Seawater-resistant PVC ship cloth coating coating equipment and preparation method

By applying the base layer and top layer in multiple layers, combined with roller dip coating and roller coating technologies, a dense adhesive layer and a high-density functional layer are formed. This solves the problems of delamination and blistering of PVC ship fabric coating under seawater immersion and external force, achieving high adhesion and uniform thickness, and meeting the usage requirements of deep-sea and high-load conditions.

CN122032816APending Publication Date: 2026-05-15SHANDONG HONGDING NEW MATERIAL TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202610369811.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-03-25
Publication Date
2026-05-15

AI Technical Summary

Technical Problem

Existing PVC ship fabric coating equipment cannot maintain the adhesion between the coating and the base fabric under long-term immersion in seawater and external force. Moreover, the coating thickness is uneven, which leads to easy delamination, blistering, and insufficient peel resistance, and cannot meet the requirements of use in deep sea and high-load conditions.

Method used

By employing a multi-coating method for the base layer and top layer, combined with roll-dip coating and roll coating technologies, a dense adhesive layer and a high-density functional layer are formed through base layer impregnation and top layer coating. Nano-titanium dioxide and mica powder are used to form a double protection, and gradient drying and cooling are combined to ensure uniform coating thickness and adhesion.

Benefits of technology

It achieves Grade 0 adhesion between the coating and the base fabric, improves seawater immersion resistance to 1500 hours, with no delamination or blistering, and has a dense and uniform coating with 50% increased mechanical strength, meeting the requirements for use in deep-sea and high-load conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122032816A_ABST
    Figure CN122032816A_ABST
Patent Text Reader

Abstract

The invention discloses seawater-resistant PVC ship cloth coating equipment and a preparation method, and belongs to the technical field of seawater-resistant ship cloth preparation. Comprising an unwinding unit, a pretreatment unit, a bottom-layer size dipping tank unit, a fixed-thickness drying unit, a cold-pressing laminating roller group, a bottom-layer coating unit, a first drying unit, a surface-layer coating unit, a second drying unit, a gradient cooling and shaping unit and a winding unit which are arranged in the coating direction of base cloth, the bottom-layer size dipping tank unit, the bottom-layer coating unit and the surface-layer coating unit are connected to a closed-loop feeding system; the fixed-thickness drying unit comprises a rolling roller pair arranged on the inner side of the bottom-layer size dipping tank unit and a centering roller pair arranged right above the rolling roller pair, and a hot air drying box is arranged between the rolling roller pair and the centering roller pair; according to the coating equipment and the preparation method of the seawater-resistant PVC ship cloth coating, the surface of the base cloth is coated with the bottom layer and the surface layer in batches, so that the adhesive force of the ship cloth and the coating can be ensured, and the weather resistance and the mechanical strength are greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention specifically relates to a coating equipment and preparation method for seawater-resistant PVC ship fabric, belonging to the field of seawater-resistant ship fabric preparation technology. Background Technology

[0002] PVC marine fabric is a core material for offshore operations and ship equipment, widely used in inflatable boats, marine tarpaulins, offshore enclosures, and aquaculture cages. Besides requiring excellent resistance to seawater immersion, salt spray, algae control, and aging, it also demands higher requirements for coating thickness and peel strength from the base fabric under complex conditions such as deep sea and high loads. Existing PVC fabrics, such as the PVC fabric publication number CN101509201A, disclose a process for preparing a PVC marine enclosure coating material. This process includes feeding the PVC fabric blank, preheating and ironing, double-sided coating treatment, pre-plasticizing and gelling, flattening and cooling, first horizontal coating, plasticizing treatment, cooling and shaping, second horizontal coating, plasticizing treatment, embossing, cooling, winding, and surface treatment. Compared to ordinary coating processes, this process allows for vertical... The process involves coating, topcoat, and bottom layers, but the resulting PVC coated fabric is unsuitable for marine operations. Existing seawater-resistant PVC marine fabric coating equipment and processes suffer from the following significant drawbacks: 1. The coating often employs surface slit coating, where the slurry adheres only to the base fabric surface and cannot penetrate the fibers. The coating and base fabric are only superficially bonded, making the coating prone to delamination and blistering under prolonged seawater immersion and external forces, resulting in insufficient peel resistance. 2. The roll-coating structure lacks sufficient thickness accuracy, leading to uneven coating thickness on both sides of the base fabric and preventing precise thickness control. 3. The upper limit of coating thickness is low; the total dry film thickness on one side of a single double-sided coating typically does not exceed 40μm. Thick coatings are prone to sagging and dripping; furthermore, thick coatings are prone to surface skinning and internal solvent residue during drying, resulting in poor coating density and allowing seawater to easily penetrate the interface layer, accelerating coating peeling. Summary of the Invention

[0003] To address the aforementioned issues, this invention proposes a seawater-resistant PVC ship fabric coating equipment and preparation method. By coating the base fabric surface with a base layer and a top layer in stages, the coating accuracy can be guaranteed, and the adhesion, weather resistance, and mechanical strength of the ship fabric and the coating can be greatly improved.

[0004] The seawater-resistant PVC ship fabric coating equipment of the present invention includes an unwinding unit, a pretreatment unit, a bottom impregnation tank unit, a thickness drying unit, a cold pressing and bonding roller group, a bottom coating unit, a first drying unit, a top coating unit, a second drying unit, a gradient cooling and shaping unit, and a winding unit arranged sequentially along the coating direction of the base fabric. The bottom impregnation tank unit, the bottom coating unit, and the top coating unit are connected to a closed-loop feeding system. The pretreatment unit is a plasma treatment device; The thickness-fixing drying unit includes rolling rollers disposed inside the bottom impregnation tank unit and centering rollers disposed directly above the rolling rollers. A hot air drying box is disposed between the rolling rollers and the centering rollers. A thickness-fixing scraper assembly is disposed between the rolling rollers and the hot air drying box. The thickness-fixing scraper assembly is disposed directly above scraper bodies disposed on both sides of the base fabric. The slurry scraped off by the scraper bodies flows back to the bottom impregnation tank unit along the base fabric. The cold-pressing and bonding roller assembly consists of mirror-finished cooling rollers arranged symmetrically on the upper and lower sides. Cooling channels are provided inside the mirror-finished cooling rollers and are connected to a cooling water circulation system. The cold-pressing and bonding roller assembly has an intermittently adjustable structure and is equipped with an independent motor for driving rotation. Constant-temperature cooling water flows inside the rollers, the surface roughness Ra≤0.2μm, and the pressing gap is purely mechanically adjustable. Both the bottom coating unit and the top coating unit include coating tubes facing each other on the top and bottom surfaces of the base fabric. The coating tubes are connected to a closed-loop feeding system. A coating head is provided on the side of the coating tube facing the base fabric, and a reverse coating roller that presses against the base fabric is provided on the output side of the coating tube. A slit extrusion coating head is provided on the side of the coating tube close to the base fabric. After the material is applied through the coating head, it is coated to a fixed thickness by the reverse coating roller. The reverse coating roller is configured to cooperate with the coating head, and the ratio of its linear speed to the running speed of the base fabric is 1.05-1.2:1. The closed-loop feeding system includes a first mixing tank and a second mixing tank. Vacuum degassing devices are connected to the first and second mixing tanks. A double-spiral belt electric stirrer is installed on the first and second mixing tanks. The first mixing tank is connected to the bottom coating unit and the bottom impregnation tank unit through a first pump group and a replenishment pump, respectively. The second mixing tank is connected to the top coating unit through a second pump group. The second drying unit includes a low-temperature pre-drying section, a medium-temperature plasticizing section, and a high-temperature shaping section arranged sequentially.

[0005] The undercoating unit first coats the base fabric surface with an undercoat, and then the topcoat unit coats the undercoat with a topcoat; the undercoat and topcoat work together to ensure the adhesion, weather resistance and mechanical strength of the seawater-resistant PVC marine fabric. By utilizing the interface transition buffering effect, the contradiction between thick coating and adhesion is resolved: after the base layer cures, a thick and dense adhesive layer is formed, with a surface smoothness far superior to that of the rough base fabric fiber surface, providing a smooth anchoring surface for the topcoat; this avoids localized thin coatings or slurry accumulation caused by fiber protrusions when the topcoat is directly coated onto the base fabric, reducing the topcoat thickness error from ±5μm to ±2μm; through the flexible adhesive system of the base layer (containing DOTP plasticizer), the internal stress during the curing of the topcoat can be buffered, reducing the risk of coating cracking caused by thick coating, and the finished product can withstand 1000 flexing cycles without cracking (a single thick coating can only withstand 300 cycles). Double-barrier anti-permeability, greatly improving seawater resistance: The bottom layer fills the gaps in the base fabric fibers, forming the first sealing barrier to prevent seawater from seeping in through the fiber gaps; the high-density functional layer on the surface (containing nano-titanium dioxide and mica powder) forms the second protective wall, blocking seawater, salt spray, and ultraviolet radiation. The two layers work together to reduce the seawater permeation rate to 0.01 g / (㎡·24h), far lower than the 0.15 g / (㎡·24h of a single coating. The seawater immersion time is increased from 1000h to 1500h without delamination; the polyurethane adhesive accelerator in the bottom layer forms a chemically compatible interface with the PVC resin in the surface layer, avoiding interlayer peeling caused by seawater penetration, and further strengthening the adhesion from level 0 (the cohesive damage rate of the coating reaches 95% when peeled). The mechanical synergy enhances the overall strength significantly. The bottom layer and the base fabric fibers form a fiber and PVC anchoring structure, while the top layer forms a rigid protective shell. When the two work together under stress, the breaking strength of the finished product is more than 50% higher than that of the base fabric itself (base fabric 4000N / 5cm - finished product 7350N / 5cm), far exceeding the sum of the strength of the base fabric and the coating. The abrasion-resistant agent (1-2 parts) in the top layer works in conjunction with the flexible system of the bottom layer to further enhance the abrasion resistance of the marine fabric surface. After 1000 cycles of friction (500g load), the coating wear is only 0.02g, which meets the requirements of high-frequency marine use scenarios.

[0006] Furthermore, the second drying unit is a segmented gradient heating suspended drying box, which is equipped with a gradient wind speed adjustable nozzle group (an upper or lower nozzle array connected to a variable frequency fan). That is, the second drying unit includes a low-temperature pre-drying section, a medium-temperature plasticizing section, and a high-temperature shaping section. The upper and lower nozzle arrays are arranged directly opposite each other on the inner top and bottom. Each set of upper and lower nozzle arrays is connected to the variable frequency fan through a duct. The input side of the variable frequency fan is connected to a temperature control box. The wind speed of the gradient wind speed adjustable nozzle group increases gradually along the running direction of the base fabric. The wind speed at the feeding end of the low-temperature pre-drying section is 2-3 m / s, and the wind speed at the discharging end is 5-6 m / s. The wind speed in the medium-temperature plasticizing section and the high-temperature shaping section increases synchronously with the degree of coating curing. The wind speed of the upper and lower nozzle arrays is independently adjustable.

[0007] Furthermore, the bottom impregnation tank unit includes a sealed impregnation tank with a constant temperature jacket, and multiple guide rollers are arranged inside the sealed impregnation tank; the gradient cooling and shaping unit consists of multiple sets of cooling rollers that gradient cool along the running direction of the base fabric, and each set of cooling rollers is connected to an independent temperature control cooling system.

[0008] Furthermore, the pretreatment unit includes a reverse brushing dust removal roller group, a plasma treatment device, a bidirectional synchronous fabric roughening roller group, and a negative pressure dust removal device arranged sequentially along the running direction of the base fabric.

[0009] Furthermore, the bidirectional synchronous fabric roughening roller group is symmetrically arranged on both sides of the base fabric. The roller surface of the bidirectional synchronous fabric roughening roller group has micron-level diamond-shaped wear-resistant protrusions. The roller surface roughness is Ra3.2-Ra6.3. The bidirectional synchronous fabric roughening roller group is equipped with an adjustable pressing cylinder. The pressing gap is 0.8-1.0 times the thickness of the base fabric. The roller surface rotation direction is opposite to the base fabric running direction. The reverse brush dust removal roller group is symmetrically arranged on both sides. The brush bristles are made of high-resilience nylon filaments. The roller surface rotation direction is opposite to the base fabric running direction.

[0010] Furthermore, fabric clamping strut chains are provided on both sides of the base fabric at the output side of the thickness-fixed scraper assembly; the fabric clamping strut chains are arranged along the coating direction of the base fabric; edge-cutting units are provided on both sides of the input end of the winding unit; the edge-cutting unit is a carbide circular blade edge-cutting machine, and the distance between the two circular blades is completely fixed by a high-precision positioning bushing, so that the width error of the base fabric after cutting is ≤±0.1mm; during the coating of the base fabric, a 15-20mm clamping edge is reserved, and the clamping edge is clamped by the fabric clamping strut chain. After clamping and traction, the width error is ≤±0.1mm. After the coating and curing are completed, the edge-cutting unit is used for cutting, and the width error of the base fabric after cutting is ≤±0.1mm.

[0011] A method for preparing seawater-resistant PVC ship fabric, using seawater-resistant PVC ship fabric coating equipment, includes the following steps: S1. Slurry preparation: The bottom adhesive layer PVC slurry and the top seawater resistant functional layer PVC slurry are respectively put into the first mixing tank and the second mixing tank. After stirring, dispersion and vacuum degassing, the temperature is kept constant and stirring is continued. S2. Base fabric unwinding: Install the high-strength polyester filament base fabric in the unwinding unit, set the unwinding tension to 4-10N, and the base fabric enters the pretreatment unit at a set linear speed. S3. Base fabric composite pretreatment: The base fabric is sequentially cleaned by reverse brushing dust removal roller group, surface activated by plasma treatment device, physical micro-roughening by bidirectional synchronous fabric roughening roller group, and dust removal by negative pressure dust removal device. After treatment, the surface tension of the base fabric is ≥48dyn / cm. S4. Full fiber deep impregnation: The base fabric enters the bottom impregnation tank unit and is fully impregnated in the constant temperature slurry along the guide roller path. The slurry completely penetrates into the fiber gaps of the base fabric and is then smoothly fed into the fixed thickness drying unit. S5. Thickness Coating and Pre-drying: The base fabric enters the thickness drying unit and is rolled by rolling rollers. Then, the base fabric is pulled vertically to the ground by the combined action of the rolling rollers and the centering rollers. At this time, the gap between the scraper bodies on both sides of the base fabric and the base fabric is completely consistent. After the base fabric has been fully impregnated and rolled, the excess slurry on the surface of the base fabric is scraped off by the scraper bodies, controlling the thickness error of the bottom dry film on both sides of the base fabric to ≤ ±0.3μm. At this time, the base fabric enters the hot air drying box. It is pre-dried at a low temperature of 40-60℃ for 30-60s to form a non-sticky bottom coating. Then, it is cold-pressed at low pressure by the cold-press bonding roller group to eliminate the micro-bubbles between the coating and the base fabric and strengthen the interfacial bonding force. S6. Undercoat coating and pre-drying: The base fabric enters the undercoat unit, and both sides of the base fabric are coated by roller coating in the undercoat unit. The roller coating thickness is 5-10μm, and the fabric is dried by the first drying unit. After the base fabric is coated with the undercoat, it enters the first drying unit and is pre-dried at a low temperature of 40-60℃ for 30-60 seconds to form a non-sticky undercoat. Then, it is cold-pressed at low pressure by the cold-pressing and bonding roller group to eliminate tiny air bubbles between the coating and the base fabric and strengthen the interfacial bonding force. S7. Topcoat: The base fabric enters the topcoat unit, and the topcoat seawater resistant functional layer slurry is applied to the bottom coating through the coating head of the topcoat unit. Then, it is uniformly coated to a fixed thickness through the reverse coating roller; the thickness error is ≤ ±2μm. S8. Segmented Gradient Drying and Curing: After the coating layer is applied, the base fabric enters the second drying unit, sequentially entering the low-temperature pre-drying section at 70-90℃, then the medium-temperature plasticizing section at 100-130℃, and finally the high-temperature setting section at 135-155℃. The total drying time is 180-300 seconds. The coating is gradually cured from the inside out using gradient airflow nozzles. S9. Gradient cooling and shaping: The dried base fabric enters the gradient cooling and shaping unit, and is gradually cooled by multiple sets of cooling rollers to eliminate the internal stress of the coating. S10, Traction and winding: The qualified base fabric is wound by the winding unit with decreasing tension to obtain the finished seawater resistant PVC ship fabric.

[0012] Further, the bottom adhesive layer PVC slurry is composed of the following components by weight: 100 parts PVC paste resin, 40-50 parts dioctyl terephthalate, 5-8 parts polyurethane adhesive accelerator, 2-3 parts calcium-zinc heat stabilizer, and 0.5-1 parts defoamer; the top seawater resistant functional layer PVC slurry is composed of the following components by weight: 100 parts PVC paste resin, 35-45 parts dioctyl terephthalate, 3-4 parts calcium-zinc heat stabilizer, 1-2 parts benzotriazole ultraviolet absorber, 2-3 parts isothiazolinone algaecide, 3-5 parts nano titanium dioxide, 5-8 parts mica powder, 1-2 parts wear-resistant agent, and 0-2 parts pigment; the slurry is dispersed at a high speed of 800-1200 r / min for 20-30 min, with a vacuum degassing degree of -0.08~-0.1 MPa and a degassing time of 15-20 min.

[0013] Furthermore, the plasma treatment device has a plasma treatment power of 3-6kW, and the treatment speed is synchronized with the linear speed of the base fabric; the temperature control of the bottom impregnation tank unit is 22-28℃, and the base fabric immersion time is ≥2s; the weight of the high-strength polyester filament base fabric is 200-500g / ㎡, and the tensile strength is ≥4000N / 5cm; the prepared seawater-resistant PVC ship fabric has a coating adhesion of 0 grade to the base fabric, is resistant to seawater immersion for 1500h without delamination, blistering, or discoloration, is resistant to neutral salt spray for 1000h without corrosion, has a tensile strength ≥6000N / 5cm, a tear strength ≥800N, and a dimensional change rate ≤0.5% after immersion in water for 72h.

[0014] Compared with the prior art, the seawater-resistant PVC ship fabric coating equipment and preparation method of the present invention have the following advantages: 1. Significant improvement in peel resistance: Since the base fabric is made of interwoven fibers, there are a large number of micron-level gaps. The base fabric is first fully impregnated and then rolled to achieve full-area deep wetting of the base fabric fibers. Combined with the physical micro-roughening structure, the coating and the base fabric form a 360° mechanical pinning structure, and the adhesion is stably improved from level 1 to level 0 (GB / T5210-2006). The seawater immersion time is improved from 1000h to 1500h, with no delamination or blistering, and the long-term stability is greatly improved. 2. More stable coating: The base layer is coated by roller dip coating, and then supplemented by roller coating to ensure the consistency of the base layer thickness and the smoothness of the surface. The roller dip coating base layer has no floating layer and no interface gaps. Then, the top layer is coated by roller coating to ensure that the thickness error of the base layer and the top layer is stably controlled within ±2μm, which meets the requirements of the ship fabric thickness under high load marine working conditions. Gradient wind speed drying avoids surface skinning and internal solvent residue of the thick coating. After thick coating, the coating is dense and uniform, without defects such as pinholes and bubbles.

[0015] 3. Superior overall performance of the finished product: Gradient cooling and shaping eliminates internal stress in the coating, avoiding coating peeling caused by stress release during long-term use.

[0016] 4. Secondary reinforcement of the bonding force between the base fabric and the bottom layer: After the bottom layer is pre-dried, it is then cold-pressed at low pressure by a cold-pressing roller group to eliminate tiny air bubbles between the coating and the base fabric and strengthen the interfacial bonding force. Attached Figure Description

[0017] Figure 1 This is a schematic diagram of one embodiment of the seawater-resistant PVC ship fabric coating equipment of the present invention.

[0018] Figure 2 This is a schematic diagram of the overall structure of the bottom coating unit of the present invention.

[0019] Figure 3 This is a schematic diagram of another embodiment of the seawater-resistant PVC ship fabric coating equipment of the present invention.

[0020] Figure 4 This is a schematic diagram of the arrangement structure of the centering rollers and the stretching chain of the present invention.

[0021] Figure 5 This is a schematic diagram of the workflow for preparing seawater-resistant PVC ship fabric according to the present invention.

[0022] Reference numerals: 1. Unwinding unit; 2. Plasma treatment device; 3. Underlayer impregnation tank unit; 4. Rolling rollers; 5. Centering rollers; 6. Hot air drying box; 7. Thickness-fixing doctor blade assembly; 8. Base fabric; 9. Cold pressing and bonding roller assembly; 10. Underlayer coating unit; 11. First drying unit; 12. Top layer coating unit; 13. Second drying unit; 14. Gradient cooling and setting unit; 15. Rewinding unit; 16. Coating tube; 17. Coating head. 18. Reverse coating roller; 19. First mixing tank; 20. Second mixing tank; 21. Vacuum degassing device; 22. First pump set; 23. Liquid replenishment pump; 24. Second pump set; 25. Low temperature pre-drying section; 26. Medium temperature plasticizing section; 27. High temperature setting section; 28. Sealed impregnation tank; 29. ​​Guide roller; 30. Reverse brushing dust removal roller set; 31. Bidirectional synchronous fabric roughening roller set; 32. Negative pressure dust removal device; 33. Fabric clamping and stretching chain. Detailed Implementation

[0023] Example 1: like Figures 1 to 4The seawater-resistant PVC marine fabric coating equipment shown includes an unwinding unit 1, a pretreatment unit, a bottom impregnation tank unit 3, a thickness drying unit, a cold pressing and bonding roller group 9, a bottom coating unit 10, a first drying unit 11, a top coating unit 12, a second drying unit 13, a gradient cooling and shaping unit 14, and a winding unit 15 arranged sequentially along the coating direction of the base fabric 8. The bottom impregnation tank unit 3, the bottom coating unit 10, and the top coating unit 12 are connected to a closed-loop feeding system. Both the unwinding unit 1 and the winding unit 15 are equipped with servo tension controllers to form a closed-loop tension control loop with a tension control accuracy of ±1N. The adjustable range of the running linear speed of the base fabric 8 is 2-25m / min. The pretreatment unit is a plasma treatment device 2; The thickness-fixing drying unit includes rolling rollers 4 disposed inside the bottom impregnation tank unit 3, and centering rollers 5 disposed directly above the rolling rollers 4. A hot air drying box 6 is disposed between the rolling rollers 4 and the centering rollers 5. A thickness-fixing scraper group 7 is disposed between the rolling rollers 4 and the hot air drying box 6. The thickness-fixing scraper group 7 is disposed directly opposite the scraper bodies disposed on both sides of the base fabric 8. The slurry scraped off by the scraper bodies flows back to the bottom impregnation tank unit 3 along the base fabric 8. The hot air drying box 6 is a segmented gradient heating type suspended drying box. A cold-pressing bonding roller group 9 is disposed at the outlet end. The cold-pressing bonding roller group 9 is a mirror cooling roller symmetrically arranged on the upper and lower sides. A cooling channel is disposed inside the mirror cooling roller, and the cooling channel is connected to the cooling water circulation system. The cold-pressing bonding roller group 9 has an intermittent adjustable structure and is equipped with an independent motor for driving rotation. Constant temperature cooling water flows inside the roller, the surface roughness Ra≤0.2μm, and the pressing gap is purely mechanically adjustable. Both the bottom coating unit 10 and the top coating unit 12 include coating tubes 16 facing each other on the top and bottom surfaces of the base fabric 8. The coating tubes 16 are connected to a closed-loop feeding system. A coating head 17 is provided on the side of the coating tube 16 facing the base fabric 8. A reverse coating roller 18 that presses against the base fabric 8 is provided on the output side of the coating tube 16. A slit extrusion coating head 17 is provided on the side of the coating tube 16 close to the base fabric 8. After the material is applied through the coating head 17, it is coated to a fixed thickness by the reverse coating roller 18. The reverse coating roller 18 is configured to cooperate with the coating head 17, and the ratio of its linear speed to the running speed of the base fabric 8 is 1.05-1.2:1. The closed-loop feeding system completes the feeding of slurry for the bottom layer and the top layer. The closed-loop feeding system includes a first mixing tank 19 and a second mixing tank 20. Vacuum degassing devices 21 are connected to the first mixing tank 19 and the second mixing tank 20. A double-spiral belt electric stirrer is provided on the first mixing tank 19 and the second mixing tank 20. The first mixing tank 19 is connected to the bottom layer coating unit 10 and the bottom layer impregnation tank unit 3 through a first pump group 22 and a replenishing pump 23, respectively. The second mixing tank 20 is connected to the top layer coating unit 12 through a second pump group 24. The second drying unit 13 includes a low-temperature pre-drying section 25, a medium-temperature plasticizing section 26, and a high-temperature shaping section 27 arranged sequentially. The second drying unit 13 is equipped with a gradient wind speed adjustable nozzle group. The wind speed at the feed end of the low-temperature pre-drying section 25 is 2.5 m / s, and the wind speed at the discharge end is 5.5 m / s. The wind speed increases gradually with the degree of curing.

[0024] The second drying unit 13 is a segmented gradient heating suspension drying box. The segmented gradient heating suspension drying box is equipped with a gradient wind speed adjustable nozzle group (the upper or lower nozzle array is connected to the variable frequency fan). That is, the second drying unit 13 includes a low temperature pre-drying section 25, a medium temperature plasticizing section 26 and a high temperature setting section 27. The upper and lower nozzle arrays are arranged directly opposite each other on the inner top and bottom. Each set of the upper and lower nozzle arrays is connected to the variable frequency fan through a duct. The input side of the variable frequency fan is connected to the temperature control box. The wind speed of the gradient wind speed adjustable nozzle group increases gradually along the running direction of the base fabric 8. The wind speed at the feeding end of the low temperature pre-drying section 25 is 2-3 m / s and the wind speed at the discharging end is 5-6 m / s. The wind speed in the medium temperature plasticizing section 26 and the high temperature setting section 27 increases synchronously with the degree of coating curing. The wind speed of the upper and lower nozzle arrays is independently adjustable.

[0025] The bottom impregnation tank unit 3 includes a sealed impregnation tank 28 with a constant temperature jacket, and multiple guide rollers 29 are arranged inside the sealed impregnation tank 28; the gradient cooling and shaping unit 14 consists of multiple sets of cooling rollers that gradient-cool along the running direction of the base fabric 8, and each set of cooling rollers is connected to an independent temperature control cooling system; the gradient cooling and shaping unit 14 consists of 3 sets of gradient cooling mirror cooling rollers, with the first set at 32°C, the second set at 22°C, and the third set at 18°C. The pretreatment unit includes a reverse brushing dust removal roller group 30, a plasma treatment device 2, a bidirectional synchronous fabric roughening roller group 31, and a negative pressure dust removal device 32, arranged sequentially along the running direction of the base fabric 8.

[0026] The bidirectional synchronous fabric roughening roller group 31 is symmetrically arranged on both sides of the base fabric 8. The roller surface of the bidirectional synchronous fabric roughening roller group 31 has micron-level diamond-shaped wear-resistant protrusions; the roller surface has micron-level diamond-shaped wear-resistant protrusions with Ra4.5. The bidirectional synchronous fabric roughening roller group 31 is equipped with an adjustable pressing cylinder, the pressing gap is 0.9 times the thickness of the base fabric 8, and the roller surface rotation direction is opposite to the running direction of the base fabric 8. The reverse brush dust removal roller group 30 is symmetrically arranged on both sides, the brush bristles are high-resilience nylon filaments, and the roller surface rotation direction is opposite to the running direction of the base fabric 8. The base fabric 8 is provided with fabric clamping strut chains 33 on both sides of the output side of the thickness-fixed scraper group 7; the fabric clamping strut chains 33 are arranged along the coating direction of the base fabric 8; the winding unit 15 is provided with edge-cutting units on both sides of the input end; the edge-cutting unit is a carbide circular blade edge-cutting machine, the distance between the two circular blades is completely fixed by a high-precision positioning bushing, and the width error of the base fabric 8 after cutting is ≤±0.1mm; when the base fabric 8 is coated, a 15-20mm clamping edge is reserved, and the clamping edge is clamped by the fabric clamping strut chains 33. After clamping and traction, the width error is ≤±0.1mm. After the coating and curing are completed, the base fabric 8 is cut by the edge-cutting unit, and the width error of the base fabric 8 after cutting is ≤±0.1mm.

[0027] Example 2: like Figure 5 As shown, the seawater-resistant PVC ship fabric preparation method of this embodiment is implemented using the seawater-resistant PVC ship fabric coating equipment described in Example 1, and the specific steps are as follows: S1. Slurry Preparation: The bottom bonding layer PVC slurry is prepared according to the following components by weight: 100 parts PVC paste resin, 45 parts dioctyl terephthalate, 6 parts polyurethane bonding accelerator, 2.5 parts calcium-zinc heat stabilizer, and 0.8 parts defoamer. The top seawater-resistant functional layer PVC slurry is prepared according to the following components by weight: 100 parts PVC paste resin, 40 parts dioctyl terephthalate, 3.5 parts calcium-zinc heat stabilizer, 1.5 parts benzotriazole UV absorber, 2.5 parts isothiazolinone algaecide, and sodium... Four parts of titanium dioxide, six parts of mica powder, 1.5 parts of wear-resistant agent, and one part of titanium dioxide were prepared. The two slurries were dispersed in a high-speed disperser at 1000 r / min for 25 min, and degassed under a vacuum of -0.09 MPa for 18 min. They were then fed into the corresponding double-spiral belt mixing tank of the closed-loop feeding system, where the temperature was set at 25℃ and the circulating stirring speed was 50 r / min for storage. The bottom slurry in the first mixing tank 19 was intermittently fed to the bottom impregnation tank unit 3, and the temperature of the bottom impregnation tank unit 3 was kept constant at 25℃. S2, Base Fabric 8 Unwinding: Select a high-strength polyester filament base fabric 8 with a weight of 300g / ㎡ and a breaking strength of 4500N / 5cm. Install it in the unwinding unit 1, leaving an 18mm clamping edge to obtain a base fabric 8 with a consistent width. Set the unwinding tension to 6N and the running linear speed of the base fabric 8 to 10m / min before entering the pretreatment unit.

[0028] S3, Base Fabric 8 Composite Pretreatment: Base Fabric 8 is sequentially cleaned and impurities removed by reverse brushing dust removal roller group 30, surface activated by plasma treatment device 232 with 4kW power, physically micro-roughened by bidirectional synchronous fabric roughening roller group 31 to form micron-level pits, and dust removed by negative pressure dust removal device 32; after treatment, the surface tension of Base Fabric 8 is 50dyn / cm, and the surface fiber hairs are upright. S4. Bottom Layer Double-Sided Synchronous Roller Coating: The pretreated base fabric 8 enters the bottom layer impregnation tank unit 3 for double-sided synchronous roller coating. In a 25℃ constant temperature impregnation tank, it is fully impregnated with the bottom layer slurry by the guide roller 29 for 3 seconds. The slurry is fully impregnated along the path of the guide roller 29, completely penetrating into the fiber gaps of the base fabric 8. Then, it is pressed and rolled by the rolling rollers 4. Next, the rolled edge of the base fabric 8 is synchronously clamped and stretched by the fabric tensioning chain 33. Through the combined traction of the rolling rollers 4 and the centering rollers 5, the base fabric 8 is brought to a perpendicular traction state with the ground. At this time, the two sides of the base fabric 8... The gap between the scraper body on the side and the base fabric 8 is completely consistent. After the base fabric 8 has been fully impregnated and rolled, the scraper body scrapes off the excess slurry on the surface of the base fabric 8, controlling the thickness error of the bottom dry film on both sides of the base fabric 8 to be ≤±0.3μm. At this time, the base fabric 8 enters the hot air drying oven 6. After being pre-dried at a low temperature of 50℃ for 40s, a non-sticky bottom coating is formed. Then, it is cold-pressed at low pressure by the cold pressing and bonding roller group 9 to eliminate the tiny air bubbles between the coating and the base fabric 8 and strengthen the interfacial bonding force. The pressing pressure of the rolling roller 4 is 0.3MPa, and the scraper body scrapes off the excess floating slurry, controlling the thickness error of the bottom dry film on one side to be ≤±0.6μm. S5. Undercoating and pre-drying: After the base fabric 8 is stretched flat by the fabric tensioner chain 33, the base fabric 8 is roller coated on both sides by the undercoating unit 10. The roller coating thickness is 8μm, and the thickness of the dry film of the undercoating on one side is controlled to be 110μm. The drying is completed by the first drying unit 11. S6. Topcoat: The base fabric 8 is pulled into the topcoat unit 12 by the fabric tensioner chain 33. The topcoat seawater resistant functional layer slurry is coated on the base coating by the coating head 17 of the topcoat unit 12. Then, it is uniformly coated to a fixed thickness by the reverse coating roller 18. The ratio of the linear speed of the reverse coating roller 18 to the speed of the base fabric 8 is 1.1:1, and the dry film thickness of the topcoat on one side is controlled to be 25μm with a thickness error ≤±1.5μm. S7. Segmented gradient drying and curing: The base fabric 8 after coating enters the second drying unit 13, and is pre-dried at 80℃ for 60s, medium-temperature plasticizing at 120℃ for 90s, and high-temperature setting at 145℃ for 60s in sequence, with a total drying time of 210s; the gradient wind speed adjustable nozzle group gradually increases the wind speed according to the degree of curing, so as to achieve the coating to be gradually cured from the inside to the outside. S8. Gradient cooling and shaping: The dried base fabric 8 enters the gradient cooling and shaping unit 14, and is gradually cooled by three sets of cooling rollers at 32℃, 22℃ and 18℃ to eliminate the internal stress of the coating. S9. Edge trimming and winding: The qualified base fabric 8 is trimmed by the edge trimming unit to remove the clamping edges on both sides, and then wound by the winding unit 15 with decreasing tension to obtain the finished seawater resistant PVC ship fabric.

[0029] Example 3: The differences between this embodiment and Embodiment 2 are as follows: The bottom adhesive layer PVC slurry consists of 100 parts PVC paste resin, 40 parts dioctyl terephthalate, 5 parts polyurethane bonding accelerator, 2 parts calcium-zinc heat stabilizer, and 0.5 parts defoamer; the top layer slurry consists of 100 parts PVC paste resin, 35 parts dioctyl terephthalate, 3 parts calcium-zinc heat stabilizer, 1 part benzotriazole UV absorber, 2 parts isothiazolinone algaecide, 3 parts nano titanium dioxide, 5 parts mica powder, and 1 part abrasion resistant agent; the base fabric 8 is a 200g / ㎡ high-strength polyester filament base fabric 8, with a 15mm clamping edge, an unwinding tension of 4N, and a running linear speed of 15m / min. n; plasma treatment power 3kW, hot air drying temperature 60℃, base fabric 8 surface tension 48dyn / cm; impregnation tank constant temperature 22℃, impregnation time 2s, roller pressing pressure 0.2MPa, single-sided bottom layer dry film thickness 100μm; single-sided top layer dry film thickness 20μm, reverse coating roller 18 linear speed to base fabric 8 speed ratio 1.05:1; second drying unit 13 is 70℃ pre-drying for 50s, 100℃ medium temperature plasticizing for 70s, 135℃ high temperature setting for 50s, total drying time 170s; traction tension 6N; the remaining steps and parameters are the same as in Example 2.

[0030] Example 4: The differences between this embodiment and Embodiment 2 are as follows: The bottom adhesive layer PVC paste consists of 100 parts PVC paste resin, 50 parts dioctyl terephthalate, 8 parts polyurethane bonding accelerator, 3 parts calcium-zinc heat stabilizer, and 1 part defoamer; the top layer paste consists of 100 parts PVC paste resin, 45 parts dioctyl terephthalate, 4 parts calcium-zinc heat stabilizer, 2 parts benzotriazole UV absorber, 3 parts isothiazolinone algaecide, 5 parts nano titanium dioxide, 8 parts mica powder, 2 parts abrasion resistant agent, and 2 parts pigment; the base fabric 8 is a 500g / ㎡ high-strength polyester filament base fabric 8 with a 20mm clamping edge, an unwinding tension of 10N, and a running linear speed of 5m / min. n; plasma treatment power 6kW, hot air drying temperature 80℃, base fabric 8 surface tension 52dyn / cm; impregnation tank constant temperature 28℃, impregnation time 5s, roller pressing pressure 0.4MPa, single-sided bottom layer dry film thickness 120μm; single-sided top layer dry film thickness 30μm, reverse coating roller 18 linear speed to base fabric 8 speed ratio 1.2:1; the second drying unit 138 is 90℃ pre-drying for 80s, 130℃ medium temperature plasticizing for 120s, 155℃ high temperature setting for 70s, total drying time 270s; traction tension 12N; the remaining steps and parameters are the same as in Example 2.

[0031] The performance tests conducted on Examples 2 to 4 yielded the results shown in Table 1.

[0032] The test results show that the present invention achieves deep wetting of the base fabric fibers and the bottom slurry through the roll-coating structure, the coating adhesion is stable at level 0, the seawater immersion resistance is greatly improved, and a high thickness of 105-130μm is achieved. The mechanical properties, aging resistance and dimensional stability are excellent, and it fully meets the requirements of use in complex marine working conditions such as deep sea and high load.

[0033] The bottom coating unit 10 of the present invention first coats the base fabric 8 with a bottom layer, and then coats the bottom layer with a top layer by the top layer coating unit 12; the bottom layer and the top layer work together to ensure the adhesion, weather resistance and mechanical strength of the seawater resistant PVC marine fabric, as detailed below: By utilizing the interface transition buffering effect, the contradiction between thick coating and adhesion is resolved: after the base layer cures, a thick and dense adhesive layer is formed, with a surface smoothness far superior to the rough fiber surface of the base fabric 8, providing a smooth anchoring surface for the topcoat; this avoids localized thin coatings or slurry accumulation caused by fiber protrusions when the base fabric 8 is directly coated with the topcoat, reducing the surface thickness error from ±5μm to ±2μm; through the flexible adhesive system of the base layer (containing DOTP plasticizer), the internal stress during the curing of the topcoat can be buffered, reducing the risk of coating cracking caused by thick coating, and the finished product can withstand 1000 flexing cycles without cracking (a single thick coating can only withstand 300 cycles). Double-barrier anti-permeability, greatly improving seawater resistance: The bottom layer fills the gaps between the 8 fibers of the base fabric, forming the first sealing barrier to prevent seawater from seeping in through the fiber gaps; the high-density functional layer on the surface (containing nano-titanium dioxide and mica powder) forms the second protective wall, blocking seawater, salt spray, and ultraviolet radiation. The two layers work together to reduce the seawater permeation rate to 0.01 g / (㎡·24h), far lower than the 0.15 g / (㎡·24h of a single coating. The seawater immersion time is increased from 1000h to 1500h without delamination; the polyurethane adhesive accelerator in the bottom layer forms a chemically compatible interface with the PVC resin in the surface layer, avoiding interlayer peeling caused by seawater penetration, and further strengthening the adhesion from level 0 (the cohesive damage rate of the coating reaches 95% when peeled). The mechanical synergy enhances the overall strength significantly. The bottom layer and the base fabric 8 fibers form a fiber and PVC anchoring structure, while the top layer forms a rigid protective shell. When the two work together under stress, the breaking strength of the finished product is more than 50% higher than that of the base fabric 8 itself (base fabric 8 4000N / 5cm - finished product 7350N / 5cm), far exceeding the sum of the strength of the base fabric 8 and the coating strength. The abrasion-resistant agent (1-2 parts) in the top layer works in conjunction with the flexible system of the bottom layer to further enhance the abrasion resistance of the marine fabric surface. After 1000 cycles of friction (500g load), the coating wear is only 0.02g, which meets the requirements of high-frequency marine use scenarios.

[0034] The above embodiments are merely preferred embodiments of the present invention. Therefore, all equivalent changes or modifications made to the structure, features and principles described in the claims of the present invention are included within the scope of the present invention.

Claims

1. A seawater-resistant PVC ship fabric coating equipment, characterized in that: The system includes an unwinding unit, a pretreatment unit, a bottom impregnation tank unit, a thickness drying unit, a cold pressing and bonding roller group, a bottom coating unit, a first drying unit, a top coating unit, a second drying unit, a gradient cooling and shaping unit, and a winding unit arranged sequentially along the base fabric coating direction. The bottom impregnation tank unit, the bottom coating unit, and the top coating unit are connected to a closed-loop feeding system. The pretreatment unit is a plasma treatment device; The thickness drying unit includes a pair of rolling rolls disposed inside the bottom impregnation tank unit, and a pair of centering rolls disposed directly above the rolling rolls. A hot air drying box is disposed between the rolling rolls and the centering rolls. A thickness-fixing scraper group is disposed between the rolling rolls and the hot air drying box. The thickness-fixing scraper group is disposed directly opposite the scraper bodies disposed on both sides of the base fabric. The cold-pressing and bonding roller assembly consists of mirror-finished cooling rollers arranged symmetrically on the upper and lower sides. The mirror-finished cooling rollers have cooling channels inside, which are connected to a cooling water circulation system. The cold-pressing and bonding roller assembly has an intermittently adjustable structure and is equipped with an independent motor for driving rotation. Both the bottom coating unit and the top coating unit include coating tubes facing each other on the top and bottom surfaces of the base fabric. The coating tubes are connected to a closed-loop feeding system. A coating head is provided on the side of the coating tube facing the base fabric, and a reverse coating roller that presses against the base fabric is provided on the output side of the coating tube. The closed-loop feeding system includes a first mixing tank and a second mixing tank. Vacuum degassing devices are connected to the first and second mixing tanks. A double-spiral belt electric stirrer is installed on the first and second mixing tanks. The first mixing tank is connected to the bottom coating unit and the bottom impregnation tank unit through a first pump group and a replenishment pump, respectively. The second mixing tank is connected to the top coating unit through a second pump group. The second drying unit includes a low-temperature pre-drying section, a medium-temperature plasticizing section, and a high-temperature shaping section arranged sequentially.

2. The seawater-resistant PVC ship fabric coating equipment according to claim 1, characterized in that: The inner top and bottom of the low-temperature pre-drying section, the medium-temperature plasticizing section, and the high-temperature shaping section are all equipped with upper and lower air nozzle arrays facing each other. Each set of upper and lower air nozzle arrays is connected to a variable frequency fan through a duct. The input side of the variable frequency fan is connected to a temperature control box.

3. The seawater-resistant PVC ship fabric coating equipment according to claim 1, characterized in that: The bottom impregnation tank unit includes a sealed impregnation tank with a constant temperature jacket, and multiple guide rollers are arranged inside the sealed impregnation tank; the gradient cooling and shaping unit consists of multiple sets of cooling rollers that gradient cool along the running direction of the base fabric, and each set of cooling rollers is connected to an independent temperature control cooling system.

4. The seawater-resistant PVC ship fabric coating equipment according to claim 1, characterized in that: The pretreatment unit includes a reverse brushing dust removal roller group, a plasma treatment device, a bidirectional synchronous fabric roughening roller group, and a negative pressure dust removal device arranged sequentially along the running direction of the base fabric.

5. The seawater-resistant PVC ship fabric coating equipment according to claim 4, characterized in that: The bidirectional synchronous fabric roughening roller group is symmetrically arranged on both sides of the base fabric, and the roller surface of the bidirectional synchronous fabric roughening roller group has micron-level diamond-shaped wear-resistant protrusions.

6. The seawater-resistant PVC ship fabric coating equipment according to claim 1, characterized in that: Fabric tensioning chains are provided on both sides of the base fabric at the output side of the thickness-fixed scraper assembly; the fabric tensioning chains are arranged along the coating direction of the base fabric.

7. The seawater-resistant PVC ship fabric coating equipment according to claim 6, characterized in that: The winding unit has trimming units on both sides of its input end.

8. A method for preparing seawater-resistant PVC ship fabric, using the seawater-resistant PVC ship fabric coating equipment as described in claim 4, characterized in that, Includes the following steps: S1. Slurry preparation: The bottom adhesive layer PVC slurry and the top seawater resistant functional layer PVC slurry are respectively put into the first mixing tank and the second mixing tank. After stirring, dispersion and vacuum degassing, the temperature is kept constant and stirring is continued. S2. Base fabric unwinding: Install the high-strength polyester filament base fabric in the unwinding unit, set the unwinding tension to 4-10N, and the base fabric enters the pretreatment unit at a set linear speed. S3. Base fabric composite pretreatment: The base fabric is sequentially cleaned by reverse brushing dust removal roller group, surface activated by plasma treatment device, physical micro-roughening by bidirectional synchronous fabric roughening roller group, and dust removal by negative pressure dust removal device. After treatment, the surface tension of the base fabric is ≥48dyn / cm. S4. Full fiber deep impregnation: The base fabric enters the bottom impregnation tank unit and is fully impregnated in the constant temperature slurry along the guide roller path. The slurry completely penetrates into the fiber gaps of the base fabric and is then smoothly fed into the fixed thickness drying unit. S5. Thickness Coating and Pre-drying: The base fabric enters the thickness drying unit and is rolled by the rolling rollers. Then, the base fabric is pulled vertically to the ground by the rolling rollers and the centering rollers. At this time, the gap between the scraper body on both sides of the base fabric and the base fabric is completely consistent. After the base fabric is fully impregnated and rolled, the excess slurry is scraped off by the scraper body. At this time, the base fabric enters the hot air drying box. After being pre-baked at a low temperature of 40-60℃ for 30-60 seconds to form a non-sticky bottom coating, it is then cold-pressed at low pressure by a cold-pressing roller group to eliminate tiny air bubbles between the coating and the base fabric and strengthen the interfacial bonding force. S6. Undercoat coating and pre-drying: The base fabric enters the undercoat unit, and both sides of the base fabric are coated by roller coating in the undercoat unit. The roller coating thickness is 5-10μm, and the fabric is dried by the first drying unit. S7. Topcoat: The base fabric enters the topcoat unit, and the topcoat seawater resistant functional layer slurry is applied to the bottom coating through the coating head of the topcoat unit. Then, it is uniformly coated to a fixed thickness by the reverse coating roller. S8. Segmented gradient drying and curing: The base fabric after coating enters the second drying unit, and then enters the low temperature pre-drying section to maintain a pre-drying temperature of 70-90℃. Next, it passes through the medium temperature plasticizing section to maintain a medium temperature plasticizing temperature of 100-130℃. Finally, it passes through the high temperature setting section to maintain a high temperature setting temperature of 135-155℃. The total drying time is 180-300 seconds. S9. Gradient cooling and shaping: The dried base fabric enters the gradient cooling and shaping unit, and is gradually cooled by multiple sets of cooling rollers to eliminate the internal stress of the coating. S10, Traction and winding: The qualified base fabric is wound by the winding unit with decreasing tension to obtain the finished seawater resistant PVC ship fabric.

9. The method for preparing seawater-resistant PVC ship fabric according to claim 8, characterized in that: The bottom adhesive layer PVC slurry is composed of the following components by weight: 100 parts PVC paste resin, 40-50 parts dioctyl terephthalate, 5-8 parts polyurethane bonding accelerator, 2-3 parts calcium-zinc heat stabilizer, and 0.5-1 parts defoamer; the top seawater resistant functional layer PVC slurry is composed of the following components by weight: 100 parts PVC paste resin, 35-45 parts dioctyl terephthalate, 3-4 parts calcium-zinc heat stabilizer, 1-2 parts benzotriazole ultraviolet absorber, 2-3 parts isothiazolinone algaecide, 3-5 parts nano titanium dioxide, 5-8 parts mica powder, 1-2 parts wear-resistant agent, 1-2 parts titanium dioxide, and 0-2 parts pigment.

10. The method for preparing seawater-resistant PVC ship fabric according to claim 8, characterized in that: The plasma treatment device has a plasma treatment power of 3-6kW and a processing speed that is synchronized with the running speed of the base fabric; the temperature control of the bottom impregnation tank unit is 22-28℃ and the impregnation time of the base fabric is ≥2s; the weight of the high-strength polyester filament base fabric is 200-500g / ㎡ and the breaking strength is ≥4000N / 5cm.