A high-strength polypropylene staple fiber for cool fabric and its preparation method

By chemically integrating weather-resistant flame retardants and nucleating agents into polypropylene staple fibers, high-strength, long-lasting weather-resistant and flame-retardant polypropylene staple fibers are prepared, solving the problem of insufficient weather resistance and flame retardancy of polypropylene staple fibers and achieving the integration of high strength and long-lasting properties.

CN121473015BActive Publication Date: 2026-11-17HUBEI BOTAO SYNTHETIC FIBER CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202511634524.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-11-10
Publication Date
2026-11-17
Estimated Expiration
2045-11-10

Smart Images

  • Figure CN121473015B_ABST
    Figure CN121473015B_ABST
Patent Text Reader

Abstract

This invention discloses a high-strength polypropylene staple fiber for cool fabrics and its preparation method, relating to the technical field of polymer rayon and similar materials. The high-strength polypropylene staple fiber for cool fabrics is prepared from raw materials comprising the following parts by weight: 100 parts polypropylene resin, 0.1-1 parts nucleating agent, 0.2-0.8 parts inorganic filler, 0.5-2 parts processing aid, 3-6 parts plasticizer, 1-5 parts lubricant, and 0.5-2 parts weather-resistant flame retardant. Compared to the problems of aging and rapid performance degradation of polypropylene staple fibers in complex environments in the prior art, the polypropylene staple fiber prepared by this invention has significantly improved weather resistance and stability, and the performance decline due to aging after long-term use is significantly slowed down.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer rayon and similar technologies, specifically to a high-strength polypropylene staple fiber for cool fabrics and its preparation method. Background Technology

[0002] Polypropylene staple fiber, with its advantages of light weight, high tensile strength, good chemical stability, and controllable cost, has become one of the core raw materials for the preparation of PVC-U fabrics, and is widely used in outdoor shading fabrics, indoor decorative fabrics, industrial filter fabrics, and vehicle interior fabrics. However, as the application environment of PVC-U fabrics becomes increasingly complex, the shortcomings of existing polypropylene staple fibers in terms of weather resistance and long-term flame retardancy are becoming increasingly prominent, becoming a key bottleneck restricting their performance upgrade.

[0003] In terms of weather resistance, polypropylene molecular chains do not contain anti-aging functional groups. Under outdoor conditions of ultraviolet radiation, high temperature and humidity, or alternating hot and cold environments, they are prone to thermo-oxidative aging and photo-oxidative degradation, leading to fiber molecular chain breakage and decreased crystallinity. This manifests as problems such as yellowing of the fabric, fiber embrittlement, and decreased tear strength during use. For example, after 1-2 years of natural exposure, outdoor sunshade fabrics often experience a loss of more than 30% in tensile strength, and the fabric surface is easily damaged, rendering it unable to continue providing protection. Even decorative fabrics used indoors are prone to fiber loosening and fabric deformation due to insufficient weather resistance when exposed to long-term air conditioning cycles.

[0004] In terms of flame retardant performance, existing polypropylene staple fibers for filter cloths mostly rely on traditional additive flame retardants. Although they can temporarily meet the basic flame retardant standards, they have significant long-term defects: these flame retardants have poor compatibility with the polypropylene matrix and are prone to migrating and precipitating from the fiber interior with changes in temperature and humidity during long-term use, leading to a gradual decline in flame retardant effect. For example, after six months of continuous use, the limiting oxygen index of industrial filter cloths often decreases, failing to meet the requirements for continuous flame retardancy. At the same time, some flame retardants can also have antagonistic effects with weather-resistant additives. Adding them not only fails to synergistically improve performance but may also accelerate fiber aging and further deteriorate weather resistance stability.

[0005] Currently, as Cool Fabrics develops towards high-end and multi-functional applications, such as outdoor durable decoration and rail transit interiors, higher requirements are placed on the weather resistance and long-term flame retardancy of materials. Existing polypropylene staple fibers can no longer meet these needs. Therefore, developing polypropylene staple fibers for Cool Fabrics that combine excellent weather resistance and long-term flame retardancy has become a technical challenge that urgently needs to be overcome in this field. Summary of the Invention

[0006] The purpose of this invention is to address the problems in the existing technology of polypropylene staple fiber for cool fabrics, such as poor weather resistance, insufficient long-term flame retardancy, poor compatibility and easy migration of traditional flame retardants with polypropylene matrix, and potential antagonism with weather-resistant additives. The invention provides a high-strength polypropylene staple fiber for cool fabrics and its preparation method, which has excellent weather resistance, long-term flame retardancy and high strength, can be adapted to the use of cool fabrics in multiple scenarios, and meets the high-end requirements of cool fabrics.

[0007] To achieve the above objectives, the technical solution adopted by the present invention is: a high-strength polypropylene short fiber for cool fabric, prepared from raw materials comprising the following parts by weight: 100 parts polypropylene resin, 0.1-1 parts nucleating agent, 0.2-0.8 parts inorganic filler, 0.5-2 parts processing aid, 3-6 parts plasticizer, 1-5 parts lubricant, and 0.5-2 parts weather-resistant flame retardant; The weather-resistant flame retardant is a compound represented by Formula 1: The structure of Equation 1 is as follows: ; In Formula 1, R1 is a substituent, and R1 is selected from any one of hydrogen, methyl, ethyl, methoxy, and cyano.

[0008] Furthermore, the nucleating agent is selected from any one of: dibenzyl sorbitol, p-methyl dibenzyl sorbitol, 2,4-di(3,4-dimethyl)benzyl sorbitol, and N,N'-dicyclohexyl-2,6-naphthalenediamide.

[0009] Furthermore, the inorganic filler is selected from silicon dioxide.

[0010] Furthermore, the processing aid is selected from any one of calcium stearate, zinc stearate, ethylene bis-stearamide, and stearamide.

[0011] Furthermore, the plasticizer is selected from any one of phthalates, epoxidized soybean oil, citrate, and phosphate esters.

[0012] Furthermore, the lubricant is selected from either ethylene wax or polyethylene wax.

[0013] Furthermore, the weather-resistant flame retardant is selected from any one of the compounds shown in the following structures: ; ; .

[0014] Furthermore, the weather-resistant flame retardant has the dual functions of weather resistance and flame retardancy.

[0015] Furthermore, the high-strength polypropylene staple fiber used in the fabric can also be enriched with polyimide.

[0016] A method for preparing high-strength polypropylene staple fiber for cool fabrics includes the following steps: S1. Mixing: Add the polypropylene resin, nucleating agent, inorganic filler, processing aid, plasticizer, lubricant and weather-resistant flame retardant to a high-speed mixer and mix for 15-40 minutes to obtain a mixture; S2. Melt extrusion granulation: The mixture is melt-blended, extruded, cooled, and pelletized using a twin-screw extruder to obtain polypropylene masterbatch; S3. Spinning: The polypropylene masterbatch is fed to a spinning machine for melt spinning, and the primary fibers are formed by metering and extrusion through a spinneret. S4. Stretching and setting: The nascent fiber is subjected to multi-stage thermal stretching and relaxation heat setting to obtain the high-strength polypropylene short fiber for the fabric.

[0017] Furthermore, the processing temperature of the twin-screw extruder is 180-250℃.

[0018] Furthermore, the spinning temperature is 230-265℃.

[0019] Furthermore, S1 is performed under a nitrogen atmosphere.

[0020] Furthermore, the multi-stage thermal stretching described in S4 specifically refers to: First stage of stretching: carried out in a warm water bath at 40-60℃, with a stretching ratio of 2.5-3.5 times; Second-stage drawing: carried out in hot air or steam at 95-105℃, with a drawing ratio of 1.5-2.0 times; The total draw ratio should be controlled between 4.0 and 6.0.

[0021] Furthermore, the relaxation heat setting temperature in S4 is 110-130℃, and the time is 5-15 minutes.

[0022] The core design of the weather-resistant and flame-retardant molecule described in this invention lies in integrating weather resistance and flame retardancy into a single molecule through chemical bonds. Its synergistic mechanism is as follows: the phenolic hydroxyl group (-OH), acting as the primary antioxidant, efficiently captures and terminates the alkyl peroxide radical (ROO·) generated by thermo-oxidative aging by providing hydrogen atoms, converting it into a stable hydroperoxide (ROOH). Meanwhile, the aromatic oxygen radicals generated by the hydroxyl group itself are highly stable due to the electron delocalization effect of the adjacent large conjugated structure, thereby effectively interrupting the polymer's oxidative chain reaction and endowing the material with excellent resistance to thermo-oxidative aging. This large conjugated structure also acts as a UV... The ultraviolet-absorbing groups absorb ultraviolet light energy and convert it into harmless heat energy, providing anti-photoaging protection for polypropylene fibers and significantly enhancing the thermal stability and structural rigidity of the entire molecule, reducing volatilization and migration, and ensuring long-lasting efficacy. The diethyl phosphonate group, acting as the flame-retardant functional center, decomposes upon heating to produce highly dehydrating phosphorus-containing species, catalyzing the dehydration and carbonization of polypropylene in the condensed phase to form a dense char layer with heat insulation and oxygen barrier properties. This physically slows down the combustion process and partially interrupts the combustion chain reaction by generating PO· free radicals to capture highly reactive H· and OH· free radicals in the gas phase. This intramolecular integrated design fundamentally avoids the problems of poor compatibility, mutual antagonism, and easy migration and precipitation that easily occur with physical blending additives. During processing and long-term use, the weather-resistant component continuously protects the integrity of the polypropylene molecular chain, laying the foundation for the formation of a solid char layer in the early stages of a fire, while the flame-retardant component provides immediate fire protection. Ultimately, this synergistic approach achieves a balance between high strength, long-lasting weather resistance, and durable flame retardancy in polypropylene staple fibers.

[0023] This invention successfully solves three major technical challenges of polypropylene fiber—poor weather resistance, difficulty in maintaining flame retardancy, and the tendency of traditional flame retardants to migrate and antagonize weather-resistant additives—through a systematic approach of "core function integration and multi-component synergy." Its core innovation lies in the use of a specially designed weather-resistant flame retardant. This agent is not a physical blend, but rather integrates a free radical-capturing phenolic hydroxyl / large conjugated structure (weather-resistant function) with a phosphonate group that promotes char formation (flame-retardant function) into a single molecule via chemical bonds. This not only fundamentally inhibits component migration and precipitation due to its large molecular weight and excellent compatibility, ensuring long-lasting flame retardancy and weather resistance, but also avoids the functional antagonism common in physical blends. The nucleating agent enhances fiber strength by refining grain size, while the inorganic filler acts as a reinforcing agent and works synergistically with the weather-resistant flame retardant to form a dense carbon layer in the condensed phase, further enhancing flame retardancy and mechanical properties. Processing aids / lubricants and plasticizers ensure processing fluidity and fiber flexibility under high-filler systems. In addition, on a polypropylene resin matrix, nitrogen-protected mixing, precisely controlled extrusion spinning temperature, and multi-stage hot stretching and relaxation heat setting processes jointly ensure the structural integrity of functional components and their uniform dispersion and directional crystallization in the fiber, ultimately producing high-end polypropylene staple fibers with high strength, excellent long-lasting weather resistance, and durable flame retardancy.

[0024] Compared with the prior art, the beneficial effects of the present invention are: 1. Superior weather resistance: Compared with the existing technology, polypropylene staple fiber is prone to aging and rapid performance degradation in complex environments. The polypropylene staple fiber prepared by this invention has significantly improved weather resistance and the performance decline caused by aging after long-term use is significantly slowed down.

[0025] 2. Better flame retardancy and long-lasting effect: Overcoming the shortcomings of traditional flame retardants in the prior art, such as easy migration, flame retardant effect decay with use time, and possible antagonistic effect with weathering additives, the flame retardant effect of polypropylene short fiber of the present invention can be maintained for a long time, and there will be no mutual interference between flame retardancy and weathering performance.

[0026] 3. Enhanced strength performance: This invention avoids the problem of negative impact on fiber strength caused by the addition of multiple additives in existing technologies. While achieving excellent weather resistance and long-lasting flame retardancy, it can stably maintain or even improve the strength performance of polypropylene staple fibers, meeting the high-strength requirements of Cool Fabric. Attached Figure Description

[0027] Figure 1 This is the NMR spectrum of weather-resistant flame retardant 1 of the present invention.

[0028] Figure 2 This is the NMR spectrum of weather-resistant flame retardant 4 of the present invention. Detailed Implementation

[0029] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are merely some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0030] Preparation Example 1 Preparation of weather-resistant flame retardant 1: ; Under nitrogen protection, 10 g of compound 1, 16.81 g of compound 2, 9.85 g of sodium tert-butoxide, and 140 ml of toluene were added sequentially to the reaction system. After stirring until homogeneous, 2.35 g of tris(dibenzylacetone)dipalladium and 0.51 g of tritert-butylphosphine were added, stirred until homogeneous, and refluxed at 110 °C for 10 h. After the reaction was completed, the mixture was filtered hot through silica gel, dried over anhydrous magnesium sulfate, and the solvent was removed using a rotary evaporator. The mixture was then purified by silica gel column chromatography using a mixture of petroleum ether and ethyl acetate as eluent to obtain 15.68 g of compound 3. The mass spectra of compound 3 were M / Z MS+1: 388.

[0031] ; Under nitrogen protection, 15.68 g of compound 3, 9.07 g of compound 4, 11.18 g of anhydrous potassium carbonate, and 200 ml of toluene were added sequentially to the reaction system. After thorough stirring, the mixture was purged twice with nitrogen. Under nitrogen protection, 2.34 g of tetra(triphenylphosphine)palladium was added to the system, and the nitrogen was purged twice. The mixture was heated to 105 °C and refluxed for 10 hours. After the reaction was completed, the mixture was filtered, the solvent was removed using a rotary evaporator, and the mixture was purified by silica gel column chromatography using a mixture of petroleum ether and ethyl acetate as eluent to obtain 16.03 g of weather-resistant flame retardant 1. The mass spectra of weather-resistant flame retardant 1 were M / Z MS+1: 494, and the NMR results are shown below. Figure 1 .

[0032] Preparation Examples 2-5 In Preparation Examples 2-5, weather-resistant flame retardant 2-weather-resistant flame retardant 5 were prepared sequentially, following the preparation method of Preparation Example 1, except that compound 4 was replaced, and the rest remained the same as in Preparation Example 1. See Table 1 for details.

[0033] Table 1.

[0034] Example 1

[0035] Preparation of a high-strength polypropylene staple fiber for cool fabric: 1. Raw material components: Polypropylene resin: 100 parts, purchased from: China Petroleum & Chemical Corporation, relative density 0.90-0.91; Nucleating agent: 0.5 parts, selected from: dibenzylsorbitol, purchased from: Shanghai Maclean Biochemical Technology Co., Ltd.; Inorganic filler: 0.5 parts, selected from: silica, purchased from: Jiangsu Puleisi Biotechnology Co., Ltd.; Processing aid: 1 part, selected from: calcium stearate, purchased from: Wuhan Jixin Yibang Biotechnology Co., Ltd.; Plasticizer: 4.5 parts, selected from phthalates, purchased from Shaanxi Didu New Materials Co., Ltd.; Lubricant: 3 parts, selected from: polyethylene wax, purchased from: Qingdao Bonni Chemical Co., Ltd., product model: Bouni ® 501; Weather-resistant flame retardant: 1 part, selected from: Weather-resistant flame retardant 1.

[0036] 2. Preparation method: S1. Mixing: Add the above polypropylene resin, nucleating agent, inorganic filler, processing aid, plasticizer, lubricant and weather-resistant flame retardant to a high-speed mixer and mix for 30 minutes under nitrogen atmosphere protection at a mixing temperature of 45°C to obtain the mixture; S2. Melt Extrusion Granulation: The mixture is fed into the feed hopper of a twin-screw extruder, and the extruder is started for melt blending. The temperatures of each section of the twin-screw extruder are set as follows: feeding section 190℃, compression section 220℃, homogenization section 240℃, and die head temperature 245℃. The screw speed is controlled at 180 r / min. After the mixture is melt-blended in the extruder for 15 minutes, it is extruded from the die head to form a continuous strip-shaped melt. The strip-shaped melt is immediately cooled to room temperature in a room temperature water bath (water temperature 25℃), and then conveyed to a pelletizer to be cut into particles with a particle size of 2-3 mm and a length of 2-2.5 mm, thus obtaining polypropylene masterbatch. S3. Spinning: The polypropylene masterbatch is first pretreated in a hot air dryer at 90°C for 3 hours to remove adsorbed moisture (moisture content ≤0.1%). The dried polypropylene masterbatch is then conveyed to the spinning machine hopper. The temperatures of each section of the spinning machine barrel are set according to process requirements: feeding section 235°C, melting section 250°C, metering section 260°C, and spinneret temperature 262°C. After the masterbatch melts in the barrel, the melt delivery rate is precisely controlled by a metering pump (speed 25 r / min). The melt is extruded through a spinneret (80 spinneret holes, 0.3 mm diameter) to form a continuous melt stream. The melt stream is immediately cooled by side blowing air (cooling air temperature 23°C, air speed 0.8 m / s) to solidify, and then wound up at a speed of 650 m / min to obtain nascent fibers. S4. Stretching and Setting: The nascent fibers undergo multi-stage hot stretching and relaxation heat setting, with the following specific steps: First-stage stretching: The nascent fibers are introduced into a 50℃ warm water bath and stretched at a speed of 120m / min under the action of a stretching machine, with the stretching ratio controlled at 3.0 times, to initially orient the fiber molecular chains; Second-stage stretching: The fibers after the first-stage stretching are sent into a hot air oven (temperature set at 100℃) and stretched again at a speed of 216m / min, with a stretching ratio of 1.8 times, and the total stretching ratio reaches 5.4 times, further improving the orientation and crystallinity of the fibers; Relaxation heat setting: The fibers that have completed multi-stage stretching are sent into a hot air setting machine and held at a temperature of 120℃ for 10 minutes, during which the fiber relaxation rate is controlled at 3%-5% to eliminate the internal stress generated during the stretching process; After setting, the fibers are naturally cooled to room temperature, and finally cut into short fibers to obtain the high-strength polypropylene short fiber for cool fabrics.

[0037] Examples 2-5 The preparation of a high-strength polypropylene staple fiber for cool fabric is carried out by referring to the preparation method of Example 1, except that weather-resistant flame retardant 1 is replaced with weather-resistant flame retardant 2-weather-resistant flame retardant 5 in sequence, and the rest is the same as in Example 1.

[0038] Comparative Example 1 The preparation of a high-strength polypropylene staple fiber for cool fabric is carried out according to the preparation method of Example 1, except that the weather-resistant flame retardant 1 is replaced with trioctyl phosphate, and the rest is the same as in Example 1.

[0039] Comparative Example 2 The preparation of a high-strength polypropylene staple fiber for cool fabric is carried out by referring to the preparation method of Example 1, except that the weather-resistant flame retardant 1 is replaced with antioxidant 1010, and the rest is the same as in Example 1.

[0040] Comparative Example 3 The preparation of a high-strength polypropylene staple fiber for cool fabric is carried out according to the preparation method of Example 1, except that the weather-resistant flame retardant 1 is replaced with 0.5 parts of trioctyl phosphate + 0.5 parts of antioxidant 1010, and the rest is the same as in Example 1.

[0041] Comparative Example 4 The preparation of a high-strength polypropylene staple fiber for cool fabric is carried out according to the preparation method of Example 1, except that the weather-resistant flame retardant 1 is replaced with 0.5 parts of diphenyl toluene phosphate + 0.5 parts of antioxidant 264, and the rest is the same as in Example 1.

[0042] Comparative Example 5 The preparation of a high-strength polypropylene staple fiber for cool fabric is carried out according to the preparation method of Example 1, except that weather-resistant flame retardant 1 is not added, and the rest is the same as in Example 1.

[0043] Comparative Example 6 The preparation of a high-strength polypropylene staple fiber for cool fabric is the same as in Example 1, except that the nucleating agent is not added.

[0044] Performance testing: Test sample: A high-strength polypropylene staple fiber for cool fabric prepared in the examples and comparative examples.

[0045] 1. Breaking strength: The breaking strength of the samples was tested according to the test method of GB / T 14344-2008 "Test method for tensile properties of chemical fiber short fiber". The data are shown in Table 2.

[0046] 2. Limiting Oxygen Index (LOI): The limiting oxygen index of the test samples was determined according to GB / T 2406.2-2009 "Determination of Combustion Behavior by Oxygen Index Method for Plastics - Part 2: Room Temperature Test". The data are shown in Table 2.

[0047] 3. Weather resistance test: The test samples are placed in a fluorescent ultraviolet aging test chamber (equipped with UVA-340 lamps, irradiation intensity 0.71W / m²). 2 • 340nm), aging cycle: 8h of light exposure (80℃) + 4h of condensation (10℃), condensation humidity: ≥95%RH. Total aging time: 3600h; after aging, the fracture strength and limiting oxygen index after aging were retested, and the fracture strength retention rate was calculated. The data are shown in Table 2.

[0048] Table 2.

[0049] Fracture strength (cN / dtex) Limiting Oxygen Index (LOI, %) Fracture strength retention rate (%) Limiting oxygen index (LOI, %) after aging Example 1 5.3 30 96 30 Example 2 5.2 29 95 28 Example 3 5.4 31 97 31 Example 4 5.3 30 96 28 Example 5 5.2 29 95 29 Comparative Example 1 4.5 26 60 22 Comparative Example 2 4.3 19 76 13 Comparative Example 3 4.4 25 70 21 Comparative Example 4 4.6 27 73 22 Comparative Example 5 4.2 18 56 10 Comparative Example 6 3.6 30 92 28 The polypropylene staple fibers prepared using weather-resistant flame retardants with different structures (weather-resistant flame retardants 1-5) showed stable overall performance in four core indicators: breaking strength, initial limiting oxygen index, retention rate of breaking strength after aging, and limiting oxygen index after aging, with no significant fluctuations. Compared with the comparative examples, the breaking strength of the examples was significantly better than that of the comparative examples using traditional flame retardants, single antioxidants, a combination of traditional flame retardants and antioxidants, and no weather-resistant flame retardants. Only the breaking strength of the comparative examples without nucleating agents was slightly close to that of the examples. The initial limiting oxygen index of the examples was higher than that of the comparative examples using single antioxidants and no weather-resistant flame retardants, and also better than that of the comparative examples using traditional flame retardants or their combination with antioxidants. The initial limiting oxygen index of the comparative examples without nucleating agents was comparable to that of the examples. The retention rate of breaking strength after aging of the examples was much higher than that of all the comparative examples. The limiting oxygen index of the examples after aging could basically maintain the initial level, while the limiting oxygen index of all the comparative examples decreased to varying degrees after aging, with the decrease being particularly significant in the comparative examples using single antioxidants and no weather-resistant flame retardants.

[0050] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A high-strength polypropylene staple fiber for cool fabrics, characterized in that, It is prepared from raw materials containing the following parts by weight: 100 parts polypropylene resin, 0.1-1 parts nucleating agent, 0.2-0.8 parts inorganic filler, 0.5-2 parts processing aid, 3-6 parts plasticizer, 1-5 parts lubricant, and 0.5-2 parts weather-resistant flame retardant; The weather-resistant flame retardant is a compound represented by Formula 1: The structure of Equation 1 is as follows: ; R1 is selected from any one of hydrogen, methyl, ethyl, methoxy, and cyano.

2. The high-strength polypropylene staple fiber for cool fabric as described in claim 1, characterized in that, The nucleating agent is selected from any one of the following: dibenzyl sorbitol, p-methyl dibenzyl sorbitol, 2,4-di(3,4-dimethyl)benzyl sorbitol, and N,N'-dicyclohexyl-2,6-naphthalenediamide.

3. The high-strength polypropylene staple fiber for cool fabric as described in claim 1, characterized in that, The inorganic filler is selected from silicon dioxide.

4. The high-strength polypropylene staple fiber for cool fabric as described in claim 1, characterized in that, The processing aid is selected from any one of the following: calcium stearate, zinc stearate, ethylene bis-stearamide, and stearamide.

5. The high-strength polypropylene staple fiber for cool fabric as described in claim 1, characterized in that, The plasticizer is selected from any one of the following: phthalates, epoxidized soybean oil, citrate, and phosphate esters.

6. The high-strength polypropylene staple fiber for cool fabric according to claim 1, characterized in that, The lubricant is selected from either ethylene wax or polyethylene wax.

7. The high-strength polypropylene staple fiber for cool fabric according to claim 1, characterized in that, The weather-resistant flame retardant is selected from any one of the compounds shown in the following structures: ; ; 。 8. A method for preparing a high-strength polypropylene staple fiber for cool fabric according to any one of claims 1-7, characterized in that, Includes the following steps: S1. Mixing: Add the polypropylene resin, nucleating agent, inorganic filler, processing aid, plasticizer, lubricant and weather-resistant flame retardant to a high-speed mixer and mix for 15-40 minutes to obtain a mixture; S2. Melt extrusion granulation: The mixture is melt-blended, extruded, cooled, and pelletized using a twin-screw extruder to obtain polypropylene masterbatch; S3. Spinning: The polypropylene masterbatch is fed to a spinning machine for melt spinning, and the nascent fibers are formed by metering and extrusion through a spinneret. S4. Stretching and setting: The nascent fiber is subjected to multi-stage hot stretching and relaxation heat setting to obtain the high-strength polypropylene short fiber for the fabric. The processing temperature of the twin-screw extruder is 180-250℃; The spinning temperature is 230-265℃; S1 is performed under a nitrogen atmosphere.

9. The method for preparing high-strength polypropylene staple fiber for cool fabric according to claim 8, characterized in that, The multi-stage thermal stretching mentioned in S4 specifically refers to: First stage of stretching: carried out in a warm water bath at 40-60℃, with a stretching ratio of 2.5-3.5 times; Second-stage drawing: carried out in hot air or steam at 95-105℃, with a drawing ratio of 1.5-2.0 times; The total draw ratio should be controlled between 4.0 and 6.

0.

10. The method for preparing high-strength polypropylene staple fiber for cool fabric according to claim 8, characterized in that, The relaxation heat setting temperature in S4 is 110-130℃, and the time is 5-15 minutes.

Citation Information

Patent Citations

  • Flame-retardant master batch, preparation method of flame-retardant master batch and method for preparing flame-retardant fiber by using flame-retardant master batch

    CN102585451A

  • Antimony-free flame-retardant polypropylene composition and preparation method therefor

    WO2021164353A1