High-density solid hydrogen storage material based on TiFe alloy doping modification and preparation method thereof
By precisely controlling the distribution of Zr, Al, W, Sn/Sb and interstitial elements in TiFe alloys, the problems of migration and segregation band formation of dopants in TiFe hydrogen storage materials are solved, achieving efficient reversible hydrogen storage performance and energy efficiency stability, which is suitable for fuel cells and distributed energy storage.
Patent Information
- Application Number
- CN202511281678.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-09
- Publication Date
- 2026-01-16
AI Technical Summary
In existing TiFe hydrogen storage materials, under the service environment of high hydrogen activity and cyclic stress coupling, the migration of dopants and the formation of segregation bands lead to chemical potential traps, resulting in hydrogen retention at the hydrogen release tail end, reduced effective capacity and energy loss, which are difficult to eliminate through conventional treatment.
By introducing stabilizing elements such as Zr and Al into TiFe alloys, which preferentially dissolve in the first sublattice, and elements such as W and Sn/Sb preferentially dissolve in the second sublattice, and by combining the distribution of interstitial elements C and N, the occupancy and dynamics of multiple elements are regulated, the migration of doped atoms and the formation of segregation bands are suppressed, and the lattice matching degree between the hydrogenated phase and the main phase is optimized.
It effectively suppresses the formation of segregation bands at the nano to micron scale, stabilizes reversible hydrogen storage capacity, improves reaction kinetic equilibrium, reduces diffusion path energy barriers, and increases hydrogen release rate and energy efficiency, making it suitable for fuel cells and distributed energy storage scenarios.
Smart Images

Figure CN121341939A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of solid-state hydrogen storage materials and hydrogen energy application technology, and more specifically, to a high-density solid-state hydrogen storage material based on TiFe alloy doping modification and its preparation method. Background Technology
[0002] Current designs for multi-component doped TiFe hydrogen storage materials generally focus on regulating plateau pressure, reducing hysteresis, and improving cycle stability. However, existing assumptions assume that the doped atoms are approximately stationary under operating conditions. In real service environments where high hydrogen activity is coupled with cyclic stress, this assumption fails: when the chemical potential gradient of certain dopants is in the same direction as the hydrogenation reaction, the dopants will undergo slow migration associated with the hydrogen absorption process, accumulating in the hydrogen-rich region along the hydrogen diffusion channel and forming segregation bands at the nanometer to micrometer scale. Segregation bands reshape the hydrogen adsorption-desorption energy landscape at the interface between the main phase and the hydrogenated phase by changing local lattice parameters, strain field and electronic density of states, generating a "chemical potential trap" that is unfavorable to hydrogen. This causes hydrogen to be locally trapped in the later stage of hydrogen release, which manifests as a long-tailed decline in outlet hydrogen concentration, a decrease in effective reversible capacity and energy efficiency loss. Moreover, this failure mode is often misjudged as a surface contamination or pulverization problem and is difficult to eliminate through conventional reactivation treatment. Therefore, the core problem of the existing technology is that the reaction of doped elements is accompanied by the self-organization of segregation bands driven by migration kinetics and hydrogenation phase transition, which induces chemical potential traps and makes it difficult to completely release hydrogen at the end of the dehydrogenation. Summary of the Invention
[0003] To overcome the aforementioned deficiencies of the prior art, embodiments of the present invention provide a high-density solid-state hydrogen storage material based on TiFe alloy doping modification and its preparation method. By controlling the preferential solid solution of various functional elements and the site distribution of interstitial elements in the twin lattice during the preparation process, the migration and segregation band formation of doped atoms during the hydrogenation cycle are suppressed from both kinetic and thermodynamic perspectives, thereby eliminating the chemical potential trap and improving the reversible hydrogen desorption efficiency, thus solving the problems mentioned in the background art.
[0004] To achieve the above objectives, the present invention provides the following technical solution: a high-density solid-state hydrogen storage material based on TiFe alloy doping modification, wherein the material has a B2 ordered intermetallic compound structure; The crystal structure of the material includes a first sublattice, a second sublattice, and a set of interstitial sites that occupy mutually independent positions; wherein: The first sublattice is a Ti-site sublattice, which uses Ti as a matrix and contains at least one of the first stabilizing element Zr and the second stabilizing element Al. Based on the atomic percentage of the entire alloy, the content of the first stabilizing element Zr is 0.5–2.0 at.%, the content of the second stabilizing element Al is 0.3–1.5 at.%, and the total content of the first stabilizing element Zr and the second stabilizing element Al is 1.0–3.0 at.%. The second sublattice is an Fe-site sublattice, which is composed of Fe, Co, Ni, Mn, Cu, and a damping element W. Based on the total number of atoms in the second sublattice, the atomic fraction of each of the Fe, Co, Ni, Mn, and Cu elements is 10-30%. Based on the total atomic percentage of the alloy, the content of the damping element W is 0.5-1.0 at.%, and based on the total number of atoms in the second sublattice, the combined atomic fraction of Ni and Mn elements is 0.35-0.55%. The high-density solid-state hydrogen storage material contains a first anti-segregating element distributed in the second sublattice. The first anti-segregating element is Sn, Sb, or a combination of Sn and Sb. The total content of the first anti-segregating element is 0.3–0.8 at.% based on the total alloy atomic percentage. The interstitial site set contains interstitial elements C and N; in atomic parts per million, the content of interstitial element C is 30-120 appm, and the content of interstitial element N is 30-120 appm. Furthermore, the occupancy of each of the above components satisfies the following constraints: the first stabilizing element Zr and the second stabilizing element Al enter the first sublattice, the damping element W and the first anti-segregation element enter the second sublattice, and the interstitial element C and the interstitial element N occupy the set of interstitial sites.
[0005] In a preferred embodiment, the atomic fractions of Fe, Co, Ni, Mn and Cu in the second sublattice are all 15-25%, and the content of the damping element W is 0.6-0.9 at.% of the total alloy atomic percentage.
[0006] In a preferred embodiment, the first antisegregating element is a combination of Sn and Sb elements, wherein the Sn element content is 0.30 to 0.60 at.% and the Sb element content is 0.05 to 0.20 at.% in terms of total alloy atomic percentage, and the atomic ratio of Sn to Sb is 3:1 to 10:1.
[0007] In a preferred embodiment, the atomic ratio of the first stabilizing element Zr to the second stabilizing element Al in the first sublattice is 1:1 to 3:1, and the atomic fraction of the Ti element is not less than 0.97 based on the total number of atoms in the first sublattice.
[0008] In a preferred embodiment, the upper limit of impurities in the all-alloy is: the sum of atomic parts per million of oxygen, sulfur and phosphorus is not higher than 300 appm, and the content of boron is not higher than 50 appm.
[0009] In a preferred embodiment, the alloy further includes an electronic structure regulating element Ta, wherein the content of the electronic structure regulating element Ta is 0.10 to 0.30 at.% of the total alloy atomic percentage. The electronic structure regulating element Ta preferentially enters the first sublattice to maintain the stability of the plateau pressure without introducing new phase separation.
[0010] A method for preparing a high-density solid-state hydrogen storage material based on TiFe alloy doping modification includes the following steps: Step 1: Weighing and Proportioning Raw Materials Based on the design formula with full alloy atomic percentage, Ti, Fe, Co, Ni, Mn, Cu, the first stabilizing element Zr, the second stabilizing element Al, the damping element W, the first anti-segregation element Sn and / or Sb, and the electronic structure adjustment element Ta, which is selected when the platform pressure needs to be adjusted, are included. Pre-alloying supports for introducing interstitial elements C and N are also prepared. The content of the first stabilizing element Zr is 0.5–2.0 at.%, the content of the second stabilizing element Al is 0.3–1.5 at.%, and the total content of Zr and Al is 1.0–3.0 at.%. The atomic fractions of Fe, Co, Ni, Mn and Cu in the second sublattice are all 10 to 30%, and the combined atomic fraction of Ni and Mn is 0.35 to 0.55, wherein the atomic fractions are calculated based on the total number of atoms in the second sublattice. The content of damping element W is 0.5–1.0 at.%; The total content of the first anti-segregating element is 0.3 to 0.8 at.%; when it is a combination of Sn and Sb, the content of Sn is 0.30 to 0.60 at.% and the content of Sb is 0.05 to 0.20 at.%, and the atomic ratio of Sn to Sb is 3:1 to 10:1. When the electronic structure regulating element Ta is selected, its content is 0.10 to 0.30 at.% and it preferentially enters the first sublattice; Interstitial element C and interstitial element N were introduced at contents ranging from 30 to 120 appm. Step 2: Pretreatment and purification: The Ti element, the first stabilizing element Zr, and the second stabilizing element Al are subjected to vacuum annealing to remove the surface oxide layer; the Fe element, Co element, Ni element, Mn element, Cu element, damping element W, and the first anti-segregation element Sn and / or Sb are subjected to acid washing and drying to ensure that the total impurity content of oxygen, sulfur and phosphorus is not higher than 300 appm and boron is not higher than 50 appm. Step 3: Alloy Melting In a vacuum induction melting furnace, all the S2-treated metal raw materials are added to the crucible at once, and then... -3 Heating to complete melting under a vacuum of less than Pa; then argon gas protection is introduced, and melting and mechanical stirring are continued to achieve the dissolution of components in the first and second sub-lattices; during the melting process, by controlling the temperature and stirring frequency, it is ensured that the first stabilizing element Zr and the second stabilizing element Al preferentially dissolve in the first sub-lattice, and the damping element W and the first anti-segregation element Sn and / or Sb preferentially dissolve in the second sub-lattice; Step 4: Introduction of gap elements: When the main alloy melt is cooled to the semi-solid temperature range, a pre-alloyed powder containing interstitial elements C and N is added in a measured amount and stirred rapidly to promote the uniform distribution of interstitial elements C and N and their occupation of interstitial sites; step four is carried out in an argon protective atmosphere to reduce the surface reaction loss of interstitial elements. Step 5, Solidification and Ingot Casting: The melt is cast into ingots under an inert atmosphere and directional cooling is used to reduce dendrite segregation; after the ingots are formed, they are slowly cooled to room temperature under an inert atmosphere. Step Six: Homogenization Heat Treatment The ingot is heated to 850–950°C under vacuum or high-purity argon protection and held for 24–72 hours to achieve diffusion of elements in the first and second sublattices. Step 7: Crushing and Shaping The heat-treated alloy is mechanically crushed to the target particle size under an inert atmosphere and then activated in an argon or hydrogen atmosphere to form an activated surface suitable for high-density solid hydrogen storage; finally, it is pressed or filled according to the requirements of the hydrogen storage device. Step 8: Finished Product Inspection The compositional distribution of the first sublattice, the second sublattice, and the interstitial site set is tested to determine whether they meet the content range and occupancy relationship defined in any one of claims 1 to 6; the reversible capacity, plateau pressure stability, and tail-end hydrogen desorption rate of the material are tested under multi-cycle hydrogen adsorption and desorption conditions to confirm that the material does not form a continuous segregation band along the hydrogen diffusion direction during cycling.
[0011] The technical effects and advantages of this invention are as follows: 1. By controlling the preferential solid-solid dissolution of the first stabilizing element Zr and the second stabilizing element Al in the first sub-lattice, and the preferential solid-solid dissolution of the damping element W and the first anti-segregation element Sn and / or Sb in the second sub-lattice, the kinetic pathway of dopant atoms migrating along the hydrogen diffusion channel is blocked under the coupled environment of high hydrogen activity and cyclic stress. This fundamentally suppresses the formation of segregation bands at the nanometer to micrometer scale, eliminates the local hydrogen retention phenomenon at the hydrogen desorption tail end, and stabilizes the reversible hydrogen storage capacity. 2. The twin-lattice oriented solid solution strategy, while ensuring structural stability, optimizes the lattice matching degree between the main phase and the hydride phase through differences in elemental radii and valence electron structures, reduces interfacial strain concentration, lowers the energy barrier of hydrogen diffusion paths during absorption and desorption, and improves the equilibrium of reaction kinetics. 3. The solid solution of damping element W in the second sublattice suppresses the propagation of microcracks induced by cyclic stress, while the anti-segregation elements Sn / Sb stabilize the electronic structure of the hydride phase by adjusting the local electronic state density, thereby reducing the rate of reversible capacity decay caused by electronic structure distortion. 4. The synergistic effect of interstitial elements C and N in the interstitial site set can optimize the local strain and chemical environment of the hydrogen diffusion path, reduce diffusion path distortion and blockage during cycling, and thus maintain a high hydrogen transport rate during long-term service: 5. By precisely controlling the temperature and stirring frequency, elements with different chemical properties and diffusion coefficients preferentially enter the target sublattice during the solid-state reaction, ensuring from a process perspective that the final material's sublattice element distribution is consistent with the designed configuration, and avoiding subsequent thermodynamic redistribution of elements. 6. TiFe alloys optimized by twin lattice doping and interstitial element adjustment exhibit low hydrogen absorption start-up delay and rapid hydrogen release rate at room temperature, avoiding long-tail decay of outlet hydrogen concentration and achieving stable energy output. They are suitable for high-cycle-frequency scenarios such as fuel cells and distributed energy storage. Attached Figure Description
[0012] Figure 1 This is a flowchart of the preparation method of the present invention. Detailed Implementation
[0013] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0014] Refer to the instruction manual appendix Figure 1 An embodiment of the present invention provides a high-density solid-state hydrogen storage material based on TiFe alloy doping modification, wherein the material has a B2 ordered intermetallic compound structure; The crystal structure of the material includes a first sublattice, a second sublattice, and a set of interstitial sites that occupy mutually independent positions; wherein: The first sublattice is a Ti-site sublattice, which uses Ti as a matrix and contains at least one of the first stabilizing element Zr and the second stabilizing element Al. Based on the atomic percentage of the entire alloy, the content of the first stabilizing element Zr is 0.5–2.0 at.%, the content of the second stabilizing element Al is 0.3–1.5 at.%, and the total content of the first stabilizing element Zr and the second stabilizing element Al is 1.0–3.0 at.%. The second sublattice is an Fe-site sublattice, which is composed of Fe, Co, Ni, Mn, Cu, and a damping element W. Based on the total number of atoms in the second sublattice, the atomic fraction of each of the Fe, Co, Ni, Mn, and Cu elements is 10-30%. Based on the total atomic percentage of the alloy, the content of the damping element W is 0.5-1.0 at.%, and based on the total number of atoms in the second sublattice, the combined atomic fraction of Ni and Mn elements is 0.35-0.55%. The high-density solid-state hydrogen storage material contains a first anti-segregating element distributed in the second sublattice. The first anti-segregating element is Sn, Sb, or a combination of Sn and Sb. The total content of the first anti-segregating element is 0.3–0.8 at.% based on the total alloy atomic percentage. The interstitial site set contains interstitial elements C and N; in atomic parts per million, the content of interstitial element C is 30-120 appm, and the content of interstitial element N is 30-120 appm. Furthermore, the occupancy of each of the above components satisfies the following constraints: the first stabilizing element Zr and the second stabilizing element Al enter the first sublattice, the damping element W and the first anti-segregation element enter the second sublattice, and the interstitial element C and the interstitial element N occupy the set of interstitial sites, so as to suppress the continuous segregation band formed along the hydrogen diffusion direction and stabilize the reversible hydrogen storage capacity during the hydrogen absorption and desorption cycle. It should be noted that this scheme precisely arranges the components around the "two sub-lattices + interstitial sites" architecture of B2 ordered intermetallic compounds: Zr and / or Al are introduced into the first sub-lattice (Ti-site sub-lattice) to stabilize the lattice parameters and local coordination environment with stabilizing elements whose atomic size and valence electron structure are close to those of the Ti sites. This reduces strain concentration caused by volume effects at the Ti sites during hydrogen absorption and desorption, and converges the energy level distribution of hydrogen-related sites within the reversible range, thereby stabilizing the plateau pressure and cyclic volume changes. In the second sub-lattice (Fe-site sub-lattice), a multi-component distribution of Fe / Co / Ni / Mn / Cu is used, with a limited total ratio of Ni and Mn. A small amount of W is added as a "dampening factor for diffusion and phase separation." The combined effect is... The configuration entropy of the second sublattice is increased, the chemical potential driving force of a single element is weakened, and the equilibrium strength of the transition metal-hydrogen interaction is maintained. At the same time, the reversible capacity and kinetics are ensured by the catalytic effect of Ni on hydrogen decomposition / recombination and the buffering effect of Mn on lattice expansion. In the same second sublattice, Sn and / or Sb with low content are used as the first anti-segregation element. Their p-block elemental characteristics can improve the nucleation work of potential segregation nuclei and increase the interface energy, making it difficult for continuous segregation along the hydrogen diffusion channel to occur or grow. Only appm-level C and N are introduced in the interstitial site set. By forming stable complexes with vacancies / dislocations, the apparent energy barrier of long-range atomic migration in the alloy is increased, "freezing" unfavorable migration kinetics without significantly sacrificing the diffusion channel. Based on the synergistic setting of site occupancy and content, the material will undergo a controlled evolution during actual hydrogen adsorption and desorption cycles as follows: First, the stable Zr / Al first sublattice provides a relatively rigid framework, reducing chemical potential fluctuations around Ti sites; subsequently, the multi-component distribution of the second sublattice and the damping effect of W together smooth out the element migration driving force caused by the hydrogen concentration gradient, and Sn / Sb further raises the segregation nucleation threshold, causing the enrichment bands that were originally easy to self-organize and form on the main hydrogen diffusion channel to lose thermodynamic and kinetic support; at the same time, the pinning effect of interstitial C / N on defects suppresses the propagation of a small number of misoccupied sites or local disturbances. The expected results are: the diffusion coefficient and site energy level of hydrogen remain spatially uniform throughout the entire volume; the hydrogen absorption and desorption plateau pressure and reversible capacity remain stable after multiple cycles; the long-tail decay of the hydrogen desorption tail is significantly compressed; and no continuous segregation bands are formed inside the material along the hydrogen diffusion direction. This mechanism chain provides the principle basis for the "suppression of segregation bands - stabilization of reversible capacity" of this scheme, and explains why the combination of each component and each sublattice is a necessary and sufficient combination.
[0015] In the second sublattice, the atomic fractions of Fe, Co, Ni, Mn, and Cu are all 15-25%, and the content of the damping element W is 0.6-0.9 at.% based on the total alloy atomic percentage. As a further approach, the atomic fractions of Fe, Co, Ni, Mn, and Cu in the second sublattice are uniformly limited to 15-25%. The core objective is to achieve a balance between high entropy distribution and lattice stability. If the proportions of each component are too low, it will be difficult to form a significant configurational entropy to smooth the chemical potential gradient, making it easy for a high-content element to segregate under the drive of the hydrogen concentration gradient. Conversely, if the proportions are too high, it will compress the occupancy opportunities of other components and reduce the solid solution stabilization effect caused by the mutual perturbation between multiple components. In conjunction with controlling the damping element W in the range of 0.6-0.9 at.%, it is based on its "dual damping effect" on diffusion and phase separation in the Fe sublattice. Within this content range, the positive enthalpy of mixing of W can increase the long-range migration barrier of solute atoms, delaying the component rearrangement accompanying the hydrogenation reaction, while preventing the precipitation of new phases or plateau pressure drift due to excessive content. Overall, this ratio setting can ensure that the second sublattice maintains a high configurational entropy global chemical potential flatness during hydrogen absorption and desorption, and under the dynamic damping effect of W, suppresses the formation of local component enrichment bands along the hydrogen diffusion direction, thus complementing the stable framework of the first sublattice and improving the material's reversible hydrogen storage performance and cycle life.
[0016] The first anti-segregating element is a combination of Sn and Sb elements. The Sn element content is 0.30 to 0.60 at.% and the Sb element content is 0.05 to 0.20 at.% in terms of total alloy atomic percentage. The atomic ratio of Sn to Sb is 3:1 to 10:1. In a further proposed scheme, the first anti-segregation element is set as a combination of Sn and Sb elements, with strict limits on their respective contents and proportions. This is based on the coupling and control principle of the coordination chemical properties of the two elements in the Fe site sub-lattice and the segregation thermodynamic effect. By controlling the Sn element content at 0.30–0.60 at.% in terms of the total alloy atomic percentage, it can ensure that its p-region metallic properties provide sufficient local electronic state perturbation in the second sub-lattice, thereby improving the interface energy for segregation nucleation. If the Sn content is below 0.30 at.%, the suppression effect is insufficient, while if it is above 0.60 at.%, a brittle phase enriched in Sn may be formed. Controlling the Sb element at 0.05–0.20 at.% utilizes its larger atomic radius and stronger electronic localization effect to form a microscopic pairing structure with Sn in the Fe sub-lattice, further improving the nucleation work of potential segregated nuclei along the hydrogen diffusion direction; the synergistic effect is not obvious below 0.05 at.%, while it is easy to induce the accumulation of lattice distortion above 0.20 at.%. Setting the atomic ratio of the two to 3:1 to 10:1 is to achieve the best synergy between the dominant interfacial energy enhancement effect of Sn and the radius distortion effect of Sb: too low a ratio will weaken the interfacial energy enhancement effect of Sn, while too high a ratio will reduce the coordination perturbation contribution of Sb. Overall, this content and ratio design can effectively raise the thermodynamic and kinetic threshold for the formation of continuous segregation bands along the hydrogen diffusion channel while ensuring solid solution stability, thereby achieving long-term stable reversible hydrogen storage capacity and plateau pressure.
[0017] In the first sublattice, the atomic ratio of the first stabilizing element Zr to the second stabilizing element Al is 1:1 to 3:1, and based on the total number of atoms in the first sublattice, the atomic fraction of the Ti element is not less than 0.97. As a further approach, the atomic ratio of the first stabilizing element Zr to the second stabilizing element Al in the first sublattice is limited to 1:1 to 3:1, and the atomic fraction of Ti is required to be no less than 0.97 based on the total number of atoms in the first sublattice. This design logic stems from the precise control of the lattice stability of Ti sites in B2 ordered intermetallic compounds. Zr and Al complement each other for Ti sites in terms of atomic radius and valence electron structure, respectively: Zr's larger atomic radius can buffer the volume expansion strain during hydrogen absorption and desorption, while Al's electronic structure can fine-tune the bonding strength between Ti sites and hydrogen. Maintaining the ratio between the two at 1:1 to 3:1 can maintain lattice stability while avoiding a decrease in orderliness or local chemical potential imbalance caused by an excess of a single element. Simultaneously, maintaining the atomic fraction of Ti at ≥0.97 ensures that the main characteristics of Ti sites are not excessively replaced, maintaining the continuity and framework support of the first sublattice during phase transitions. When the Ti percentage is lower than this value, the Zr / Al substitution ratio becomes too high, potentially causing plateau pressure shifts and distortion of the hydrogen diffusion path. In summary, this ratio and content setting can enable Zr and Al to achieve synergistic size and electronic effects without damaging the main structure of Ti sites, thereby stabilizing the platform pressure, reducing cyclic stress concentration, and enhancing the structural integrity of the material during multiple hydrogen adsorption and desorption processes.
[0018] The upper limit of impurities in the full alloy is: the total atomic parts per million of oxygen, sulfur and phosphorus is not higher than 300 appm, and the content of boron is not higher than 50 appm. It should be noted that this approach aims to control the content of non-designed elements that could compromise the reversibility of hydrogen storage and lattice stability at the source. Oxygen, sulfur, and phosphorus are high-affinity nonmetallic elements that readily react with reactive metals such as Ti, Zr, and Al during smelting and cycling to form oxides, sulfides, or phosphides. These inclusions are typically located at grain boundaries or dislocations, weakening the diffusion path of hydrogen in the lattice and becoming crack initiation sources. When the total content is controlled below 300 appm, the volume fraction of these inclusions is sufficiently low to prevent the formation of a through-brittle phase under cyclic loading. Boron at the ppm level can act as an interstitial element affecting the lattice stress field, but when the content exceeds 50 appm, B atoms may segregate at grain boundaries and form stable brittle compounds (such as TiB2), thereby reducing the material's toughness and cyclic impact resistance. Therefore, this impurity limit is set to prevent non-designed elements from forming irreversible chemical bonds and structural defects at sublattices or grain boundaries, ensuring the long-term structural integrity and performance stability of this alloy during high-density hydrogen absorption and desorption.
[0019] It also includes an electronic structure regulating element Ta, with the content of the electronic structure regulating element Ta being 0.10 to 0.30 at.% based on the atomic percentage of the whole alloy. The electronic structure regulating element Ta preferentially enters the first sub-lattice to maintain the stability of the plateau pressure without introducing new phase separation. Furthermore, the scheme introduces an additional electronic structure regulating element, Ta, into the full alloy, limiting its content to 0.10–0.30 at.%, and requiring it to preferentially enter the first sublattice (Ti site sublattice). The aim is to stabilize the hydrogen adsorption / desorption plateau pressure of the material by adjusting the electronic state distribution of the first sublattice without inducing unfavorable phase structure changes. As a transition metal, Ta exhibits controllable hybridization of its 5d orbitals with the 3d orbitals of Ti in terms of energy levels and spatial distribution. When Ta is dissolved in trace amounts at Ti sites, it can refine the electron density distribution around the Ti sites, thereby adjusting the binding energy of the Ti–H bond and stabilizing the enthalpy of hydrogen adsorption-desorption reaction at a certain level. Within the target range, significant drift in plateau pressure during multiple cycles should be avoided. When the content is below 0.10 at.%, this electronic state regulation effect is insufficient, making it difficult to effectively fine-tune the plateau pressure. When it is above 0.30 at.%, the large atomic radius and strong metallic bonds of Ta may disrupt the order of the Ti site lattice, inducing the precipitation of additional phases or local disorder of the B2 phase. Preferentially allocating Ta to the first sublattice ensures that the electronic state regulation effect is concentrated on the Ti site framework that determines the thermodynamic properties of hydrogenation. This maintains the kinetic activity of hydrogen absorption and desorption reactions without introducing the risk of new phase separation, thus achieving a dual guarantee of plateau pressure stability and structural integrity.
[0020] A method for preparing a high-density solid-state hydrogen storage material based on TiFe alloy doping modification includes the following steps: Step 1: Weighing and Proportioning Raw Materials Based on the design formula with full alloy atomic percentage, high-purity Ti, Fe, Co, Ni, Mn, Cu, the first stabilizing element Zr, the second stabilizing element Al, the damping element W, the first anti-segregation element Sn and / or Sb, and the electronic structure adjustment element Ta, which is used when the platform pressure needs to be adjusted, are selected. Pre-alloying supports for introducing interstitial elements C and N are also prepared. Among these: The content of the first stabilizing element Zr is 0.5–2.0 at.%, the content of the second stabilizing element Al is 0.3–1.5 at.%, and the total content of Zr and Al is 1.0–3.0 at.%. The atomic fractions of Fe, Co, Ni, Mn and Cu in the second sublattice are all 10 to 30%, and the combined atomic fraction of Ni and Mn is 0.35 to 0.55, wherein the atomic fractions are calculated based on the total number of atoms in the second sublattice. The content of damping element W is 0.5 to 1.0 at.% (preferably 0.6 to 0.9 at.%). The total content of the first anti-segregating element is 0.3 to 0.8 at.%; when it is a combination of Sn and Sb, the content of Sn is 0.30 to 0.60 at.% and the content of Sb is 0.05 to 0.20 at.%, and the atomic ratio of Sn to Sb is 3:1 to 10:1. When the electronic structure regulating element Ta is selected, its content is 0.10 to 0.30 at.% and it preferentially enters the first sublattice; Interstitial element C and interstitial element N were introduced at contents ranging from 30 to 120 appm. Step 2: Pretreatment and purification: The Ti element, the first stabilizing element Zr, and the second stabilizing element Al are subjected to vacuum annealing to remove the surface oxide layer; the Fe element, Co element, Ni element, Mn element, Cu element, damping element W, and the first anti-segregation element Sn and / or Sb are subjected to acid washing and drying to ensure that the total impurity content of oxygen, sulfur and phosphorus is not higher than 300 appm and boron is not higher than 50 appm. Step 3: Alloy Melting In a vacuum induction melting furnace, all the S2-treated metal raw materials are added to the crucible at once, and then... -3 Heating to complete melting under a vacuum of less than Pa; then purging with high-purity argon gas for protection, continuing melting and mechanical stirring to achieve uniform dissolution of the components in the first and second sub-lattices; during the melting process, by controlling the temperature and stirring frequency, ensuring that the first stabilizing element Zr and the second stabilizing element Al preferentially dissolve in the first sub-lattice, and the damping element W and the first anti-segregation element Sn and / or Sb preferentially dissolve in the second sub-lattice; Regarding S3, it should be noted that the temperature and stirring frequency control mentioned above are intended to artificially adjust the chemical potential difference and diffusion kinetics of different elements during alloy solidification. This allows the first stabilizing element Zr and the second stabilizing element Al to preferentially enter the first sublattice (Ti site sublattice), and the damping element W and the first anti-segregation element Sn and / or Sb to preferentially enter the second sublattice (Fe site sublattice). Specifically, after the raw materials are completely melted, the melt temperature is controlled in the high superheated zone above the liquidus line and held for a short time to eliminate initial local segregation. Subsequently, the temperature is lowered to the range close to the solidus line, where the B2 short-range ordered structure begins to form. During this stage, the order of the Ti site sublattice is rapidly established, and the chemical potential of the Ti site increases, which is beneficial to the atomic radius. Zr and Al, whose electronic structures match those of Ti sites, are dissolved into the first sublattice. At this point, low-to-medium frequency continuous stirring is used to maintain a stable local ordered environment and reduce interference from Fe site elements. Then, as solidification is about to be completed, the temperature is maintained within a range that can activate atomic migration without destroying the already formed ordered structure. At the same time, high-frequency pulse stirring is switched to promote rapid homogenization of the liquid phase composition around the Fe sites, allowing W and Sn / Sb, which have higher mixing enthalpy and coordination matching degree with Fe sites, to preferentially dissolve into the second sublattice. Finally, this occupancy difference is "frozen" by controlled cooling, and after ingot formation, a short-term heat treatment is performed at a homogenization temperature below the instability threshold of the ordered structure to return a small number of misoccupied atoms to their thermodynamically preferred positions, further enhancing this selective solid solution effect. Step 4: Introduction of gap elements: When the main alloy melt is cooled to the semi-solid temperature range, a pre-alloyed powder containing interstitial elements C and N is added in a measured amount and stirred rapidly to promote the uniform distribution of interstitial elements C and N and their occupation of interstitial sites; step four is carried out in an argon protective atmosphere to reduce the surface reaction loss of interstitial elements. Step 5, Solidification and Ingot Casting: The melt is cast into ingots under an inert atmosphere and directional cooling is used to reduce dendrite segregation. After the ingot is formed, it is slowly cooled to room temperature under an inert atmosphere to ensure the high-entropy second sub-lattice structure and the stable occupancy of interstitial elements. Step Six: Homogenization Heat Treatment The ingot is heated to 850–950°C under vacuum or high-purity argon protection and held for 24–72 hours to achieve diffusion of elements in the first and second sublattices. Step 7: Crushing and Shaping The heat-treated alloy is mechanically crushed to the target particle size (including but not limited to 50-150 μm) under an inert atmosphere, and then activated in an argon or hydrogen atmosphere to form an activated surface that can be used for high-density solid hydrogen storage; finally, it is pressed or filled according to the requirements of the hydrogen storage device. Step 8: Finished Product Inspection The compositional distribution of the first sublattice, the second sublattice, and the interstitial site set is tested to determine whether they meet the content range and occupancy relationship defined in any one of claims 1 to 6; the reversible capacity, plateau pressure stability, and tail-end hydrogen desorption rate of the material are tested under multi-cycle hydrogen adsorption and desorption conditions to confirm that the material does not form a continuous segregation band along the hydrogen diffusion direction during cycling.
[0021] This solution includes, but is not limited to, the following embodiments: Example 1 (Sn+Sb used together; Ta-free; total Zr+Al = 1.5 at.%): 1) Formula and Placement: First sublattice (Ti sublattice, total 50 at.%): Total alloy content: Ti 48.5 at.%, Zr 1.0 at.%, Al 0.5 at.% (Ti atomic fraction in the first sublattice = 97.0%). Second sublattice (Fe site sublattice, total 50 at.%): W 0.70 at.%, Sn 0.45 at.%, Sb 0.10 at.%; Sublattice distribution (based on the total number of atoms in the second sublattice): Fe=23.0%, Co=20.0%, Ni=22.0%, Mn=18.0%, Cu=14.5%, W+Sn+Sb=2.5% (where Ni+Mn=40.0%, satisfying 0.35~0.55); Note: The content of each of the above five elements (Fe / Co / Ni / Mn / Cu) is in the range of 10% to 30%; Gap position set: C60appm, N80appm; 2) Key points of preparation (numerical window corresponding to the method): Vacuum induction melting: base vacuum ≤ 5 × 10 -4 Pa; superheat 120-150K (above the liquidus), hold for 6-10 minutes; Cool to the range of (solid line +20~35K); stir continuously at medium and low frequency at 180~240rpm (to maintain a short-range ordered environment at Ti sites) for 10~15min; Switch to pulse stirring at the end of solidification: 600-800 rpm, 2s on / 3s off, cycle for 2-4 min (to homogenize the composition of the Fe site neighborhood). Add C / N pre-alloyed powder to the semi-solid zone: stir continuously for 60-90 seconds after addition; argon gas 99.999% protection (dew point ≤ -60℃); Directional solidification and slow cooling; Homogenization heat treatment: 900℃×48h (Ar protection), furnace cooling to 600℃ followed by air cooling; Inertly pulverize to 50–150 μm, and activate under H2 / Ar (volume fraction 1% / 99%) for 30–60 min; 3) Structure and composition confirmation: XRD / Rietveld: B2 ordered phase, no second phase diffraction peaks; EPMA / EDS line scan (section ≥ 500 μm): W, Sn, Sb fluctuations in the thickness direction < 0.3 at.%; Sublattice site fitting: Zr / Al is located at Ti sites; W / Sn / Sb is located at Fe sites (consistent with the claims constraints); 4) Key points for hydrogen absorption / desorption verification: Sieverts process: 200 cycles of hydrogen absorption (3.0 MPa, 30°C) / hydrogen release (0.1 MPa, 30°C); Observations: The tail of the hydrogen desorption curve was within the baseline noise and there was no continuous long tail; the reversible capacity decay tended to be a linear and slight decay; no signs of continuous segregation bands were observed. Example 2 (Sn only; containing Ta = 0.20 at.%; total Zr + Al + Ta = 1.0 at.%): 1) Formula and Placement: First sublattice (total 50 at.%): All alloy composition: Ti 49.0 at.%, Zr 0.5 at.%, Al 0.3 at.%, Ta 0.2 at.% (Ti atomic fraction in the first sublattice = 98.0%). Second sublattice (total 50 at.%): All alloy composition: W 0.90 at.%, Sn 0.60 at.%; Sublattice distribution: Fe=17.0%, Co=14.0%, Ni=28.0%, Mn=22.0%, Cu=16.0%, W+Sn=3.0% (Ni+Mn=50.0%, within 0.35~0.55; each of the five elements 10~30%). Gap position set: C30appm, N60appm; 2) Key points of preparation: The smelting and atmosphere control are the same as in Example 1; The temperature / stirring strategy is the same as in Example 1; Homogenization heat treatment: 900℃ for 36 to 48 hours; The other steps are the same; 3) Structure and composition confirmation XRD: B2 ordered phase; Quantitative EDS / WDS: Ta is preferentially located in the neighborhood of Ti sites (consistent with the requirement of "preferential entry into the first sublattice"); Inside the second sub-lattice: Ni / Mn high ratio (total 50%) but no second phase induced; 4) Key points for hydrogen absorption / desorption verification: Repeated testing under the same conditions; Observations: The platform pressure stability improved; the hydrogen release tail converged rapidly; no identifiable continuous segregation bands appeared in the depth distribution of elements after cycling; Example 3 (Sb only; low W; total Zr + Al = 1.0 at.%): 1) Formula and Placement: First sublattice (total 50 at.%): All alloy composition: Ti 49.0 at.%, Zr 0.5 at.%, Al 0.5 at.% (Ti atomic fraction in the first sublattice = 98.0%). Second sublattice (total 50 at.%): All alloy composition: W 0.50 at.%, Sb 0.30 at.%; Sublattice distribution: Fe=27.0%, Co=24.0%, Ni=19.0%, Mn=16.0%, Cu=12.4%, W+Sb=1.6% (Ni+Mn=35.0%, within 0.35~0.55; each of the five elements 10~30%). Gap site set: C120appm, N30appm (boundary value combination, used to confirm site occupancy and diffusion stability); 2) Key points of preparation: The smelting window is the same as in Example 1; After adding C / N in a semi-solid state, stir rapidly for 90 seconds. Homogenization heat treatment: 880~900℃×48h (lower temperature to avoid short-range orderly fluctuations under low W); 3) Structure and composition confirmation: XRD: B2 phase, peak width and lattice constant are stable within statistical error; EPMA: Sb is uniform at grain boundaries / within grains, with no continuous enriched bands; Even under low W conditions, the requirement of 10-30% sub-lattice distribution of each of the five elements is still met; 4) Key points for hydrogen absorption / desorption verification: After 100 cycles, the EPMA line scan was repeated, and the elemental fluctuation was still <0.4 at.%; The hydrogen expulsion curve shows no long tail; the tail rate shows no significant tailing. Example 4 (Sn+Sb combined; high W and high Ni+Mn; total Zr+Al = 1.5 at.%) 1) Formula and Placement: First sublattice (total 50 at.%): All alloy composition: Ti 48.5 at.%, Zr 0.6 at.%, Al 0.9 at.% (Ti atomic fraction in the first sublattice = 97.0%). Second sublattice (total 50 at.%): All alloy composition: W 1.00 at.%, Sn 0.64 at.%, Sb 0.16 at.% (Sn∶Sb=4∶1, satisfying 3∶1~10∶1; Sn+Sb=0.80 at.%) Sublattice composition: Ni=30.0%, Mn=25.0% (Ni+Mn=55.0%, near the upper limit of 0.35~0.55), Fe=18.0%, Co=13.0%, Cu=10.4%, W+Sn+Sb=3.6% (each of the five elements is 10~30%). Gap position set: C90appm, N90appm; 2) Key points of preparation: The superheat is set at 130–150 K; Continuous stirring at low to medium frequency 200-240 rpm (Ti site directional solid solution stage) → pulse stirring 700-800 rpm (Fe site homogenization stage); Homogenize at 910℃ for 48 hours after directional solidification; 3) Structure and composition confirmation: Rietveld: B2 phase ratio ≈100%, no precipitation peaks; EPMA surface scan: Total fluctuation of W / Sn / Sb < 0.5 at.%; no continuous segregation bands were generated; 4) Key points for hydrogen absorption / desorption verification: Under the combination of high Ni+Mn and high W, the hydrogen desorption platform remains stable and there is no long tail in the tail section; After a long period (≥200 times), the reversible capacity remained stable, and no delayed hydrogen release phenomenon was observed.
[0022] In Example 1, XRD / Rietveld refinement first confirmed that the sample only exhibited the B2 ordered phase, with no second-phase diffraction peaks detected. This indicates that the synergistic control of melting and temperature / stirring successfully achieved stable solid solution of Zr and Al in the Ti sublattice, and ordered distribution of W, Sn, and Sb in the Fe sublattice. Subsequently, EPMA / EDS was used to perform a depth scan of ≥500 μm on the cross-section. The results showed that the content fluctuations of W, Sn, and Sb in the thickness direction were all less than 0.3 at.%. This uniformity stemmed from the rapid local composition homogenization brought about by high-frequency pulse stirring at the end of solidification, and the suppression of diffusion-driven segregation growth by the directional solidification-slow cooling process. In external hydrogen absorption and desorption cycling tests, the Sieverts method was used to cycle 200 times under conditions of hydrogen absorption at 3.0 MPa and 30 °C and hydrogen desorption at 0.1 MPa and 30 °C. The reversible capacity retention rate remained between 96% and 98%, and the convergence time of the tail end of the hydrogen desorption curve did not increase with the increase of cycles. This stability is due to the anti-segregation effect formed by Sn / Sb at the Fe site, which inhibits the formation of chemical potential traps on the hydrogen diffusion channel and fundamentally blocks the self-organization process of continuous segregation bands. The overall results show that the multi-component synergistic site occupation strategy of this formulation effectively maintains structural homogeneity and hydrogen desorption kinetic stability in long-term cycling, proving its feasibility and ingenuity in the anti-segregation mechanism. In Example 2, 0.20 at.% Ta was additionally introduced into the first sublattice. XRD analysis showed that the sample was a single B2 ordered phase, indicating that the addition of Ta did not introduce new phase separation. WDS quantitative analysis showed that Ta was mainly distributed in the vicinity of Ti sites, which is consistent with its role in electronic structure regulation, namely, stabilizing the plateau pressure by increasing the local binding energy of Ti sites. In 200 cycles of hydrogen adsorption and desorption experiments, the relative drift of the plateau pressure remained within ±4%, while the normalized area change at the end of the hydrogen desorption phase was not significant, and the capacity retention rate was 95%–97%. This stability can be attributed to two aspects: firstly, Ta, Zr, and Al jointly occupy the Ti sublattice, reducing the sensitivity of the plateau pressure to hydrogen concentration; secondly, the presence of Sn in the Fe sites continues to play an anti-segregation role, keeping the long-range diffusion path of hydrogen unobstructed and avoiding the formation of segregation bands. No continuous enrichment bands of Sn were observed in the depth scan after cycling, indicating that while the plateau stability was improved, the anti-segregation mechanism remained effective, verifying the feasibility of the formulation in achieving dual objectives (pressure stabilization and anti-segregation). Example 3 uses an anti-segregation elemental system containing only Sb, with the W content reduced to 0.50 at.%, and the C / N interstitial element ratio set as a boundary value (C=120 appm, N=30 appm) to verify the robustness of the scheme. XRD results show that the peak width and lattice constant of the B2 phase do not change significantly within the statistical error, indicating that the combination of low W and boundary interstitial elements does not destroy the overall phase structure. EPMA analysis shows that Sb is uniformly distributed at grain boundaries and within grains, with a fluctuation range of less than 0.4 at.%, which is consistent with the stirring at the end of solidification. The homogenization and interstitial element freezing effect are closely related. C and N form a composite defect at the interstitial site, which increases the migration kinetic energy barrier of Sb, thereby suppressing its segregation along the hydrogen diffusion direction. In the 100-cycle hydrogen adsorption and desorption experiment, there was no obvious long tail at the end of the hydrogen desorption curve, the release rate was comparable to the initial value, and the capacity retention rate was between 95% and 96%. This shows that even under low W and extreme interstitial element ratios, the anti-segregation mechanism and the interstitial freezing effect can still work synergistically, proving the feasibility and universality of this strategy under different formulation boundary conditions. Example 4 employed a combination of high W (1.00 at.%) and high Ni+Mn (55%), with Sn and Sb used as anti-segregation elements, totaling 0.80 at.%. Rietveld refinement results showed that the B2 phase accounted for approximately 100% of the sample, with no precipitation peaks, indicating that high W and high Ni+Mn did not induce phase separation or unfavorable short-range order. EPMA surface scan data showed that the total fluctuation of W / Sn / Sb across the entire cross-section was less than 0.5 at.%, which is attributed to the synergistic effect of the Fe site sublattice mixing enthalpy normalization brought about by high W and the Sn / Sb anti-segregation effect. During 200 hydrogen absorption and desorption cycles, the plateau pressure change fell within the instrument measurement error range, no obvious long tail was observed in the hydrogen desorption tail, and the capacity retention rate was 94%–96%. In-depth profile analysis confirmed that no continuous segregation bands appeared in the hydrogen diffusion direction, indicating that even when the elemental proportions were close to the upper limit, the chemical potential balance and anti-segregation mechanism still operated effectively. This result verified the feasibility of the scheme under the upper limit of the formulation.
[0023] In addition, it should be noted that the formation of this scheme is based on a targeted improvement strategy proposed after a systematic analysis of the limitations of the hydrogen storage performance of TiFe alloys. Based on our preliminary research and multiple rounds of experiments, our R&D team identified problems such as insufficient hydrogen absorption and desorption rates of TiFe alloys at room temperature and susceptibility to impurities and structural degradation affecting cycle stability. These problems were addressed in the solution through technical descriptions of material composition, microstructure, and preparation process. In response to these issues, the proposed solution adopted a multi-component doping modification approach, introducing stabilizing elements, damping elements, anti-segregation elements, and electronic structure adjustment elements into the TiFe alloy system in specific proportions to improve lattice stability and regulate the thermodynamic and kinetic conditions for hydride formation. The rationale for this approach lies in the following: on the one hand, the directional solid solution of doping elements in different sublattices can effectively weaken the lattice distortion and phase transition barriers during the hydrogenation reaction; on the other hand, the synergistic effect between elements can optimize the electronic structure, thereby improving hydrogen storage performance without significantly increasing the preparation cost. In terms of implementation steps, the scheme ensures the uniformity of alloy composition and the stability of structure by successively carrying out steps such as raw material weighing, mechanical alloying, vacuum melting, and annealing; argon gas protection is introduced in key steps to reduce the surface reaction loss of interstitial elements, and specific elements are preferentially dissolved in the target sublattice by controlling temperature and stirring frequency. Secondly, in terms of operating mechanism, the modified TiFe alloy exhibits lower hydrogenation reaction resistance during the hydrogen absorption stage due to enhanced lattice stability, while maintaining high phase structure reversibility during the hydrogen release stage, reducing capacity decay during cycling. In practical applications, this material can be used in high-density solid-state hydrogen storage modules, suitable for fuel cell vehicles, distributed energy storage, and emergency hydrogen supply scenarios, demonstrating the ability to rapidly absorb and release hydrogen at room temperature and a long cycle life.
[0024] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A high-density solid-state hydrogen storage material based on TiFe alloy doping modification, the material having a B2 ordered intermetallic compound structure, characterized in that: the crystal structure of the material comprises a first sub-lattice, a second sub-lattice and a set of interstitial sites independently occupying each other; wherein: the first sub-lattice is a Ti-site sub-lattice, the Ti-site sub-lattice has a Ti element as a matrix and contains at least one of a first stabilizing element Zr and a second stabilizing element Al; the content of the first stabilizing element Zr is 0.5-2.0 at.%, the content of the second stabilizing element Al is 0.3-1.5 at.%, and the total content of the first stabilizing element Zr and the second stabilizing element Al is 1.0-3.0 at.%, all in terms of total alloy atomic percentage; the second sub-lattice is a Fe-site sub-lattice, the Fe-site sub-lattice is composed of Fe element, Co element, Ni element, Mn element, Cu element and damping element W; the atomic fraction of each of the Fe element, Co element, Ni element, Mn element and Cu element is 10-30% based on the total number of atoms in the second sub-lattice; the content of the damping element W is 0.5-1.0 at.%, all in terms of total alloy atomic percentage, and the total atomic fraction of the Ni element and the Mn element is 0.35-0.55 based on the total number of atoms in the second sub-lattice; the high-density solid-state hydrogen storage material contains a first counter segregation element distributed in the second sub-lattice, the first counter segregation element is Sn element, Sb element or a combination of Sn element and Sb element; the total content of the first counter segregation element is 0.3-0.8 at.%, all in terms of total alloy atomic percentage; the set of interstitial sites contains interstitial element C and interstitial element N; the content of the interstitial element C is 30-120 appm and the content of the interstitial element N is 30-120 appm, both in terms of atomic parts per million; and the occupation of each component satisfies the following constraints: the first stabilizing element Zr and the second stabilizing element Al enter the first sub-lattice, the damping element W and the first counter segregation element enter the second sub-lattice, and the interstitial element C and the interstitial element N occupy the set of interstitial sites. 2.The high-density solid-state hydrogen storage material based on TiFe alloy doping modification according to claim 1, characterized in that: the atomic fraction of the Fe element, Co element, Ni element, Mn element and Cu element in the second sub-lattice is 15-25%, and the content of the damping element W is 0.6-0.9 at.%, all in terms of total alloy atomic percentage. 3.The high-density solid-state hydrogen storage material based on TiFe alloy doping modification according to claim 1, characterized in that: The first counter segregation element is a combination of Sn and Sb, the content of Sn is 0.30-0.60 at.%, the content of Sb is 0.05-0.20 at.%, and the atomic ratio of Sn to Sb is 3:1-10:
1. 4.The high-density solid-state hydrogen storage material based on TiFe alloy doped and modified according to claim 1, characterized in that: The atomic ratio of the first stabilizing element Zr to the second stabilizing element Al in the first sublattice is 1:1-3:1, and the atomic fraction of the Ti element is not less than 0.97 based on the total number of atoms in the first sublattice. 5.The high-density solid-state hydrogen storage material based on TiFe alloy doped and modified according to claim 1, characterized in that: The upper limit of impurities in the whole alloy is that the total atomic percentage of oxygen, sulfur and phosphorus is not higher than 300 appm, and the content of boron is not higher than 50 appm. 6.The high-density solid-state hydrogen storage material based on TiFe alloy doped and modified according to any one of claims 1-5, characterized in that: It further comprises an electronic structure adjusting element Ta, the content of the electronic structure adjusting element Ta is 0.10-0.30 at.%, the electronic structure adjusting element Ta preferentially enters the first sublattice to maintain the stability of the platform pressure without introducing new phase separation.
7. A method for preparing high-density solid-state hydrogen storage material based on TiFe alloy doped modification, characterized in that, It comprises the following steps: Step one, raw material weighing and proportioning: According to the design formula of the whole alloy atomic percentage, Ti element, Fe element, Co element, Ni element, Mn element, Cu element, first stabilizing element Zr, second stabilizing element Al, damping element W, first counter segregation element Sn and / or Sb, and electronic structure adjusting element Ta when needed to adjust the platform pressure are selected, and pre-alloyed carriers of gap element introduction sources C and N are prepared; wherein: The content of the first stabilizing element Zr is 0.5-2.0 at.%, the content of the second stabilizing element Al is 0.3-1.5 at.%, and the total content of Zr and Al is 1.0-3.0 at.%; The atomic fraction of Fe element, Co element, Ni element, Mn element and Cu element in the second sublattice is 10-30%, and the total atomic fraction of Ni element and Mn element is 0.35-0.55, wherein the atomic fraction is calculated based on the total number of atoms in the second sublattice; The content of the damping element W is 0.5-1.0 at.%; The total content of the first counter segregation element is 0.3-0.8 at.%, when it is a combination of Sn and Sb, the content of Sn is 0.30-0.60 at.%, the content of Sb is 0.05-0.20 at.%, and the atomic ratio of Sn to Sb is 3:1-10:1; When the electronic structure adjusting element Ta is selected, its content is 0.10-0.30 at.% and it preferentially enters the first sublattice; The interstitial element C and the interstitial element N are introduced in a content of 30-120 appm respectively; Step two, pretreatment and purification: The Ti element, the first stabilizing element Zr, and the second stabilizing element Al are vacuum annealed to remove the surface oxide layer; the Fe element, the Co element, the Ni element, the Mn element, the Cu element, the damping element W, and the first anti-segregation element Sn and / or Sb are pickled and dried to ensure that the total impurity content of oxygen element, sulfur element, and phosphorus element is not higher than 300 appm, and the boron element is not higher than 50 appm; Step three, alloy smelting: In a vacuum induction melting furnace, all the metal raw materials after S2 treatment are added into the crucible at one time, and heated to complete melting under a vacuum degree below 10 -3 argon gas protection, continue to melt and mechanically stir to realize the dissolution of components in the first and second sublattices; during the melting process, by controlling the temperature and stirring frequency, ensure that the first stabilizing element Zr and the second stabilizing element Al are preferentially solid-solved in the first sublattice, and the damping element W and the first anti-segregation elements Sn and / or Sb are preferentially solid-solved in the second sublattice; Step four, interstitial element introduction: When the main alloy melt is cooled to the semi-solid temperature zone, the pre-alloy powder containing the interstitial element C and the interstitial element N is added quantitatively, and rapid stirring is performed to promote the uniform distribution of the interstitial element C and the interstitial element N and occupy the interstitial site set; step four is carried out in an argon protective atmosphere to reduce the surface reaction loss of the interstitial element; Step five, solidification and ingot casting: The melt is poured into an ingot under the protection of an inert atmosphere, and directional cooling is used to reduce dendritic segregation; after the ingot is formed, it is slowly cooled to room temperature under an inert atmosphere; Step six, homogenization heat treatment: The ingot is heated to 850-950℃ under vacuum or high-purity argon protection, and is kept for 24-72 hours to realize the diffusion of each element in the first sublattice and the second sublattice; Step seven, crushing and forming: The heat-treated alloy is mechanically crushed to the target particle size under the protection of an inert atmosphere, and is activated in an argon or hydrogen atmosphere to form an activated surface that can be used for high-density solid-state hydrogen storage; finally, it is pressed or packed according to the requirements of the hydrogen storage device; Step eight, finished product inspection: Detect whether the component distribution of the first sublattice, the second sublattice, and the interstitial site set meets the content range and occupation relationship defined in any one of claims 1-6; test the reversible capacity, platform pressure stability, and tail hydrogen release rate of the material under the condition of multiple cycle hydrogen absorption and release, to confirm that the material does not form a continuous segregation band along the hydrogen diffusion direction during the cycle process.