A silver-coated copper powder, its preparation method and application

By using amphiphilic block copolymers and polyethylene glycol succinate (VES) as dispersants, the silver ion addition rate was controlled, thus solving the inhomogeneity and safety hazards of silver-coated copper powder prepared by chemical plating and producing silver-coated copper powder with excellent antioxidant and electrical conductivity.

CN121732790BActive Publication Date: 2026-11-10HUNAN ZHONGWEI NEW SILVER MATERIAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202511849447.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-12-09
Publication Date
2026-11-10
Estimated Expiration
2045-12-09

AI Technical Summary

Technical Problem

Existing chemical plating methods for preparing silver-coated copper powder have problems such as localized aggregation of silver atoms, uneven silver plating, safety hazards, and poor oxidation resistance.

Method used

Using amphiphilic block copolymers and polyethylene glycol succinate (VES) as dispersants, and controlling the silver ion addition rate, silver was uniformly deposited on the surface of copper powder by chemical plating, thus preparing silver-coated copper powder with good oxidation resistance and low resistivity.

Benefits of technology

This method achieves uniform deposition of silver atoms on the surface of copper powder, improves the oxidation resistance and electrical conductivity of silver-coated copper powder, avoids the use of toxic reagents, and enhances safety and the uniformity of silver plating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

This invention discloses a silver-coated copper powder, its preparation method, and its applications, relating to the field of metal materials technology. The preparation method of the silver-coated copper powder includes the following steps: preparing a dispersion of copper powder, an amphiphilic block copolymer, polyethylene glycol succinate (VES), a reducing agent, and a complexing agent; adding a soluble silver ion solution to the dispersion; and reacting to obtain the silver-coated copper powder. The mass ratio of the amphiphilic block copolymer to VES is 1:(0.8-4.5); the addition rate of the soluble silver ions is 0.01 g / min-0.1 g / min. This preparation method can produce silver-coated copper powder with good antioxidant properties and low silver content.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metallic materials technology, and in particular to a silver-coated copper powder, its preparation method, and its application. Background Technology

[0002] Silver-coated copper powder combines the properties of copper and silver, possessing advantages such as high electrical conductivity, high thermal conductivity, and strong oxidation resistance, and is relatively inexpensive. Reported methods for preparing silver-coated copper powder include spray pyrolysis, electron beam radiation, vapor phase spark ablation, and chemical plating. Among these, chemical plating has advantages such as simple process and low cost compared to other methods. However, chemical plating for preparing silver-coated copper powder has the following problems: (1) The reduction rate of silver ions is fast, and silver atoms are prone to local aggregation on the surface of copper powder, forming a dotted, discontinuous, loose silver layer that cannot completely cover the surface of copper powder, resulting in a reduced coating rate and decreased oxidation resistance of the silver-coated copper powder. (2) In the liquid-phase reaction system, copper powder is prone to agglomeration due to its high surface energy, forming tiny gaps. The dispersant is unevenly distributed, and the silver plating rate varies at different locations on the surface of the copper powder aggregates, resulting in uneven silver plating. (3) To improve dispersibility and silver plating uniformity, some processes use organic solvents such as ethylene glycol and oleylamine, which pose safety hazards such as flammability and high volatility. Therefore, there is a need to provide a method for preparing silver-coated copper powder with high safety, good oxidation resistance and low resistivity through chemical plating. Summary of the Invention

[0003] The present invention aims to at least solve one of the technical problems existing in the prior art. To this end, the present invention proposes a method for preparing silver-coated copper powder.

[0004] The present invention also provides silver-coated copper powder prepared by the above preparation method.

[0005] The present invention also provides applications of the above-mentioned silver-coated copper powder.

[0006] A method for preparing silver-coated copper powder according to a first aspect of the present invention includes the following steps: A dispersion of copper powder, amphiphilic block copolymer, vitamin E succinate polyethylene glycol (TPGS), reducing agent, and complexing agent is prepared. A soluble silver ion solution is added to the dispersion, and the reaction is carried out to obtain the silver-coated copper powder. The mass ratio of the amphiphilic block copolymer to the vitamin E succinate polyethylene glycol ester is 1:(0.8-4.5). The addition rate of the soluble silver ions is 0.01 g / min to 0.1 g / min.

[0007] The preparation method according to embodiments of the present invention has at least the following beneficial effects: This preparation method is simple, mild, and does not require the use of toxic reagents, making it highly safe. Silver atoms are uniformly deposited on the surface of copper powder, resulting in silver-coated copper powder with good oxidation resistance and low resistivity.

[0008] According to some embodiments of the present invention, the mass ratio of the amphiphilic block copolymer to polyethylene glycol succinate is 1:(0.8-4.5). For example, it can be 1:0.8, 1:1, 1:1.2, 1:1.4, 1:1.6, 1:1.8, 1:2, 1:2.2, 1:2.4, 1:2.6, 1:2.8, 1:3, 1:3.2, 1:3.4, 1:3.6, 1:3.8, 1:4, 1:4.2, 1:4.4, or 1:4.5.

[0009] According to some embodiments of the present invention, the total mass of the amphiphilic block copolymer and the polyethylene glycol succinate (VES) is 1.5 wt%-5 wt% of the copper powder. For example, it can be 1.5 wt%, 1.6 wt%, 1.7 wt%, 1.8 wt%, 1.9 wt%, 2 wt%, 2.1 wt%, 2.2 wt%, 2.3 wt%, 2.4 wt%, 2.5 wt%, 2.6 wt%, 2.7 wt%, 2.8 wt%, 2.9 wt%, 3 wt%, 3.1 wt%, 3.2 wt%, 3.3 wt%, 3.4 wt%, 3.5 wt%, 3.6 wt%, 3.7 wt%, 3.8 wt%, 3.9 wt%, 4 wt%, 4.1 wt%, 4.2 wt%, 4.3 wt%, 4.4 wt%, 4.5 wt%, 4.6 wt%, 47 wt%, 4.8 wt%, 4.9 wt%, or 5 wt%.

[0010] According to some embodiments of the present invention, the amphiphilic block copolymer includes polyethylene glycol-polycaprolactone block copolymer and polyethylene oxide. At least one of the polyaspartic acid block copolymers.

[0011] According to some embodiments of the present invention, the concentration of copper powder in the dispersion is 5wt%-15wt%. For example, it can be 5wt%, 5.5wt%, 6wt%, 6.5wt%, 7wt%, 7.5wt%, 8wt%, 8.5wt%, 9wt%, 9.5wt%, 10wt%, 10.5wt%, 11wt%, 11.5wt%, 12wt%, 12.5wt%, 13wt%, 13.5wt%, 14wt%, 14.5wt%, or 15wt%.

[0012] According to some embodiments of the present invention, the particle size of the copper powder is 2 μm-10 μm. For example, it can be 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm, 9.5 μm, or 10 μm.

[0013] According to some embodiments of the present invention, the copper powder is copper powder that has undergone deoxidation treatment.

[0014] According to some embodiments of the present invention, the deoxidation treatment includes the following steps: The copper powder was treated in a dilute acid solution and then washed.

[0015] According to some embodiments of the present invention, the dilute acid solution includes, but is not limited to, dilute nitric acid aqueous solution, dilute sulfuric acid aqueous solution, or dilute acetic acid aqueous solution.

[0016] According to some embodiments of the present invention, the acid concentration in the dilute acid solution is 2 (v / v)%-15 (v / v)%. For example: it can be 2(v / v)%, 2.5(v / v)%, 3(v / v)%, 3.5(v / v)%, 4(v / v)%, 4.5(v / v)%, 5(v / v)%, 5.5(v / v)%, 6(v / v)%, 6.5(v / v)%, 7(v / v)%, 7.5(v / v)%, 8(v / v)%, 8.5(v / v )%, 9(v / v)%, 9.5(v / v)%, 10(v / v)%, 10.5(v / v)%, 11(v / v)%, 11.5(v / v)%, 12(v / v)%, 12.5(v / v)%, 13(v / v)%, 13.5(v / v)%, 14(v / v)%, 14.5(v / v)% or 15(v / v)%.

[0017] According to some embodiments of the present invention, the deoxidation treatment time is 10 min to 30 min. For example, it can be 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, 16 min, 17 min, 18 min, 19 min, 20 min, 21 min, 22 min, 23 min, 24 min, 25 min, 26 min, 27 min, 28 min, 29 min, or 30 min.

[0018] According to some embodiments of the present invention, the deoxidation treatment is an ultrasonic treatment. The power of the ultrasonic treatment is 50 W-80 W. For example, it can be 50 W, 51 W, 52 W, 53 W, 54 W, 55 W, 56 W, 57 W, 58 W, 59 W, 60 W, 61 W, 62 W, ​​63 W, 64 W, 65 W, 66 W, 67 W, 68 W, 69 W, 70 W, 71 W, 72 W, 73 W, 74 W, 75 W, 76 W, 77 W, 78 W, 79 W, or 80 W.

[0019] According to some embodiments of the present invention, the deoxidation treatment is carried out under stirring. The stirring speed is 250 rpm to 600 rpm. For example: it can be 250 rpm, 260 rpm, 270 rpm, 280 rpm, 290 rpm, 300 rpm, 310 rpm, 320 rpm, 330 rpm, 340 rpm, 350 rpm, 360 rpm, 370 rpm, 380 rpm, 390 rpm, 400 rpm, 410 rpm, 420 rpm, 430 rpm, 440 rpm, 450 rpm, 460 rpm, 470 rpm, 480 rpm, 490 rpm, 500 rpm, 510 rpm, 520 rpm, 530 rpm, 540 rpm, 550 rpm, 560 rpm, 570 rpm, 580 rpm, 590 rpm or 600 rpm.

[0020] According to some embodiments of the present invention, the reducing agent includes at least one of ascorbic acid, glucose, and glutamic acid.

[0021] According to some embodiments of the present invention, the concentration of the reducing agent in the dispersion is 0.5wt%-8wt%. For example, it can be 0.5wt%, 0.6wt%, 0.8wt%, 1wt%, 1.2wt%, 1.4wt%, 1.6wt%, 1.8wt%, 2wt%, 2.2wt%, 2.4wt%, 2.6wt%, 2.8wt%, 3wt%, 3.2wt%, 3.4wt%, 3.6wt%, 3.8wt%, 4wt%, 4.2wt%, 4.4wt%, 4.6wt%, 4.8wt%, 5wt%, 5.2wt%, 5.4wt%, 5.6wt%, 5.8wt%, 6wt%, 6.2wt%, 6.4wt%, 6.6wt%, 6.8wt%, 7wt%, 7.2wt%, 7.4wt%, 7.6wt%, 7.8wt%, or 8wt%.

[0022] According to some embodiments of the present invention, the complexing agent includes at least one of EDTA-2Na, ethylenediamine, and ammonia.

[0023] According to some embodiments of the present invention, the concentration of the complexing agent in the dispersion is 0.5wt%-5wt%. For example, it can be 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt%, 1.6wt%, 1.7wt%, 1.8wt%, 1.9wt%, 2wt%, 2.2wt%, 2.4wt%, 2.6wt%, 2.8wt%, 3wt%, 3.2wt%, 3.4wt%, 3.6wt%, 3.8wt%, 4wt%, 4.2wt%, 4.4wt%, 4.6wt%, 4.8wt%, or 5wt%.

[0024] According to some embodiments of the present invention, the solvent of the dispersion is water.

[0025] According to some embodiments of the present invention, the concentration of soluble silver ions in the soluble silver ion solution is 0.1 g / mL to 1 g / mL. For example, it can be 0.1 g / mL, 0.15 g / mL, 0.2 g / mL, 0.25 g / mL, 0.3 g / mL, 0.35 g / mL, 0.4 g / mL, 0.45 g / mL, 0.5 g / mL, 0.55 g / mL, 0.6 g / mL, 0.65 g / mL, 0.7 g / mL, 0.75 g / mL, 0.8 g / mL, 0.85 g / mL, 0.9 g / mL, 0.95 g / mL, or 1 g / mL. The balance of the soluble silver ion solution is water.

[0026] According to some embodiments of the present invention, the sources of the soluble silver ions include, but are not limited to, silver nitrate, silver sulfate, or silver ammonia.

[0027] According to some embodiments of the present invention, the addition rate of the soluble silver ions is 0.01 g / min to 0.1 g / min. For example, it can be 0.01 g / min, 0.015 g / min, 0.02 g / min, 0.025 g / min, 0.03 g / min, 0.035 g / min, 0.04 g / min, 0.045 g / min, 0.05 g / min, 0.055 g / min, 0.06 g / min, 0.065 g / min, 0.07 g / min, 0.075 g / min, 0.08 g / min, 0.085 g / min, 0.09 g / min, 0.095 g / min, or 0.1 g / min.

[0028] According to some embodiments of the present invention, the molar ratio of the soluble silver ions to the reducing agent is (1-2):1. For example, it can be 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, or 2:1.

[0029] According to some embodiments of the present invention, the amount of soluble silver ions added is 30wt%-60wt% of the copper powder. For example, it can be 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wt%, 36wt%, 37wt%, 38wt%, 39wt%, 40wt%, 41wt%, 42wt%, 43wt%, 44wt%, 45wt%, 46wt%, 47wt%, 48wt%, 49wt%, 50wt%, 51wt%, 52wt%, 53wt%, 54wt%, 55wt%, 56wt%, 57wt%, 58wt%, 59wt%, or 60wt%.

[0030] According to some embodiments of the present invention, the reaction temperature is 20°C-30°C. For example, it can be 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, or 30°C.

[0031] According to some embodiments of the present invention, the reaction time after adding the soluble silver ion solution is 30 min to 60 min. For example, it can be 30 min, 31 min, 32 min, 33 min, 34 min, 35 min, 36 min, 37 min, 38 min, 39 min, 40 min, 41 min, 42 min, 43 min, 44 min, 45 min, 46 min, 57 min, 48 min, 49 min, 50 min, 51 min, 52 min, 53 min, 54 min, 55 min, 56 min, 57 min, 58 min, 59 min, or 60 min.

[0032] According to some embodiments of the present invention, the preparation method further includes post-reaction treatment. The post-reaction treatment includes filtration, washing, and drying.

[0033] A silver-coated copper powder according to a second aspect of the present invention is prepared by the preparation method described in the first aspect embodiment.

[0034] The application of silver-coated copper powder as described in the second aspect embodiment of the present invention in conductive paste.

[0035] Other features and advantages of the invention will be set forth in the description which follows, and will be apparent in part from the description, or may be learned by practicing the invention. Attached Figure Description

[0036] Figure 1 This is a scanning electron microscope image of the silver-coated copper powder prepared in Example 1 of the present invention; Figure 2 This is a scanning electron microscope image of the silver-coated copper powder obtained in Example 2 of the present invention; Figure 3 This is a scanning electron microscope image of the silver-coated copper powder prepared in Comparative Example 1 of this invention. Figure 4 This is a scanning electron microscope image of the silver-coated copper powder prepared in Comparative Example 2 of this invention; Figure 5 This is a scanning electron microscope image of the silver-coated copper powder prepared in Comparative Example 3 of this invention; Figure 6 This is a scanning electron microscope image of the silver-coated copper powder prepared in Comparative Example 4 of this invention. Figure 7 This is a scanning electron microscope image of the silver-coated copper powder prepared in Comparative Example 5 of this invention; Figure 8 This is a scanning electron microscope image of the silver-coated copper powder prepared in Comparative Example 6 of this invention. Detailed Implementation

[0037] The following will describe the concept and technical effects of the present invention clearly and completely with reference to embodiments, so as to fully understand the purpose, features and effects of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are all within the scope of protection of the present invention.

[0038] Unless otherwise specified in the examples, the procedures should be performed under standard conditions or conditions recommended by the manufacturer. Reagents or instruments whose manufacturers are not specified are all commercially available products.

[0039] When a numerical range is disclosed herein, the range is considered continuous and includes the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values ​​of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.

[0040] "And / or" is used to indicate that one or both of the described situations may occur, for example, A and / or B includes (A and B) and (A or B).

[0041] Unless otherwise specified, "about" in this invention means that the allowable error is within ±2%.

[0042] Unless otherwise specified, "room temperature" in this invention means (25±5)℃.

[0043] Example 1 This example provides a method for preparing silver-coated copper powder, the steps of which are as follows: S1, 10 g of particles with a diameter (D) 50 Copper powder with a particle size of 4 μm was placed in an 8 (v / v)% sulfuric acid aqueous solution and ultrasonically treated for 40 min at a rotation speed of 300 rpm and an ultrasonic power of 80 W. After washing with deionized water until the pH was neutral, wet copper powder with a water content of about 12% was obtained by pressure filtration.

[0044] S2. At room temperature, the above wet copper powder, 100 g deionized water, 0.05 g polyethylene glycol-polycaprolactone block copolymer, 0.2 g TPGS, 3.7 g ascorbic acid, and 1.5 g EDTA-2Na were ultrasonically dispersed to obtain a dispersion. 10 mL of 0.52 g / mL silver nitrate aqueous solution was added dropwise to the dispersion at a dropping rate of 0.06 mL / min. After the addition was completed, the mixture was stirred for another 45 min (stirring speed 300 rpm), filtered, washed with deionized water, and dried to obtain silver-coated copper powder.

[0045] Example 2 This example provides a method for preparing silver-coated copper powder, the steps of which are as follows: S1, 10 g of particles with a diameter (D) 50 Copper powder with a particle size of 4 μm was placed in a 4 (v / v)% sulfuric acid aqueous solution and ultrasonically treated for 70 min at a rotation speed of 500 rpm and an ultrasonic power of 50 W. After washing with deionized water until the pH was neutral, wet copper powder with a water content of about 13% was obtained by pressure filtration.

[0046] S2. At room temperature, the above wet copper powder, 100 g deionized water, 0.1 g polyethylene glycol-polycaprolactone block copolymer, 0.3 g TPGS, 5 g ascorbic acid, and 1.5 g EDTA-2Na were ultrasonically dispersed to obtain a dispersion. 10 mL of 0.69 g / mL silver nitrate aqueous solution was added dropwise to the dispersion at a dropping rate of 0.08 mL / min. After the addition was completed, the mixture was stirred for another 45 min (stirring speed 300 rpm), filtered, washed with deionized water, and dried to obtain silver-coated copper powder.

[0047] Example 3 This example provides a method for preparing silver-coated copper powder, the steps of which are as follows: S1, 10 g of particles with a diameter (D) 50 Copper powder with a particle size of 2 μm was placed in a 12 (v / v)% sulfuric acid aqueous solution and ultrasonically treated for 50 min at a rotation speed of 600 rpm and an ultrasonic power of 50 W. After washing with deionized water until the pH was neutral, wet copper powder with a water content of about 11% was obtained by pressure filtration.

[0048] S2. At room temperature, mix the above-mentioned wet copper powder, 100 g of deionized water, and 0.1 g of polyethylene oxide. Polyaspartic acid block copolymer, 0.1 g TPGS, 6.2 g ascorbic acid, and 1.5 g EDTA-2Na were ultrasonically dispersed to obtain a dispersion. 10 mL of 0.86 g / mL silver nitrate aqueous solution was added dropwise to the dispersion at a dropping rate of 0.1 mL / min. After the addition was complete, the mixture was stirred for another 45 min (stirring speed 300 rpm), filtered, washed with deionized water, and dried to obtain silver-coated copper powder.

[0049] Comparative Example 1 This example provides a method for preparing silver-coated copper powder, which is basically the same as that in Example 1, except that TPGS is replaced with an equal mass of Tween-80.

[0050] Comparative Example 2 This example provides a method for preparing silver-coated copper powder, which is basically the same as that in Example 1, except that the polyethylene glycol-polycaprolactone block copolymer is replaced with an equal mass of sodium dodecylbenzenesulfonate.

[0051] Comparative Example 3 This example provides a method for preparing silver-coated copper powder, which is basically the same as that in Example 1, except that the polyethylene glycol-polycaprolactone block copolymer and TPGS are omitted in the default step S2.

[0052] Comparative Example 4 This example provides a method for preparing silver-coated copper powder, which is basically the same as that in Example 1, except that the amount of polyethylene glycol-polycaprolactone block copolymer is adjusted from 0.05 g to 0.3 g.

[0053] Comparative Example 5 This example provides a method for preparing silver-coated copper powder, which is basically the same as that in Example 1, except that the amount of polyethylene glycol-polycaprolactone block copolymer is adjusted from 0.05 g to 0.15 g and the amount of TPGS is adjusted from 0.2 g to 0.6 g.

[0054] Comparative Example 6 This example provides a method for preparing silver-coated copper powder, which is basically the same as that in Example 1, except that the dropping rate of the silver nitrate aqueous solution in step S2 is adjusted from 0.06 mL / min to 0.6 mL / min.

[0055] Detection example (1) The silver-coated copper powders prepared in Examples 1-3 and Comparative Examples 1-6 were characterized by scanning electron microscopy and the particle size was tested.

[0056] (2) Acid resistance time: 5 g of the silver-coated copper powder prepared in Examples 1-3 and Comparative Examples 1-6 were placed in 30 g of acetic acid solution (10 wt% water, 90 wt% acetic acid), stirred thoroughly for 30 s, and the color change time of the supernatant was observed.

[0057] The results are shown in Table 1 and Figures 1-8 As shown.

[0058] Table 1

[0059] In the preparation methods of Examples 1-3, the polyethylene glycol succinate and the amphiphilic block copolymer provide a significant steric hindrance effect and a stable interfacial environment, which helps to promote copper powder dispersion and reduce particle aggregation. Combined with an appropriate silver ion droplet acceleration rate, this improves the uniform adsorption and deposition of elemental silver on the copper powder surface. Substituting, omitting, or overusing either the polyethylene glycol succinate or the amphiphilic block copolymer, or using silver ions at an excessively high addition rate, will significantly degrade the coating effect and electrical properties of the silver-coated copper powder.

[0060] The embodiments of the present invention have been described in detail above with reference to the examples. However, the present invention is not limited to the above embodiments. Within the scope of knowledge possessed by those skilled in the art, various changes can be made without departing from the spirit of the present invention.

Claims

1. A method for preparing silver-coated copper powder, characterized in that, Includes the following steps: A dispersion of copper powder, an amphiphilic block copolymer, polyethylene glycol succinate containing vitamin E, a reducing agent, and a complexing agent is prepared. A soluble silver ion solution is added to the dispersion, and the mixture is reacted to obtain the silver-coated copper powder. The reducing agent includes at least one of ascorbic acid, glucose, and glutamic acid. The total mass of the amphiphilic block copolymer and polyethylene glycol succinate containing vitamin E is 1.5 wt%-5 wt% of the copper powder. The mass ratio of the amphiphilic block copolymer to the vitamin E succinate polyethylene glycol ester is 1:(0.8-4.5). The addition rate of the soluble silver ions is 0.01 g / min to 0.1 g / min.

2. The preparation method according to claim 1, characterized in that, The amphiphilic block copolymer includes polyethylene glycol-polycaprolactone block copolymer and polyethylene oxide. At least one of the polyaspartic acid block copolymers.

3. The preparation method according to claim 1, characterized in that, The concentration of the reducing agent in the dispersion is 0.5wt%-8wt%.

4. The preparation method according to claim 1, characterized in that, The complexing agent includes at least one of EDTA-2Na, ethylenediamine, and ammonia water; and / or, the concentration of the complexing agent in the dispersion is 0.5wt%-5wt%.

5. The preparation method according to claim 1, characterized in that, The concentration of soluble silver ions in the soluble silver ion solution is 0.1 g / mL to 1 g / mL; and / or, the molar ratio of the soluble silver ions to the reducing agent is (1-2):

1.

6. The preparation method according to claim 1, characterized in that, The sources of the soluble silver ions include at least one of silver nitrate, silver sulfate, and silver ammonia.

7. The preparation method according to claim 1, characterized in that, The reaction temperature is 20℃-30℃.

8. A silver-coated copper powder, characterized in that, The silver-coated copper powder is prepared by the preparation method according to any one of claims 1 to 7.

9. The application of the silver-coated copper powder according to claim 8 in conductive paste.

Citation Information

Patent Citations

  • Silver-coated copper powder with low-temperature sintering activity as well as preparation method and application of silver-coated copper powder

    CN119870490A

  • Preparation method of silver-coated copper composite powder with high oxidation resistance

    CN120696413A