A method for coating particle dispersed fuel granules in a molding state in combination with split molding
By combining anhydrous ethanol wet ball milling and split molding with SPS sintering technology, the problem of uneven distribution of TRISO particles in SiC matrix was solved, and uniform distribution of TRISO particles in gas-cooled microreactor chips was achieved, improving reactor safety and preparation efficiency.
Patent Information
- Application Number
- CN202511321677.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-16
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2045-09-16
AI Technical Summary
Existing technologies make it difficult to achieve uniform distribution of TRISO particles in the SiC matrix, leading to a sudden increase in local temperature and thermal stress in the gas-cooled microreactor core, which affects reactor safety.
Anhydrous ethanol is used as a solvent, and a uniform mixture of TRISO particles and SiC powder is formed by wet ball milling and stirring. Combined with split molding and SPS sintering technology, the uniform distribution of TRISO particles in each core layer is ensured.
It significantly improves the uniformity of TRISO particle distribution in the matrix, enhances the temperature distribution of dispersed fuel and reactor safety, simplifies the preparation process, and improves the precision of pellet quality control.
Smart Images

Figure CN121354992B_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of nuclear fuel preparation technology, and in particular relates to a method for combining the molding of coated particulate dispersed fuel agglomerates with separate forming. Background Technology
[0002] The uniformity of TRISO fuel particle distribution in the matrix has a significant impact on the in-core heat distribution of dispersed fuel for gas-cooled microreactors. The agglomeration of fuel particles causes a sudden increase in local temperature of the fuel pellets, an increase in internal temperature gradient and thermal stress. When a certain limit is exceeded, it will lead to pellet cracking, endangering the safe operation of the reactor.
[0003] The traditional preparation process for coated particulate fuel involves uniformly mixing TRISO particles with SiC matrix powder and then molding them. However, due to the differences in density and flowability between TRISO particles and SiC powder, as well as the effect of gravity, during the loading process into the mold, the denser TRISO particles or coated TRISO particles separate from the SiC matrix powder, ultimately leading to local aggregation of TRISO particles. Furthermore, as the amount of TRISO particles in the matrix increases, this non-uniformity becomes more severe. Since the volume ratio of TRISO particles in the core of a gas-cooled microreactor needs to be no less than 40%, the above molding method cannot meet the requirements of uniform fuel particle distribution in the fuel pellets of a gas-cooled microreactor.
[0004] In the prior art, Chinese patent CN202211523928.9 discloses a method for preparing FCM chip gel molding. This method involves injecting a SiC-based slurry into a mold, adding TRISO particles to the slurry, curing it in a water bath to obtain a chip preform, drying and debinding the chip to obtain a semi-finished preform, and then sintering the semi-finished preform to obtain the FCM chip. The slurry mixture uses alcohol and water as solvents, N-carboxymethylacrylamide as the monomer, ammonium polyacrylate as the dispersant, and methylenebisacrylamide as the crosslinking agent. The method includes the following steps: The mixed powder, mixed solvent, monomer, dispersant, and crosslinking agent are ball-milled and mixed. After ball milling, ammonium persulfate solution as an initiator and tetramethylethylenediamine as a catalyst are added to the mixed slurry, and vacuum degassing is performed to obtain SiC slurry; After defoaming, slowly pour the slurry into the mold along the mold wall, then add TRISO granules into the mold and shake well. Heat in a water bath for 10 minutes to solidify the semi-finished product; Place the mold in an oven to dry for 24 hours. After demolding the sample, continue drying for another 20 hours. After drying, the glue needs to be removed, and the glue removal time should be more than 24 hours.
[0005] The drawbacks of this method are: due to the addition of a large amount of organic matter, salts and other substances, a long drying and debinding time is required, resulting in low pellet preparation efficiency. At the same time, the relevant substances inevitably remain in the pellets, and the relevant impact of these substances on the reactor is difficult to assess.
[0006] Chinese patent CN201711391729.6 discloses a method for preparing a toroidal FCM chip, including the following steps: A layer of binder is coated on the surface of TRISO particles. The binder is glycerol diluted with anhydrous ethanol. TRISO particles coated with binder are mixed with silicon carbide powder to coat the surface of the TRISO particles with a layer of silicon carbide powder. The molding die is used to press the molding material; The core is densified and sintered by spark plasma.
[0007] The drawback of this method is that, during the preparation of FCM chips using this method, no matter how uniformly the TRISO particles and silicon carbide powder are mixed in the early stage, the TRISO particles may agglomerate during the molding process due to the differences in density and flowability between the two and the effect of gravity, which may affect the working performance of the FCM chips. Summary of the Invention
[0008] The purpose of this application is to provide a method for overcoming the limitations of existing technologies by combining a coating of dispersed fuel pellets with a modular molding process, thereby improving the uniformity of TRISO particle distribution within the overall fuel pellet and enhancing the temperature distribution of this type of dispersed fuel within the reactor and the safety of the reactor.
[0009] To achieve the above objectives, this application provides the following technical solution: A method for coating particulate dispersed fuel agglomerates using a combination of molding and split forming, comprising: Step 1: Mix SiC powder with sintering aids Al2O3 and Y2O3, then wet-mill with anhydrous ethanol, dry, and sieve to obtain uniform SiC matrix powder; Step 2: Coat the TRISO particles with SiC powder using anhydrous ethanol; Step 3: Mix TRISO particles with SiC powder to form granules, then pack them into a mold and stir twice to ensure uniformity; shape the pieces according to the sintering pressure distribution, adjust the pressure of each part to match the green body density, and ensure the joint strength and no gaps at the joints; Step 4: After assembling the formed multi-layer core and the fuel-free zone sleeve cover plate into a single unit, SPS sintering is performed.
[0010] According to one embodiment of this application, step 1 specifically includes: Step 1.1: Al2O3 powder and Y2O3 powder, which are sintering aids, are mixed with 40nm~500nm SiC powder by wet ball milling with anhydrous ethanol. Step 1.2: Add anhydrous ethanol at a rate of 50ml / 100g to 150ml / 100g of the mixed powder, mix evenly, and then dry in an oven. After drying, sieve through a 50-200 mesh sieve to obtain the mixed matrix powder.
[0011] According to one embodiment of this application, 20g to 40g of 40nm to 90nm SiC powder, 25g to 50g of 100nm to 500nm SiC powder, 2g to 4g of Al2O3 powder, and 1g to 3g of Y2O3 powder are weighed.
[0012] According to one embodiment of this application, in step 1.2, the mixing time is 4h~8h, and the drying time is 40℃~60℃ for 12h~24h.
[0013] According to one embodiment of this application, step 3 specifically includes: Step 3.1: Weigh SiC powder and TRISO particles one by one, add anhydrous ethanol and stir to form a granular mixture. After loading into the mold, mechanically stir a second time to ensure uniformity. Step 3.2: Set the molding pressure for different regions of the core according to the sintering pressure distribution, and ensure uniform distribution of fuel particles and seamless connection at the joints by segmented molding.
[0014] According to one embodiment of this application, 1.2g~2.5g of SiC mixed matrix powder and 1.4g~2.7g of coated TRISO particles are weighed, and 0.1g~0.25g of anhydrous ethanol is added dropwise.
[0015] According to one embodiment of this application, a stirring and mixing device is used to stir and mix the above-mentioned particles, powder and solvent. The stirring speed is 10 r / min to 30 r / min and the mixing time is 1 min to 2 min. Finally, the TRISO particles and silicon carbide powder are in a uniformly mixed granular state between dry powder and slurry. The above materials are then subjected to secondary mechanical stirring, with the stirring speed controlled at 10 r / min to 20 r / min and the mixing time at 1 min to 2 min.
[0016] According to one embodiment of this application, the core forming pressure is 7MPa~12MPa, which is more than 1 / 2 different from the final sintering pressure.
[0017] According to one embodiment of this application, the core pressure at the end is controlled at 7MPa~9MPa, and the core pressure in the middle is controlled at 10MPa~12MPa. The core is formed by splitting 4~8 pieces.
[0018] According to one embodiment of this application, the maximum SPS sintering temperature is 1700℃~2000℃, the maximum pressure is 30MPa~50MPa, the temperature is 1400℃~1600℃, and the holding time is 3min~8min every 100℃ interval, with the maximum holding time being 10min~30min.
[0019] Compared with the prior art, the method of coating particulate dispersed fuel agglomerates combined with split molding provided in this application has the following advantages: This application ensures the consistency of the total amount of TRISO particles within each layer of the separate pellet by controlling the split molding process. Anhydrous ethanol is added for stirring and mixing, resulting in a two-phase homogeneous "agglomerate" state where the TRISO particles and silicon carbide powder are mixed. Ultimately, the combination of these two processes improves the uniformity of TRISO particle distribution within the overall pellet, further enhancing the temperature distribution of this type of dispersed fuel within the reactor and improving reactor safety.
[0020] The solvent system used in this application is simple, completely removable, and has no additional impact on reactor performance. Existing preparation methods require the addition of significant amounts of organic matter, salts, and other substances, which inevitably remain in the fuel pellet, and their impact on the reactor is difficult to assess. In contrast, the method used in this application employs a simple anhydrous ethanol solvent. During the SPS sintering process, the core is directly sintered, and the anhydrous ethanol vapor is completely volatilized and removed by high-purity argon gas replacement.
[0021] This application greatly simplifies the preparation process and achieves high efficiency in core block preparation. Compared with existing preparation methods, this invention mainly controls the state of the mixture by optimizing the type and amount of solvent added, eliminating the need for lengthy drying and debinding processes. Furthermore, it does not adhere to the weighing fixtures and molds, making the overall operation simple, ensuring precise and reliable core block quality control, and facilitating large-scale application.
[0022] Furthermore, the uniformity of fuel particle distribution was significantly improved. By adding anhydrous ethanol and stirring, the TRISO particles in each individual pellet were mixed with the silicon carbide powder to form a two-phase homogeneous "agglomerate" state (see...). Figure 2 Furthermore, the split molding control ensures the consistency of the total amount of TRISO particles in each layer of split pellets. The combination of these two methods significantly improves the uniformity of TRISO particle distribution in the overall pellet, greatly improves the temperature distribution of this type of dispersed fuel in the reactor, enhances the safety of related reactors, and provides a very effective control approach for the uniform distribution of fuel phases in all similar dispersed fuels. Attached Figure Description
[0023] To more clearly illustrate the technical solution of this application, the accompanying drawings used in the technical description will be briefly introduced below.
[0024] Figure 1 A flowchart of the method for combining particle-state molding and split forming of coated particulate dispersed fuel agglomerates provided in this application; Figure 2 This is a flowchart of the silicon carbide matrix powder preparation process provided in this application; Figure 3 The flowchart for the preparation of the agglomerated molding combined with the split molding core provided in this application; Figure 4 A schematic diagram showing the distribution of the TRISO particles and silicon carbide powder agglomerates in the mold provided in this application; Figure 5 A simplified process flow diagram for preparing coated particulate dispersion fuel pellets provided in this application; Figure 6 CT microscopic images of TRISO particle distribution provided for this application (lower limit of parameters); Figure 7 CT microscopic images of TRISO particle distribution provided for this application (maximum parameters); Figure 8 A schematic diagram comparing the uniformity of TRISO particle distribution in core blocks prepared by combining traditional molding and granular molding with split molding, as provided in this application. Detailed Implementation
[0025] The following detailed description provides further details on specific implementation methods.
[0026] like Figures 1 to 5 As shown, this application provides a method for coating particulate dispersed fuel agglomerates using a combination of granular molding and split forming, comprising: Step 1: Preparation of SiC matrix powder. SiC powder is mixed with sintering aids Al2O3 and Y2O3, and then wet-milled with anhydrous ethanol, dried, and sieved to obtain uniform SiC matrix powder.
[0027] Step 2: TRISO particle coating. Anhydrous ethanol is used to coat the TRISO particles with SiC powder. During the coating process, the spindle speed is 100 r / min to 350 r / min, the spray pressure is 0.4 MPa to 0.6 MPa, the slurry pump speed is 80 r / min to 300 r / min, and the drying temperature is 40℃ to 60℃.
[0028] Step 3: Granular Formation Combined with Separate Molding. TRISO particles and SiC powder are mixed and stirred into granules before being molded. The mixture is stirred a second time to ensure uniformity. The pieces are then shaped according to the sintering pressure distribution, and the pressure in each part is adjusted to match the density of the green blank, ensuring strong and seamless joints.
[0029] Step 4: Integrated Assembly and SPS Sintering. The multi-layered core and the fuel-free zone sleeve cover plate, as described above, are integrated and then subjected to SPS sintering. The maximum SPS sintering temperature is 1700℃~2000℃, the maximum pressure is 30MPa~50MPa, and the temperature is maintained at 1400℃~1600℃ for 3min~8min at 100℃ intervals. The maximum holding time at the highest temperature is 10min~30min. The uniformity of TRISO particle distribution in the final prepared core is tested as shown in the figure. Figure 6 , Figure 7 As shown.
[0030] Step 1 specifically includes: Step 1.1: The sintering aids Al2O3 powder and Y2O3 powder are mixed with 40nm~500nm SiC powder by wet ball milling with anhydrous ethanol. Specifically, 20g~40g of 40nm~90nm SiC powder, 25g~50g of 100nm~500nm SiC powder, 2g~4g of Al2O3 powder, and 1g~3g of Y2O3 powder are weighed.
[0031] Step 1.2: Add anhydrous ethanol at a rate of 50ml / 100g~150ml / 100g of the mixed powder, mix for 4~8 hours, and after uniform mixing, place in an oven and dry at 40℃~60℃ for 12~24 hours. After drying, obtain the mixed matrix powder through a 50~200 mesh sieve.
[0032] Step 3 specifically includes: Step 3.1: Granular Formation Molding. Weigh SiC powder and TRISO particles piece by piece, add anhydrous ethanol and stir to form a granular mixture. After molding, perform secondary mechanical stirring to ensure homogeneity, providing a precise and reliable granular matrix for subsequent molding. Details are as follows: To ensure accurate and reliable uranium loading in each core, the materials in the core are weighed and stirred piece by piece. For example, 1.2g to 2.5g of SiC mixed matrix powder and 1.4g to 2.7g of coated TRISO particles are weighed, and 0.1g to 0.25g of anhydrous ethanol is added dropwise.
[0033] The above-mentioned particles, powder and solvent are stirred and mixed using a stirring and mixing device at a stirring speed of 10 r / min to 30 r / min and a mixing time of 1 min to 2 min. Finally, the TRISO particles and silicon carbide powder are in a uniform mixed granular state between dry powder and slurry. The above materials are directly loaded into a steel mold and then subjected to secondary mechanical stirring at a stirring speed of 10 r / min to 20 r / min and a mixing time of 1 min to 2 min.
[0034] Step 3.2: Segmented Molding. Based on the sintering pressure distribution, the molding pressure is set for different regions of the core, with lower pressure at the ends and higher pressure in the middle to match the green density and sintering pressure transmission characteristics. Segmented molding ensures uniform distribution of fuel particles and seamless connection at the joints.
[0035] Based on the final SPS sintering pressure distribution of the core, the forming pressure of each part of the core is selected for separate forming. For example, the core forming pressure is 7MPa~12MPa, which is more than 1 / 2 different from the final sintering pressure, to ensure good connection strength and no gaps at the final core assembly splicing.
[0036] Because the final SPS sintering pressure transmission has a situation where it is greater at both ends and smaller in the middle, the core pressure at the ends is controlled at 7MPa~9MPa, and the core pressure in the middle is controlled at 10MPa~12MPa, so as to ensure the matching of the green density of the split core and the final SPS sintering pressure distribution; according to the fuel particle uniformity requirements, the core is split into 4~8 pieces.
[0037] This application mixes TRISO particles with matrix powder by adding an appropriate amount of suitable solvent, so that the TRISO particles and silicon carbide powder are in a uniformly mixed "granular" state between dry powder and slurry. This is a polymer form formed by the bonding of particles of different phases together, which can effectively reduce the density and flowability differences between the two phases and ensure the uniformity of TRISO particles in each core layer.
[0038] This application adopts the concept of the finite element method, namely "breaking down the whole into parts and assembling the parts into a whole," to divide the complete core into separate parts for shaping. This ensures the consistency of the total amount of TRISO particles within each layer of the core. By precisely controlling the molding parameters of each single layer and performing multi-layer density-matching stacking and sintering, the uniformity of TRISO dispersed fuel distribution in the coated particles is improved, ultimately enhancing the temperature distribution of this type of dispersed fuel within the reactor and improving reactor safety. The process flow diagram for preparing the silicon carbide matrix powder is shown below. Figure 2 The preparation process of the granular molding combined with the split molding core is as follows: Figure 2 ; Figure 4 This is a schematic diagram showing the distribution of a mixture of TRISO particles and silicon carbide powder agglomerates in a mold. The diagram shows micro "agglomerate" unit 1, silicon carbide-coated TRISO particles 2, silicon carbide powder 3, and anhydrous ethanol 4. Figure 3 This is a complete process flow diagram for preparing coated particulate dispersion fuel pellets.
[0039] By adding an appropriate amount of anhydrous ethanol solvent, TRISO particles with significant differences in density and flowability are uniformly mixed with silicon carbide powder to form a moist "agglomerate" state, which significantly improves the uniformity of TRISO particle distribution in the matrix. Simultaneously, combined with pre-shaping of individual components and controllable matching of the green density of each layer, the assembled components are well-bonded after sintering, with no gaps on the cylindrical surfaces. Micro-CT and neutron radiography revealed that the prepared gas-cooled microreactor pellets exhibited high particle distribution uniformity and good integrity. The uniformity of particle number between different layers (1 - standard deviation / average) reached over 93.02%, meeting the TRISO particle distribution uniformity requirements for coated particulate fuel in gas-cooled microreactors. The fuel particle distribution uniformity test results of the pellets are shown in […]. Figure 6 , Figure 7 As shown.
[0040] Example 1 This embodiment implements the above method, and the specific operation steps are as follows: (1) The sintering aid Al2O3 powder and Y2O3 powder were mixed with 40nm and 100nm SiC powder by wet ball milling with anhydrous ethanol. Among them, 20g of 40nm SiC powder, 25g of 100nm SiC powder, 2g of Al2O3 powder and 1g of Y2O3 powder were weighed.
[0041] (2) Add anhydrous ethanol to the powder in step (1). The amount of anhydrous ethanol added is 50 ml / 100 g of mixed powder. The mixing time is 4 hours. After uniform mixing, put it into an oven and dry at 40°C for 12 hours. After drying, sieve through a 50-mesh sieve to obtain the mixed matrix powder.
[0042] (3) Use a garmenting machine to coat the surface of TRISO particles with anhydrous ethanol to make them wet, and then coat the powder from step (2) onto the surface of TRISO particles. During the garmenting process, the spindle speed is 100 r / min, the spray pressure is 0.4 MPa, the slurry pump speed is 80 r / min, and the drying temperature is 40℃.
[0043] (4) In order to ensure the accuracy and reliability of the uranium loading of a single core, the core material is weighed and stirred piece by piece. In this embodiment, 2.5g of the powder prepared in step (2) and 2.7g of the coated TRISO particles prepared in step (3) are weighed and 0.2g of anhydrous ethanol is added.
[0044] (5) The mixture in step (4) is stirred using a mixing device. The stirring speed is 10 r / min and the mixing time is 1 min. Finally, the TRISO particles and silicon carbide powder are in a uniformly mixed granular state between dry powder and slurry. The above materials are directly loaded into the steel mold and then subjected to secondary mechanical stirring. The stirring speed is controlled at 10 r / min and the mixing time is 1 min.
[0045] (6) The core is divided into 4 pieces for split molding. The pressure of the two core pieces at both ends is controlled at 7MPa, and the pressure of the two core pieces in the middle is controlled at 10MPa, so as to ensure the matching of the green density of the split molding core with the final SPS sintering pressure distribution, and to prevent the particles at both ends from gathering towards the center and becoming disordered again.
[0046] (7) After the multi-layer core and the fuel-free zone sleeve cover plate formed in step (6) are integrated and assembled, SPS sintering is carried out. The maximum SPS sintering temperature is 1700℃, the maximum pressure is 30MPa, the temperature is 1400℃~1600℃ for 3 minutes every 100℃ interval, and the maximum temperature holding time is 10 minutes. The uniformity of fuel particle distribution in the final prepared core is shown in the figure. Figure 6 .
[0047] Example 2 This embodiment implements the above method, and the specific operation steps are as follows: (1) The sintering aid Al2O3 powder and Y2O3 powder were mixed with 200nm and 400nm SiC powder by wet ball milling with anhydrous ethanol. Among them, 30g of 50nm SiC powder, 35g of 400nm SiC powder, 3g of Al2O3 powder and 2g of Y2O3 powder were weighed.
[0048] (2) Add anhydrous ethanol to the powder in step (1). The amount of anhydrous ethanol added is 150 ml / 100 g of mixed powder. The mixing time is 8 hours. After uniform mixing, put it into an oven and dry at 50°C for 18 hours. After drying, sieve through 100 mesh to obtain mixed matrix powder.
[0049] (3) Use a garmenting machine to coat the surface of TRISO particles with anhydrous ethanol to make them wet, and then coat the powder from step (2) onto the surface of TRISO particles. The spindle speed during the garmenting process is 200 r / min, the spray pressure is 0.5 MPa, the pump speed is 200 r / min, and the drying temperature is 50℃.
[0050] (4) In order to ensure the accuracy and reliability of the uranium loading of a single core, the core material is weighed and stirred piece by piece. In this embodiment, 1.7g of the powder prepared in step (2) and 1.8g of the coated TRISO particles prepared in step (3) are weighed and 0.2g of anhydrous ethanol is added.
[0051] (5) The mixture in step (4) is stirred using a mixing device. The stirring speed is 20 r / min and the mixing time is 1.5 min. Finally, the TRISO particles and silicon carbide powder are in a uniformly mixed granular state between dry powder and slurry. The above materials are directly loaded into the steel mold and then subjected to secondary mechanical stirring. The stirring speed is controlled at 15 r / min and the mixing time is 1.5 min.
[0052] (6) The core is divided into 6 pieces for split molding. The pressure of the 4 core pieces at both ends is controlled at 8MPa, and the pressure of the 2 core pieces in the middle is controlled at 11MPa, so as to ensure the matching of the green density of the split molding core with the final SPS sintering pressure distribution, and to prevent the particles at both ends from gathering towards the center and becoming disordered again.
[0053] (7) After the multi-layer core and the fuelless area sleeve cover plate formed in step (6) are integrated and assembled, SPS sintering is carried out. The maximum temperature of SPS sintering is 1850℃, the maximum pressure is 50MPa, the temperature is 1400℃~1600℃ for 8 minutes every 100℃ interval, and the maximum temperature holding time is 20 minutes.
[0054] Example 3 (1) The sintering aids Al2O3 powder and Y2O3 powder were mixed with 100nm and 500nm SiC powder by wet ball milling with anhydrous ethanol. Among them, 40g of 90nm SiC powder, 50g of 500nm SiC powder, 4g of Al2O3 powder and 3g of Y2O3 powder were weighed.
[0055] (2) Add anhydrous ethanol to the powder in step (1). The amount of anhydrous ethanol added is 150 ml / 100 g of mixed powder. The mixing time is 8 hours. After uniform mixing, put it into an oven and dry at 60°C for 24 hours. After drying, sieve through 200 mesh to obtain mixed matrix powder.
[0056] (3) Use a garmenting machine to coat the surface of TRISO particles with anhydrous ethanol to make them wet, and then coat the powder from step (2) onto the surface of TRISO particles. During the garmenting process, the spindle speed is 350 r / min, the spray pressure is 0.6 MPa, the pump speed is 300 r / min, and the drying temperature is 60℃.
[0057] (4) In order to ensure the accuracy and reliability of the uranium loading of a single core, the core material is weighed and stirred piece by piece. In this embodiment, 1.2g of the powder prepared in step (2) and 1.4g of the coated TRISO particles prepared in step (3) are weighed and 0.2g of anhydrous ethanol is added.
[0058] (5) The mixture in step (4) is stirred using a mixing device at a speed of 30 r / min and a mixing time of 2 min. The TRISO particles and silicon carbide powder will eventually be in a uniformly mixed granular state between dry powder and slurry. The above materials are directly loaded into the steel mold and then subjected to secondary mechanical stirring at a speed of 20 r / min and a mixing time of 2 min.
[0059] (6) The core is divided into 8 pieces for split molding. The pressure of the 3 core pieces at both ends is controlled at 9MPa, and the pressure of the 2 core pieces in the middle is controlled at 12MPa, so as to ensure the matching of the green density of the split molding core with the final SPS sintering pressure distribution, and to prevent the particles at both ends from gathering towards the center and becoming disordered again.
[0060] (7) After the multi-layer core and the fuelless zone sleeve cover plate formed in step (6) are integrated and assembled, SPS sintering is carried out. The maximum SPS sintering temperature is 2000℃, the maximum pressure is 50MPa, the temperature is 1400℃~1600℃ for 8 minutes every 100℃ interval, and the maximum temperature holding time is 30 minutes. The uniformity of TRISO particle distribution in the final prepared core block is shown in the figure. Figure 7 .
[0061] Figure 6 and Figure 7 The micro-CT results show the distribution of TRISO particles in gas-cooled microreactor pellets prepared using a combination of granular molding and split molding. The micro-CT scan was performed in 24 layers. The uniformity of particle number between different layers in pellets prepared with the lower parameter limit (1 - standard deviation / average) reached 94.95%; the uniformity of particle number between different layers in pellets prepared with the upper parameter limit (1 - standard deviation / average) reached 93.05%; while the uniformity of particle number between different layers in pellets prepared using the traditional method (1 - standard deviation / average) was only 46.51%. This demonstrates that the TRISO particle distribution uniformity of pellets prepared using a combination of granular molding and split molding significantly increases compared to the traditional molding method, and this uniformity fully meets the TRISO particle distribution uniformity requirements for this type of fuel in gas-cooled microreactors. Figure 8 A comparison of the uniformity of TRISO particle distribution in core blocks prepared by combining traditional molding with granular molding.
[0062] Therefore, this application provides a process and mixing parameters for directly molding a "granular" mixture. By adding as few additives as possible, TRISO particles and silicon carbide powder are in a uniformly mixed "granular" state, which is between dry powder and slurry. Micro-CT detection revealed that the uniformity of TRISO particle distribution in the matrix under this state is significantly improved compared to the dry mixing method of matrix powder and TRISO particles. Directly molding this uniform mixture and determining the relative distribution position of the particles in the mold lays a solid foundation for the uniform distribution of TRISO particles in the matrix.
[0063] This application provides a split-forming process and density matching parameters for each core layer. By drawing on the finite element method—"breaking down the whole into parts and then integrating them"—the complete core is split and shaped. Based on the distribution of sintering pressure, the green density of each core layer is controlled and matched by precisely controlling the single-layer split-forming parameters. This ensures the consistency of TRISO particle movement during pressing, avoiding a situation where TRISO particles are uniformly distributed during preforming but become disordered after spark plasma (SPS) sintering due to pressure conduction issues at different locations, causing particles at both ends to aggregate towards the center. Simultaneously, the pre-formed green density of the core is controlled to be significantly lower than the density after sintering densification. Finally, through multi-layer stacking and assembly with spark plasma sintering, the seams between different core layers are eliminated, resulting in a smooth, complete, and seamless cylindrical surface.
[0064] This application uses anhydrous ethanol for coating TRISO particles and wet mixing TRISO particles with the matrix silicon carbide powder to form agglomerated particles. The system is simple, and the anhydrous ethanol can fully volatilize during the sintering process, avoiding the introduction of other elements into the fuel pellets and ensuring the safe and stable operation of the reactor.
[0065] The above description is only a specific embodiment of this application, but the protection scope of this application is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this application should be included within the protection scope of this application.
Claims
1. A method for combining encapsulated particulate dispersed fuel agglomerates with split molding, characterized in that, include: Step 1: Mix SiC powder with sintering aids Al2O3 and Y2O3, then wet-mill with anhydrous ethanol, dry, and sieve to obtain uniform SiC matrix powder; Step 2: Coat the TRISO particles with SiC powder using anhydrous ethanol to obtain coated TRISO particles; Step 3: After mixing and stirring the coated TRISO granules with SiC powder to form granules, the mixture is placed into a mold and stirred a second time to ensure uniformity. The mixture is then sintered and formed into sheets according to the sintering pressure distribution, adjusting the pressure at each part to match the green body density, ensuring strong and seamless joints. Step 3 specifically includes: Step 3.1: Weigh SiC powder and coated TRISO granules piece by piece, add anhydrous ethanol and stir to form a uniform granular mixture between dry powder and slurry. After molding, mechanically stir a second time to ensure uniformity; Specifically, weigh 1.2g~2.5g of SiC mixed matrix powder and 1.4g~2.7g of coated TRISO granules, and add 0.1g~0.25g of anhydrous ethanol dropwise. Step 3.2: Set the forming pressure for the core in different regions according to the sintering pressure distribution. Ensure uniform distribution of fuel particles and seamless connection at the splicing points by forming in sections. The core forming pressure is 7MPa~12MPa, with the core pressure at the ends controlled at 7MPa~9MPa and the core pressure in the middle controlled at 10MPa~12MPa. Step 4: After the formed multi-layer core and the fuel-free zone sleeve cover plate are assembled into one unit, SPS sintering is carried out. The maximum SPS sintering temperature is 1700℃~2000℃, the maximum pressure is 30MPa~50MPa, the temperature is 1400℃~1600℃, and the holding time is 3min~8min every 100℃ interval. The maximum holding time is 10min~30min.
2. The method for coating particulate dispersed fuel agglomerates and combining granular molding with split forming according to claim 1, characterized in that, Step 1 specifically includes: Step 1.1: Al2O3 powder and Y2O3 powder, which are sintering aids, are mixed with 40nm~500nm SiC powder by wet ball milling with anhydrous ethanol; Step 1.2: Add anhydrous ethanol at a rate of 50ml / 100g to 150ml / 100g of the mixed powder, mix evenly, and then dry in an oven. After drying, sieve through a 50-200 mesh sieve to obtain the mixed matrix powder.
3. The method for coating particulate dispersed fuel agglomerates and combining granular molding with split forming according to claim 2, characterized in that, In step 1.1, weigh out 20g~40g of 40nm~90nm SiC powder, 25g~50g of 100nm~500nm SiC powder, 2g~4g of Al2O3 powder, and 1g~3g of Y2O3 powder.
4. The method for coating particulate dispersed fuel agglomerates and combining granular molding with split forming according to claim 2, characterized in that, In step 1.2, the mixing time is 4h~8h, and the drying time is 40℃~60℃ for 12h~24h.
5. The method for coating particulate dispersed fuel agglomerates and combining granular molding with split forming according to claim 1, characterized in that, In step 3.1, a mixing device is used to mix the coated TRISO particles, SiC powder, and anhydrous ethanol. The mixing speed is 10 r / min to 30 r / min, and the mixing time is 1 min to 2 min. The final result is that the coated TRISO particles and silicon carbide powder are in a uniformly mixed granular state between dry powder and slurry. The above materials are then subjected to secondary mechanical stirring, with the stirring speed controlled at 10 r / min to 20 r / min and the mixing time at 1 min to 2 min.
6. The method for coating particulate dispersed fuel agglomerates and combining granular molding with split forming according to claim 1, characterized in that, In step 3.2, the core is formed by splitting it into 4 to 8 pieces.
Citation Information
Patent Citations
Method for preparing annular FCM pellet
CN108249926A
Gel injection molding preparation method of FCM fuel pellet
CN115862913A
SPS (spark plasma sintering) silicon-carbide-particle-reinforced aluminum-based composite and preparing method thereof
CN105154705A
Rapid sintering method of silicon carbide matrix dispersion pellet
CN116417169A