High-efficiency titanium steel composite plate assembling method
By using modular splicing with short frames and specific welding processes, the problems of frame deformation and low welding efficiency in the production of titanium-steel composite panels have been solved, achieving efficient and low-cost production of titanium-steel composite panels and ensuring the bonding strength and quality of the finished products.
Patent Information
- Application Number
- CN202511185667.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-08-22
- Publication Date
- 2025-12-19
AI Technical Summary
In the current production of titanium-steel composite plates, frame deformation leads to high processing difficulty, large welding filler volume and low efficiency, poor weld quality, and unstable bonding strength of the finished product.
It adopts a short-frame modular splicing, with a sharp corner structure on the outer side of the frame. It uses a combination of argon arc welding and carbon dioxide gas shielded welding to reduce the amount of welding filler and ensure welding quality and sealing.
It effectively avoids frame deformation, reduces welding filler and cost, improves billet assembly efficiency, ensures weld strength and interface cleanliness, and enhances the bonding strength of the finished product.
Smart Images

Figure CN121156438A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of titanium-steel composite plate production technology, and in particular to a high-efficiency method for assembling titanium-steel composite plates. Background Technology
[0002] Titanium-steel composite plates, possessing the superior properties of both titanium and steel, have been widely used in petroleum, chemical, and marine engineering fields. The main production methods for titanium-steel composite plates include explosive bonding, diffusion bonding, explosive-rolling, and rolling bonding. Among these, rolling bonding has become the primary development direction for titanium-steel composite plate production due to its environmental friendliness, high efficiency, and low cost.
[0003] The main process for producing titanium-steel composite plates using the rolling composite method is as follows: surface treatment of the titanium composite and the base steel → welding the titanium composite and the base steel together to form a raw billet → heating the raw billet → rolling the raw billet into a titanium-steel composite plate or coil → (uncoiling the composite coil →) separating the plates → straightening → finished titanium-steel composite plate. Compared to rolling a single metal, rolling titanium-steel composite plates involves an additional billet assembly process, and the quality of the assembly directly affects the final bonding strength of the product.
[0004] Figure 1 The diagram shows a typical assembly method for rolling titanium-steel composite plates, known as symmetrical assembly. This assembly method avoids warping caused by mismatched deformation between the two materials. Here, the titanium-steel contact surface is called the bonding surface, and the titanium-titanium contact surface is called the separating surface. Before assembly, the titanium and steel plates must undergo surface treatment to remove oxide scale and oil, ensuring a clean interface. A release agent is applied between the titanium plates to facilitate separation of the upper and lower titanium-steel composite plates after rolling. The upper and lower substrates are welded to the surrounding frame, and a vacuum treatment is performed internally.
[0005] Existing typical material assembly methods have the following technical drawbacks: 1. Frame deformation leads to high processing and assembly difficulties: Traditional methods using integral frames of the same length as the billet often result in ultra-long thin-walled structures (e.g., a typical cross-section of 50×50×5000mm), which inevitably bend during processing and welding, and may even pose a risk of incomplete vacuum sealing. 2. Large welding filler volume and low efficiency: The wide contact surface between the traditional rectangular cross-section frame and the steel billet requires a large amount of welding material to fill the weld. This results in long welding times and high material costs. 3. Poor weld quality leads to interface contamination. In traditional high-filler welding, to improve efficiency, if high-current welding (such as MIG welding) is used directly, spatter can easily enter the cavity and contaminate the titanium-steel interface; if the number of weld layers is insufficient, it is prone to cracking during rolling.
[0006] In summary, existing technologies suffer from low assembly efficiency, high cost, and unstable bonding strength of finished products due to processing and welding problems caused by the frame structure. Summary of the Invention
[0007] To address the aforementioned problems, the present invention aims to provide a high-efficiency method for assembling titanium-steel composite plates, which can effectively avoid frame deformation and reduce welding filler, thereby improving production efficiency and reducing production costs.
[0008] The technical solution adopted in this invention is as follows: The present invention proposes a high-efficiency titanium-steel composite plate assembly method, comprising the following steps: S1. Raw material preparation: two titanium plates as composite materials, two steel billets as base materials, and multiple frame segments; the length of a single frame segment is ≤1500mm, and the multiple frame segments are spliced end to end to form a closed frame; the outer end face of each frame segment is set as an outwardly arched pointed corner structure, and the angle between the slope surface of the pointed corner structure and the horizontal plane of the steel billet is 30°-60°; and a hole is opened in the middle of the frame segment at the end and a steel pipe is welded on it; S2. Coating the titanium surface with a release agent: After wiping the surface of the titanium plate clean, apply a release agent to one side of the titanium plate, i.e. the titanium-titanium contact surface, and let it stand to dry. S3. Frame fixing: The frame is welded to the upper surface of the lower steel billet in sequence, with the sharp corners of the frame facing outwards. S4, Titanium and Steel Billet Assembly: Place two titanium plates with the release agent coated on one side facing each other inside the frame, so that the center point of the titanium plate coincides with the center point of the steel billet; then place the upper steel billet, coinciding with the lower steel billet; S5. Welding and Vacuuming: (a) First, use argon arc welding to seal the upper steel billet to the upper end face of the frame, so that a closed cavity is formed between the upper steel billet, the frame, and the lower steel billet; (b) Connect the vacuum equipment to the steel pipe and evacuate to an internal vacuum degree ≤1×10 -2 Pa is used to seal the steel pipe; (c) 3-4 passes are welded with electric welding rods, and then carbon dioxide gas shielded welding is used to build up the weld until the sharp corner structure of the outer end face of the frame is flush with the edge of the steel billet.
[0009] Furthermore, in step S1, the thickness of the substrate and composite material is determined by the finished product specifications and the reduction amount, which must be ≥80%.
[0010] Furthermore, in step S1, the total width of a single frame is 50-60mm, and the width of the horizontal surface that contacts the upper and lower end faces of the frame with the upper and lower steel billets is 18-22mm.
[0011] Furthermore, in step S1, the frame height is (2×h+Δh), where h is the thickness of the titanium plate and Δh=0.5-3mm.
[0012] Furthermore, the two ends of the frame have chamfers of 25°-35°.
[0013] Furthermore, in step S2, the release agent is uniformly coated with a coating thickness of 0.5 mm to 1.5 mm.
[0014] Furthermore, step S3 specifically includes: first, spot welding all the frame edges to fix them, and then checking the straightness and flatness; then, using an alternating welding sequence to complete the frame weld splicing, and filling the corners at the ends of adjacent frame edges fully; the weld height does not exceed the upper surface of the frame edge.
[0015] Furthermore, in step S5, the amount of carbon dioxide gas shielded welding is based on completely covering the sharp corner structure and being flush with the edge of the steel billet.
[0016] Compared with the prior art, the present invention has the following advantages: 1. Completely solves the problem of frame deformation: In large-scale industrial production, titanium plates are often quite long. For example, a 5m frame would result in an ultra-long, thin-walled structure. During machining, the straightness deviation of the frame could reach 3-5mm / m, causing assembly gaps that would severely affect subsequent welding quality. Achieving this level of precision requires extremely high machining precision, inevitably increasing manufacturing costs. This invention uses modular splicing with short frames (≤1500mm), eliminating deformation during the machining of ultra-long, thin-walled parts and reducing machining difficulty. 2. The amount of filler material is reduced by more than 50%, resulting in a reduction of welding time and material consumption by more than 50%. Figure 6 and Figure 7 As shown; 3. Improved weld strength and sealing performance: The combination of argon arc welding for sealing, electric electrode for root pass, and CO2 welding for surfacing results in high welding efficiency, zero spatter contamination, and a clean interface, which is beneficial to improving the bonding strength of the composite plate. 4. Significant overall benefits: Improved billet assembly efficiency, shorter welding time, reduced welding material consumption, and guaranteed interface cleanliness help reduce costs, ensure quality, and improve overall performance. Attached Figure Description
[0017] Figure 1 This is a schematic diagram of the assembly method for conventional rolled titanium-steel composite plates; Figure 2 This is a schematic diagram of the material assembly method of the present invention; Figure 3 This is a schematic diagram of the frame structure in this invention; Figure 4 for Figure 3 A top-view structural diagram; Figure 5 This is a top view of the structure at the adjacent ends of the border. Figure 6 This is a schematic diagram of the welding filler amount of the present invention; Figure 7 This is a schematic diagram of the welding filler amount in the original preform assembly method.
[0018] In the attached drawings, the following labels are used: 1-steel billet; 2-titanium plate; 3-release agent; 4-frame; 5-steel pipe; 6-sealing part; 7-frame contact surface; 8-sharp corner structure; 9-welding area. Detailed Implementation
[0019] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0020] See appendix Figure 1-2 The present invention proposes a high-efficiency titanium-steel composite plate assembly method, which specifically includes the following steps: S1. Raw material preparation: two titanium plates 2 as composite materials, two steel billets 1 as base materials, and several frame frames 4. The length of a single frame 4 is ≤1500mm, preferably within 1000mm; multiple frame segments are spliced end to end to form a closed frame; the outer end face of each frame 4 is set as an outwardly arched pointed corner structure 8; the total width of a single frame 4 is 50-60mm, and the width of the horizontal plane that contacts the upper and lower end faces of the frame 4 with the upper and lower steel billets 1 is 18-22mm; the angle between the slope of the pointed corner structure 8 on the outer end face of the frame 4 and the horizontal plane of the steel billet 1 is 30°-60°; the height of the frame 4 is (2×h+Δh), where h is the thickness of the titanium plate 2, and Δh=0.5-3mm; the two ends of the frame 4 are chamfered at 25°-35°.
[0021] A hole is made in the middle of a frame 4 at the tail end, and a steel pipe 5 with a diameter of φ10-φ15mm is pre-welded to it to facilitate subsequent vacuum treatment of the interior. The thickness of the substrate and composite is determined by the finished product specifications and the reduction amount. The reduction amount needs to be controlled above 80%. Taking a rolled finished product with a thickness of 2mm TA2+8mm Q235 as an example, if the reduction amount is selected as 92%, the thickness of the titanium plate is 25mm and the thickness of the Q235mm plate is 100mm.
[0022] S2. Coating the titanium surface with a release agent: Wipe the oil stains off the surface of the titanium plate with anhydrous ethanol, and then coat the titanium plate 2 with release agent 3 on one side, i.e. the titanium-titanium contact surface, and let it stand to dry; the release agent 3 is usually composed of powdered metal oxides and organic substances such as binders and dispersants; The release agent 3 should be applied evenly with a thickness of 0.5mm to 1.5mm. If the coating thickness is less than 0.5mm, there is a risk of adhesion, and it will not be able to separate the two titanium plates 2. If the thickness is greater than 1.5mm, it will easily fall off after drying.
[0023] S3, Frame fixing: The frame 4 is welded to the upper surface of the lower steel billet 1 in sequence, with the sharp corner structure 8 of the frame 4 facing the outside of the billet assembly; First, spot weld all four edges of the frame. After confirming that the straightness and flatness are correct, proceed with the welding. Fill the included angle between the ends of two adjacent edges of the frame with full fill. During welding, alternate the four edges of the frame to avoid deformation caused by concentrated heat in one place. The weld height should not exceed the upper surface of the edge of the frame. After the edge of the frame is welded, if any part exceeds the plane, it needs to be removed with an angle grinder to ensure that it is level. Otherwise, the gap between the upper steel billet 1 and the edge of the frame will be too large. After the frame 4 is fixed, clean the oil stains and welding slag spatter on the inner surface of the lower steel billet 1 and the frame 4 again.
[0024] S4, Titanium and Steel Billet Assembly: Place two titanium plates 2 with the release agent 3 facing each other in the frame 4, so that the center point of the titanium plate 2 coincides with the center point of the steel billet 1; then place the upper steel billet 1, which coincides with the lower steel billet 1 longitudinally. S5. Welding and Vacuuming: Weld the upper steel billet 1 to the frame 4, then connect the vacuum equipment to the steel pipe 5 on the tail frame 4 to perform internal vacuuming. When the vacuum degree is ≤1×10 -2 After Pa, the steel pipe 5 is sealed to maintain the internal vacuum.
[0025] When welding the upper steel billet 1 and the frame 4, argon arc welding without spatter is used first. After the upper steel billet 1 and the upper end face of the frame 4 are completely connected and a closed cavity is formed between the upper steel billet, the frame and the lower steel billet, other methods can be used to continue welding to prevent spatter such as welding slag from entering the interior of the billet assembly and having an adverse effect on the rolling composite. After the argon arc welding is completed, 3-4 passes are welded with electric welding rods, followed by carbon dioxide gas shielded welding for overlay welding. The welding amount is based on the standard that the sharp corner structure of the outer end face of the frame is flush with the edge of the steel billet. If the welding amount is too small, the weld strength will be insufficient, and cracking will occur during the subsequent heating and rolling process. If it is too large, it will result in waste of raw materials.
[0026] The working principle of this invention is as follows: To avoid frame deformation, the frame dimensions of this invention are relatively fixed, with only the height varying with the thickness of the titanium billet. The length is relatively short, and the frames are welded together to form a whole. This avoids the problem of excessively long thin-walled structures caused by the excessive length of the integral frame (which is usually the same as the length of the billet) in traditional methods (for example, processing a 50×50×5000mm strip will inevitably result in bending, and the straightness will not meet the assembly requirements).
[0027] The reduction in fill is a benefit derived from the geometry of the border design based on this invention. Traditional or conventional borders (also called edge strips) are typically rectangular.
[0028] The effects of the present invention will be further illustrated below through specific embodiments and comparative examples: Example 1 Finished 2mm TA2 + 8mm Q235 composite plate blank: Based on the finished product specifications, the titanium plate thickness is selected as 10mm, and the Q235 raw material billet thickness is 40mm. The reduction is designed to be 80%; the frame width is 50mm, and the height is 2*10+2=22mm. The titanium plate dimensions are 1600×5000mm, and the steel billet dimensions are 1700×5100mm. Based on the substrate length, 10 1000mm long frames and 4 850mm long frames are machined, for the length and width directions respectively. The frame machining shape is as follows... Figure 3 As shown. The frame is welded to the lower steel billet, and the overall straightness of the assembled frame is ≤0.5mm. After cleaning the interior again, a titanium plate is placed inside. After the billet assembly is completed, argon arc welding is used for sealing, ensuring no spatter is generated during the sealing process and guaranteeing the cleanliness of the cavity. Then, three passes of electric welding are performed, followed by MIG welding to fill the gaps between the sharp corners of the frame and the upper and lower steel billets. The vacuum degree inside the assembled billet is 0.002Pa.
[0029] After rolling, the titanium-titanium interface separated smoothly, the titanium-steel interface bonded well with no delamination, and the average shear strength was 233 MPa.
[0030] Example 2 Finished 1.2mm TA2 + 10mm Q235 composite plate blank: Based on the finished product specifications, the titanium plate thickness is selected as 15mm, the Q235 raw material billet thickness is 125mm, the reduction is designed to be 92%, the frame width is 60mm, and the height is 2*15+3=33mm. The titanium plate dimensions are 1550×5000mm, and the steel billet dimensions are 1670×5120mm. Based on the base material length, 10 frames of 1000mm length and 4 frames of 835mm length are machined, for length and width directions respectively. The frame machining shape is as follows... Figure 3 As shown. The frame is welded to the lower steel billet, and the overall straightness of the assembled frame is ≤0.5mm. After cleaning the interior again, a titanium plate is placed inside. After the billet assembly is completed, argon arc welding is used for sealing, with no spatter generated during the sealing process to ensure the cleanliness of the cavity. Then, four passes are welded using electric welding rods, followed by MIG welding. After welding, no sharp corners of the frame are visible, and the vacuum degree inside the assembled billet is 0.009Pa.
[0031] After rolling, the titanium-titanium interface separated smoothly, the titanium-steel interface bonded well with no delamination, and the average shear strength was 269 MPa.
[0032] Example 3 Finished 1.0mm TA2 + 5mm Q235 composite plate blank: Based on the finished product specifications, the titanium plate thickness is selected as 20mm, the Q235 raw material billet thickness is 100mm, the reduction is designed to be 95%, the frame width is 50mm, and the height is 2*20+1=41mm. The titanium plate dimensions are 1700×5000mm, and the steel billet dimensions are 1800×5100mm. Based on the base material length, 10 1000mm long frames and 4 900mm long frames are processed, for length and width directions respectively. The frame processing shape is as follows... Figure 3 As shown. The frame is welded to the lower steel billet, and the overall straightness of the frame after splicing is ≤0.5mm. After cleaning the interior again, a titanium plate is placed inside. After the billet assembly is completed, argon arc welding is used for sealing. No spatter is generated during sealing, ensuring the cleanliness of the cavity. After welding three times with electric welding rods, MIG welding is used to weld the frame and the upper and lower steel billets together. After welding, no sharp corners of the frame are visible, and the vacuum degree inside the assembled billet is 0.006Pa.
[0033] After rolling, the titanium-titanium interface separated smoothly, the titanium-steel interface bonded well with no delamination, and the average shear strength was 302 MPa.
[0034] Comparative Example 1 Finished 2mm TA2 + 8mm Q235 composite plate blank (insufficient frame welding strength): Based on the finished product specifications, the titanium plate thickness is selected as 10mm, the Q235 raw material billet thickness is 40mm, the reduction is designed to be 80%, the frame width is 50mm, and the height is 2*10+1=21mm. The titanium plate dimensions are 1600×5000mm, and the steel billet dimensions are 1700×5100mm. Based on the base material length, 10 frames of 1000mm length and 4 frames of 850mm length are machined, for length and width directions respectively. The frame machining shape is as follows... Figure 3 As shown, the contact surface width between the billet and the billet is 35mm. After the billet assembly is completed, argon arc welding is used for sealing, then two passes are welded with electric welding rods, and then the frame and the upper and lower billets are stacked together with MIG welding. The vacuum degree inside the billet assembly is 0.002Pa.
[0035] During rolling, due to insufficient weld depth on the frame, the weld cracked during the third rolling pass. Air entered the titanium-steel interface, resulting in a finished product shear strength of less than 140 MPa.
[0036] Comparative Example 2 Finished 1.2mm TA2 + 10mm Q235 composite plate blank (reduction less than 80%, vacuum degree > 0.01Pa): Based on the finished product specifications, the titanium plate thickness is selected as 5mm, the Q235 raw material billet thickness is 42mm, the reduction is only 76%, the frame width is 60mm, and the height is 2*5+1=11mm. The titanium plate size is 1550×5000mm, and the steel billet size is 1670×5120mm. Based on the substrate length, 10 1000mm long frames and 4 835mm long frames are processed, for length and width directions respectively. The frame processing shape is as follows... Figure 3 As shown, after the frame is welded to the lower steel billet, the interior is cleaned again and a titanium plate is placed inside. After the billet assembly is completed, argon arc welding is used for sealing, and then MIG welding is used to weld the frame and the upper and lower steel billets together. After welding, no sharp corners of the frame are visible, and the vacuum degree inside the billet assembly is 0.6 Pa.
[0037] After rolling, the titanium-titanium interface separated smoothly, but the titanium-steel interface showed partial delamination, and the shear strength was less than 140 MPa.
[0038] Comparative Example 3 Finished 1.0mm TA2+5mm Q235 composite plate blank (welding spatter entering the blank): Based on the finished product specifications, the titanium plate thickness is selected as 20mm, the Q235 raw material billet thickness is 100mm, the reduction is designed to be 95%, the frame width is 50mm, and the height is 2*20+1=41mm. The titanium plate dimensions are 1700×5000mm, and the steel billet dimensions are 1800×5100mm. Based on the substrate length, 10 1000mm long frames and 4 900mm long frames are machined, for length and width directions respectively. The frame machining shape is as follows... Figure 3 As shown, after the billet assembly is completed, the frame and the upper and lower billets are welded together using MIG welding. During welding, spatter enters the interior of the assembled billet. No sharp corners of the frame are visible after welding, and the vacuum degree inside the assembled billet is 0.006 Pa.
[0039] After rolling, the titanium-titanium interface separation was successful. However, due to the impact of spatter, delamination occurred in the 500mm edge and some areas in the middle of the titanium-steel interface, and complete bonding was not achieved.
[0040] Comparative Example 4 Finished 1.0mm TA2 + 5mm Q235 composite plate blank (frames are too long and deformed, welding strength is insufficient): Based on the finished product specifications, the titanium plate thickness was chosen to be 20mm, the Q235 raw material billet thickness was 100mm, the reduction was designed to be 95%, the frame width was 35mm, and the height was 2*20+1=41mm. The titanium plate dimensions were 1700×5000mm, and the steel billet dimensions were 1800×5100mm. Two 5000mm long and two 900mm long frames were machined according to the substrate length, for the length and width directions respectively. The frames were conventional cuboid structures. After assembly, significant deformation of the frames was observed, with a maximum deformation of 11mm, resulting in a welding depth of only 9mm in this area. After assembly, argon arc welding was first used for sealing, followed by three passes of electric welding, and then MIG welding was used to fill the gaps between the frames and the upper and lower steel billets. The internal vacuum degree of the assembled billet was 0.006Pa.
[0041] When the rolling deformation is 30%, the weld cracks, air enters the titanium-steel interface, resulting in the finished product having a shear strength of less than 140 MPa.
[0042] Comparative Example 5 Under the same conditions as Example 1, but with a rectangular cross-section, the frame specifications are: length 1000mm, total width 50mm, rectangular cross-section, and no sharp corners. Compared to Example 1, it consumes 19.4kg more welding wire and increases welding time by 7 hours. There is no cracking during the rolling process, but the overall cost is higher.
[0043] All matters not covered in this invention are common knowledge.
[0044] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.
Claims
1. A high-efficiency method for assembling titanium-steel composite plates, characterized in that: The method includes the following steps: S1. Raw material preparation: two titanium plates as composite materials, two steel billets as base materials, and multiple frame segments; the length of a single frame segment is ≤1500mm, and the multiple frame segments are spliced end to end to form a closed frame; the outer end face of each frame segment is set as an outwardly arched pointed corner structure, and the angle between the slope surface of the pointed corner structure and the horizontal plane of the steel billet is 30°-60°; and a hole is opened in the middle of the frame segment at the end and a steel pipe is welded on it; S2. Coating the titanium surface with a release agent: After wiping the surface of the titanium plate clean, apply a release agent to one side of the titanium plate, i.e. the titanium-titanium contact surface, and let it stand to dry. S3. Frame fixing: The frame is welded to the upper surface of the lower steel billet in sequence, with the sharp corners of the frame facing outwards. S4, Titanium and Steel Billet Assembly: Place two titanium plates with the release agent coated on one side facing each other inside the frame, so that the center point of the titanium plate coincides with the center point of the steel billet; then place the upper steel billet, coinciding with the lower steel billet; S5. Welding and Vacuuming: (a) First, use argon arc welding to seal the upper steel billet to the upper end face of the frame, so that a closed cavity is formed between the upper steel billet, the frame, and the lower steel billet; (b) Connect the vacuum equipment to the steel pipe and evacuate to an internal vacuum degree ≤1×10 -2 Pa is used to seal the steel pipe; (c) 3-4 passes are welded with electric welding rods, and then carbon dioxide gas shielded welding is used to build up the weld until the sharp corner structure of the outer end face of the frame is flush with the edge of the steel billet.
2. The method for assembling a high-efficiency titanium-steel composite plate according to claim 1, characterized in that: In step S1, the thickness of the substrate and composite material is determined by the finished product specifications and the reduction amount, which must be ≥80%.
3. The method for assembling a high-efficiency titanium-steel composite plate according to claim 1, characterized in that: In step S1, the total width of a single frame is 50-60mm, and the width of the horizontal surface that contacts the upper and lower end faces of the frame with the upper and lower steel billets is 18-22mm.
4. The method for assembling a high-efficiency titanium-steel composite plate according to claim 3, characterized in that: In step S1, the frame height is (2×h+Δh), where h is the thickness of the titanium plate and Δh=0.5-3mm.
5. The method for assembling a high-efficiency titanium-steel composite plate according to claim 4, characterized in that: The two ends of the frame have chamfers of 25°-35°.
6. The method for assembling a high-efficiency titanium-steel composite plate according to claim 1, characterized in that: In step S2, the release agent is uniformly coated with a coating thickness of 0.5 mm to 1.5 mm.
7. The method for assembling a high-efficiency titanium-steel composite plate according to claim 1, characterized in that: Step S3 specifically includes: first, spot welding all the frame edges to fix them, and then checking the straightness and flatness; then, using an alternating welding sequence to complete the frame weld splicing, and filling the corners at the ends of adjacent frame edges fully; the weld height should not exceed the upper surface of the frame edge.
8. The method for assembling a high-efficiency titanium-steel composite plate according to claim 1, characterized in that: In step S5, the amount of carbon dioxide gas shielded welding is based on completely covering the sharp corner structure and being flush with the edge of the steel billet.