coated molecular sieve structure. The core structure uses a molecular sieve with a micron-sized particle size and nano-sized internal pores. The outer SiOC aerogel is prepared using methyltrimethoxysilane (MTMS) and vinyltriethoxysilane (VTES) as silicon sources via a sol-gel method, following the steps described below:

[0009] Step 1, Preparation of SiOC aerogel precursor sol

[0010] Methyltrimethoxysilane and vinyltriethoxysilane were uniformly dispersed in a mixed solution of deionized water, ethanol, and N,N-dimethylformamide. Glacial acetic acid solution was added dropwise to adjust the pH to 5-6 while stirring. Ammonia water was slowly added dropwise to adjust the pH to 8.5-9.5, and stirring continued to disperse the solution, thus obtaining the precursor sol. The components were: 20-25 parts methyltrimethoxysilane, 15-20 parts vinyltriethoxysilane, 10-15 parts deionized water, and 35-40 parts anhydrous ethanol by volume.

[0011] In step 1, the mass percentage concentration of ammonia water is 25% to 28%.

[0012] In step 1, glacial acetic acid solution is added dropwise to adjust the pH to 5-6, and stirring is carried out simultaneously for 40-60 hours. Ammonia water is then slowly added dropwise to the solution to adjust the pH to 8.7-9.3, and stirring is continued for 8-12 minutes.

[0013] In step 1, the stirring speed is 100-500 revolutions per minute.

[0014] In step 1, by volume, there are 23-25 ​​parts of methyltrimethoxysilane, 15-17 parts of vinyltriethoxysilane, 13-15 parts of deionized water, and 35-36 parts of anhydrous ethanol.

[0015] Step 2, surface coating of molecular sieve

[0016] Molecular sieves were placed in a funnel containing filter material, and the SiOC aerogel precursor sol obtained in step 1 was added until the molecular sieves were completely immersed in the SiOC aerogel precursor sol. The mixture was then subjected to vacuum filtration. After vacuum filtration, the solid material in the funnel was transferred to a container, and ethanol was added. The mixture was then ultrasonically dispersed and soaked. The soaked solid material was dried under normal pressure at a temperature of 60–80°C for 48–72 hours to obtain a solid composite material of molecular sieves coated with precursor gel. The mass ratio of molecular sieves to SiOC aerogel precursor sol obtained in step 1 was 1:(1–3).

[0017] In step 2, ethanol is added and ultrasonically dispersed for 10-30 minutes, followed by soaking for 20-30 hours, during which the ethanol solution is replaced every 10-15 hours.

[0018] In step 2, the mass ratio of the molecular sieve to the SiOC aerogel precursor sol obtained in step 1 is 1:1.

[0019] Step 3, Formation of the coating structure

[0020] The solid composite material obtained in step 2 was calcined in an inert atmosphere to obtain a coated SiOC aerogel-molecular sieve composite material. The temperature was increased from room temperature (20-30°C) to the calcination temperature at a rate of 5-10°C / min. The calcination temperature was 800-850°C. The calcination temperature was maintained for 1-5 hours and then cooled in the furnace.

[0021] In step 3, the inert atmosphere is nitrogen, helium, or argon.

[0022] In step 3, the calcination temperature is 800-820℃, and the calcination time is maintained at the calcination temperature for 1.5-2.5 hours.

[0023] In the above preparation method, SBA-15 or ZSM-5 is used for molecular screening. The molecular screening is performed by multiple ultrasonic water washings and a final alcohol washing before use.

[0024] The SiOC aerogel-molecular sieve composite material with a coating structure of the present invention is used in a methane gas sensor. It is filled into the sensor protective shell as a filter material at the top of the methane sensor, and then the protective shell is assembled with the methane sensor to form a sensor assembly with a protective shell.

[0025] The packing thickness of the SiOC aerogel-molecular sieve composite material with the coating structure is 1.0-2.0 mm.

[0026] The sensor protective housing is made of PP, ABS, or PC materials, which are compatible with the sensor, and features a top opening.

[0027] The methane sensor protective material prepared by the technical solution of this invention can effectively improve the selectivity and anti-poisoning performance of the methane sensor without affecting the response speed and stability of the methane sensor itself. This invention prepares an aerogel-molecular sieve composite material with a multi-level porous structure. While not affecting the methane gas response, this material effectively isolates or adsorbs organic interfering gases, thereby improving the sensor's selectivity for methane gas. Simultaneously, the composite aerogel can avoid poisoning and contamination by hexamethyldisiloxane vapor, thus improving the stability and service life of the sensor.

[0028] The methane sensor with a protective layer obtained in this invention was tested for its gas-sensing performance. It exhibits good anti-interference performance, with a sensitivity of 1.02 for interfering gases such as 2000 ppm ethanol, 1.02 for 2000 ppm acetic acid, and 1.03 for 2000 ppm acetone. The sensor also demonstrates a sensitivity of 8.72 for 4000 ppm methane gas with a response time of 5 seconds, exhibiting high selectivity and rapid response. This protective layer design represents a convenient, efficient, and highly valuable functional optimization scheme for methane sensors. Attached Figure Description

[0029] Figure 1 These are scanning electron microscope (SEM) images of the SiOC aerogel-molecular sieve coated composite material samples obtained in Examples 1-4 of this invention, where (a)-(d) correspond to Examples 1-4 respectively.

[0030] Figure 2 This is a comparison of the response curves of a standard methane sensor with and without protective material (as described in Example 4) to 2000 ppm ethanol and 4000 ppm methane.

[0031] Figure 3 The bar chart shows the test results of the selective sensitivity characteristics of a regular methane sensor with and without protective material (Example 4) to interfering gases such as methane and ethanol. Detailed Implementation

[0032] The technical solution of the present invention will be further described below with reference to specific embodiments. Two types of molecular sieves are coated with SiOC aerogel: SBA-15 and ZSM-5. SBA-15 has a columnar structure with distributed axial micropores; ZSM-5 has a sheet-like structure with micropores distributed on its surface.

[0033] Example 1:

[0034] The specific preparation method of the SiOC aerogel-molecular sieve composite material in this embodiment is as follows:

[0035] (1) Selection of molecular sieve: SBA-15 molecular sieve with a size of 50 micrometers and an internal pore size of 10 nanometers was selected. The molecular sieve was subjected to multiple ultrasonic water washings and a final alcohol washing before use.

[0036] (2) Preparation of SiOC aerogel precursor sol: 23 parts by volume of MTMS, 17 parts by volume of VTES, 13 parts by volume of deionized water, and 36 parts by volume of anhydrous ethanol were weighed. Methyltrimethoxysilane (MTMS) and vinyltriethoxysilane (VTES) were dispersed in a mixed solution of deionized water, ethanol, and DMF (DMF as the solvent atmosphere). Glacial acetic acid solution was added to adjust the pH to 5, and the mixture was stirred continuously for 42 h. Ammonia water with a mass percentage (concentration) of 25% was slowly added dropwise to the solution to adjust the pH to 8.7. The mixture was stirred for 12 min to obtain the precursor sol.

[0037] (3) Surface coating of molecular sieve: The molecular sieve cleaned in step (1) was placed in a funnel with filter paper, and an equal mass of the precursor sol prepared in step (2) was added. After the molecular sieve was completely immersed in the sol, it was filtered under reduced pressure. After filtration, the solid in the funnel was transferred to a container containing ethanol, sonicated for 30 min, and then soaked for 24 h, with the solution being changed every 12 h. Finally, the treated solid material was dried at 60 °C under normal pressure for 72 h to obtain a solid composite material with precursor gel coating on the surface of the molecular sieve.

[0038] (4) Formation of the coating structure: The solid composite material obtained in step (3) is heated to 800℃ at 5℃ / min under nitrogen atmosphere and held for 2h, and then cooled and calcined in the furnace to obtain the SiOC aerogel-molecular sieve composite material with the coating structure.

[0039] (5) Assembly of gas sensor: The SiOC aerogel-molecular sieve composite material obtained in step (4) is tightly packed into the PP material sensor protective shell with a top opening at a thickness of 1.5mm, and the protective shell is assembled with the methane sensor to obtain a sensor assembly with a protective shell.

[0040] The microstructure of the coated composite material is shown in the attached figure. Figure 1 As shown in (a), the sensor characteristics are shown in Appendix Table 1.

[0041] Example 2:

[0042] The experimental steps are the same as in Example 1, but the difference is as follows: In step (1), SBA-15 molecular sieve with a size of 30 micrometers and an internal pore size of 10 nanometers is selected. In step (2), glacial acetic acid solution is added to adjust the pH to 6 and stirred continuously for 48 hours. Ammonia water is slowly added dropwise to the solution to adjust the pH to 9.3, and stirred for 8 minutes to obtain the precursor sol. In step (4), the sintering temperature is maintained at 800℃ for 2.5 hours. In step (5), the composite material is tightly packed into the ABS sensor protective shell with a top opening at a thickness of 1.0 mm.

[0043] The microstructure of the coated composite material is shown in the attached figure. Figure 1 As shown in (b), the sensor characteristics are shown in Appendix Table 1.

[0044] Example 3:

[0045] The experimental steps are the same as in Example 1, but the difference is as follows: In step (1), SBA-15 molecular sieve with a size of 40 micrometers and an internal pore size of 20 nanometers is selected. In step (2), glacial acetic acid solution is added to adjust the pH to 5.4 and stirred continuously for 40 hours. Ammonia water is slowly added dropwise to the solution to adjust the pH to 9, and stirred for 10 minutes to obtain the precursor sol. In step (3), after 25 minutes of ultrasonic treatment, it is soaked for 30 hours, and the ethanol solution is replaced every 15 hours. The aged solid is dried under normal pressure at a drying temperature of 70°C for 36 hours. In step (5), the composite material is tightly packed into the PC material sensor protective shell with a top opening at a thickness of 2.0 mm.

[0046] The microstructure of the coated composite material is shown in the attached figure. Figure 1 As shown in (c), the sensor characteristics are shown in the attached table.

[0047] Example 4:

[0048] The experimental steps were the same as in Example 1, but with the following differences: In step (1), ZSM-5 molecular sieves with a diameter of 10 micrometers and an internal pore size of 0.5 nanometers were selected. In step (2), glacial acetic acid solution was added to adjust the pH to 5.6, and stirring was continued for 40 hours. Ammonia water was slowly added dropwise to the solution to adjust the pH to 9, and stirring was carried out for 8 minutes to obtain the precursor sol. In step (3), after 15 minutes of ultrasonic treatment, the solution was soaked for 30 hours, and the ethanol solution was replaced every 10 hours. The aged solid was dried under normal pressure at a temperature of 70°C for 36 hours.

[0049] The microstructure of the coated composite material is shown in the attached figure. Figure 1 As shown in (d), the sensor's gas sensitivity characteristics are as shown in the attached diagram. Figure 2-3 .

[0050] From the appendix Figure 1 Scanning electron microscope (SEM) images of the SiOC aerogel-molecular sieve coated composite material samples obtained in Examples 1-4 show that the molecular sieve is coated with SiOC aerogel, highlighting the coating structure of the composite material. This indicates that SiOC aerogel-molecular sieve coated composite materials can be prepared by following the preparation method and by changing the molecular sieve material.

[0051] Current residential natural gas alarms are essentially methane gas sensors, but these sensors are also sensitive to volatile organic gases such as ethanol and acetic acid. In daily life, cooking inevitably involves adding spirits like baijiu, cooking wine, and vinegar, which produce ethanol and acetic acid gases, easily triggering false alarms from methane sensors. While activated carbon and other materials are used as protective agents, the application of aerogel and molecular sieve composite materials is currently unexplored. (See attached image) Figure 2 and 3 The response curves of ordinary methane sensors without protective material and with protective material from Example 4 to 2000ppm ethanol and 4000ppm methane, as well as the test results of the selective sensitivity characteristics of ordinary methane sensors without protective material and with protective material from Example 4 to interfering gases such as methane and ethanol, show that the SiOC aerogel-molecular sieve coated composite material of the present invention can effectively filter interfering gases such as ethanol and acetic acid, while ensuring the timeliness and accuracy of methane sensing. As the top filter material of the methane sensor, see the response characteristic test results table below.

[0052] Table 1 shows the test results of the sensor response characteristics.

[0053]

[0054] The aerogel-molecular sieve composite material prepared using the technical solution of this invention has a multi-level porous structure. While not affecting the methane gas response, it can effectively isolate or adsorb interfering gases, thereby improving the sensor's selectivity for methane gas. Simultaneously, the aerogel-molecular sieve composite material can avoid poisoning and contamination by hexamethyldisiloxane vapor, thus improving the sensor's stability and lifespan. The material preparation process of this invention is simple, and the raw material cost is low, making it an ideal material for sensor protective layers.

[0055] By adjusting the preparation process parameters according to the present invention, SiOC aerogel-molecular sieve composite materials can be prepared, and the results, after testing, exhibit performance that is essentially consistent with the examples provided. The present invention has been described above as exemplary. It should be noted that any simple modifications, alterations, or other equivalent substitutions that can be made by those skilled in the art without creative effort, without departing from the core of the present invention, fall within the protection scope of the present invention.

Claims

1. A SiOC aerogel-molecular sieve composite material with a protective coating structure for methane gas sensors, characterized in that, A molecular sieve structure with SiOC aerogel coating was adopted. The core structure uses molecular sieves with micron-sized particles and nano-sized internal pores. The outer SiOC aerogel coating was prepared by sol-gel method using methyltrimethoxysilane and vinyltriethoxysilane as silicon sources, according to the following steps: Step 1, Preparation of SiOC aerogel precursor sol Methyltrimethoxysilane and vinyltriethoxysilane were uniformly dispersed in a mixed solution of deionized water, ethanol, and N,N-dimethylformamide. Glacial acetic acid solution was added dropwise to adjust the pH to 5-6 while stirring. Ammonia water was slowly added dropwise to adjust the pH to 8.5-9.5, and stirring continued to disperse the solution, thus obtaining the precursor sol. The components were: 20-25 parts methyltrimethoxysilane, 15-20 parts vinyltriethoxysilane, 10-15 parts deionized water, and 35-40 parts anhydrous ethanol by volume. Step 2, surface coating of molecular sieve Molecular sieves were placed in a funnel containing filter material, and the SiOC aerogel precursor sol obtained in step 1 was added until the molecular sieves were completely immersed in the SiOC aerogel precursor sol. Vacuum filtration was then performed. After the vacuum filtration was completed, the solid material in the funnel was transferred to a container, and ethanol was added and ultrasonically dispersed and soaked. The soaked solid material was then dried at normal pressure at a temperature of 60–80°C for 48–72 h to obtain a solid composite material of molecular sieves coated with precursor gel. The mass ratio of molecular sieve to SiOC aerogel precursor sol obtained in step 1 is 1:(1-3); Step 3, Formation of the coating structure The solid composite material obtained in step 2 was calcined in an inert atmosphere to obtain a coated SiOC aerogel-molecular sieve composite material. The temperature was increased from room temperature (20-30°C) to the calcination temperature at a rate of 5-10°C / min. The calcination temperature was 800-850°C. The calcination temperature was maintained for 1-5 hours and then cooled in the furnace.

2. The SiOC aerogel-molecular sieve composite material for protective coating of a methane gas sensor according to claim 1, characterized in that, Molecular screening was performed using SBA-15 or ZSM-5, followed by multiple ultrasonic water washings and a final alcohol washing before use.

3. The SiOC aerogel-molecular sieve composite material for protective coating of a methane gas sensor according to claim 1, characterized in that, In step 1, the mass percentage concentration of ammonia water is 25%–28%; by volume, there are 23–25 parts of methyltrimethoxysilane, 15–17 parts of vinyltriethoxysilane, 13–15 parts of deionized water, and 35–36 parts of anhydrous ethanol; glacial acetic acid solution is added dropwise to adjust the pH to 5–6, and stirring is carried out simultaneously for 40–60 hours; ammonia water is slowly added dropwise to the solution to adjust the pH to 8.7–9.3, and stirring is continued for 8–12 minutes; the stirring speed is 100–500 revolutions per minute.

4. The SiOC aerogel-molecular sieve composite material for protective coating of a methane gas sensor according to claim 1, characterized in that, In step 2, ethanol is added and ultrasonically dispersed for 10-30 min, followed by soaking for 20-30 h, with the ethanol solution being replaced every 10-15 h; the mass ratio of molecular sieve to SiOC aerogel precursor sol obtained in step 1 is 1:

1.

5. The SiOC aerogel-molecular sieve composite material for protective coating of a methane gas sensor according to claim 1, characterized in that, In step 3, the inert atmosphere is nitrogen, helium or argon; the calcination temperature is 800-820℃, and the calcination temperature is maintained for 1.5-2.5h.

6. A method for preparing a SiOC aerogel-molecular sieve composite material with a protective coating structure for methane gas sensors, characterized in that, The sol-gel method was used to prepare the product using methyltrimethoxysilane and vinyltriethoxysilane as silicon sources, and the following steps were performed: Step 1, Preparation of SiOC aerogel precursor sol Methyltrimethoxysilane and vinyltriethoxysilane were uniformly dispersed in a mixed solution of deionized water, ethanol, and N,N-dimethylformamide. Glacial acetic acid solution was added dropwise to adjust the pH to 5-6 while stirring. Ammonia water was slowly added dropwise to adjust the pH to 8.5-9.5, and stirring continued to disperse the solution, thus obtaining the precursor sol. The components were: 20-25 parts methyltrimethoxysilane, 15-20 parts vinyltriethoxysilane, 10-15 parts deionized water, and 35-40 parts anhydrous ethanol by volume. Step 2, surface coating of molecular sieve Molecular sieves were placed in a funnel containing filter material, and the SiOC aerogel precursor sol obtained in step 1 was added until the molecular sieves were completely immersed in the SiOC aerogel precursor sol. Vacuum filtration was then performed. After the vacuum filtration was completed, the solid material in the funnel was transferred to a container, and ethanol was added and ultrasonically dispersed and soaked. The soaked solid material was then dried at normal pressure at a temperature of 60–80°C for 48–72 h to obtain a solid composite material of molecular sieves coated with precursor gel. The mass ratio of molecular sieve to SiOC aerogel precursor sol obtained in step 1 is 1:(1-3); Step 3, Formation of the coating structure The solid composite material obtained in step 2 was calcined in an inert atmosphere to obtain a coated SiOC aerogel-molecular sieve composite material. The temperature was increased from room temperature (20-30°C) to the calcination temperature at a rate of 5-10°C / min. The calcination temperature was 800-850°C. The calcination temperature was maintained for 1-5 hours and then cooled in the furnace.

7. The method for preparing a SiOC aerogel-molecular sieve composite material with a protective coating structure for a methane gas sensor according to claim 6, characterized in that, In step 1, the mass percentage concentration of ammonia water is 25%–28%; by volume, there are 23–25 parts of methyltrimethoxysilane, 15–17 parts of vinyltriethoxysilane, 13–15 parts of deionized water, and 35–36 parts of anhydrous ethanol; glacial acetic acid solution is added dropwise to adjust the pH to 5–6, and stirring is carried out simultaneously for 40–60 hours; ammonia water is slowly added dropwise to the solution to adjust the pH to 8.7–9.3, and stirring is continued for 8–12 minutes; the stirring speed is 100–500 revolutions per minute.

8. The method for preparing a SiOC aerogel-molecular sieve composite material with a protective coating structure for a methane gas sensor according to claim 6, characterized in that, In step 2, ethanol is added and ultrasonically dispersed for 10-30 min, followed by soaking for 20-30 h, with the ethanol solution being replaced every 10-15 h; the mass ratio of molecular sieve to SiOC aerogel precursor sol obtained in step 1 is 1:1; in step 3, the inert atmosphere is nitrogen, helium or argon; the calcination temperature is 800-820℃, and the calcination temperature is maintained for 1.5-2.5 h.

9. The method for preparing a SiOC aerogel-molecular sieve composite material with a protective coating structure for a methane gas sensor according to claim 6, characterized in that, Molecular screening was performed using SBA-15 or ZSM-5, followed by multiple ultrasonic water washings and a final alcohol washing before use.

10. The application of the SiOC aerogel-molecular sieve composite material with a protective coating structure for a methane gas sensor as described in claims 1-5 in a methane gas sensor, characterized in that, It is filled into the sensor protective shell as the top filter material of the methane sensor, and then the protective shell is assembled with the methane sensor to form a sensor assembly with a protective shell; the filling thickness of the SiOC aerogel-molecular sieve composite material with the encapsulation structure is 1.0-2.0mm; the sensor protective shell is made of PP, ABS, or PC materials, which are compatible with the sensor and have a top opening.