Diazo naphthoquinone type photosensitive compound, preparation method and application of diazo naphthoquinone type photosensitive compound in photoresist
By combining ion exchange resins and alkaline compounds, the problem of chloride ion impurities in diazonoquinone-type photosensitive compounds was solved, enabling the preparation of high-purity photosensitive compounds and improving the performance and stability of photoresists.
Patent Information
- Application Number
- CN202511615389.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-11-06
- Publication Date
- 2026-03-20
AI Technical Summary
Existing technologies make it difficult to prepare diazonaphthoquinone-type photosensitive compounds with extremely low levels of ionic impurities, which affects the resolution, film retention, and other properties of photoresists. Furthermore, the chloride ions introduced by traditional synthesis methods can lead to corrosion and contamination of metal substrates.
A synthesis method combining ion exchange resin and basic compound was adopted. The reaction was carried out in an organic solvent, followed by treatment with acidic substances, filtration and vacuum drying to prepare a diazonoquinone-type photosensitive compound, thereby reducing the chloride ion content.
This study achieved efficient synthesis of photosensitive compounds with extremely low levels of ionic impurities, reduced the chloride ion concentration in the photoresist, improved the resolution and film retention of the photoresist, and reduced the risk of corrosion on the metal substrate.
Smart Images

Figure CN121698783A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of organic synthesis technology, specifically to diazonoquinone-type photosensitive compounds, their preparation methods, and their applications in photoresists. Background Technology
[0002] Positive photoresists composed of diazononaphthoquinone (DNQ)-type photosensitive compounds (PACs) and phenolic / polyimide (PI) resins have been widely used in G / I line lithography processes. The reaction mechanism of DNQ-type photosensitive agents involves the release of N₂ to generate indanic acid via the Wolff rearrangement under illumination. These photosensitive agents exhibit excellent photosensitivity to light sources at wavelengths of 436 nm and 365 nm, and their unique structural variations make DNQ an ideal photosensitive compound for G / I line photoresists.
[0003] Meanwhile, DNQ molecules can also form intermolecular hydrogen bonds with functional groups (-OH, -COOH, etc.) in the resin, reducing the resin's solubility in the solvent. When DNQ is exposed to ultraviolet light, its structure changes, the intermolecular hydrogen bonds are broken, leading to an increase in the solubility of the polymer molecules. Therefore, the exposed photoresist can be dissolved and removed, thus completing the transfer of the photolithographic pattern. Therefore, DNQ-type photosensitive compounds are also widely used as dissolution inhibitors in positive photosensitive polyimide (PSPI) photoresist solutions.
[0004] With the rapid development of the semiconductor industry and the advancement of photoresist technology, the demand for purer raw materials is increasing. To meet the extremely low contaminant levels required by today's photoresists, raw materials must be prepared to be cleaner. However, residual ionic impurities can affect a range of issues, including photosensitivity, particle formation, etching, and dark film loss. Furthermore, the purity of the photosensitive compound directly impacts the resolution, film retention, edge roughness, and defect rate of the photoresist lithography pattern.
[0005] The classic synthesis method for DNQ-type photosensitive compounds involves the dehydrochlorination of diazonaphthoquinone (DNQ) sulfonyl chloride and phenolic compounds under the action of a large amount of alkaline compounds. This process introduces chloride ions, which can affect the resolution and film retention of the photoresist, and cause long-term corrosion of the metal substrate. In addition, excessive alkaline compounds can generate a large number of byproducts, causing some pollution.
[0006] Current techniques address this problem by using an excessive amount of pure water for washing, or by repeated dissolution and reprecipitation. However, this technique still does not yet solve the problem of preparing ions with extremely low levels (Cl-). - The problem lies in the presence of impurities in PAC. Therefore, the existing technology needs further development. Summary of the Invention
[0007] To address the shortcomings of existing technologies and solve the aforementioned problems, a diazononaphthoquinone-type photosensitive compound, its preparation method, and its application in photoresists are proposed, along with the following technical solutions: A method for preparing a diazononaphthoquinone-type photosensitive compound includes: mixing diazononaphthoquinone sulfonyl chloride and a phenolic compound in an organic solvent, then adding an ion exchange resin and a basic compound to react and obtain the diazononaphthoquinone-type photosensitive compound.
[0008] Furthermore, the ion exchange resin is at least one of Amberjet 4000CL, Amberjet 1200 Na, Amberlite IRA67, Amberlite IRA96, Amberlite IRA401, Amberjet UP4000, Amberlyst A21, Amberlyst 15, Amberlite IRC50, Amberlite 719, Lanxess MonoPlus MP 64, Lanxess MonoPlus MP68, Lanxess MonoPlus M500, Mitsubishi SA10ALLP, Mitsubishi WA30LL, Purolite A100, Purolite A105, Purolite A830, and Purolite A103 Plus.
[0009] Furthermore, the mass ratio of the amount of ion exchange resin to the amount of diazonoquinone sulfonyl chloride is 1:1-4.
[0010] Furthermore, the molar ratio of the amount of ion exchange resin to the amount of alkaline compound is 2-4:1.
[0011] Furthermore, the alkaline compound is at least one selected from triethylamine, 2-isopropylamine, tripropylamine, ethylenediamine, pyridine, 1,4-diazabicyclo[2.2.2]octane, 1,8-diazabicyclo[5.4.0]undec-7-ene, N,N-dimethylaniline, tetramethylammonium hydroxide, sodium methoxide, sodium ethoxide, lithium diisopropylamino, sodium carbonate, sodium bicarbonate, sodium hydroxide, potassium carbonate, potassium bicarbonate, potassium hydroxide, ammonium hydroxide, and sodium hydride.
[0012] Further, after the reaction, the mixture is filtered, an acidic substance is added to the filtrate, stirred and filtered again. The filtrate obtained after the second filtration is added to a poor solvent for the diazononaphthoquinone type photosensitive compound, stirred and filtered to obtain the diazononaphthoquinone type photosensitive compound. The acidic substance is at least one of organic acid, inorganic acid, and acidic ion exchange resin; the unsuitable solvent is at least one of methanol, ethanol, isopropanol, and ultrapure water.
[0013] Furthermore, the reaction is carried out under an inert gas protective atmosphere, the reaction temperature is 10–60 °C, and the reaction time is 0.5–8 h.
[0014] Furthermore, the organic solvent is at least one selected from dichloromethane, tetrahydrofuran, 1,4-dioxane, γ-butyrolactone, γ-valerolactone, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, acetone, toluene, acetonitrile, methanol, and ethanol.
[0015] This invention provides a diazonoquinone-type photosensitive compound prepared by the above-described method.
[0016] This invention also provides an application of a diazonaphthoquinone-type photosensitive compound in photoresists.
[0017] Beneficial effects: 1. This invention combines ion exchange resin and alkaline compounds. The ion exchange resin not only has adsorption properties but also catalyzes the reaction in synergy with the alkaline compounds. The combined effect of these two components enables the production of ions with extremely low Cl- levels. - This enables the efficient synthesis of photosensitive compounds containing impurities, and since ion exchange resins can be recycled without generating large amounts of waste, the synthesis of ultrapure diazonaphthoquinone-type photosensitive compounds can be achieved.
[0018] 2. This invention investigates the effect of the ratio between ion exchange resin and basic compound on chloride ion content. When the molar ratio of the amount of basic ion exchange resin to the amount of basic compound is 1-4:1, a small amount of alkali and basic ion exchange resin are added to the reaction system simultaneously. The small amount of alkali can synergistically activate the deactivated basic ion exchange resin in the reaction system and promote the reaction cycle. Attached Figure Description
[0019] Figure 1 This is a synthetic route diagram of a diazononaphthoquinone-type photosensitive compound of the present invention; Figure 2 Here are the metallographic microscope test results of the PSPI-1 photoresist of this invention: Figure 3 This is a metallographic microscope test result of the PSPI-7 photoresist of the present invention. Detailed Implementation
[0020] To enable those skilled in the art to better understand the technical solutions of the present invention, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Based on the embodiments in this application, other similar embodiments obtained by those skilled in the art without creative effort should all fall within the scope of protection of this application.
[0021] According to embodiments of the present invention, a method for preparing a diazonoquinone-type photosensitive compound is provided, comprising: as follows Figure 1 Diazonaphthoquinone sulfonyl chloride and phenolic compounds are mixed in an organic solvent, then added to an ion exchange resin and a basic compound to react and obtain a diazononaphthoquinone-type photosensitive compound. This invention combines an ion exchange resin and a basic compound. The ion exchange resin not only has adsorption properties but also catalyzes the reaction in synergy with the basic compound. The combined effect of both enables the production of photosensitizing compounds with extremely low levels of Cl- ions. - This method enables the efficient synthesis of PACs containing impurities, and since ion exchange resins can be recycled without generating large amounts of waste, it allows for the synthesis of ultrapure diazonaphthoquinone-type photosensitive compounds.
[0022] The ion exchange resin is at least one of Amberjet 4000CL, Amberjet 1200 Na, Amberlite IRA67, Amberlite IRA96, Amberlite IRA401, Amberjet UP4000, Amberlyst A21, Amberlyst 15, Amberlite IRC50, Amberlite 719, Lanxess MonoPlus MP 64, Lanxess MonoPlus MP 68, Lanxess MonoPlus M500, Mitsubishi SA10ALLP, Mitsubishi WA30LL, Purolite A100, Purolite A105, Purolite A830, and Purolite A103 Plus, more preferably, at least one or more of Lanxess MonoPlus MP 64, Amberlite IRA67, Purolite A105, and Mitsubishi SA10ALLP.
[0023] The organic solvents mentioned include at least one or more of the following: dichloromethane, tetrahydrofuran, 1,4-dioxane, γ-butyrolactone, γ-valerolactone, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, acetone, toluene, acetonitrile, methanol, and ethanol. The alkaline compound includes, but is not limited to, at least one of triethylamine, 2-isopropylamine, tripropylamine, ethylenediamine, pyridine, 1,4-diazabicyclo[2.2.2]octane, 1,8-diazabicyclo[5.4.0]undec-7-ene, N,N-dimethylaniline, tetramethylammonium hydroxide, sodium methoxide, sodium ethoxide, lithium diisopropylamino, sodium carbonate, sodium bicarbonate, sodium hydroxide, potassium carbonate, potassium bicarbonate, potassium hydroxide, ammonium hydroxide, and sodium hydride, preferably at least one or more of triethylamine, 1,4-diazabicyclo[2.2.2]octane, 1,8-diazabicyclo[5.4.0]undec-7-ene, and sodium bicarbonate.
[0024] Phenolic compounds can be single benzene rings, heterocycles, or aromatic rings and heterocycles with different substituents (alkyl, halogen, etc.), as well as aromatic rings and heterocycles with multiple symmetrical or asymmetrical structures.
[0025] Preferred phenolic compounds may be selected from at least one of the following structural compounds: The diazononaphthoquinone-type photosensitive compound obtained above also undergoes the following post-processing: the diazononaphthoquinone-type photosensitive compound system is filtered, and the filtrate is collected. Then, an appropriate amount of acidic substance is added to the filtrate and stirred to remove salts from the system. The filtered reaction product is added to a poor solvent. The aqueous PAC slurry is stirred and filtered. It is then washed with deionized water to obtain diazononaphthoquinone sulfonate compounds; the diazononaphthoquinone sulfonate products are dried in a vacuum drying oven to obtain the diazononaphthoquinone-type photosensitive compound (PAC).
[0026] Acidic substances include formic acid, acetic acid, propionic acid, butyric acid, valeric acid, hexanoic acid, heptanoic acid, octanoic acid, nonanoic acid, decanoic acid, oxalic acid, maleic acid, methylmalonic acid, adipic acid, gallic acid, trimellitic acid, arachidonic acid, 2-ethylhexanoic acid, oleic acid, stearic acid, linoleic acid, salicylic acid, benzoic acid, p-aminobenzoic acid, benzenesulfonic acid, monochloroacetic acid, dichloroacetic acid, trichloroacetic acid, trifluoroacetic acid, malonic acid, citric acid, tartaric acid, sulfuric acid, hydrochloric acid, nitric acid, hydrofluoric acid, phosphoric acid, and acidic ion exchange resins such as Lanxess MonoPlus S107NS, MonoPlus S108, MonoPlus S108H, S80, C 249, MonoPlus SP 112, Purolite C100, C104, C107, C115, C145, C150, C160, and Amberlite. The resin contains at least one or more of various organic acids, inorganic acids, and acidic ion exchange resins, such as IR100Na, Amberlite 732, AmberliteIR120H, AmberLite™ HPR650H, Amberlyst 15, and DIAION™AMP03, preferably formic acid, acetic acid, malonic acid, sulfuric acid, phosphoric acid, Amberlite 732, Amberjet 1200H, Purolite C100, and Amberlyst 15.
[0027] Undesirable solvents include at least one or more of methanol, ethanol, isopropanol, and ultrapure water. Preferably, undesirable solvents are a mixture of methanol and ultrapure water in a ratio of methanol:ultrapure water = 2:8-4:6.
[0028] The preferred vacuum drying oven is set with a negative pressure of 10–600 mbar and a temperature of 30–50°C to further improve the vacuum drying efficiency.
[0029] This application provides a diazononaphthoquinone-type photosensitive compound, which has the structure shown in Formula I below: Ar can be a single benzene ring, heterocycle, or an aromatic ring and heterocycle with different substituents (alkyl, halogen, etc.), as well as an aromatic ring and heterocycle with multiple symmetrical or asymmetrical structures, etc. R represents hydrogen, halogen, alkyl chain, aromatic hydrocarbon, unsaturated hydrocarbon group, benzene ring, aromatic heterocycle, etc.
[0030] Furthermore, the diazonoquinone-type photosensitive compound may be selected from at least one of the following compounds: in, The diazonaphthoquinone-type photosensitive compound of this application can be used in photoresists. The photoresist composition includes a resin, a diazonaphthoquinone-type photosensitive compound, a thermal crosslinking agent, and an adhesion promoter. Specifically, the resin is a polyimide resin, the thermal crosslinking agent is a polyphenol compound, and the adhesion promoter is 3-aminopropyltriethoxysilane. The weight-average molecular weight M of the resin is... w The concentration ranges from 2000 to 40000. The mass percentage of diazonoquinone-type photosensitive compounds in the photoresist composition is 0.5% to 10.0%.
[0031] Example 1 This embodiment provides a method for preparing the diazonaphthoquinone (DNQ) type photosensitive compound PAC-1. The reaction formula for its preparation is shown below, and the specific steps include: Under nitrogen protection, 21.23 g of polyphenol compound (A-1) and 33.84 g of diazonaquinone sulfonyl chloride (DNQ-1) were dissolved in 200 mL of 1,4-dioxane solution. Then, 3.0 g of 1,8-diazabicyclo[5.4.0]undec-7-ene was added in portions below 40 °C. Next, 40 g of dry ion exchange resin Amberlite IRA67 was slowly added. After the addition was complete, the reaction was carried out for 1-3 h, and the ion exchange resin was filtered off. 2 mL of dilute sulfuric acid was added to the reaction mixture and stirred for 1 hour. The mixture was then filtered, and the filtrate was added to 400 mL of aqueous methanol. The reaction mixture was stirred for 30 minutes and filtered to obtain a solid. The solid was washed three times thoroughly with pure water to obtain the diazonaquinone-type photosensitizing compound (PAC-1). Finally, PAC-1 was dried in a vacuum oven at 35-40 °C to obtain the solid product. HPLC analysis showed that the effective content of the esterified compound was 99.3%.
[0032] Example 2 This embodiment provides a method for preparing the diazonaphthoquinone (DNQ) type photosensitive compound PAC-2. The reaction formula for its preparation is shown below, and the specific steps include: Under nitrogen protection, 11.5 g of polyphenol compound (A-2) and 33.84 g of diazonaquinone sulfonyl chloride (DNQ-1) were dissolved in 200 mL of 1,4-dioxane solution. Then, 3.0 g of 1,8-diazabicyclo[5.4.0]undec-7-ene was added in portions below 40 °C. Next, 40 g of dry ion exchange resin Amberlite IRA67 was slowly added. After the addition was complete, the reaction was carried out for 1-3 h, and the ion exchange resin was filtered off. 2 mL of dilute sulfuric acid was added to the reaction mixture and stirred for 1 hour. The mixture was then filtered, and the filtrate was added to 400 mL of aqueous methanol. The reaction mixture was stirred for 30 minutes and filtered to obtain a solid. The solid was washed three times thoroughly with pure water to obtain a diazonaquinone-type photosensitive compound (PAC-2). Finally, PAC-2 was dried in a vacuum oven at 35-40 °C to obtain the solid product.
[0033] The preparation method in Example 2 differs from that in Example 1 in that the polyphenol compound (A-1) is replaced with 11.5 g of the raw material (A-2), while other conditions remain unchanged. Solid product PAC-2 was obtained, and HPLC analysis showed that the effective ester content was 99.2%.
[0034] Example 3 This embodiment provides a method for preparing the diazonaphthoquinone (DNQ) type photosensitive compound PAC-3. The reaction formula for its preparation is shown below, and the specific steps include: Under nitrogen protection, 11.5 g of polyphenol compound (A-2) and 33.84 g of diazonaquinone sulfonyl chloride (DNQ-1) were dissolved in 200 mL of 1,4-dioxane solution. Then, 3.0 g of 1,8-diazabicyclo[5.4.0]undec-7-ene was added in portions below 40 °C. Next, 40 g of dry ion exchange resin Amberlite IRA67 was slowly added. After the addition was complete, the reaction was carried out for 1-3 h, and the ion exchange resin was filtered off. 1 mL of dilute sulfuric acid and 10 g of ion exchange resin Amberjet 120H were added to the reaction mixture, and the mixture was stirred for 1 hour. The mixture was then filtered, and the filtrate was added to 400 mL of aqueous methanol. The reaction mixture was stirred for 30 minutes and filtered to obtain a solid. The solid was washed three times thoroughly with pure water to obtain a diazonaquinone-type photosensitizing compound (PAC-3). Finally, PAC-3 was dried in a vacuum oven at 35-40 °C to obtain the solid product.
[0035] The difference between the preparation method in Example 3 and Example 2 is that "adding 2 mL of dilute sulfuric acid to the reaction" is changed to "adding 1 mL of dilute sulfuric acid and 10 g of ion-exchange resin Amberjet 120H to the reaction". HPLC analysis showed that the effective content of the esterified compound was 99.3%.
[0036] Example 4 Under nitrogen protection, 21.23 g of polyphenol compound (A-1) and 50 g of diazonaquinone sulfonyl chloride (DNQ-1) were dissolved in 200 mL of 1,4-dioxane solution. Then, 7.65 g of 1,4-diazabicyclo[2.2.2]octane was added in portions below 40 °C. Next, 50 g of dry ion exchange resin Amberlite IRA67 was slowly added. After the addition was complete, the reaction was carried out for 1-3 h, and the ion exchange resin was filtered off. 2 mL of dilute sulfuric acid was added to the reaction mixture and stirred for 1 hour. The mixture was then filtered, and the filtrate was added to 400 mL of aqueous methanol. The reaction mixture was stirred for 30 minutes and filtered to obtain a solid. The solid was washed three times thoroughly with pure water to obtain a diazonaquinone-type photosensitive compound. Finally, the diazonaquinone-type photosensitive compound was dried in a vacuum oven at 35-40 °C to obtain a solid product.
[0037] The preparation method in Example 4 differs from that in Example 1 in that the mass ratio of dried ion exchange resin Amberlite IRA67 to diazonaphthoquinone sulfonyl chloride (DNQ-1) is changed to 1:1; the molar ratio of dried ion exchange resin Amberlite IRA67 to 1,8-diazabicyclo[5.4.0]undec-7-ene is changed to 2:1, while other conditions remain unchanged. HPLC analysis showed that the effective content of the esterified compound was 99.3%.
[0038] Example 5 Under nitrogen protection, 21.23 g of polyphenol compound (A-1) and 50 g of diazonaquinone sulfonyl chloride (DNQ-1) were dissolved in 200 mL of 1,4-dioxane solution. Then, 7.65 g of 1,8-diazabicyclo[5.4.0]undec-7-ene was added in portions below 40 °C. Next, 100 g of dry ion exchange resin Amberlite IRA67 was slowly added. After the addition was complete, the reaction was carried out for 1-3 h, and the ion exchange resin was filtered off. 2 mL of dilute sulfuric acid was added to the reaction mixture and stirred for 1 hour. The mixture was then filtered, and the filtrate was added to 400 mL of aqueous methanol. The reaction mixture was stirred for 30 minutes and filtered to obtain a solid. The solid was washed three times thoroughly with pure water to obtain a diazonaquinone-type photosensitive compound. Finally, the diazonaquinone-type photosensitive compound was dried in a vacuum oven at 35-40 °C to obtain a solid product.
[0039] The preparation method in Example 5 differs from that in Example 1 in that the mass ratio of dried ion exchange resin Amberlite IRA67 to diazonaphthoquinone sulfonyl chloride (DNQ-1) is changed to 3:1; the molar ratio of dried ion exchange resin Amberlite IRA67 to 1,8-diazabicyclo[5.4.0]undec-7-ene is changed to 4:1, while other conditions remain unchanged. HPLC analysis revealed an effective ester content of 99.2%.
[0040] Example 6 This embodiment provides a method for preparing the diazonaphthoquinone (DNQ) type photosensitive compound PAC-1. The reaction formula for its preparation is shown below, and the specific steps include: Under nitrogen protection, 21.23 g of polyphenol compound (A-1) and 33.84 g of diazonaquinone sulfonyl chloride (DNQ-1) were dissolved in 200 mL of 1,4-dioxane solution. Then, 2.2 g of 1,4-diazabicyclo[2.2.2]octane was added in portions below 40 °C. Next, 40 g of Purolite A100 was slowly added. After the addition was complete, the reaction was carried out for 1-3 h, and the ion exchange resin was filtered off. 2 mL of dilute sulfuric acid was added to the reaction mixture and stirred for 1 hour. The mixture was then filtered, and the filtrate was added to 400 mL of aqueous methanol. The reaction mixture was stirred for 30 minutes and filtered to obtain a solid. The solid was washed three times thoroughly with pure water to obtain a diazonaquinone-type photosensitive compound. Finally, the obtained product was dried in a vacuum oven at 35-40 °C to obtain a solid product. HPLC analysis showed that the effective content of the esterified compound was 99.3%.
[0041] The preparation method in Example 6 differs from that in Example 1 in that the dried ion exchange resin Amberlite IRA67 is replaced with Purolite A100; and 1,8-diazabicyclo[5.4.0]undec-7-ene is replaced with 1,4-diazabicyclo[2.2.2]octane, while other conditions remain unchanged. HPLC analysis showed that the effective content of the esterified compound was 99.2%.
[0042] Comparative Example 1 This comparative example provides a conventional method for preparing the diazonaphthoquinone (DNQ) type photosensitive compound PAC-4. The reaction formula for its preparation is shown below, and the specific steps include: Under nitrogen protection, 21.23 g of polyphenol compound (A-1) and 33.84 g of diazonoquinone sulfonyl chloride (DNQ-1) were dissolved in 200 mL of 1,4-dioxane solution. Then, triethylamine (40 g dissolved in 50 mL of 1,4-dioxane) was slowly added dropwise. The solution was stirred at 40 °C for 2 hours, and then 1.0 wt% dilute hydrochloric acid was slowly added. After stirring for 1 hour, the solid was filtered off, and the filtrate was added to 800 mL of ultrapure water and stirred. After filtration, the filter cake was washed repeatedly with 800 mL of ultrapure water more than three times. Finally, it was dried in a vacuum drying oven to obtain solid product PAC-4. HPLC analysis showed that the effective ester content was 99.5%.
[0043] Comparative Example 2 This comparative example provides a conventional method for preparing the diazonoquinone (DNQ) type photosensitive compound PAC-5. The reaction formula for its preparation is shown below, and the specific steps include: Under nitrogen protection, 11.5 g of polyphenol compound (A-2) and 33.84 g of diazonoquinone sulfonyl chloride (DNQ-1) were dissolved in 200 mL of 1,4-dioxane solution. Then, triethylamine (40 g dissolved in 50 mL of 1,4-dioxane) was slowly added dropwise. The solution was stirred at 40 °C for 2 hours, and then 1.0 wt% dilute hydrochloric acid was slowly added. After stirring for 1 hour, the solid was filtered off, and the filtrate was added to 800 mL of ultrapure water and stirred. After filtration, the filter cake was washed repeatedly with 800 mL of ultrapure water at least three times. Finally, it was dried in a vacuum drying oven to obtain the solid product PAC-5.
[0044] The preparation method of Comparative Example 2 differs from that of Comparative Example 1 in that the polyphenol compound (A-1) is replaced with 11.5 g of the raw material (A-2), while other conditions remain unchanged. Solid product PAC-5 was obtained, and HPLC analysis showed that the effective content of the esterified compound was 99.2%.
[0045] Comparative Example 3 This comparative example provides a conventional method for preparing a diazononaphthoquinone (DNQ) type photosensitive compound. The reaction formula for its preparation is shown below, and the specific steps include: Under nitrogen protection, 21.23 g of polyphenol compound (A-1) and 33.84 g of diazonaquinone sulfonyl chloride (DNQ-1) were dissolved in 200 mL of 1,4-dioxane solution. Then, 40 g of dry ion-exchange resin Amberlite IRA67 was slowly added. After the addition was complete, the reaction proceeded for 1–3 h, and the ion-exchange resin was filtered off. 2 mL of dilute sulfuric acid was added to the reaction mixture, and the mixture was stirred for 1 hour. The mixture was then filtered, and the filtrate was added to 400 mL of aqueous methanol. The reaction mixture was stirred for 30 minutes and filtered to obtain a solid. The solid was washed three times thoroughly with pure water to obtain the diazonaquinone-type photosensitizing compound (PAC-1). Finally, PAC-1 was dried in a vacuum oven at 35–40 °C to obtain the solid product. HPLC analysis showed that the effective content of the esterified compound was 99.3%.
[0046] The preparation method of Comparative Example 3 differs from that of Example 1 in that the basic compound 1,8-diazabicyclo[5.4.0]undec-7-ene was not added, while other conditions remained unchanged. A solid product was obtained, and the effective content of the esterified product was determined by HPLC to be 99.2%.
[0047] Comparative Example 4 This comparative example provides a conventional method for preparing a diazononaphthoquinone (DNQ) type photosensitive compound. The reaction formula for its preparation is shown below, and the specific steps include: Under nitrogen protection, 21.23 g of polyphenol compound (A-1) and 33.84 g of diazonaquinone sulfonyl chloride (DNQ-1) were dissolved in 200 mL of 1,4-dioxane solution. Then, 2.0 g of 1,8-diazabicyclo[5.4.0]undec-7-ene was added in portions below 40 °C. After the addition was complete, the reaction was carried out for 1-3 h, and the ion exchange resin was filtered off. 2 mL of dilute sulfuric acid was added to the reaction mixture and stirred for 1 hour. The mixture was then filtered, and the filtrate was added to 400 mL of aqueous methanol. The reaction mixture was stirred for 30 minutes and filtered to obtain a solid. The solid was washed three times thoroughly with pure water to obtain the diazonaquinone-type photosensitive compound (PAC-1). Finally, PAC-1 was dried in a vacuum oven at 35-40 °C to obtain the solid product. HPLC analysis showed that the effective content of the esterified compound was 99.2%.
[0048] The preparation method of Comparative Example 4 differs from that of Example 1 in that the ion exchange resin Amberlite IRA67 was not added, while other conditions remained unchanged. A solid product was obtained, and HPLC analysis showed that the effective content of the esterified compound was 99.2%.
[0049] The diazonoquinone-type photosensitive compounds obtained in Examples 1-5 and Comparative Examples 1-4 were tested. The main method for detecting ion content was ion chromatography. The detection results of chloride ions in the diazonoquinone-type photosensitive compounds are shown in Tables 1 and 2 below: Table 1. Ion concentrations in diazonoquinone-type photosensitive compounds from Examples 1-5 Table 2 Ion concentrations in diazonoquinone-type photosensitive compounds of Examples 1-3 and Comparative Examples 1-4 Example 1 uses a combination of ion exchange resin and basic compound, followed by acid washing with dilute sulfuric acid. Example 2 differs from Example 1 in that it uses other polyphenolic substances in the reaction. Example 3 uses dilute sulfuric acid and acidic ion exchange resin for acid washing. In Example 3, acidic ion exchange resin is added to neutralize the remaining alkali in the reaction and simultaneously remove residual chloride ions and other metal ions from the system. The addition of acid and acidic ion exchange resin can have a synergistic effect; the acid can not only neutralize the alkali but also reactivate some of the deactivated acidic ion exchange resin to continue working. Examples 4-5 change the ratio of ion exchange resin, diazonoquinone sulfonyl chloride, and basic compound. The chloride ion concentration in the resulting diazonoquinone-type photosensitive compound is much lower than that in the comparative examples, indicating that within the scope of protection of this application, changing the ratio can still effectively reduce the chloride ion concentration. Comparative Examples 1 and 2 do not use ion exchange resin and basic compound, Comparative Example 3 does not use basic compound, and Comparative Example 2 does not use ion exchange resin. The comparative examples show that the chloride ion concentration in the diazonaphthoquinone-type photosensitive compound prepared using ion exchange resin in the examples is significantly reduced. Furthermore, the addition of acidic ion exchange resin in Example 3 can further reduce the cation concentration in the reaction system. The results demonstrate that this synthesis process is not only simple and convenient, but also significantly reduces the chloride ions generated during the reaction, thus avoiding the impact of chloride ions on the dielectric properties, resolution, and film retention of the photoresist, as well as the corrosion of the metal substrate due to prolonged reaction time.
[0050] The high-purity diazonaphthoquinone (DNQ) type photosensitive compounds provided in Examples 1-5 above, the products in Comparative Examples 1-4, and commercially available 2,3,4,4'-tetrahydroxybenzophenone-2,1,5-diazonaphthoquinone sulfonate (PAC-6) were used as photosensitizers and mixed with polyimide resin, thermal crosslinking agent, adhesion promoter, and solvent to form a photosensitive polyimide photoresist solution. Based on 100 parts by weight of the photoresist solution, the solvent was 60 parts, the polyimide resin was 32 parts, the photosensitizer was 6 parts, the thermal crosslinking agent was 1.5 parts, and the adhesive was 0.5 parts. The solvent was N-methylpyrrolidone, the thermal crosslinking agent was a polyphenol compound, and the adhesion promoter was 3-aminopropyltriethoxysilane.
[0051] The resin is a type of polyimide resin, and its preparation reaction formula is shown below. The specific steps include: In a 250 mL round-bottom flask, 18.31 g of 6FAP was dissolved in 80 mL of NMP. While maintaining the flask at 0–5 °C, 15.51 g of ODPA was slowly added, and the mixture was stirred at 0–5 °C for 16 hours. After polymerization, 80 mL of NMP and 50 mL of toluene were added to the flask. The resulting polyamic acid was thermally imidized at 160 °C for 4–6 hours. Simultaneously, the water produced by the ring-closing reaction was separated as a toluene azeotrope. After the reaction was complete, the solution was slowly poured into an ethanol-water mixture to obtain a precipitate. The precipitate was filtered and washed three times with an aqueous ethanol solution. The solid was collected and dried in a vacuum oven at 40 °C for 48 hours to obtain solid PI.
[0052] 3.2 g of PI resin was dissolved in 6 g of N-methylpyrrolidone solution. 0.6 g of diazonoquinone-type photosensitive compound, 0.15 g of thermal crosslinking agent, and 0.05 g of binder were added to the above solution and stirred until dissolved. The resulting solution was then filtered through a 0.2 μm polytetrafluoroethylene filter to provide 11 different PSPI photoresist compositions: PSPI-1, PSPI-2, PSPI-3, PSPI-4, PSPI-5, PSPI-6, PSPI-7, PSPI-8, PSPI-9, PSPI-10, and PSPI-11.
[0053] The different PSPI photoresist solutions mentioned above were then subjected to photolithography using the following method: First, the PSPI photoresist solution was spin-coated onto a silicon wafer and pre-baked at 120 °C for 2 minutes to obtain a film approximately 3 μm thick. A photomask was then vacuum-pressed onto the coated silicon wafer, and the wafer was irradiated with filtered ultraviolet light at a wavelength of 365 nm emitted from a high-pressure mercury lamp. After exposure, it was developed with a 2.38 wt% tetramethylammonium hydroxide aqueous solution for 40 seconds. After rinsing with water for 60 seconds, it was post-baked at 170 °C and 220 °C for 30 minutes each to form the photoresist pattern. The photoresist pattern was inspected using a metallographic microscope to compare the resolution of the photoresist, with the minimum achievable linewidth as the standard. Film thickness was measured using a step meter. The metallographic microscopy test results of the PSPI-1 photoresist are shown below. Figure 2 Metallurgical microscopy test results of PSPI-7 photoresist are as follows: Figure 3 The resolution test results and film retention rates of different photoresist patterns are shown in Table 3.
[0054] Table 3. Resolution test results and film retention rate of photoresist patterns The photoresists in Examples 1-5 comprehensively outperformed those in Comparative Examples 1-2 and the commercially available PSPI-8. This demonstrates the significant advantages of the novel diazonaphthoquinone (DNQ)-type photosensitive compounds synthesized in these examples in improving photoresist resolution and lifespan (reflected in film retention). Example 1 performed best: its resolution (3.2 μm) was significantly higher than that of the commercially available PSPI-11 (6.1 μm), nearly doubling its performance. The comparative examples performed worst: Comparative Examples 1 and 2 exhibited the worst resolution, which is related to their synthesis route or product purity. This indicates that their photosensitive compounds had low photochemical reaction efficiency, resulting in insufficient dissolution contrast during exposure, leading to blurred edges and difficulty in resolving fine lines.
[0055] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
Claims
1. A method for preparing a diazonoquinone-type photosensitive compound, characterized in that, include: Diazonaphthoquinone sulfonyl chloride and phenolic compounds are mixed in an organic solvent, then added to an ion exchange resin and a basic compound to react and obtain a diazononaphthoquinone-type photosensitive compound.
2. The method for preparing the diazonoquinone-type photosensitive compound according to claim 1, characterized in that, The ion exchange resin is an alkaline ion exchange resin, and the alkaline ion exchange resin is at least one of Amberjet 4000CL, Amberjet 1200Na, Amberlite IRA67, Amberlite IRA96, Amberlite IRA401, Amberjet UP4000, Amberlyst A21, Amberlyst 15, Amberlite IRC50, Amberlite 719, Lanxess MonoPlus MP 64, Lanxess MonoPlus MP 68, Lanxess MonoPlus M500, Mitsubishi SA10ALLP, Mitsubishi WA30LL, Purolite A100, Purolite A105, Purolite A830, and Purolite A103 Plus.
3. The method for preparing the diazonoquinone-type photosensitive compound according to claim 1, characterized in that, The mass ratio of the amount of ion exchange resin to the amount of diazonaphthoquinone sulfonyl chloride is 1-4:
1.
4. The method for preparing the diazonoquinone-type photosensitive compound according to claim 1, characterized in that, The molar ratio of the amount of ion exchange resin to the amount of basic compound is 2-8:
1.
5. The method for preparing the diazonoquinone-type photosensitive compound according to claim 1, characterized in that, The alkaline compound is at least one of the following: triethylamine, 2-isopropylamine, tripropylamine, ethylenediamine, pyridine, 1,4-diazabicyclo[2.2.2]octane, 1,8-diazabicyclo[5.4.0]undec-7-ene, N,N-dimethylaniline, tetramethylammonium hydroxide, sodium methoxide, sodium ethoxide, lithium diisopropylamino, sodium carbonate, sodium bicarbonate, sodium hydroxide, potassium carbonate, potassium bicarbonate, potassium hydroxide, ammonium hydroxide, and sodium hydride.
6. The method for preparing the diazonoquinone-type photosensitive compound according to claim 1, characterized in that, After the reaction, the mixture is filtered. An acidic substance is added to the filtrate, and the mixture is stirred and filtered again. The filtrate obtained after the second filtration is added to a poor solvent for the diazononaphthoquinone type photosensitive compound, stirred, and filtered to obtain the diazononaphthoquinone type photosensitive compound. The acidic substance is at least one of organic acid, inorganic acid, and acidic ion exchange resin, and the unsuitable solvent is at least one of methanol, ethanol, isopropanol, and ultrapure water.
7. The method for preparing the diazonoquinone-type photosensitive compound according to claim 1, characterized in that, The reaction is carried out under an inert gas protective atmosphere, at a temperature of 10–60 °C, and for a time of 0.5–8 h.
8. The method for preparing the diazonoquinone-type photosensitive compound according to claim 1, characterized in that, The organic solvent is at least one of dichloromethane, tetrahydrofuran, 1,4-dioxane, γ-butyrolactone, γ-valerolactone, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, acetone, toluene, acetonitrile, methanol, and ethanol.
9. A diazononaphthoquinone-type photosensitive compound prepared by the method described in any one of claims 1-8.
10. The application of the diazonaphthoquinone type photosensitive compound of claim 9 in photoresist.