Through the optimization of composite adsorption materials and processes, the deep removal and resource utilization of fluorine in the wet zinc smelting process has been achieved, solving the problem of fluorine circulation and enrichment within the system, generating high-purity calcium fluoride products, ensuring stable system operation and reducing costs.
Patent Information
- Application Number
- CN202610048728.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-01-15
- Publication Date
- 2026-04-21
AI Technical Summary
Existing technologies make it difficult to achieve deep removal and resource recovery of fluorine in the hydrometallurgical zinc smelting process, resulting in the accumulation of fluorine in the system, which corrodes equipment and threatens the stable operation of the system, while also posing resource waste and environmental risks.
Targeted adsorption and fluoride removal using composite adsorption materials, combined with efficient desorption and material regeneration, generates high-purity calcium fluoride precipitate through multi-stage countercurrent contact and gentle desorption, realizing a closed-loop resource recycling of fluorine.
It achieves deep fluoride removal (F-<50mg/L), high selectivity (Zn loss <1.0%) and long material life, producing high-purity calcium fluoride products, reducing operating costs and hazardous waste generation, and ensuring stable system operation.
Smart Images

Figure CN121894743A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the fields of non-ferrous metal hydrometallurgy, environmental functional materials, and secondary resource recycling. Specifically, it provides a method for deep defluorination and fluorine resource recovery of electrolytic zinc leaching solutions based on innovative adsorption materials and process design. This method is used for the efficient and deep removal of fluoride ions from leaching solutions in electrolytic zinc production systems and the simultaneous high-value recovery of fluorine. Background Technology
[0002] In the hydrometallurgical zinc smelting process, fluoride from the raw materials enters the solution system during the leaching process. Fluoride ions are one of the harmful impurities in zinc electrolysis. When their concentration exceeds 100 mg / L, they severely corrode the cathode plate, destroy its surface passivation film, leading to difficulties in peeling off deposited zinc, decreased current efficiency, and a sharp increase in cathode plate consumption. Furthermore, fluoride ions accelerate the corrosion of pumps, pipelines, valves, and other equipment, threatening the long-term stable operation of the system. Therefore, deep defluorination is a crucial step in ensuring the efficient, economical, and safe operation of hydrometallurgical zinc smelting.
[0003] Currently, commonly used industrial defluorination methods mainly include lime precipitation and rare earth adsorption precipitation. Lime precipitation is simple to operate, but the resulting calcium fluoride precipitate particles are fine, have high water content, and are heavily contaminated with zinc, forming hazardous sludge that is difficult to dispose of. Furthermore, the fluoride is not utilized, resulting in resource waste and secondary environmental risks. Rare earth adsorption precipitation has higher defluorination efficiency, but the resulting defluorination slag is rich in zinc and usually needs to be returned to the pyrometallurgical system for treatment. During this process, fluoride re-evaporates at high temperatures and returns to the wet process with the flue gas purification system, causing fluoride to continuously circulate and accumulate throughout the "wet-pyrometallurgical" system, failing to fundamentally "open the loop."
[0004] In recent years, while research on various adsorbent materials (such as activated alumina, bone char, and certain modified resins) has made progress, they generally suffer from problems such as low adsorption capacity, poor selectivity (easily adsorbing zinc leading to metal loss), difficult regeneration, complex regeneration solution treatment, or inability to adapt to the low pH, high salt, and high impurity environment of hydrometallurgical zinc refining systems. There is a lack of a method that can simultaneously meet the requirements of deep defluorination (F... - A feasible technology that achieves concentrations of <50 mg / L, high selectivity (extremely low zinc loss), long adsorbent lifespan, and ultimately, stable separation of fluorine from the production system in the form of a high-value product.
[0005] Therefore, developing a novel adsorption material and a matching process to completely solve the "open circuit" problem of fluorine and realize the resource utilization of fluorine is of great significance and an urgent industrial need for promoting technological progress, resource recycling and green development in the hydrometallurgical zinc industry. Summary of the Invention
[0006] The purpose of this invention is to overcome the shortcomings of existing technologies and provide a highly efficient, stable, economical, and environmentally friendly method for deep defluorination and fluorine resource recovery from electrolytic zinc leaching solutions. This method not only pursues deep fluorine removal but also, through material innovation and process optimization, forms a complete resource recovery chain for fluorine, encompassing "adsorption and enrichment - desorption and transfer - precipitation and recovery," thereby achieving permanent fluorine recovery and value enhancement.
[0007] The technical solution of this invention is achieved as follows: a method for deep defluorination and fluorine resource recovery of electrolytic zinc leaching solution, the process comprising the following steps: (1) Targeted adsorption for fluoride removal: Electrolytic zinc leaching solution with a pH of 2.0-4.5 is subjected to at least two stages of countercurrent contact adsorption with a composite adsorbent material at 20-50°C. The composite adsorbent material is effective against fluoride ions (F... - The adsorption capacity is ≥40mg / g, and the concentration of fluoride ions in the liquid after adsorption is stably reduced to below 50mg / L; (2) High-efficiency desorption and material regeneration: The composite adsorbent material saturated by adsorption in step (1) is desorbed by sodium hydroxide solution with a concentration of 0.5-2.0 mol / L at 30-60℃ to obtain a high-concentration sodium fluoride desorption solution. The desorbed composite adsorbent material is treated with a specific regeneration solution and its adsorption performance recovery rate is ≥95%, and it is returned to step (1) for recycling. (3) Closed-loop precipitation and fluorine resource utilization: The high-concentration sodium fluoride desorption solution obtained in step (2) is mixed with lime milk at a calcium-fluoride molar ratio of 1.0-1.2:1 and subjected to causticization precipitation reaction at 40-80℃ to generate high-purity calcium fluoride precipitate. After filtration, washing and drying, the precipitate is used to obtain pure calcium fluoride product. The precipitate liquid is returned to step (2) for recycling as regenerated alkali liquid, realizing the closed loop within the alkali medium system. Preferably, the composite adsorbent material in step (1) includes one or more of modified salt-based activated carbon, metal-based ion exchange resin, and magnetic nano-iron composite adsorbent; Preferably, in the modified salt-based activated carbon, the active metal component exists in a highly dispersed crystalline form on the surface and inside the pores of the activated carbon, and its metal oxide loading is 5-20 wt%. Preferably, the metal-based ion exchange resin has an exchange capacity ≥ 2.0 mmol F. - / g, and its adsorption performance for fluoride ions remains stable in the pH range of 2.0-5.0; Preferably, the magnetic nano-iron composite adsorbent has an average particle size of 20-80 nm, and can achieve rapid solid-liquid separation within 5 minutes by applying an external magnetic field; Preferably, the adsorption process in step (1) is achieved using a 2-4 stage countercurrent adsorption tower or a series stirred tank, with a total contact time of 30-90 minutes and a zinc loss rate of <1.0% during the adsorption stage; Preferably, in step (2), the specific regeneration solution used is a modified salt-based activated carbon as the composite adsorbent and a 0.05-0.2 mol / L dilute hydrochloric acid or dilute sulfuric acid solution as the regeneration solution; or a metal-based ion exchange resin as the composite adsorbent and a 0.1-0.5 mol / L mixed solution of NaOH and NaCl as the regeneration solution; or a magnetic nano-iron composite adsorbent and a 0.5-1.0 mol / L NaOH solution as the regeneration solution. Preferably, the causticization precipitation reaction in step (3) is carried out in a reaction vessel, the pH at the reaction endpoint is controlled at 8.0-10.0, the reaction time is 60-120 minutes, and the calcium fluoride precipitate has high crystallinity and is easy to filter and wash. Preferably, the modified salt-based activated carbon is made of ≥1200m 2 Using high specific surface area activated carbon as a carrier, nano-scale alkaline earth metal / rare earth metal oxide active sites are loaded through in-situ precipitation-atmosphere calcination technology to form a composite material with hierarchical pore structure and strong fluoride ion coordination ability; the metal-based ion exchange resin is based on polymer or inorganic silica gel as a framework, and metal-organic elements with clear fluoride ion recognition function are grafted through coordination bonds to form an adsorption resin with both ion exchange and specific complexation capabilities; the magnetic nano-iron composite adsorbent is based on magnetic Fe3O4 nanoparticles as the core, and is coated and functionalized with a hydrated lanthanum oxide shell to form a core-shell structure, a nanocomposite material with both high adsorption capacity and magnetic separation characteristics.
[0008] The core innovation of this invention lies in: Innovation in Adsorption Materials: Moving beyond traditional single adsorption methods, a series of high-performance composite adsorption materials with multiple functions including physical adsorption, chemical coordination, and ion exchange have been prepared. These materials possess precise selectivity, achieved through optimization of the active sites on the material surface, enabling them to adsorb large amounts of Zn. 2+ Mg 2+ Ca 2+ Even with the coexistence of cations, it still affects F. - It exhibits extremely high binding capacity and adsorption capacity. Through the hierarchical pores or core-shell structure of the material, it provides abundant mass transfer channels and a huge specific surface area, ensuring an adsorption capacity of over 40 mg / g and a rapid adsorption rate. It also demonstrates excellent cycle stability and easy separation. The material structure is robust, and its performance decays very little after several adsorption-desorption cycles. The solid-liquid separation process is energy-efficient and has low energy consumption.
[0009] The optimized and innovative process system organically couples three units: "multi-stage countercurrent adsorption," "high-efficiency and mild desorption," and "precipitation and crystallization resource utilization," forming a closed-loop process system. Multi-stage countercurrent adsorption maximizes adsorbent utilization, ensuring stable and compliant effluent quality. High-efficiency and mild desorption achieves complete fluoride desorption using low-concentration alkaline solutions, resulting in a high fluoride concentration in the desorbent, creating favorable conditions for subsequent precipitation. A proprietary regeneration process ensures the long-term effectiveness of the adsorbent. Closed-loop precipitation and resource utilization involves reacting the high-concentration fluoride desorbent with lime slurry to generate easily filterable high-purity calcium fluoride, achieving fluoride solidification and commercialization. The mother liquor (NaOH solution) is returned to the desorption process, achieving zero-discharge recycling of the alkaline medium.
[0010] The method described in this invention has the following significant beneficial effects: (1) Solving the problem of fluorine open circuit: For the first time, fluorine is permanently separated in the form of solid calcium fluoride in the hydrometallurgical zinc smelting process, eliminating the risk of systemic cyclic enrichment of fluorine.
[0011] (2) Leading technical indicators: Defluorination depth (F - Key indicators such as adsorption capacity (≥40mg / g), selectivity (Zn loss <1.0%), and material cycle life are significantly superior to existing technologies.
[0012] (3) Outstanding resource utilization benefits: turning waste into treasure, producing high-purity calcium fluoride, creating direct economic benefits; at the same time, the closed-loop circulation of alkaline media greatly reduces operating costs.
[0013] (4) Environmentally friendly: No new hazardous waste or wastewater is generated throughout the entire process, achieving clean production.
[0014] (5) Broad prospects for industrialization: The process is modular, can be flexibly embedded into existing production lines, has low modification difficulty, and is stable and reliable in operation. Attached Figure Description
[0015] Figure 1 This is a process flow diagram of the present invention. Detailed Implementation Example 1:
[0016] Raw material: Neutral leaching supernatant from a zinc smelter, F - Concentration 200 mg / L, Zn 2+ Concentration 55 g / L, pH 4.0; Material: Modified basic (magnesium-lanthanum) activated carbon with a specific surface area of 1150 m² 2 / g, with MgO and La2O3 loadings of 8wt% and 5wt%, respectively; Adsorption: Carried out in a three-stage countercurrent fixed adsorption column, operated at room temperature, with an average effluent F -The concentration remained stable at 28 mg / L, with a zinc loss rate of <0.8%. Desorption and regeneration: The saturated adsorption column was desorbed with 1.0 mol / L NaOH. The average F of the desorption solution was... - The concentration reached 8.2 g / L; After desorption, the adsorption capacity was regenerated by washing with 50 mL of 0.1 mol / L H₂SO₄, and the adsorption capacity recovery rate was 99.5%. Fluorine precipitation: Take the desorption solution, add 1.1 times the theoretical amount of lime milk, stir at 60℃ for 90 min, filter and dry to obtain CaF2, with a chemical analysis purity of 95.2%. Example 2:
[0017] Raw material: Circulating electrolyte from a zinc smelter, F - Concentration 176 mg / L, Zn 2+ Concentration 120 g / L, H2SO4 concentration 160 g / L; Material: Core-shell type M@Fe3O4 magnetic nanocomposite material, with an average particle size of 50 nm; Adsorption: Batch adsorption was carried out in a stirred tank at a dosage of 2 g / L. The pH was adjusted to 3.0, and the reaction was carried out at 30°C for 40 min to achieve solid-liquid separation. The effluent was F. - The zinc concentration was reduced to 15 mg / L, with a zinc loss rate of 0.45%.
[0018] Desorption and regeneration: The magnetic material was desorbed using 1.5 mol / L NaOH at 50℃ for 30 min. Esorption solution F - Concentration 12.5 g / L. The material was washed with deionized water and then reused directly.
[0019] Fluorine precipitation: The desorption solution reacts with lime milk to obtain CaF2 with a purity of 96.05%.
[0020] Example 3: Raw material: Neutral leachate from a zinc smelter, F - Concentration 185 mg / L, Zn 2+ Concentration 85 g / L, pH 3.8, contains trace amounts of Mg 2+ Ca 2+ Impurity ions, etc.
[0021] Materials: A metal-based ion exchange resin (FJR-01) was used, with cross-linked polystyrene as the backbone and R-group organic functional groups grafted onto the surface. The exchange capacity was 2.3 mmol F. - / g, with a particle size range of 0.4–0.6 mm, and stable adsorption performance for fluoride ions in the pH range of 2.0–5.0.
[0022] Adsorption: The adsorption was carried out in a two-stage series fixed-bed adsorption column with a resin packing volume of 2 L, a feed flow rate of 4 BV / h, and an operating temperature of 35 °C. After 120 hours of continuous operation, the average effluent F... - The concentration was stable at 32 mg / L, and the zinc loss rate was <0.5%.
[0023] Desorption and regeneration: The adsorption-saturated resin was dynamically desorbed using a 0.3 mol / L NaOH solution at a flow rate of 2 BV / h and a temperature of 45℃. The average F of the desorbed solution was... - The concentration reached 7.8 g / L, and the desorption rate reached 98.2%. After static soaking in the same regeneration solution for 2 hours, it can be directly returned to the adsorption process for recycling.
[0024] Fluorine precipitation: Take 1 L of the above desorption solution and add lime milk at a calcium-to-fluorine molar ratio of 1.1:1. React at 70°C with stirring for 100 min, with the final pH being 9.2. After the reaction is complete, perform solid-liquid separation and dry at 105°C to obtain a white powdered calcium fluoride product with a purity of 95.82%.
[0025] In summary, the embodiments of the present invention demonstrate that, in a complex and realistic zinc smelting solution environment, by optimizing materials and processes, highly efficient and deep removal and resource recovery of fluorine are achieved, with results far superior to traditional methods, solving the long-standing problem of fluorine open circuits in the industry. The above descriptions are merely preferred embodiments of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for deep defluorination and fluorine resource utilization of electrolytic zinc leaching solution, characterized in that, The process includes the following steps: (1) Targeted adsorption for fluoride removal: The electrolytic zinc leaching solution with a pH value of 2.0-4.5 is subjected to at least two stages of countercurrent contact adsorption with the composite adsorption material at 20-50℃. The composite adsorption material has an adsorption capacity of fluoride ions ≥40mg / g, and the fluoride ion concentration in the liquid after adsorption is stably reduced to below 50mg / L. (2) High-efficiency desorption and material regeneration: The composite adsorbent material saturated by adsorption in step (1) is desorbed by sodium hydroxide solution with a concentration of 0.5-2.0 mol / L at 30-60℃ to obtain a high-concentration sodium fluoride desorption solution. The desorbed composite adsorbent material is treated with a specific regeneration solution and its adsorption performance recovery rate is ≥95%, and it is returned to step (1) for recycling. (3) Closed-loop precipitation and fluorine resource utilization: The high-concentration sodium fluoride desorption solution obtained in step (2) is mixed with lime milk at a calcium-fluoride molar ratio of 1.0-1.2:1 and subjected to causticization precipitation reaction at 40-80℃ to generate high-purity calcium fluoride precipitate. After filtration, washing and drying, the precipitate is used to obtain pure calcium fluoride product. The precipitate liquid is returned to step (2) for recycling as regenerated alkali liquid, realizing the closed loop within the system of alkali medium.
2. The method for deep defluorination and fluorine resource utilization of electrolytic zinc leaching solution according to claim 1, characterized in that: The composite adsorbent material mentioned in step (1) includes one or more of the following: modified salt-based activated carbon, metal-based ion exchange resin, and magnetic nano-iron composite adsorbent.
3. The method for deep defluorination and fluorine resource utilization of electrolytic zinc leaching solution according to claim 2, characterized in that: In the modified salt-based activated carbon, the active metal component exists in a highly dispersed crystalline form on the surface and inside the pores of the activated carbon, and its metal oxide loading is 5-20 wt%.
4. The method for deep defluorination and fluorine resource utilization of electrolytic zinc leaching solution according to claim 2, characterized in that: The metal-based ion exchange resin has an exchange capacity ≥2.0 mmol F. - / g, and its adsorption performance for fluoride ions remains stable in the pH range of 2.0-5.
0.
5. The method for deep defluorination and fluorine resource utilization of electrolytic zinc leaching solution according to claim 2, characterized in that: The magnetic nano-iron composite adsorbent has an average particle size of 20-80 nm and can achieve rapid solid-liquid separation within 5 minutes by applying an external magnetic field.
6. The method for deep defluorination and fluorine resource utilization of electrolytic zinc leaching solution according to claim 1, characterized in that: The adsorption process in step (1) is achieved by using a 2-4 stage countercurrent adsorption tower or a series stirred tank, with a total contact time of 30-90 minutes and a zinc loss rate of <1.0% during the adsorption stage.
7. The method for deep defluorination and fluorine resource utilization of electrolytic zinc leaching solution according to claim 2, characterized in that: The specific regeneration solution mentioned in step (2) is a 0.05-0.2 mol / L dilute hydrochloric acid or dilute sulfuric acid solution when the composite adsorbent is modified salt-based activated carbon; a 0.1-0.5 mol / L mixed solution of NaOH and NaCl when the composite adsorbent is metal-based ion exchange resin; and a 0.5-1.0 mol / L NaOH solution when the composite adsorbent is magnetic nano-iron composite adsorbent.
8. The method for deep defluorination and fluorine resource utilization of electrolytic zinc leaching solution according to claim 1, characterized in that: The causticization precipitation reaction described in step (3) is carried out in a reaction vessel. The final pH of the reaction is controlled at 8.0-10.0, and the reaction time is 60-120 minutes. The calcium fluoride precipitate has high crystallinity and is easy to filter and wash.
9. A method for deep defluorination and fluorine resource utilization of electrolytic zinc leaching solution according to claim 2, 3, 4, or 5, characterized in that: The modified salt-based activated carbon is made with ≥1200m ² Using high specific surface area activated carbon as a carrier, nano-scale alkaline earth metal / rare earth metal oxide active sites are loaded through in-situ precipitation-atmosphere calcination technology to form a composite material with hierarchical pore structure and strong fluoride ion coordination ability; the metal-based ion exchange resin is based on polymer or inorganic silica gel as a framework, and metal-organic elements with clear fluoride ion recognition function are grafted through coordination bonds to form an adsorption resin with both ion exchange and specific complexation capabilities; the magnetic nano-iron composite adsorbent is based on magnetic Fe3O4 nanoparticles as the core, and is coated and functionalized with a hydrated lanthanum oxide shell to form a core-shell structure, a nanocomposite material with both high adsorption capacity and magnetic separation characteristics.