A single-crystal ternary cathode material, its preparation method and application

By doping molybdenum and barium into nickel-cobalt-manganese cathode materials, a cubic single-crystal ternary cathode material is formed, which solves the problems of grain boundary cracking and interface stability of traditional materials, and achieves battery performance with high capacity, high rate performance and good stability.

CN121641941BActive Publication Date: 2026-11-10YIBIN LIBODE NEW MATERIAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202511828964.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-12-05
Publication Date
2026-11-10
Estimated Expiration
2045-12-05

AI Technical Summary

Technical Problem

Traditional polycrystalline ternary cathode materials suffer from problems such as grain boundary cracking and pulverization during charge and discharge. Monocrystalline ternary materials face issues such as insufficient monocrystalline material, uneven particle size, and poor interface stability. In particular, the structure and thermal stability of high-nickel ternary materials decline, affecting the cycle life and safety performance of the battery.

Method used

By doping molybdenum and barium elements into nickel-cobalt-manganese cathode materials and controlling the single crystal morphology in a specific ratio, a cubic single-crystal ternary cathode material is formed. The grains are mainly based on the (104) crystal plane. Combined with oxygen atmosphere sintering process, the defects of Li/Ni mixing are controlled and Li+ transport is promoted.

Benefits of technology

It improves the capacity and rate performance of single-crystal ternary cathode materials, enhances Li+ transport performance and interface stability, and improves the energy density, cycle stability and safety of batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121641941B_ABST
    Figure CN121641941B_ABST
Patent Text Reader

Abstract

This invention discloses a single-crystal ternary cathode material, its preparation method, and its application, belonging to the field of battery material technology. The single-crystal ternary cathode material comprises LiNi... x Co y Mn z The cathode material of O2 and its doping elements; among which, 0.8
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery materials, and specifically, relates to a single-crystal ternary positive electrode material, the preparation method and application thereof. Background Art

[0002] Lithium-ion batteries are widely used in electric vehicles, portable electronic devices and other fields due to their advantages such as high energy density, long cycle life and environmental friendliness. With the rapid development of electric vehicles, the requirements for the energy density and cruising range of lithium-ion batteries are continuously increasing. Ternary positive electrode materials have become one of the mainstream positive electrode materials for lithium-ion batteries because of their high capacity, low cost and good rate performance. However, traditional polycrystalline ternary positive electrode materials have problems such as grain boundary cracking and pulverization during charge and discharge processes, which seriously affect the cycle stability and safety of batteries; in addition, single-crystal ternary materials also face many challenges, such as insufficient single-crystallization degree of the material, non-uniform particle size, poor interface stability, etc. Especially for high-nickel ternary materials, the increase in nickel content leads to the decrease of structural stability and thermal stability of the material, which further affects the cycle life and safety performance of batteries.

[0003] In view of this, the present invention is specially proposed. Summary of the Invention

[0004] The objective of the present invention is to provide a single-crystal ternary positive electrode material, the preparation method and application thereof, so as to solve or ameliorate the above technical problems.

[0005] The present invention can be implemented as follows: In a first aspect, the present invention provides a single-crystal ternary positive electrode material, the single-crystal ternary positive electrode material comprises a positive electrode material body and doping elements; wherein the molecular formula of the positive electrode material body is LiNi x Co y Mn z O2, 0.8<x<0.96, 0<y<0.1, z=1-x-y; the doping elements comprise molybdenum and barium, the doping amount of molybdenum is 2000ppm to 10000ppm, and the doping amount of barium is 1000ppm to 5000ppm.

[0006] In an optional embodiment, the doping amount of molybdenum is 3000ppm, and the doping amount of barium is 2000ppm.

[0007] In an optional embodiment, the single-crystal ternary positive electrode material has a cubic structure, and the crystal grains in the single-crystal ternary positive electrode material are dominated by the (104) crystal plane.

[0008] In a second aspect, the present invention provides a preparation method of the above single-crystal ternary positive electrode material, comprising the following steps: mixing a lithium source, a ternary positive electrode material precursor and a dopant, followed by sintering; wherein the molecular formula of the ternary positive electrode material precursor is Ni x Co y Mn z (OH)₂, 0.8<x<0.96, 0<y<0.1, z=1-x-y; the dopant includes a molybdenum source providing molybdenum element and a barium source providing barium element.

[0009] In an optional embodiment, in terms of molar amount, (Ni+Co+Mn):Li=1:(1.04~1.08).

[0010] In an optional embodiment, the lithium source includes lithium hydroxide; and / or, the molybdenum source includes molybdenum oxide; and / or, the barium source includes at least one of barium hydroxide, barium carbonate, barium chloride and barium nitrate.

[0011] In an optional embodiment, the sintering comprises: first treating at 450°C to 560°C for 2h to 4h, then heating up to 700°C to 800°C for 3h to 6h, then heating up to 880°C to 1000°C for 1h to 5h, and cooling down to 700°C to 800°C for further treatment for 2h to 5h.

[0012] In an optional embodiment, the heating rate during the sintering process is 2°C / min to 6°C / min.

[0013] In an optional embodiment, the sintering atmosphere is an oxygen atmosphere.

[0014] In a third aspect, the present invention further provides a battery, which contains the above single-crystal ternary positive electrode material.

[0015] The beneficial effects of the present invention include: According to the present invention, by specifically doping molybdenum element and barium element in a certain proportion in the nickel-cobalt-manganese positive electrode material to jointly regulate the single crystal morphology, the defect that high-concentration Mo 6+ doping significantly inhibits the growth of single crystal grains is effectively avoided. After Ba element doping, the surface energy of the (104) plane of the nickel-cobalt-manganese ternary positive electrode material is reduced to a greater extent, which is beneficial to promoting the formation of more (104) crystal planes that are favorable for Li + transport, and thus is beneficial to improving the capacity and rate performance of the positive electrode material.

[0016] The single-crystal ternary positive electrode material has a cubic structure, and the crystal grains are dominated by the (104) crystal plane; the single-crystal ternary positive electrode material has a low concentration of Li / Ni anti-site defects, the single crystals of the ternary positive electrode material grow uniformly, and have excellent Li +With its superior transmission performance, excellent interface and structural stability, batteries containing this single-crystal ternary cathode material can achieve higher rate performance and energy density, while also improving cycle stability and safety. Attached Figure Description

[0017] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0018] Figure 1 The NCM(104) atomic structure model is used. Figure 2 The image shows the SEM image of the Mo and Ba co-doped NCM material in Example 1. Figure 3 The image shows the XRD pattern of the Mo and Ba co-doped NCM material in Example 1. Figure 4 The image shows the SEM image of the Mo-doped NCM material in Comparative Example 2. Detailed Implementation

[0019] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0020] The following is a detailed description of the single-crystal ternary cathode material proposed in this invention, its preparation method, and its application.

[0021] The single-crystal ternary cathode material provided by this invention includes the cathode material body and doping elements.

[0022] The molecular formula of the cathode material is LiNi. x Co y Mn z O2, 0.8 <x<0.96,0<y<0.1,z=1-x-y。

[0023] Doping elements include molybdenum and barium.

[0024] It should be noted that the particle morphology of single-crystal ternary cathode materials can be controlled by molybdenum doping. However, introducing high concentrations of high-valence Mo... 6+High concentrations of molybdenum ions can lead to more Li / Ni mixing defects and make single-crystal particle growth difficult in single-crystal cathode materials. The inventors specifically combined molybdenum doping with barium doping to jointly control the single-crystal morphology, effectively avoiding the problems associated with high-concentration Molybdenum doping. 6+ Doping significantly inhibits single-crystal grain growth. The NCM(104) atomic structure model is as follows: Figure 1 As shown. The surface energy of the nickel-cobalt-manganese ternary cathode material (104) before and after doping was calculated using density functional theory (MatterCraft software), proving that barium is the optimal doping element for promoting the formation of the (104) active crystal facet. After Ba doping, the surface energy of the nickel-cobalt-manganese ternary cathode material (104) decreased more significantly, which is beneficial for promoting grain formation and more favorable for Li. + The (104) crystal plane of the transmission is beneficial to improving the capacity and rate performance of the cathode material.

[0025] In some alternative embodiments, the molybdenum doping amount is 2000ppm to 10000ppm, such as 2000ppm, 2500ppm, 3000ppm, 3500ppm, 4000ppm, 4500ppm, 5000ppm, 5500ppm, 6000ppm, 7000ppm, 8000ppm, 9000ppm or 10000ppm, or other values ​​in the range of 2000ppm to 10000ppm.

[0026] The barium doping amount is 1000ppm to 5000ppm, such as 1000ppm, 1500ppm, 2000ppm, 2500ppm, 3000ppm, 3500ppm, 4000ppm, 4500ppm or 5000ppm, or other values ​​in the range of 1000ppm to 5000ppm.

[0027] In some preferred embodiments, the molybdenum doping level is 3000 ppm and the barium doping level is 2000 ppm.

[0028] If the molybdenum doping amount is too low, it is not conducive to the formation of a cubic single crystal with the (104) crystal plane as the dominant crystal; if the molybdenum doping amount is too high, it is not conducive to grain growth. If the barium doping amount is too low, it is not conducive to the formation of a cubic single crystal with the (104) crystal plane as the dominant crystal; if the barium doping amount is too high, it will lead to a decrease in material capacity.

[0029] According to the doping range provided by the present invention, simultaneous doping of molybdenum and barium in the above positive electrode material body can effectively improve the particle morphology of the single-crystal ternary positive electrode material, reduce the Li / Ni anti-site defect concentration, and promote the uniform growth of the ternary single-crystal positive electrode material. This single-crystal ternary positive electrode material has a cubic structure, and the crystal grains in the single-crystal ternary positive electrode material are dominated by the (104) crystal plane.

[0030] Correspondingly, the present invention further provides a preparation method of the above single-crystal ternary positive electrode material, comprising the following step: mixing a lithium source, a ternary positive electrode material precursor and a dopant, followed by sintering.

[0031] Wherein, the molecular formula of the ternary positive electrode material precursor is Ni x Co y Mn z (OH)₂, 0.8<x<0.96, 0<y<0.1, z=1-x-y. The molecular formula of this precursor corresponds to the molecular formula of the positive electrode material body in the single-crystal ternary positive electrode material.

[0032] In the present invention, the lithium source includes lithium hydroxide.

[0033] The dopant includes a molybdenum source providing molybdenum element and a barium source providing barium element. The molybdenum source may include, for example, molybdenum oxide; the barium source may include, for example, at least one of barium hydroxide, barium carbonate, barium chloride and barium nitrate.

[0034] In some optional embodiments, in terms of molar amount, (Ni+Co+Mn):Li=1:(1.04~1.08), such as 1:1.04, 1:1.05, 1:1.06, 1:1.07 or 1:1.08, etc., and may also be other values within the range of 1:(1.04~1.08).

[0035] In the present invention, the sintering process is carried out in an oxygen atmosphere, and the heating rate of the entire sintering process may be 2°C / min to 6°C / min (such as 2°C / min, 3°C / min, 4°C / min, 5°C / min or 6°C / min, etc.).

[0036] In some alternative embodiments, sintering includes: first treating at 450°C to 560°C (e.g., 450°C, 480°C, 500°C, 550°C, or 560°C) for 2 hours to 4 hours (e.g., 2 hours, 3 hours, or 4 hours), then heating to 700°C to 800°C (e.g., 700°C, 750°C, or 800°C) for 3 hours to 6 hours (e.g., 3 hours, 4 hours, 5 hours, or 6 hours), then heating to 880°C to 1000°C (e.g., 880°C, 900°C, 950°C, or 1000°C) for 1 hour to 5 hours (e.g., 1 hour, 2 hours, 3 hours, 4 hours, or 5 hours), and then cooling to 700°C to 800°C (e.g., 700°C, 750°C, or 800°C) for another 2 hours to 5 hours (e.g., 2 hours, 3 hours, 4 hours, or 5 hours).

[0037] The sintering at 450℃~560℃ primarily serves as pre-sintering, ensuring uniform contact between materials and guaranteeing a sufficient and uniform reaction during subsequent sintering. Sintering at 700℃~800℃ mainly facilitates the formation of a layered phase structure. Sintering at 880℃~1000℃ primarily promotes grain growth. Cooling down to 700℃~800℃ primarily serves as annealing, making the structure formed after the initial sintering more stable and reducing defects.

[0038] Furthermore, after sintering, the material is naturally cooled to room temperature, and then the sintered product is subjected to jaw crusher, roller crusher, airflow pulverizer and sieve to obtain single crystal ternary cathode material.

[0039] In addition, the present invention also provides a battery containing the above-mentioned monocrystalline ternary cathode material.

[0040] The single-crystal ternary cathode material based on the present invention has excellent Li... + With its superior transmission performance, excellent interface and structural stability, batteries containing this single-crystal ternary cathode material can achieve higher rate performance and energy density, while also improving cycle stability and safety.

[0041] The features and performance of the present invention will be further described in detail below with reference to embodiments.

[0042] Example 1 This embodiment provides a single-crystal ternary cathode material, the preparation method of which includes: Lithium source (LiOH) and ternary cathode material precursor Ni 0.9 Co 0.05 Mn 0.05 (OH)2 and dopants (molybdenum oxide and barium hydroxide) are mixed evenly in a high-speed mixer to obtain a mixture.

[0043] In molar amounts, (Ni+Co+Mn):Li=1:1.06; the molybdenum doping amount is 3000ppm and the barium doping amount is 2000ppm.

[0044] The mixture was placed in a crucible and sintered in a high-temperature atmosphere box furnace using oxygen as the sintering atmosphere. The heating rate during sintering was 3°C / min. The sintering process included: initial treatment at 500°C for 3 hours, followed by heating to 780°C for 5 hours, then heating to 950°C for 2 hours, and finally cooling to 780°C for 4 hours. After sintering, the mixture was allowed to cool naturally to room temperature. Subsequently, the sintered product was subjected to jaw crusher, roller mill, airflow milling, and sieving to obtain single-crystal ternary cathode material.

[0045] The SEM image of the single-crystal ternary cathode material in this embodiment is as follows: Figure 2 As shown, the XRD pattern is as follows Figure 3 As shown.

[0046] Example 2 The difference between this embodiment and Embodiment 1 is that the Mo doping amount is 2000 ppm by mass percentage.

[0047] Example 3 The difference between this embodiment and Embodiment 1 is that the Mo doping amount is 6000 ppm by mass percentage.

[0048] Example 4 The difference between this embodiment and Embodiment 1 is that the Ba doping amount is 1000 ppm by mass percentage.

[0049] Example 5 The difference between this embodiment and Embodiment 1 is that the Ba doping amount is 5000 ppm by mass percentage.

[0050] Example 6 The difference between this embodiment and Embodiment 1 is that, in molar terms, Li:(Ni+Co+Mn) = 1.04:1; and the barium source is barium chloride.

[0051] Example 7 The difference between this embodiment and Embodiment 1 is that, in molar terms, Li:(Ni+Co+Mn) = 1.08:1; and the barium source is barium nitrate.

[0052] Example 8 The difference between this embodiment and Embodiment 1 is that the sintering includes: first, treating at 450°C for 4 hours, then raising the temperature to 700°C for 6 hours, then raising the temperature to 880°C for 5 hours, and finally cooling to 700°C for another 5 hours.

[0053] Example 9 The difference between this embodiment and Embodiment 1 is that the sintering includes: first, treating at 560°C for 2 hours, then raising the temperature to 800°C for 3 hours, then raising the temperature to 1000°C for 1 hour, and then cooling down to 800°C for another 2 hours.

[0054] Experimental Example 1 The effects of different doping elements on the surface energy of the single-crystal ternary cathode material (104) are studied below, and the results are shown in Table 1.

[0055] Specifically, taking Example 1 as an example, the ratio of the molar amount of the dopant element in the dopant to the total molar amount of nickel, cobalt and manganese in the ternary cathode material precursor is controlled to 1:0.03, and the other conditions are kept consistent with Example 1.

[0056] Table 1. Calculation results of NCM(104) surface energy before and after elemental doping.

[0057] As can be seen from Table 1, by doping with Ba, the surface energy of NCM (104) can be significantly reduced compared with Mg, Al, Y and Mo.

[0058] Comparative Example 1 The difference between this comparative example and Example 1 is that the dopant is only a barium source (barium hydroxide), and the Ba doping amount is 5000 ppm.

[0059] Comparative Example 2 The difference between this comparative example and Example 1 is that the dopant is only a molybdenum source (molybdenum oxide), and the Mo doping amount is 5000 ppm.

[0060] The SEM image of the single-crystal ternary cathode material in this comparative example is shown below. Figure 4 As shown.

[0061] Comparative Example 3 The difference between this comparative example and Example 1 is that, by mass percentage, the Mo doping amount is 1000 ppm and the Ba doping amount is 4000 ppm.

[0062] Comparative Example 4 The difference between this comparative example and Example 1 is that, by mass percentage, the Mo doping amount is 3000 ppm and the Ba doping amount is 6000 ppm.

[0063] Comparative Example 5 The difference between this comparative example and Example 1 is that the sintering process includes: first treating at 500°C for 3 hours, and then heating to 780°C for 11 hours.

[0064] Comparative Example 6 The difference between this comparative example and Example 1 is that the sintering process includes: first, treating at 500°C for 3 hours, then raising the temperature to 950°C for 7 hours, and then cooling to 780°C for 4 hours.

[0065] Experimental Example 2 The single-crystal ternary cathode materials prepared in Examples 1-9 and Comparative Examples 1-6 were assembled into batteries in the following manner and their electrochemical performance was tested.

[0066] The assembly method is as follows: The assembled battery is a CR2032 coin cell, whose main components include a positive electrode, a separator, a negative electrode, and an electrolyte. NCM positive electrode material, polyvinylidene fluoride, and acetylene black (mass ratio 90:5:5) are mixed uniformly. After adding N-methylpyrrolidone, a homogenate is formed. Then, using a scraper, the positive electrode slurry is coated onto aluminum foil to a thickness of 200 μm and transferred to a vacuum drying oven for 12 hours. After drying, the positive electrode sheet is cut into 14 mm diameter discs and transferred to a glove box (argon atmosphere, oxygen and water content both less than 0.1 ppm). The coin cell assembly is carried out in the glove box. The positive electrode is a pre-prepared NCM positive electrode sheet, the negative electrode is graphite, the separator is polyethylene, and the electrolyte includes ethylene carbonate, methyl ethyl carbonate, and LiFP6, assembled into a coin cell.

[0067] Test conditions included: voltage range of 2.8V to 4.3V, battery charge / discharge rates of 0.1C, 0.2C, 0.33C, 0.5C, and 1C, and room temperature of 25℃.

[0068] The test results are shown in Table 2.

[0069] Table 2 Test Results

[0070] As can be seen from Table 2, the single-crystal ternary cathode material prepared by the method provided by the present invention can be further used to prepare batteries with higher energy density, better rate performance and cycle stability.

[0071] In summary, this invention effectively avoids the problems associated with high-concentration Mo by specifically doping molybdenum and barium elements in a certain proportion into the nickel-cobalt-manganese cathode material to jointly control the single-crystal morphology. 6+ Doping significantly suppresses defects in single-crystal grain growth. After co-doping with Ba and Mo, the surface energy of the nickel-cobalt-manganese ternary cathode material (104) decreases more significantly, which is beneficial for promoting grain formation and increasing the potential for Li... +The (104) crystal plane of the transported material is beneficial to improving the capacity and rate performance of the cathode material. This single-crystal ternary cathode material has a cubic structure, with grains dominated by the (104) crystal plane; the single-crystal ternary cathode material has a low concentration of Li / Ni mixed-displacement defects and uniform growth, exhibiting excellent Li... + It exhibits excellent transmission performance, as well as good interface and structural stability. Batteries containing this single-crystal ternary cathode material can achieve higher rate performance and energy density, while also improving cycle stability and safety.

[0072] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A single-crystal ternary cathode material, characterized in that, The single-crystal ternary positive electrode material comprises a positive electrode material body and doping elements; wherein the molecular formula of the positive electrode material body is LiNi x Co y Mn z O2, 0.8<x<0.96, 0<y<0.1, z=1-x-y; the doping elements include molybdenum and barium; The molybdenum doping amount is 3000ppm, and the barium doping amount is 2000ppm; the single-crystal ternary cathode material has a cubic structure, and the grains in the single-crystal ternary cathode material are mainly (104) crystal planes; The preparation method of the single-crystal ternary positive electrode material comprises the following steps: mixing a lithium source, a ternary positive electrode material precursor and a dopant, followed by sintering; wherein the molecular formula of the ternary positive electrode material precursor is Ni x Co y Mn z (OH)₂, 0.8<x<0.96, 0<y<0.1, z=1-x-y; the dopant includes a molybdenum source providing molybdenum element and a barium source providing barium element; the sintering process includes: first treating at 450°C to 560°C for 2h to 4h, then heating up to 700°C to 800°C for 3h to 6h, then heating up to 880°C to 1000°C for 1h to 5h, and cooling down to 700°C to 800°C for further treatment for 2h to 5h.

2. A method for preparing a single-crystal ternary cathode material as described in claim 1, characterized in that, Includes the following steps: mixing a lithium source, a ternary positive electrode material precursor and a dopant, followed by sintering; wherein the molecular formula of the ternary positive electrode material precursor is Ni x Co y Mn z (OH)2, 0.8<x<0.96, 0<y<0.1, z=1-x-y; the dopant includes a molybdenum source providing molybdenum element and a barium source providing barium element; The sintering process includes: first, treating at 450℃~560℃ for 2h~4h, then raising the temperature to 700℃~800℃ for 3h~6h, then raising the temperature to 880℃~1000℃ for 1h~5h, and finally cooling down to 700℃~800℃ for another 2h~5h.

3. The preparation method according to claim 2, characterized in that, In molar quantities, Li:(Ni+Co+Mn)= (1.04~1.08):

1.

4. The preparation method according to claim 2, characterized in that, The lithium source includes lithium hydroxide; and / or, the molybdenum source includes molybdenum oxide; and / or, the barium source includes at least one of barium hydroxide, barium carbonate, barium chloride, and barium nitrate.

5. The preparation method according to claim 2, characterized in that, The heating rate during the sintering process is 2℃ / min to 6℃ / min.

6. The preparation method according to claim 2, characterized in that, The sintering atmosphere is an oxygen atmosphere.

7. A battery, characterized in that, The battery contains the single-crystal ternary cathode material as described in claim 1.

Citation Information

Patent Citations

  • Monocrystal nickel-cobalt-manganese ternary material as well as preparation method and application thereof

    CN118600555A