A semi-solid battery separator with a modified LLZO coating and its preparation method

By using a Y- and Ca co-doped LLZO garnet-type electrolyte coating in the semi-solid battery separator, the problems of separator-electrode interface stability and high-temperature performance were solved, achieving higher ionic conductivity and battery stability.

CN121688356BActive Publication Date: 2026-11-10HEFEI CHANGYANG NEW ENERGY TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202610191228.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-02-10
Publication Date
2026-11-10
Estimated Expiration
2046-02-10

AI Technical Summary

Technical Problem

In existing semi-solid battery separators, the interfacial stability between the solid electrolyte and electrode materials is poor, and the ionic conductivity needs further optimization, especially since battery performance may degrade during high temperatures and long-term use.

Method used

LLZO garnet-type solid electrolyte modified by co-doping with Y and Ca is used as the membrane coating. The lattice structure is adjusted by doping elements to optimize lithium-ion migration channels and interface stability, thereby reducing high-temperature thermal expansion.

Benefits of technology

It improves the ionic conductivity and high-temperature stability of the separator, enhances electrode interface contact, reduces internal resistance, and improves the power density and cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of battery separators, and discloses a semi-solid battery separator with a modified LLZO coating and its preparation method, comprising a base film and a modified LLZO coating coated on the surface of the base film; the modified LLZO coating includes a modified LLZO electrolyte with the general formula Li7La. 3‑x‑γ Y x Ca γ Zr2O 12 Where 0.25 < X < 1, 0.5 < γ < 2. This invention uses a Y- and Ca-co-doped LLZO garnet-type solid electrolyte as the separator coating, which can effectively improve the ionic conductivity of the separator and enhance the interfacial stability between the separator and the lithium metal anode, reducing the increase in internal resistance caused by poor interface during battery operation. Simultaneously, the doping elements can reduce the thermal expansion of the separator at high temperatures, improving its high-temperature stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery separator technology, and in particular to a semi-solid battery separator with a modified LLZO coating and its preparation method. Background Technology

[0002] Semi-solid-state batteries utilize semi-solid electrolytes, which improve energy density while effectively enhancing battery safety. They avoid the leakage risks inherent in traditional liquid batteries and overcome some of the difficulties in solid-state battery manufacturing. The high energy density of semi-solid-state batteries makes them a promising candidate for applications in electric vehicles and energy storage systems. Numerous studies have shown that semi-solid-state batteries not only offer longer driving range but also exhibit better stability and greater adaptability in high-temperature environments.

[0003] In existing semi-solid-state battery separators, a layer of solid electrolyte is typically coated onto the surface of a polyolefin separator. For example, a semi-solid-state battery disclosed in patent CN120033329A includes a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte, with the separator located between the positive and negative electrodes, and at least one surface of the separator having a solid electrolyte coating. However, in existing semi-solid-state battery separators, the interfacial stability between the solid electrolyte and the electrode materials is poor, and the ionic conductivity of the separator still needs further optimization, especially during high temperatures and long-term use, when battery performance may degrade or decrease. Summary of the Invention

[0004] This invention aims to overcome the aforementioned problems existing in the semi-solid battery separators of the prior art, and provides a semi-solid battery separator with a modified LLZO coating and its preparation method. The LLZO garnet-type solid electrolyte, modified by co-doping with Y and Ca, is used as the separator coating, which can effectively improve the ionic conductivity of the separator and enhance the interfacial stability between the separator and the lithium metal anode, reducing the increase in internal resistance caused by poor interface during battery operation. Simultaneously, the doping elements can reduce the thermal expansion problem of the separator at high temperatures, improving the high-temperature stability of the separator.

[0005] To achieve the above objectives, the present invention adopts the following technical solution: A semi-solid-state battery separator with a modified LLZO coating includes a base film and a modified LLZO coating coated on the surface of the base film; the modified LLZO coating includes a modified LLZO electrolyte with the general formula Li7La. 3-x-γ Y x Ca γ Zr2O 12 , where 0.25 < X < 1, 0.5 < γ < 2.

[0006] The separator of this invention uses a Y and Ca co-doped modified LLZO electrolyte as a coating. Yttrium (Y) doping increases the channels for lithium-ion migration, thereby improving the ionic conductivity of the material. Calcium (Ca) doping modifies the LLZO lattice structure, optimizes its lattice defects, and affects the oxygen vacancy structure of the crystal, allowing lithium ions to move more freely and thus improving conductivity. Furthermore, the co-doping of Y and Ca effectively improves the crystal structure of LLZO, making it more compact and thus enhancing its thermal stability. By optimizing the lattice structure, the doping elements reduce the thermal expansion problem of the material under high-temperature environments, thereby improving the performance of LLZO over a wide temperature range, especially its stability at high temperatures. Simultaneously, Y and Ca doping also helps improve the interface stability between LLZO and the lithium metal anode, reducing the increase in internal resistance caused by poor interface during battery operation. Good interface contact helps improve the power density and cycle life of the battery.

[0007] Preferably, the modified LLZO electrolyte has a particle size D50 of 0.5~8 μm. This particle size range ensures good particle rearrangement during compression molding (tap density > 2.3 g / cm³). 3 It can also effectively suppress stress concentration caused by particle size differences during subsequent cold isostatic pressing.

[0008] Preferably, the coating thickness of the modified LLZO coating is 0.5~10μm.

[0009] Preferably, the base film is a thermoplastic resin porous film with a thickness of 10~40μm, more preferably 10~25μm.

[0010] Preferably, the puncture strength of the semi-solid battery separator is ≥200 kgf / cm. 2 .

[0011] The present invention also provides a method for preparing the above-mentioned semi-solid battery separator with modified LLZO coating, comprising the following steps: (1) The precursor of the modified LLZO electrolyte was prepared by the sol-gel method; (2) The precursor was subjected to gradient sintering in an inert atmosphere and then mechanically crushed and sieved to obtain the modified LLZO electrolyte; (3) The modified LLZO electrolyte is made into a coating slurry, coated on at least one side of the base membrane, and dried to obtain the semi-solid battery separator.

[0012] Preferably, the method for preparing the precursor in step (1) is as follows: A) Dissolve yttrium chloride and calcium chloride in anhydrous ethanol to obtain a mixed ionic solution; B) Lithium carbonate, lanthanum oxide, and zirconium dioxide were mixed and ball-milled to obtain a mixed powder; C) The mixed ionic solution is added to the mixed powder under stirring, and citric acid is added. The mixture is stirred to form a sol system, and then dried to obtain the precursor.

[0013] Preferably, the cation concentration in the mixed ionic solution in step A) is 0.2~0.4 mol / L; and the amount of citric acid added in step C) is 1.0~1.5 times the total molar amount of cations.

[0014] Preferably, the gradient sintering in step (2) is carried out under inert gas protection throughout the process. The gradient sintering method is as follows: First, raise the temperature from room temperature to 300-500℃ at a rate of 1-3℃ / min and hold for 60-120 min; then slowly raise the temperature to remove residual organic solvents, moisture and organic matter from the sol-gel to prevent the sample from bursting. Then, the temperature is increased to 800-1000℃ at a rate of 2-5℃ / min and held for 60-120 min; then, the temperature is increased at a medium rate to promote the decomposition of the precursor into oxide components and the formation of initial crystal nuclei. Then, the temperature is increased to 1100-1300℃ at a rate of 2-4℃ / min and held for 120-240 min; the high-temperature section is heated slowly and held for a long time to promote the formation of LLZO cubic phase and material densification. Finally, the temperature is reduced to room temperature at a rate of ≤1℃ / min; the cooling is controlled to avoid thermal stress causing material cracking.

[0015] The key to the technology of Y and Ca co-doped modified LLZO solid electrolyte lies in optimizing material properties through precise control of doping concentration and sintering process. The sintering process requires optimized temperature and time to ensure the compactness and structural stability of LLZO, and the uniform distribution of doped elements is crucial for improving conductivity. This invention employs a multi-stage heating / cooling strategy during sintering to regulate grain growth kinetics and suppress element segregation; this temperature control process effectively promotes the cubic phase Li7La3Zr2O. 12 Grain boundary reconstruction was achieved, and ionic conductivity optimization (>1×10⁻⁶) was achieved by regulating oxygen vacancy concentration. -3 S / cm). After sintering, a stepped slow cooling process is performed to finally obtain a densified electrolyte ceramic body. An inert gas is introduced throughout the sintering process to suppress lithium volatilization and prevent the formation of impurity phases (such as La₂Zr). 27 ).

[0016] Preferably, the inert atmosphere is a high-purity argon gas (oxygen content <1 ppm) protective atmosphere; the argon gas flow rate is maintained at ≥50 mL / min during sintering to ensure the uniformity of the atmosphere inside the furnace.

[0017] Preferably, by weight, the components of the coating slurry in step (3) include: 10-20 parts modified LLZO electrolyte, 1-10 parts binder, 30-50 parts water, 1-5 parts dispersant, and 1-10 parts thickener.

[0018] Preferably, the binder is at least one of polyvinylidene fluoride, polysulfide rubber, and polyvinyl alcohol; the dispersant is at least one of sodium tripolyphosphate, BYK, sodium polyacrylate, and guar gum; and the thickener is at least one of sodium chloride, hydroxypropyl methylcellulose, chitosan, and guar gum.

[0019] Therefore, the present invention has the following beneficial effects: using Y and Ca co-doped modified LLZO electrolyte as a coating in the separator helps to adjust the LLZO lattice structure, improve the lithium-ion migration path, enhance the conductivity of the material, and stabilize the cubic structure of LLZO to prevent phase transition; in addition, doping can also improve the interfacial contact stability between the electrolyte and the electrode, reduce the interfacial resistance, reduce side reactions, and improve the overall performance and safety of the semi-solid-state battery; in terms of electrochemical performance, Y and Ca doping can improve the ionic conductivity and cycle stability of LLZO, especially under high temperature and high voltage environments, showing good stability, and is suitable for high energy density and high safety semi-solid-state battery applications. Detailed Implementation

[0020] The present invention will be further described below with reference to specific embodiments.

[0021] In this invention, unless otherwise specified, all equipment and raw materials are available from the market or commonly used in the industry. The methods in the following embodiments are conventional methods in the field unless otherwise specified.

[0022] Example 1: A method for preparing a semi-solid battery separator with a modified LLZO coating, comprising the following steps: (1) Preparation of precursors for modified LLZO electrolytes using the sol-gel method: A) Dissolve 5 parts by weight of yttrium chloride (YCl3) and 8 parts by weight of calcium chloride (CaCl2·2H2O) in 30 parts by weight of anhydrous ethanol to obtain a mixed ionic solution with a cation concentration of 0.5 mol / L. B) Seven parts of lithium carbonate (Li2CO3), seven parts of lanthanum oxide (La2O3) and four parts of zirconium dioxide (ZrO2) were wet-milled at 600 rpm for 5 hours using a planetary ball mill to achieve nanoscale powder mixing, thus obtaining mixed powder; C) Under magnetic stirring conditions, the mixed ion solution was added to the mixed powder at a rate of 4 mL / min through a constant pressure dropping funnel, and 3 parts of citric acid were added. The mixture was stirred continuously for 12 h to form a sol system, and finally the precursor was obtained by vacuum drying at 80 °C. (2) The precursor powder was placed in a high-temperature corundum crucible and subjected to gradient sintering in a protective atmosphere of high-purity argon (oxygen content < 1 ppm). The argon flow rate was maintained at ≥ 50 mL / min. The gradient sintering method was as follows: First, raise the temperature from room temperature to 400℃ at a rate of 2℃ / min and hold for 90 min; Then, the temperature is increased to 900℃ at a rate of 5℃ / min and held for 120 min. Then raise the temperature to 1200℃ at a rate of 3℃ / min and hold for 120~240 min; Finally, the temperature was lowered to room temperature at a rate of ≤1℃ / min; ultimately, a densified modified LLZO electrolyte with the general formula Li7La was obtained. 1.6 Y 0.6 Ca 0.8 Zr2O 12 ; (3) The sintered and densified modified LLZO electrolyte was mechanically crushed by a planetary ball mill (zirconia mill jar with φ3 / 5mm zirconia grinding balls, ethanol medium, 300 rpm×4 h), and then particle size was classified by a vibrating sieve. After removing agglomerates by coarse sieving with 400~600 mesh (38~23μm), it was then finely sieved with 10000~30000 mesh (1.5~0.5μm) to obtain modified LLZO electrolyte powder with D50 = 0.5~1.0μm (measured by Malvern laser particle size analyzer) and monodisperse distribution. (4) By weight, 10 parts of modified LLZO electrolyte powder, 5 parts of BYK-190 and 5 parts of polyvinylidene fluoride are mixed in 30 parts of deionized water and stirred into a uniform suspension to obtain a coating slurry; the coating slurry is coated on one side of the base film (PE, 15μm thickness) with a coating thickness of 2μm, and after baking, a coating is formed. The film is then rolled up to obtain a semi-solid battery separator with a modified LLZO coating.

[0023] Example 2: A method for preparing a semi-solid battery separator with a modified LLZO coating, comprising the following steps: (1) Preparation of precursors for modified LLZO electrolytes using the sol-gel method: A) Dissolve 10 parts by weight of yttrium chloride (YCl3) and 8 parts by weight of calcium chloride (CaCl2·2H2O) in 30 parts by weight of anhydrous ethanol to obtain a mixed ionic solution with a cation concentration of 0.5 mol / L. B) 15 parts of lithium carbonate (Li2CO3), 10 parts of lanthanum oxide (La2O3) and 6 parts of zirconium dioxide (ZrO2) were wet-milled at 600 rpm for 5 hours using a planetary ball mill to achieve nanoscale powder mixing and obtain mixed powder; C) Under magnetic stirring conditions, the mixed ion solution was added to the mixed powder at a rate of 4 mL / min through a constant pressure dropping funnel, and 3 parts of citric acid were added. The mixture was stirred continuously for 12 h to form a sol system, and finally the precursor was obtained by vacuum drying at 80 °C. (2) The precursor powder was placed in a high-temperature corundum crucible and subjected to gradient sintering in a protective atmosphere of high-purity argon (oxygen content < 1 ppm). The argon flow rate was maintained at ≥ 50 mL / min. The gradient sintering method was as follows: First, raise the temperature from room temperature to 400℃ at a rate of 2℃ / min and hold for 90 min; Then, the temperature is increased to 900℃ at a rate of 5℃ / min and held for 120 min. Then raise the temperature to 1200℃ at a rate of 3℃ / min and hold for 120~240 min; Finally, the temperature was lowered to room temperature at a rate of ≤1℃ / min; ultimately, a densified modified LLZO electrolyte with the general formula Li was obtained. 14 La 1.5 Y 1.2 CaZr3O 11 ; (3) The modified LLZO electrolyte, which has been sintered and densified, is mechanically crushed by a planetary ball mill (zirconia grinding jar with φ3 / 5mm zirconia grinding balls, ethanol medium, 300 rpm×4 h), and then particle size is classified by a vibrating sieve. After removing agglomerates by coarse sieving with 400~600 mesh (38~23μm), it is then finely sieved with 3000~7500 mesh (5~2μm) to obtain modified LLZO electrolyte powder with D50 =2~4μm (measured by Malvern laser particle size analyzer) and monodisperse distribution. (4) By weight, 10 parts of modified LLZO electrolyte powder, 5 parts of BYK-190, 5 parts of coconut oil diethanolamide and 5 parts of polyvinylidene fluoride are mixed in 30 parts of deionized water and stirred into a uniform suspension to obtain a coating slurry; the coating slurry is coated on one side of the base film (PE, 20 μm thickness) with a coating thickness of 4 μm, and after baking, a coating is formed. The film is then wound up to obtain a semi-solid battery separator with a modified LLZO coating.

[0024] Example 3: A method for preparing a semi-solid battery separator with a modified LLZO coating, comprising the following steps: (1) Preparation of precursors for modified LLZO electrolytes using the sol-gel method: A) Dissolve 2 parts by weight of yttrium chloride (YCl3) and 4 parts by weight of calcium chloride (CaCl2·2H2O) in 30 parts by weight of anhydrous ethanol to obtain a mixed ionic solution with a cation concentration of 0.5 mol / L. B) Five parts of lithium carbonate (Li2CO3), three parts of lanthanum oxide (La2O3) and one part of zirconium dioxide (ZrO2) were wet-milled at 600 rpm for 5 hours using a planetary ball mill to achieve nanoscale powder mixing, thus obtaining mixed powder; C) Under magnetic stirring conditions, the mixed ion solution was added to the mixed powder at a rate of 4 mL / min through a constant pressure dropping funnel, and 3 parts of citric acid were added. The mixture was stirred continuously for 12 h to form a sol system, and finally the precursor was obtained by vacuum drying at 80 °C. (2) The precursor powder was placed in a high-temperature corundum crucible and subjected to gradient sintering in a protective atmosphere of high-purity argon (oxygen content < 1 ppm). The argon flow rate was maintained at ≥ 50 mL / min. The gradient sintering method was as follows: First, raise the temperature from room temperature to 400℃ at a rate of 2℃ / min and hold for 90 min; Then, the temperature is increased to 900℃ at a rate of 5℃ / min and held for 120 min. Then raise the temperature to 1200℃ at a rate of 3℃ / min and hold for 120~240 min; Finally, the temperature was lowered to room temperature at a rate of ≤1℃ / min; ultimately, a densified modified LLZO electrolyte with the general formula Li6La was obtained. 1.2 Y 0.4 Ca 0.5 Zr 0.8 O 10 ; (3) The modified LLZO electrolyte, which has been sintered and densified, is mechanically crushed by a planetary ball mill (zirconia grinding jar with φ3 / 5mm zirconia grinding balls, ethanol medium, 300 rpm×4 h), and then particle size is classified by a vibrating sieve. After removing agglomerates by coarse sieving with 400~600 mesh (38~23μm), it is then finely sieved with 1500~3000 mesh (10~5μm) to obtain modified LLZO electrolyte powder with D50 = 5~8μm (measured by Malvern laser particle size analyzer) and monodisperse distribution. (4) By weight, 10 parts of modified LLZO electrolyte powder, 5 parts of BYK-190, 5 parts of coconut oil diethanolamide and 5 parts of polyvinylidene fluoride are mixed in 30 parts of deionized water and stirred into a uniform suspension to obtain a coating slurry; the coating slurry is coated on one side of the base film (PE, 20 μm thickness) with a coating thickness of 6 μm, and after baking, a coating is formed. The film is then wound up to obtain a semi-solid battery separator with a modified LLZO coating.

[0025] Example 4: A method for preparing a semi-solid battery separator with a modified LLZO coating, comprising the following steps: (1) Preparation of precursors for modified LLZO electrolytes using the sol-gel method: A) Dissolve 5 parts by weight of yttrium chloride (YCl3) and 8 parts by weight of calcium chloride (CaCl2·2H2O) in 30 parts by weight of anhydrous ethanol to obtain a mixed ionic solution with a cation concentration of 0.5 mol / L. B) 10 parts of lithium carbonate (Li2CO3), 7 parts of lanthanum oxide (La2O3) and 3 parts of zirconium dioxide (ZrO2) were wet-milled at 600 rpm for 5 hours using a planetary ball mill to achieve nanoscale powder mixing and obtain mixed powder; C) Under magnetic stirring conditions, the mixed ion solution was added to the mixed powder at a rate of 4 mL / min through a constant pressure dropping funnel, and 3 parts of citric acid were added. The mixture was stirred continuously for 12 h to form a sol system, and finally the precursor was obtained by vacuum drying at 80 °C. (2) The precursor powder was placed in a high-temperature corundum crucible and subjected to gradient sintering in a protective atmosphere of high-purity argon (oxygen content < 1 ppm). The argon flow rate was maintained at ≥ 50 mL / min. The gradient sintering method was as follows: First, raise the temperature from room temperature to 400℃ at a rate of 2℃ / min and hold for 90 min; Then, the temperature is increased to 900℃ at a rate of 5℃ / min and held for 120 min. Then raise the temperature to 1200℃ at a rate of 3℃ / min and hold for 120~240 min; Finally, the temperature was lowered to room temperature at a rate of ≤1℃ / min; ultimately, a densified modified LLZO electrolyte with the general formula Li8La was obtained. 1.5 Y 0.6 Ca 0.8 Zr 1.6 O 12 ; (3) The modified LLZO electrolyte, which has been sintered and densified, is mechanically crushed by a planetary ball mill (zirconia grinding jar with φ3 / 5mm zirconia grinding balls, ethanol medium, 300 rpm×4 h), and then particle size is classified by a vibrating sieve. After removing agglomerates by coarse sieving with 400~600 mesh (38~23μm), it is then finely sieved with 1500~3000 mesh (10~5μm) to obtain modified LLZO electrolyte powder with D50 = 5~8μm (measured by Malvern laser particle size analyzer) and monodisperse distribution. (4) By weight, 5 parts of modified LLZO electrolyte powder, 5 parts of BYK-190, 5 parts of coconut oil diethanolamide and 5 parts of polyvinylidene fluoride are mixed in 30 parts of deionized water and stirred into a uniform suspension to obtain a coating slurry; the coating slurry is coated on one side of the base film (PE, 25 μm thickness) with a coating thickness of 8 μm, and after baking, a coating is formed. The film is then rolled up to obtain a semi-solid battery separator with a modified LLZO coating.

[0026] Comparative Example 1: The difference between Comparative Example 1 and Example 1 is that yttrium chloride was not added when preparing the precursor of the modified LLZO electrolyte; otherwise, they were the same as in Example 1.

[0027] Comparative Example 2: The difference between Comparative Example 2 and Example 1 is that calcium chloride was not added when preparing the precursor of the modified LLZO electrolyte; otherwise, they were the same as in Example 1.

[0028] Comparative Example 3: The difference between Comparative Example 3 and Example 1 is that barium oxide was used instead of calcium oxide when preparing the precursor for the modified LLZO electrolyte; otherwise, they were the same as in Example 1.

[0029] Comparative Example 4 (excessive Y doping): The difference between Comparative Example 4 and Example 1 is that 8 parts of yttrium chloride were added when preparing the precursor for the modified LLZO electrolyte, resulting in a modified LLZO electrolyte with the general formula Li7La. 1.6 Y 1.3 Ca 0.8 Zr2O 12 Everything else is the same as in Example 1.

[0030] Comparative Example 5 (excessive Ca doping): The difference between Comparative Example 5 and Example 1 is that 10 parts of calcium chloride were added when preparing the precursor of the modified LLZO electrolyte, and the general formula of the resulting modified LLZO electrolyte is Li7La. 1.5 Y 0.5 Ca 1.4 Zr 1.4 O 12 Everything else is the same as in Example 1.

[0031] Comparative Example 6 (without using the gradient sintering process of this invention): The difference between Comparative Example 6 and Example 1 is that Comparative Example 6 is not performed by gradient sintering, but is directly heated from room temperature to 1200°C at a rate of 2°C / min, held for 180 min, and then cooled naturally; the rest is the same as in Example 1.

[0032] The diaphragms prepared in the above embodiments and comparative examples were cut into A4 size, and various mechanical and thermal properties were tested. The results are shown in Table 1. The test methods are as follows: (1) Average thickness: The thickness of the diaphragm at different locations was measured using a micrometer screw gauge, and the average value was calculated; (2) Tensile strength: The longitudinal and transverse tensile strength of the diaphragm was tested using the Xieqiang CTM universal testing machine. Five specimens were tested in each direction and the average value was calculated. (3) Puncture strength: The puncture strength of the diaphragm was tested using the Xieqiang CTM universal testing machine. Five specimens were tested and their average value was calculated. (4) Porosity: The mass of a 10 cm × 10 cm sample was tested using an analytical balance, and the porosity of the modified LLZO coated PE membrane was calculated. Five samples were tested and their average value was calculated. (5) Ionic conductivity: The composite membrane was assembled into a coin cell using the Chenhua electrochemical workstation, and the ionic conductivity of the five semi-solid cells was measured by AC impedance method. (6) The membrane rupture temperature was tested using a hot stage microscope. The temperature of the membrane at the beginning of melting was recorded. Five samples were tested and their average value was calculated.

[0033] Table 1. Test results of diaphragm performance

[0034] As shown in Table 1, the semi-solid composite battery separator solution provided by this invention can significantly improve the ionic conductivity of the separator without affecting porosity, membrane rupture temperature, and mechanical strength. Compared with the prior art, simultaneous doping with yttrium (Y) and calcium (Ca) can improve the ionic conductivity and lattice structure of traditional LLZO, increase lithium-ion migration channels, optimize lattice defects, and improve conductivity. Y and Ca co-doping makes the LLZO crystal structure more compact, enhances thermal stability, reduces thermal expansion at high temperatures, and improves performance over a wide temperature range. The doping of Y and Ca helps improve the interface stability between LLZO and the lithium metal anode, reduces internal resistance, and increases battery power density and cycle life. The composite separators in Examples 1-4 show better mechanical properties and porosity. The ionic conductivity of Example 1 is significantly higher than that of Examples 2-4. Furthermore, the separator thickness of Example 1 is thinner, meeting practical application requirements. Overall, Example 1 demonstrates excellent performance and ease of processing, making it the most ideal solution in this invention.

[0035] In Comparative Examples 1 and 2, without Y or Ca doping, the tensile and puncture strength properties of the diaphragm were significantly reduced compared to Example 1. In Comparative Example 3, Ba was used instead of Ca for doping, and calcium ions (Ca...)... 2+The ionic radius of the ion (approximately 1.00 Å) is smaller than that of the barium ion (Ba). 2+ The ionic radius of Ba is approximately 1.35 Å. When the larger Ba... 2+ When doping is introduced into the LLZO lattice, it causes more significant lattice expansion and structural distortion. This disrupts the migration channels of lithium ions, increasing the energy barrier and resistance for lithium ions to jump within the lattice. This structural perturbation typically significantly reduces the overall lithium-ion conductivity of the material, weakening the advantage of the separator coating in improving ion transport efficiency.

[0036] In Comparative Examples 4 and 5, excessive Y and Ca doping occurred. The initial intention of Y / Ca co-doping was to optimize the cubic phase stability and lithium-ion transport channels of LLZO through synergistic effects. However, excessive Y / Ca content disrupts this balance, primarily through negative impacts on the lattice structure (excessive shrinkage, phase transition, and impurity phase precipitation) and an imbalance in lithium vacancy concentration. This significantly reduces the migration rate of lithium ions in the separator coating, leading to increased internal resistance and decreased electrochemical performance (such as rate performance and capacity retention) of the entire solid-state battery. Mechanical properties and interface stability may also be indirectly negatively affected.

[0037] Comparative Example 6 shows that the performance of the diaphragm deteriorates in all aspects because it is not sintered using a gradient sintering method.

[0038] The above description is merely a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention. All equivalent variations and modifications made based on the content of the present invention are covered within the patent scope of the present invention.

Claims

1. A semi-solid battery separator with a modified LLZO coating, characterized in that, Including the base film and the modified LLZO coating applied to the surface of the base film; The modified LLZO coating includes a modified LLZO electrolyte with the general formula Li7La. 3-x-γ Y x Ca γ Zr2O 12 , where 0.25 < X < 1, 0.5 < γ < 2.

2. The semi-solid battery separator with a modified LLZO coating according to claim 1, characterized in that, The modified LLZO electrolyte has a particle size D50 of 0.5~8μm; the modified LLZO coating has a coating thickness of 0.5~10μm.

3. The semi-solid battery separator with a modified LLZO coating according to claim 1 or 2, characterized in that, The base film is a thermoplastic resin porous membrane with a thickness of 10~40μm.

4. The semi-solid battery separator with modified LLZO coating according to claim 1, characterized in that, The puncture strength of the semi-solid battery separator is ≥200 kgf / cm. 2 .

5. A method for preparing a semi-solid battery separator with a modified LLZO coating as described in any one of claims 1 to 4, characterized in that, Includes the following steps: (1) The precursor of the modified LLZO electrolyte was prepared by the sol-gel method; (2) The precursor was subjected to gradient sintering in an inert atmosphere and then mechanically crushed and sieved to obtain the modified LLZO electrolyte; (3) The modified LLZO electrolyte is made into a coating slurry, coated on at least one side of the base membrane, and dried to obtain the semi-solid battery separator.

6. The method for preparing a semi-solid battery separator with a modified LLZO coating according to claim 5, characterized in that, The method for preparing the precursor in step (1) is as follows: A) Dissolve yttrium chloride and calcium chloride in anhydrous ethanol to obtain a mixed ionic solution; B) Lithium carbonate, lanthanum oxide, and zirconium dioxide were mixed and ball-milled to obtain a mixed powder; C) The mixed ionic solution is added to the mixed powder under stirring, and citric acid is added. The mixture is stirred to form a sol system, and then dried to obtain the precursor.

7. The method for preparing a semi-solid battery separator with a modified LLZO coating according to claim 6, characterized in that, In step A), the cation concentration in the mixed ionic solution is 0.2~0.4 mol / L; in step C), the amount of citric acid added is 1.0~1.5 times the total molar amount of cations.

8. The method for preparing a semi-solid battery separator with a modified LLZO coating according to claim 5, characterized in that, In step (2), the gradient sintering process is carried out entirely under inert gas protection. The gradient sintering method is as follows: First, raise the temperature from room temperature to 300-500℃ at a rate of 1-3℃ / min, and hold for 60-120 min; Then, increase the temperature to 800-1000℃ at a rate of 2-5℃ / min and hold for 60-120 min. Then raise the temperature to 1100-1300℃ at a rate of 2-4℃ / min and hold for 120-240 min; Finally, it is cooled to room temperature at a rate of ≤1℃ / min.

9. The method for preparing a semi-solid battery separator with a modified LLZO coating according to claim 5, characterized in that, By weight, the components of the coating slurry in step (3) include: 10-20 parts modified LLZO electrolyte, 1-10 parts binder, 30-50 parts water, 1-5 parts dispersant, and 1-10 parts thickener.

10. The method for preparing a semi-solid battery separator with a modified LLZO coating according to claim 9, characterized in that, The binder is at least one of polyvinylidene fluoride, polysulfide rubber, and polyvinyl alcohol; the dispersant is at least one of sodium tripolyphosphate, BYK, sodium polyacrylate, and guar gum; and the thickener is at least one of sodium chloride, hydroxypropyl methylcellulose, chitosan, and guar gum.

Citation Information

Patent Citations

  • Semi-solid-state battery

    CN120033329A

  • Solid electrolyte material and preparation method thereof

    CN106129463A

  • Garnet structure solid electrolyte material and preparation method thereof

    CN107887640A

  • Preparation method of modified separator for lithium ion battery

    CN109119573A