An integrated Fenton-like material, its preparation method and application
By preparing integrated Fenton-like materials, the problems of spatiotemporal separation of oxidant and catalyst and oxidant burst release in traditional Fenton-like technologies have been solved, realizing the microscopic integration of oxidant and catalyst, and ensuring efficient and durable remediation of groundwater and soil.
Patent Information
- Application Number
- CN202610320047.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-03-16
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2046-03-16
AI Technical Summary
Traditional Fenton-like technologies suffer from spatial and temporal separation of oxidants and catalysts, as well as the problem of oxidant burst release, resulting in low remediation efficiency, low reagent utilization, and high treatment costs for groundwater pollutants, making it impossible to achieve sustainable and efficient remediation.
By preparing an integrated Fenton-like material, a nano-calcium peroxide core is coated with a polymer containing amide groups to form a slow-release layer, and an iron sulfide catalyst is chemically anchored on its surface to construct a core-bridge-shell structure, thereby achieving microscopic integration of oxidant and catalyst, and possessing self-supplying oxidant and self-catalytic functions.
It achieves a long-lasting and stable synergistic effect between oxidants and catalysts in underground environments, prolongs the release cycle of H2O2, improves remediation efficiency, and reduces reagent consumption, making it suitable for efficient and long-lasting in-situ remediation of groundwater and soil.
Smart Images

Figure CN122183704B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of water treatment technology, and in particular to an integrated Fenton-like material, its preparation method, and its application. Background Technology
[0002] Organic pollutants in groundwater, such as chlorinated hydrocarbons and petroleum hydrocarbons, have always posed a major challenge to in-situ remediation due to their strong concealment, wide migration and diffusion range, and stable chemical properties. These pollutants are difficult to degrade naturally and can remain in aquifers for a long time, posing a persistent threat to the ecological environment and drinking water safety. In-situ chemical oxidation technology is one of the mainstream methods to address the above challenges. Among them, Fenton-like advanced oxidation technology, which uses solid calcium peroxide (CaO2) as a slow-release source of hydrogen peroxide (H2O2), has been widely used due to its advantages such as strong oxidation capacity, simple operation and high safety. However, the traditional application mode of this technology has the following fundamental defects that are interrelated, which seriously restrict its remediation effect and engineering application value: (1) The problem of spatiotemporal separation of oxidant and catalyst: Existing technologies usually separate solid CaO2 (or its nano-form nCaO2) from iron-based catalysts (such as Fe) 2+ Fe 0 FeS, etc.) are injected into the ground. Due to the significant differences in their physicochemical behavior (such as migration rate and soil adsorption retention) in the complex underground environment, it is difficult for them to achieve and maintain a long-lasting, stable and fully contacted in the target pollution area according to the optimal reaction ratio. This spatiotemporal separation of "oxidant-catalyst" directly causes low reaction efficiency and serious ineffective consumption of reagents; (2) The problem of "burst release" of oxidant and short action cycle: Traditional CaO2 materials, especially the early developed nCaO2, release H2O2 too quickly in the groundwater environment. This "burst release" phenomenon causes the oxidant to decompose rapidly before it can fully react with the pollutants within the pollution plume, resulting in a limited effective action radius. It is unable to cope with the continuous desorption and release of pollutants from soil particles, and may also have an inhibitory effect on the indigenous microbial ecosystem due to the high H2O2 concentration in the short term. The above two major problems of "oxidant-catalyst" separation and "burst release" of oxidant are superimposed, which together lead to incomplete remediation reaction and pollutant rebound, low reagent utilization efficiency and high treatment cost. Summary of the Invention
[0003] In view of this, the purpose of this invention is to provide an integrated Fenton-like material, its preparation method, and its application. The integrated Fenton-like material prepared by this invention achieves the integration of self-supplying oxidant (slow-release H2O2), catalysis (low-valence iron), and pollutant degradation at the microscopic scale. It can migrate autonomously in underground environments and has both long-term slow-release oxidation and high-efficiency catalytic functions, enabling efficient in-situ remediation of soil / groundwater.
[0004] To achieve the above-mentioned objectives, the present invention provides the following technical solution: This invention provides a method for preparing an integrated Fenton-like material, comprising the following steps: A polymer with amide groups, water, and sodium hydroxide are mixed and hydrolyzed to obtain a hydrolyzed reaction solution; the hydrolysis reaction is carried out under conditions of pH ≥ 11. The hydrolysis reaction solution is mixed with a soluble calcium salt to carry out an ion exchange reaction, thereby obtaining an ion exchange reaction solution; The ion-displacement reaction solution was mixed with hydrogen peroxide solution to carry out a metathesis reaction, thereby obtaining a slow-release nano-calcium peroxide material. A precipitation reaction was carried out on a ferrous salt solution under conditions of pH ≥ 12 to obtain a ferrous hydroxide insoluble system. The slow-release nano-calcium peroxide material was mixed with the ferrous hydroxide insoluble system and a coordination reaction was carried out to obtain an integrated Fenton-like material precursor. The integrated Fenton-like material precursor is mixed with sodium borohydride and sodium sulfide and then subjected to in-situ reduction-sulfidation to obtain the integrated Fenton-like material.
[0005] Preferably, the polymer having amide groups includes one or more of polyacrylamide, polyvinylpyrrolidone, and poly(N-isopropylacrylamide); the hydrolysis reaction takes 2-4 hours.
[0006] Preferably, the mass ratio of the polymer with amide groups to the soluble calcium salt used to prepare the hydrolysis reaction solution is (0~25):6, and the mass ratio is not 0:6; the ion exchange reaction time is 2~5h.
[0007] Preferably, the metathesis reaction takes 2 to 4 hours.
[0008] Preferably, the concentration of ferrous salt in the ferrous salt solution is 10-15 g / L, the solvent of the ferrous salt solution is an aqueous methanol solution, and the volume fraction of methanol in the aqueous methanol solution is 30%.
[0009] Preferably, the mass ratio of iron in the slow-release nano-calcium peroxide material to the ferrous hydroxide insoluble system is 1:(0.1~0.3); the coordination reaction time is 0.5~3h.
[0010] Preferably, the molar ratio of sulfur in the sodium sulfide to iron in the integrated Fenton-like material precursor is (0~0.4):1, and the amount of sulfur is not 0; the in-situ reduction-sulfidation time is 0.5~2h.
[0011] This invention provides an integrated Fenton-like material prepared by the preparation method described above. The integrated Fenton-like material includes a slow-release nano-calcium peroxide and an iron-based catalyst anchored on the surface of the slow-release nano-calcium peroxide. The slow-release nano-calcium peroxide includes nano-calcium peroxide and a polymer slow-release layer anchored on the surface of the nano-calcium peroxide. The iron-based catalyst is an iron sulfide.
[0012] Preferably, the particle size of the integrated Fenton-like material is <500nm.
[0013] This invention provides the application of the integrated Fenton-like material described above in soil and groundwater remediation.
[0014] This invention provides a method for preparing an integrated Fenton-like material. The invention utilizes functional groups (such as carboxylate groups formed by the hydrolysis of amide groups) in a polymer bridge layer to chemically anchor the calcium peroxide core and the iron / sulfur precursor sequentially, synthesizing and loading a catalyst in situ, thus achieving structural stability and functional integration. Specifically, this invention creatively selects a polymer coating as the functional "bridge" layer. The unsaturated functional groups abundant in its molecular chain first tightly encapsulate and anchor the nano-calcium peroxide "core" through electrostatic adsorption and cross-linking, forming an intermediate layer with slow-release function (slow-release nano-calcium peroxide material). Subsequently, the same functional groups serve as active sites, chemically adsorbing and fixing iron precursor ions, synthesizing and loading an iron sulfide catalyst "shell" layer in situ. This invention designs an integrated Fenton-like material with a "core-bridge-shell" three-layer structure based on chemical anchoring, as described above. This design, at the nanoscale, achieves stable encapsulation of the oxidant (nano-calcium peroxide) core and strong bonding of the catalyst shell through the functional groups of the same polymer, thereby pre-constructing a microenvironment tightly coupled with the oxidant's slow release and catalytic reaction within a single particle. This invention has the following beneficial effects: (1) It fundamentally solves the problem of "spatiotemporal separation" between oxidant and catalyst, ensuring that the two always work synergistically in the optimal spatial relationship in complex underground environments; (2) It utilizes the controllable diffusion characteristics of polymer layers to achieve sustained and gradual release of H2O2, overcoming the problem of "explosive release"; (3) The prepared material is a nanoscale, mobile, self-supplying oxidant and self-catalyzing remediation material. When injected into the strata, it can migrate autonomously and construct a continuous, Fenton-like reaction zone in situ with both long-term slow-release oxidation and efficient self-catalysis functions, thereby achieving efficient, thorough and sustained in-situ remediation of organic pollution in groundwater, without relying on external continuous supply of agents or the creation of complex engineering. Attached Figure Description
[0015] Figure 1 SEM image of the integrated Fenton-like material prepared in Example 1 using poly(N-isopropylacrylamide) as the core and shell (S / Fe molar ratio = 0.2). Figure 2 SEM image of the integrated Fenton-like material prepared using polyvinylpyrrolidone as the core and shell in Example 2 (S / Fe molar ratio = 0.3). Figure 3 SEM image of the integrated Fenton-like material prepared using polyacrylamide as the core and shell in Example 3 (S / Fe molar ratio = 0.3). Figure 4 Particle size distribution of an integrated Fenton-like material prepared using poly(N-isopropylacrylamide) as the core and shell (S / Fe molar ratio = 0.2). Figure 5 The particle size distribution of an integrated Fenton-like material prepared using polyvinylpyrrolidone as the core and shell (S / Fe molar ratio = 0.3). Figure 6 Particle size distribution of an integrated Fenton-like material prepared using polyacrylamide as the core and shell (S / Fe molar ratio = 0.3). Figure 7 The infrared spectrum of the integrated Fenton-like material prepared using poly(N-isopropylacrylamide), polyvinylpyrrolidone, and polyacrylamide as the core and shell in the example is shown. Figure 8 The XRD spectrum of the integrated Fenton-like material prepared by using poly(N-isopropylacrylamide), polyvinylpyrrolidone and polyacrylamide as the core and shell in the example is shown. Figure 9 The image shows the effect of integrated Fenton-like materials prepared under different degrees of vulcanization using poly(N-isopropylacrylamide) as the core and shell in Example 1 on the degradation of trichlorophenol (S / Fe molar ratio = 0, 0.1, 0.2, 0.3, 0.4, temperature = 25℃, pH 0 = 7). Figure 10 The image shows the effect of integrated Fenton-like materials prepared under different degrees of vulcanization using polyvinylpyrrolidone as the core and shell in Example 2 on the degradation of trichlorophenol (S / Fe molar ratio = 0, 0.1, 0.2, 0.3, 0.4, temperature = 25℃, pH 0 = 7). Figure 11 The image shows the effect of integrated Fenton-like material prepared under different degrees of vulcanization with polyacrylamide as the core and shell in Example 3 on the degradation of trichlorophenol (S / Fe molar ratio = 0, 0.1, 0.2, 0.3, 0.4, temperature = 25℃, pH 0 = 7). Figure 12 This is a schematic diagram of a two-dimensional sandbox model for removing trichlorophenol from groundwater by in-situ injection of an integrated Fenton-like material in an embodiment. Figure 13The time relationship between the release of nano-calcium peroxide encapsulated with polyacrylamide, polyvinylpyrrolidone, poly(N-isopropylacrylamide) and unencapsulated nano-calcium peroxide is shown in the figure (temperature = 25℃, pH 0 = 7). Detailed Implementation
[0016] This invention provides a method for preparing an integrated Fenton-like material, comprising the following steps: A polymer with amide groups, water, and sodium hydroxide are mixed and hydrolyzed to obtain a hydrolyzed reaction solution; the hydrolysis reaction is carried out under conditions of pH ≥ 11. The hydrolysis reaction solution is mixed with a soluble calcium salt to carry out an ion exchange reaction, thereby obtaining an ion exchange reaction solution; The ion-displacement reaction solution was mixed with hydrogen peroxide solution to carry out a metathesis reaction, thereby obtaining a slow-release nano-calcium peroxide material. A precipitation reaction was carried out on a ferrous salt solution under conditions of pH ≥ 12 to obtain a ferrous hydroxide insoluble system. The slow-release nano-calcium peroxide material was mixed with the ferrous hydroxide insoluble system and a coordination reaction was carried out to obtain an integrated Fenton-like material precursor. The integrated Fenton-like material precursor is mixed with sodium borohydride and sodium sulfide and then subjected to in-situ reduction-sulfidation to obtain the integrated Fenton-like material.
[0017] Unless otherwise specified, all raw materials involved in this invention are commercially available products well known in the art.
[0018] This invention involves mixing a polymer with amide groups, water, and sodium hydroxide to perform a hydrolysis reaction, thereby obtaining a hydrolysis reaction solution.
[0019] In this invention, the polymer having amide groups preferably includes one or more of polyacrylamide, polyvinylpyrrolidone, and poly(N-isopropylacrylamide). The weight-average molecular weight of the polymer having amide groups is preferably 58,000 to 5,000,000. In specific embodiments of this invention, the weight-average molecular weight of the polyacrylamide is 5,000,000, the weight-average molecular weight of the polyvinylpyrrolidone is 58,000, and the weight-average molecular weight of the poly(N-isopropylacrylamide) is 300,000. This invention uses polymers having amide groups as the core-shell of nano-calcium peroxide. In this invention, the water is preferably ultrapure water; in specific embodiments of this invention, the ratio of the polymer having amide groups to water is 2.0 to 3.0 g: 100 mL, which can be 2.0 g: 100 mL, 2.5 g: 100 mL, or 3.0 g: 100 mL.
[0020] In this invention, the hydrolysis reaction is carried out under conditions where the pH value is ≥11 (e.g., 11.0, 11.5, 12.0), and the amount of sodium hydroxide added is determined to meet the above pH requirement. Preferably, the polymer with amide groups is dissolved in water, and sodium hydroxide is added to it under stirring at room temperature to adjust the pH value of the system to ≥11; the sodium hydroxide can be added dropwise in the form of a sodium hydroxide solution, and the concentration of the sodium hydroxide solution can be 5 mol / L.
[0021] Under alkaline conditions with a pH ≥ 11, the unsaturated functional groups (partially amide groups) in the polymer molecular chain undergo hydrolysis, exposing abundant carboxylate ions. These carboxylate ions combine with sodium ions (provided by sodium hydroxide) in the solution to form a -R-COONa structure. In this invention, the hydrolysis reaction time is preferably 2-4 hours, which can be 2, 3, or 4 hours, to ensure complete transformation of the functional groups. The hydrolysis reaction is preferably carried out at room temperature with continuous stirring. In this invention, the resulting hydrolysis reaction solution can also be referred to as a pretreated polymer solution.
[0022] After obtaining the hydrolysis reaction solution, the present invention mixes the hydrolysis reaction solution with a soluble calcium salt to carry out an ion exchange reaction to obtain an ion exchange reaction solution.
[0023] In this invention, the soluble calcium salt can be calcium chloride, and it can be added in the form of an aqueous solution of calcium salt, with a concentration of 1~1.2 mol / L. In this invention, the preferred mass ratio of the polymer with amide groups to the soluble calcium salt used in preparing the hydrolysis reaction solution is (0~25):6 (and the mass ratio is not 0:6), and can be 2:6, 3:6, 5:6, 10:6, 15:6, 20:6, or 25:6. Preferably, the soluble calcium salt is added to the hydrolysis reaction solution.
[0024] In this invention, the preferred time for the ion exchange reaction is 2-5 hours, specifically 2, 3, 4, or 5 hours. The ion exchange reaction is preferably carried out at room temperature with stirring. In this invention, the pH value is above 11 during the ion exchange reaction. Specifically, in an alkaline environment, calcium ions undergo an ion exchange reaction with sodium ions in -R-COONa to form a [-R-COO-]2Ca crosslinked structure with calcium ions as the bridging center. This invention establishes a stable crosslinked network between polymer chains through calcium ions, providing anchoring sites for the subsequent heterogeneous nucleation and growth of calcium peroxide.
[0025] After obtaining the ion-exchange reaction solution, the present invention mixes the ion-exchange reaction solution with hydrogen peroxide solution to carry out a metathesis reaction to obtain a slow-release nano-calcium peroxide material.
[0026] In this invention, the mass fraction of the hydrogen peroxide solution is preferably 30%, and the hydrogen peroxide solution is preferably in excess. Preferably, the hydrogen peroxide solution is slowly added dropwise to the ion exchange reaction solution under ice-water bath conditions (controlling the reaction temperature to not exceed 25°C to prevent hydrogen peroxide decomposition); after the addition is complete, the ice-water bath is removed, and the metathesis reaction is carried out under stirring.
[0027] In this invention, the metathesis reaction time is preferably 2-4 hours, but can be 2, 3, or 4 hours. During the metathesis reaction, calcium ions anchored on the polymer network combine with peroxide ions diffused into the network, generating calcium peroxide precipitate in situ on the polymer network framework. The key mechanism is that the surface of the newly generated calcium peroxide nanocrystals has a large number of unsaturated coordinated calcium ions. These surface calcium ions have a strong coordination tendency and will further combine with carboxylate ions in the polymer network that have been cross-linked by calcium ions in the solution, forming a more stable "surface calcium carboxylate complex". This process achieves chemical bonding between the calcium peroxide crystals and the polymer network, rather than simple physical encapsulation.
[0028] After the metathesis reaction is completed, the present invention preferably subjectes the resulting reaction solution to solid-liquid separation, solid-phase washing, and drying sequentially to obtain a slow-release nano-calcium peroxide material. In this invention, the solid-liquid separation can be performed by centrifugation at 3000 rpm for 10 minutes; the solid-phase washing preferably uses anhydrous ethanol as the washing reagent, and the washing can be performed three times to remove impurities and soluble salts; the drying temperature is preferably 60°C, and the drying time is preferably 8 hours, and the drying can be carried out in a vacuum drying oven.
[0029] This invention involves precipitating a ferrous salt solution under conditions of pH ≥ 12 to obtain a ferrous hydroxide insoluble system.
[0030] In this invention, the ferrous salt in the ferrous salt solution can be ferrous sulfate heptahydrate, and the concentration of the ferrous salt in the ferrous salt solution is preferably 10~15 g / L; the solvent of the ferrous salt solution is preferably an aqueous methanol solution, and the volume fraction of methanol in the aqueous methanol solution is preferably 30%, and the methanol in the aqueous methanol solution is used to slow down the oxidation of iron ions under subsequent strong alkaline conditions.
[0031] In this invention, the pH value ≥ 12 (which can be 12 or 12.5) is preferably obtained by adjusting with sodium hydroxide solution, and the concentration of the sodium hydroxide solution can be 5 mol / L. This high pH environment serves multiple purposes: first, it forms positively charged ferrous hydroxide particles, which readily electrostatically adsorb with the negatively charged carboxylate and other functional groups on the surface of the aforementioned slow-release nano-calcium peroxide; second, it creates a strongly alkaline environment to inhibit the hydrolysis of calcium peroxide in the subsequently added slow-release nano-calcium peroxide, maintaining its structural stability; and third, it inhibits the occurrence of Fenton-like reactions, preventing the reaction of hydrogen peroxide generated from the trace hydrolysis of calcium peroxide with low-valence iron, thereby maintaining the stability of the system.
[0032] In this invention, the entire precipitation reaction is carried out under continuous nitrogen gas flow to prevent the oxidation of ferrous ions. In this invention, the precipitation reaction forms an insoluble ferrous hydroxide (ferrous hydroxide colloid or precipitate). After the precipitation reaction is completed, the next reaction is immediately carried out.
[0033] After obtaining the ferrous hydroxide insoluble system, the present invention mixes the slow-release nano-calcium peroxide material with the ferrous hydroxide insoluble system to carry out a coordination reaction to obtain an integrated Fenton-like material precursor.
[0034] In this invention, the slow-release nano-calcium peroxide material is preferably added to the ferrous hydroxide insoluble system under nitrogen protection. In this invention, the mass ratio of the slow-release nano-calcium peroxide material to the iron in the ferrous hydroxide insoluble system is preferably 1:(0.1~0.3), but can be 1:0.1, 1:0.15, or 1:0.2. In this invention, the coordination reaction time is preferably 0.5~3 hours, but can be 1 hour. The coordination reaction is preferably carried out at room temperature with stirring. Specifically, in this invention, the coordination reaction involves the coordination of carboxylate groups on the surface of the slow-release nano-calcium peroxide material with iron atoms on the surface of the ferrous hydroxide insoluble material, thereby achieving chemical anchoring of the iron precursor on the carrier surface. After the coordination reaction, the next step is directly performed.
[0035] After obtaining the integrated Fenton-like material precursor, the present invention mixes the integrated Fenton-like material precursor with sodium borohydride and sodium sulfide for in-situ reduction-sulfidation to obtain the integrated Fenton-like material.
[0036] In this invention, the amount of sodium borohydride added is sufficient to reduce the ferrous ions in the integrated Fenton-like material to zero-valent iron (Fe). 0 The standard is based on the following equation: .
[0037] In this invention, the molar ratio of sulfur in the sodium sulfide to iron in the integrated Fenton-like material precursor is preferably (0~0.4):1 (and the amount of sulfur is not zero), and can be 0.1:1, 0.2:1, 0.3:1, or 0.4:1. In an embodiment of this invention, the sodium sulfide is added in the form of Na2S·9H2O, and the sodium borohydride and sodium sulfide are added in the form of a mixed aqueous solution containing sodium borohydride and sodium sulfide. Specifically, under nitrogen protection, the mixed aqueous solution containing sodium borohydride and sodium sulfide is added dropwise to the integrated Fenton-like material precursor.
[0038] In this invention, the in-situ reduction-sulfidation time is preferably 0.5~2 hours, and can be 1 hour. The in-situ reduction-sulfidation time is calculated from the point when sodium borohydride and sodium sulfide are completely added. In this invention, the reaction occurring during the in-situ reduction-sulfidation process is as follows: the iron precursor previously fixed through coordination is reduced to zero-valent iron (Fe) by sodium borohydride. 0 The catalyst consists of nanoparticles; simultaneously, the sulfur source provided by sodium sulfide reacts with iron species to generate iron sulfides in situ. Crucially, the entire reduction and sulfidation reaction occurs on iron species coordinated with carboxylate groups on the surface of the support (slow-release nano-calcium peroxide material). This ensures that the newly generated iron sulfide nanoparticles are firmly "anchored" to the support surface through direct surface coordination, thus achieving a stable integration of the catalyst and the slow-release oxidant support. This invention, by precisely controlling the dosage of sodium sulfide, can prepare a series of iron sulfide catalysts with different S / Fe molar ratios (e.g., 0, 0.1:1, 0.2:1, 0.3:1, or 0.4:1) (in this invention, iron sulfides with different S / Fe molar ratios are also referred to as FeS) to optimize their catalytic performance.
[0039] After the in-situ reduction-sulfurization is completed, the present invention preferably performs solid-liquid separation, solid-phase washing, and drying sequentially on the obtained reaction solution to obtain the integrated Fenton-like material. In the present invention, the solid-liquid separation can be centrifugation, which is preferably carried out under nitrogen protection, at a speed of 3000 rpm for 10 min; the solid-phase washing is preferably performed three times with deoxyethanol to remove residual reactants and byproducts; the drying temperature is preferably 60°C, and the drying time is preferably 8 h, which can be carried out in a vacuum drying oven.
[0040] This invention constructs an integrated Fenton-like material by loading an iron sulfide catalyst onto the surface of a slow-release nano-calcium peroxide material through surface impregnation and chemical reduction.
[0041] Currently, traditional in-situ chemical oxidation technology, based on the separate injection of oxidant and catalyst, is one of the main methods for remediating organic pollution in groundwater. However, this technology has a key limitation: the injected oxidant and catalyst exhibit significantly different migration and retention behaviors in the formation, making it impossible for them to achieve and maintain effective spatiotemporal contact within the target contaminated area. This separation of "oxidant-catalyst" severely restricts the efficiency of Fenton-like reactions, leading to problems such as poor remediation effects, low reagent utilization, short effective period, and pollutant rebound. Therefore, this invention aims to focus on solving the core technical problem of "how to ensure that the oxidant and catalyst can work synergistically and persistently in a near-optimal reaction ratio in complex underground environments," in order to overcome the technical bottlenecks of low remediation efficiency, poor reagent utilization, short action time, and easy pollutant rebound caused by the separation of the two in traditional in-situ chemical oxidation technology. This invention creates a nanocomposite material with a "core (nCaO2)-bridge (polymer coating)-shell (catalyst)" structure. This single material simultaneously possesses the functions of a calcium peroxide slow-release oxidant and an iron-based catalyst, achieving integration of self-supplying oxidant (slow-release H2O2), self-catalysis (low-valence iron), and pollutant degradation at the microscale. This material can be directly injected into underground contaminated areas, autonomously migrating within porous media at the nanoscale to construct dispersed, mobile, and long-lasting Fenton-like reaction zones in situ. It eliminates the need for continuous external addition of reactants, representing a fundamental leap from "fixed reactors / devices" to "intelligent reactive remediation materials," making it particularly suitable for the complex needs of in-situ soil / groundwater remediation.
[0042] This invention provides an integrated Fenton-like material prepared by the preparation method described above. The integrated Fenton-like material includes a slow-release nano-calcium peroxide and an iron-based catalyst anchored on the surface of the slow-release nano-calcium peroxide. The slow-release nano-calcium peroxide includes nano-calcium peroxide and a polymer slow-release layer anchored on the surface of the nano-calcium peroxide. The iron-based catalyst is an iron sulfide.
[0043] In this invention, the particle size of the integrated Fenton-like material is <500nm.
[0044] This invention provides the application of the integrated Fenton-like material described above in soil and groundwater remediation. In this invention, the pollutants in the soil and groundwater are preferably organic pollutants, such as chlorinated hydrocarbons and benzene series pollutants. Trichlorophenol is used as an example in the embodiments of this invention.
[0045] This invention provides a novel material solution that systematically overcomes the core shortcomings of current in-situ chemical oxidation technologies for groundwater through innovative design at three levels: "structural integration," "controllable release," and "autonomous function." Ultimately, it achieves efficient, sustainable, economical, and environmentally friendly in-situ remediation of organic pollution in groundwater. Details are as follows: 1. Solve the spatiotemporal separation of "oxidant-catalyst" to achieve integrated microscale contact and highly efficient catalysis. The biggest bottleneck in existing technologies lies in the physical separation of the oxidant (CaO2 / H2O2) and the catalyst (such as FeS) in the underground environment, which makes it difficult to form a reaction interface and results in low efficiency. This invention fundamentally changes this situation by creating a three-layer nanocomposite material with a "core (nCaO2)-bridge (polymer coating)-shell (FeS)" structure. The core solution is: Chemical anchoring and structural integration: Utilizing the electronegativity of functional groups such as carboxylate groups after hydrolysis on the polymer coating surface (e.g., polyvinylpyrrolidone (PVP)), a slow-release layer (bridge) is first formed by cross-linking and coating a nano-calcium peroxide core. Subsequently, using the same functional group as an active site, iron and sulfur precursor ions are chemically adsorbed, and a catalyst shell (shell) supported by ferrous sulfide (FeS) is synthesized and stabilized in situ. This design, at the nanoscale, integrates the oxidant and catalyst into a stable composite unit through chemical action rather than physical mixing.
[0046] Achieving long-term synergy: This structure ensures that after the material is injected underground, no matter how it migrates, the oxidant release point (core) and the catalytic reaction site (shell) always maintain close contact and a fixed ratio at the nanoscale, eliminating the separation problem caused by the difference in migration between the two in traditional methods, and providing the optimal microscopic reaction environment for continuous and efficient Fenton-like reactions.
[0047] 2. Solve the problem of "burst release" of oxidants and achieve long-term, controllable, and sustained release of H2O2. Traditional nCaO2 releases H2O2 too quickly, resulting in a short reaction period and limited effective radius. This invention provides a solution through the design of a functionalized polymer "bridge" layer: Controlled diffusion barrier: The polymer coating forms a hydrophilic gel layer with controllable porosity and thickness on the nCaO2 surface. This layer acts as a smart diffusion barrier, effectively slowing down the rate of water molecule penetration into the core and the rate of H2O2 diffusion outward.
[0048] Achieving sustained oxidant supply: By controlling the thickness of the polymer coating, the release kinetics of H2O2 can be precisely controlled, transforming "burst release" into a gradual and sustained "slow release". This makes the release rate of H2O2 more compatible with the mass transfer and degradation rate of pollutants in groundwater, thereby significantly extending the effective action time of the material and expanding its radius of influence.
[0049] 3. Overcoming limitations in material migration and functional dependence to achieve in-situ, long-term, autonomous repair. Existing improved materials are either too large to migrate or have limited functionality and rely on external conditions. This invention provides a "smart reactive remediation material" that integrates self-supplying oxidant, self-catalysis, and excellent migration properties. Functional integration and self-driving: A single composite particle is a complete "micro-reaction station" that integrates an oxidant slow-release source (nCaO2 core) and a catalyst (FeS shell). It does not rely on the continuous addition of H2O2 or iron salts from the outside, thus realizing the self-powered and self-driving of the reaction system.
[0050] Nanoscale and mobility: The material is nanoscale in size (<500nm), which enables it to migrate and diffuse effectively in the soil pore media of underground aquifers. This allows it to construct a widely distributed, uniform, and mobile "Fenton-like reaction zone" in situ within the target contaminated area (such as a contamination plume) through injection wells, rather than a fixed treatment point or a limited reaction zone.
[0051] Adaptable to complex environments: This design concept makes the present invention particularly suitable for remediating groundwater contaminated with chlorinated hydrocarbons, benzene compounds, and other pollutants that are difficult to remediate and have a wide range of contamination. The material can migrate to the core contaminated area and downstream by flowing groundwater or through active injection. Through the sustained release of H2O2 and the in-situ highly efficient catalytic FeS, it continuously generates strong oxidizing free radicals (such as ·OH), achieving efficient degradation of pollutants and effectively suppressing the concentration rebound problem caused by the continuous release of pollutants from the source or incomplete remediation.
[0052] To further illustrate the present invention, the integrated Fenton-like material, its preparation method, and its application provided by the present invention are described in detail below with reference to examples, but these should not be construed as limiting the scope of protection of the present invention.
[0053] Example 1 Preparation of a poly(N-isopropylacrylamide)-based integrated Fenton-like material. The amide groups of poly(N-isopropylacrylamide) hydrolyze to carboxylate groups under alkaline conditions. After crosslinking with calcium ions, a thermosensitive hydrogel network is formed, which is beneficial for controlling the release rate of calcium peroxide. The specific preparation steps are as follows: Step 1: Preparation of slow-release nano-calcium peroxide Polymer pretreatment: Weigh 2.0 g of poly(N-isopropylacrylamide) (weight average molecular weight: 300,000) and dissolve it in 100 mL of ultrapure water. Under stirring at room temperature, slowly add 5 M sodium hydroxide solution dropwise to adjust the pH of the system to 11.5. Under these alkaline conditions, continue stirring and hydrolyzing for 3 h to convert the amide groups (-CONH-) on the poly(N-isopropylacrylamide) chains to carboxylate groups (-COONa). The solution viscosity may increase slightly at this point.
[0054] Calcium ion crosslinking: Add 50 mL of an aqueous solution containing 0.05 mol of calcium chloride (CaCl2) to the above pretreatment solution. Stir continuously for 3 hours. During this process, Ca... 2+ It undergoes ion exchange with -COONa to form a (-COO)2Ca cross-linked structure.
[0055] Preparation of calcium peroxide deposition: Under ice-water bath conditions (controlling the reaction temperature not to exceed 25℃ to prevent hydrogen peroxide decomposition), 30 mL of 30 wt% hydrogen peroxide (H2O2) solution was slowly added dropwise to the above system. After the addition was complete, the ice-water bath was removed, and the reaction was continued to be stirred for 3 h to allow calcium peroxide to nucleate heterogeneously in the cross-linked network. Subsequently, the mixture was centrifuged at 3000 rpm for 10 min, and the supernatant was discarded. The precipitate was washed three times with anhydrous ethanol (50 mL each time), and finally placed in a vacuum drying oven and dried at 60℃ for 8 h to obtain a white powder of poly(N-isopropylacrylamide) embedded slow-release nano-calcium peroxide.
[0056] Step 2: Supporting the FeS catalyst Iron precursor adsorption: Dissolve 1.0 g of ferrous sulfate heptahydrate (FeSO4·7H2O) in 100 mL of 30% (v / v) methanol / water solution. Purge with nitrogen (N2) for 20 min to remove oxygen. Under nitrogen protection, add 5 M NaOH dropwise to adjust the pH to 12.5, forming a dark green precipitate of ferrous hydroxide. Immediately add 2.0 g of the powder prepared in step one, and stir for 1 h to allow the carboxyl groups on the support surface to fully adsorb Fe. 2+ / Fe(OH)2.
[0057] Reduction and Sulfidation: Under a nitrogen atmosphere, slowly add 50 mL of a mixed solution containing 0.03 mol sodium borohydride (NaBH4) and varying amounts of sodium sulfide (Na2S·9H2O) dropwise to the resulting suspension. Calculate the amount of sodium sulfide to be added based on the target S / Fe molar ratio (e.g., 0.2). After the addition is complete, continue the reaction for 1 h to reduce the iron species to Fe. 0 FeS was generated. Subsequently, the mixture was centrifuged under nitrogen protection (3000 rpm, 10 min), the solid was washed three times with deoxyethanol, and vacuum dried (60 °C, 8 h) to obtain poly(N-isopropylacrylamide) integrated Fenton-like material.
[0058] Example 2 The preparation steps for polyvinylpyrrolidone-based integrated Fenton-like materials are as follows: Step 1: Polymer pretreatment: Weigh 3.0 g of polyvinylpyrrolidone (weight average molecular weight: 58000) and dissolve it in 100 mL of ultrapure water. Adjust the pH to 12.0 using 5 M NaOH. Stir and hydrolyze for 4 h to expose the carboxyl groups and form a -COONa structure.
[0059] Calcium ion crosslinking: 50 mL of a solution containing 0.06 mol of calcium chloride (CaCl2) was slowly added to the hydrolyzed polyvinylpyrrolidone solution. The reaction was stirred continuously for 2 hours. During this process, Ca... 2+ It undergoes ion exchange with -COONa to form a (-COO)2Ca cross-linked structure.
[0060] Preparation of calcium peroxide deposition: Under ice-water bath conditions (controlling the reaction temperature not to exceed 25℃ to prevent hydrogen peroxide decomposition), 30 mL of 30 wt% hydrogen peroxide (H2O2) solution was slowly added dropwise to the above system. After the addition was complete, the ice-water bath was removed, and the reaction was continued with stirring for 3 h to allow calcium peroxide to nucleate heterogeneously in the cross-linked network. Subsequently, the mixture was centrifuged at 3000 rpm for 10 min, and the supernatant was discarded. The precipitate was washed three times with anhydrous ethanol (50 mL each time), and finally placed in a vacuum drying oven and dried at 60℃ for 8 h to obtain a white powder of sustained-release nano-calcium peroxide embedded in polyvinylpyrrolidone.
[0061] Step 2: Supporting the FeS catalyst Iron precursor adsorption: 1.5 g FeSO4·7H2O was dissolved in 100 mL of 30% (v / v) methanol / water solution. Nitrogen gas (N2) was bubbled through for 20 min to remove oxygen. Under nitrogen protection, 5 M NaOH was added dropwise to adjust the pH to 12.5, forming a dark green precipitate of ferrous hydroxide. Immediately, 2.0 g of the powder prepared in step one was added, and the mixture was stirred for 1 h to allow the carboxyl groups on the support surface to fully adsorb Fe. 2+ / Fe(OH)2.
[0062] Reduction and Sulfidation: Under a nitrogen atmosphere, slowly add 50 mL of a mixed solution containing 0.03 mol sodium borohydride (NaBH4) and varying amounts of sodium sulfide (Na2S·9H2O) dropwise to the resulting suspension. Calculate the amount of sodium sulfide to be added based on the target S / Fe molar ratio (e.g., 0.3). After the addition is complete, continue the reaction for 1 h to reduce the iron species to Fe. 0 FeS was generated. Subsequently, the mixture was centrifuged under nitrogen protection (3000 rpm, 10 min), the solid was washed three times with deoxyethanol, and vacuum dried (60 °C, 8 h) to obtain polyvinylpyrrolidone-based integrated Fenton-like material.
[0063] Example 3 The preparation steps for polyacrylamide-based integrated Fenton-like materials are as follows: Step 1: Polymer Pretreatment: Weigh 2.5g of polyacrylamide (weight average molecular weight: 5,000,000) and disperse it in 100mL of ultrapure water (polyacrylamide has limited solubility in water, so vigorous stirring is required to form an emulsion). Adjust the pH to 11.0 using 5M NaOH. Stir and hydrolyze for 4 hours to hydrolyze the acrylate end groups to generate carboxylate (-COONa) (observe whether the system becomes clear).
[0064] Calcium ion crosslinking: Slowly add 50 mL of a solution containing 0.06 mol of calcium chloride (CaCl2) to the system. Continue stirring for 2 hours. During this process, Ca... 2+ It undergoes ion exchange with -COONa to form a (-COO)2Ca cross-linked structure.
[0065] Preparation of calcium peroxide by deposition: Under ice-water bath conditions (controlling the reaction temperature not to exceed 25℃ to prevent decomposition of hydrogen peroxide), 30 mL of 30 wt% hydrogen peroxide (H2O2) solution was slowly added dropwise to the above system. After the addition was complete, the ice-water bath was removed, and the reaction was continued to be stirred for 3 h to allow calcium peroxide to nucleate heterogeneously in the cross-linked network. Subsequently, the mixture was centrifuged at 3000 rpm for 10 min, the supernatant was discarded, and the precipitate was washed three times with anhydrous ethanol (50 mL each time). Finally, it was placed in a vacuum drying oven and dried at 60℃ for 8 h to obtain a white powder of sustained-release nano-calcium peroxide embedded in polyacrylamide.
[0066] Step 2: Supporting the FeS catalyst Iron precursor adsorption: Dissolve 1 g of FeSO4·7H2O in 100 mL of 30% (v / v) methanol / water solution. Purge with nitrogen (N2) for 20 min to remove oxygen. Under nitrogen protection, add 5 M NaOH dropwise to adjust the pH to 12.5, forming a dark green ferrous hydroxide precipitate. Immediately add 2.0 g of the powder prepared in step one, and stir for 1 h to allow the carboxyl groups on the support surface to fully adsorb Fe. 2+ / Fe(OH)2.
[0067] Reduction and Sulfidation: Under a nitrogen atmosphere, slowly add 50 mL of a mixed solution containing 0.03 mol sodium borohydride (NaBH4) and varying amounts of sodium sulfide (Na2S·9H2O) dropwise to the resulting suspension. Calculate the amount of sodium sulfide to be added based on the target S / Fe molar ratio (e.g., 0.3). After the addition is complete, continue the reaction for 1 h to reduce the iron species to Fe. 0FeS was generated. Subsequently, the mixture was centrifuged under nitrogen protection (3000 rpm, 10 min), the solid was washed three times with deoxyethanol, and then vacuum dried (60 °C, 8 h) to obtain a polyacrylamide-based integrated Fenton-like material.
[0068] Figure 1 The image shows a SEM image of the integrated Fenton-like material prepared in Example 1 using poly(N-isopropylacrylamide) as the core and shell (S / Fe molar ratio = 0.2). Figure 2 The image shows a SEM image of the integrated Fenton-like material prepared using polyvinylpyrrolidone as the core and shell in Example 2 (S / Fe molar ratio = 0.3). Figure 3 The image shows a SEM image of the integrated Fenton-like material prepared in Example 3 using polyacrylamide as the core and shell (S / Fe molar ratio = 0.3). The integrated Fenton-like materials prepared using poly(N-isopropylacrylamide) and polyvinylpyrrolidone as the core and shell both exhibit regular spherical structures, while the integrated Fenton-like material prepared using polyacrylamide as the core and shell shows a clustered development. The average particle size of the three materials was measured using a laser particle size analyzer, and the results are as follows: Figures 4-6 As shown ( Figure 4 The particle size distribution of an integrated Fenton-like material prepared using poly(N-isopropylacrylamide) as the core and shell (S / Fe molar ratio = 0.2). Figure 5 The particle size distribution of an integrated Fenton-like material prepared using polyvinylpyrrolidone as the core and shell (S / Fe molar ratio = 0.3). Figure 6 The particle size distribution of the integrated Fenton-like material prepared using polyacrylamide as the core and shell (S / Fe molar ratio = 0.3) is shown. The average particle sizes of the three materials are 368, 390 and 413 nm, respectively, all exhibiting nanoscale characteristics, which is beneficial for their migration in soil and groundwater.
[0069] The surface functional groups of the three integrated Fenton-like materials (i.e., integrated Fenton-like materials prepared using poly(N-isopropylacrylamide), polyvinylpyrrolidone, and polyacrylamide as core and shell materials) were observed using infrared spectroscopy, and the results are as follows: Figure 7 As shown, amide groups (CN) and unsaturated carboxylate groups (-COO-) after hydrolysis were clearly observed on the surface of the polymer materials in all three materials. These functional groups not only constitute the main framework of the polymer encapsulation layer, but also play a dual role in the material construction process: First, the negatively charged groups such as carboxylate groups generated after hydrolysis achieve chemical bonding with calcium ions on the surface of the core nano-calcium peroxide through ion exchange and coordination, forming a stable "core-shell" connection; second, these electron-rich functional groups exposed on the shell surface provide active sites for the subsequent chemical adsorption and coordination fixation of iron precursors.
[0070] Furthermore, the surface crystal structure of the three integrated Fenton-like materials was further determined by XRD patterns (see results). Figure 8 The dominant peaks of the prepared integrated Fenton-like material at 2θ = 30.2°, 35.5°, 47.3°, 52.6°, 53.1°, and 60.8° correspond to the (002), (110), (112), (200), (103), and (202) crystal planes of the reference spectrum of CaO2 (JCPDS-03-0865), respectively. Some characteristic peaks of the prepared integrated Fenton-like material are basically the same as the XRD characteristic peaks of CaO2, which means that the embedding of the three polymers has little effect on the crystal phase of nCaO2. Characteristic peaks of CaCO3 (JCPDS-99-0022) were found at 2θ = 29.1° and 49.8°, and the formation of CaCO3 is mainly related to CO2 in the air. Furthermore, characteristic peaks of FeS (JCPDS-80-1026) were observed at 2θ = 31.1° and 51.2°, corresponding to its (121) and (231) crystal planes, respectively. This further confirms that the sulfur source provided by sodium sulfide successfully reacted with the iron precursor fixed on the support surface through coordination, generating the target catalyst FeS in situ. The characteristic crystal phases of CaO2 and FeS were clearly detected simultaneously in the XRD results, strongly confirming the core design concept of this invention: that is, through the chemical anchoring effect of the polymer "bridge" layer, the slow-release oxidant (nCaO2) and the high-efficiency catalyst (FeS) were successfully integrated at the nanoscale, constructing a core-shell integrated material with both "slow-release" and "catalytic" functions. The presence of the FeS characteristic peak, coexisting with the CaO2 peak, rules out the possibility of simple physical mixing or independent generation of the catalyst. Instead, it indicates that FeS has become an inherent component of the composite material, forming a complete chemically bonded system with the polymer-coated nCaO2 core, laying the material basis for achieving efficient and durable in-situ Fenton-like reactions.
[0071] To further verify the application performance of integrated Fenton-like materials in the remediation of organic pollution in soil and groundwater, a static simulation experiment on the removal of organic pollution in groundwater was conducted. The results are as follows: Figures 9-11 As shown, Figure 9 The image shows the effect of integrated Fenton-like material prepared under different degrees of vulcanization using poly(N-isopropylacrylamide) as the core and shell in Example 1 on the degradation of trichlorophenol (S / Fe molar ratio = 0, 0.1, 0.2, 0.3, 0.4, temperature = 25℃, pH 0 = 7). Figure 10 The image shows the effect of integrated Fenton-like materials prepared under different degrees of vulcanization using polyvinylpyrrolidone as the core and shell in Example 2 on the degradation of trichlorophenol (S / Fe molar ratio = 0, 0.1, 0.2, 0.3, 0.4, temperature = 25℃, pH 0 = 7). Figure 11The image shows the degradation effect of the integrated Fenton-like material prepared under different degrees of sulfidation using polyacrylamide as the core and shell in Example 3 on trichlorophenol (S / Fe molar ratio = 0, 0.1, 0.2, 0.3, 0.4, temperature = 25℃, pH 0 = 7). In this experiment, a trichlorophenol solution (10 mg / L, 100 mL) was used as simulated groundwater. 0.1 g of the integrated Fenton-like material was added to a 200 mL Erlenmeyer flask for degradation testing. Materials with different degrees of sulfidation (S / Fe molar ratio) were prepared before the experiment to optimize the catalytic composition. The results showed that when S / Fe = 0.3, the degradation rates of trichlorophenol by the integrated Fenton-like materials prepared using poly(N-isopropylacrylamide), polyvinylpyrrolidone, and polyacrylamide as core and shell materials were 82.5%, 94.2%, and 91.8%, respectively. This is mainly attributed to the effective reduction of iron ions by low-valence sulfides, thereby further promoting the Fenton-like reaction. In conclusion, the integrated Fenton-like material prepared by polymer coating has great application potential for in-situ remediation of organically contaminated groundwater.
[0072] In addition, a two-dimensional sandbox model was constructed in the experiment, with a blank control group A1 and an experimental group A2. For example... Figure 12 The simulated contaminated groundwater entered a water tank from left to right, with an outlet at the right end of the tank. A water intake was placed every 10 cm on the front of the two-dimensional sandbox model. Initially, the saturation concentration of the simulated groundwater contaminant was tested at each intake. The groundwater contaminant used in this simulation experiment was trichlorophenol at a concentration of 10 mg / L. -1 An integrated Fenton-like material (S / Fe=0.3) prepared using polyvinylpyrrolidone as the core and shell in the optimal static simulation experiment was selected as the oxidizing material. The integrated Fenton-like material was directly injected into the leftmost side of the contaminated area using a simulated injection well method, allowing it to gradually migrate and form an in-situ reaction zone under the action of water flow. After 24 hours of operation, the trichlorophenol concentration in the blank control group remained essentially unchanged, while the A2 trichlorophenol removal rate in the experimental group reached 87.6%.
[0073] In addition, a sustained-release experiment was conducted: sustained-release nano-calcium peroxide prepared from the three polymers mentioned above—polyacrylamide, polyvinylpyrrolidone, and poly(N-isopropylacrylamide)—was tested (step one in Examples 1-3). 0.02 g of each material was added to 200 mL of ultrapure water. Figure 13 As shown ( Figure 13The graph shows the release time relationship between nano-calcium peroxide encapsulated with polyacrylamide, polyvinylpyrrolidone, and poly(N-isopropylacrylamide) and unencapsulated nano-calcium peroxide (temperature = 25℃, pH 0 = 7). It can be seen that the release time of unencapsulated nano-calcium peroxide is about 3 minutes, while the release times of slow-release nano-calcium peroxide encapsulated with poly(N-isopropylacrylamide), polyvinylpyrrolidone, and polyacrylamide are about 60, 90, and 90 minutes, respectively. This shows that polymer coating can effectively alleviate the burst release phenomenon of nano-calcium peroxide. Figure 13 Preparation process of unpolymer-coated nano-calcium peroxide: 6g CaCl2 was weighed and dispersed in 60mL of ultrapure water and stirred at 250rpm using a magnetic stirrer; the pH of the solution was adjusted to 10 by adding 25wt% ammonia water, and this mixed solution was labeled A1; then excess H2O2 (30mL, 30wt%) was added to the A1 solution, and the mixture was stirred continuously for 2h to ensure that it reacted fully. After centrifugation, the precipitate was collected, washed three times with ethanol, and then dried in a vacuum drying oven for 8h.
[0074] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing an integrated Fenton-like material, characterized in that, Includes the following steps: A polymer with amide groups, water, and sodium hydroxide are mixed and hydrolyzed to obtain a hydrolyzed reaction solution; the hydrolysis reaction is carried out under conditions of pH ≥ 11. The hydrolysis reaction solution is mixed with a soluble calcium salt to carry out an ion exchange reaction, thereby obtaining an ion exchange reaction solution; The ion-displacement reaction solution was mixed with hydrogen peroxide solution to carry out a metathesis reaction, thereby obtaining a slow-release nano-calcium peroxide material. A precipitation reaction was carried out on a ferrous salt solution under conditions of pH ≥ 12 to obtain a ferrous hydroxide insoluble system. The slow-release nano-calcium peroxide material was mixed with the ferrous hydroxide insoluble system and a coordination reaction was carried out to obtain an integrated Fenton-like material precursor. The integrated Fenton-like material precursor is mixed with sodium borohydride and sodium sulfide and then subjected to in-situ reduction-sulfidation to obtain the integrated Fenton-like material.
2. The preparation method according to claim 1, characterized in that, The polymer having amide groups includes one or more of polyacrylamide, polyvinylpyrrolidone, and poly(N-isopropylacrylamide); the hydrolysis reaction takes 2-4 hours.
3. The preparation method according to claim 1, characterized in that, The mass ratio of the polymer with amide groups to the soluble calcium salt used in preparing the hydrolysis reaction solution is (0~25):6, and the mass ratio is not 0:6; the time for the ion exchange reaction is 2~5h.
4. The preparation method according to claim 1, characterized in that, The time for the metathesis reaction is 2-4 hours.
5. The preparation method according to claim 1, characterized in that, The concentration of ferrous salt in the ferrous salt solution is 10~15g / L, and the solvent of the ferrous salt solution is an aqueous methanol solution, wherein the volume fraction of methanol in the aqueous methanol solution is 30%.
6. The preparation method according to claim 1, characterized in that, The mass ratio of iron in the controlled-release nano-calcium peroxide material to the ferrous hydroxide insoluble system is 1:(0.1~0.3); the coordination reaction time is 0.5~3h.
7. The preparation method according to claim 1, characterized in that, The molar ratio of sulfur in the sodium sulfide to iron in the integrated Fenton-like material precursor is (0~0.4):1, and the amount of sulfur is not zero; the in-situ reduction-sulfidation time is 0.5~2h.
8. The integrated Fenton-like material prepared by the preparation method according to any one of claims 1 to 7, wherein the integrated Fenton-like material comprises a slow-release nano-calcium peroxide and an iron-based catalyst anchored on the surface of the slow-release nano-calcium peroxide, wherein the slow-release nano-calcium peroxide comprises nano-calcium peroxide and a polymer slow-release layer anchored on the surface of the nano-calcium peroxide, and the iron-based catalyst is an iron sulfide.
9. The integrated Fenton-like material according to claim 8, characterized in that, The particle size of the integrated Fenton-like material is <500nm.
10. The application of the integrated Fenton-like material as described in claim 8 or 9 in soil and groundwater remediation.
Citation Information
Patent Citations
Sustained-release nano-calcium peroxide materials, preparation thereof, and method for removing chlorohydrocarbon and / or benzene series from underground water through sustained-release nano-calcium peroxide materials
CN110759319A
Slow-release nano material with tea polyphenol complexed with ferric iron coated calcium peroxide and application of slow-release nano material
CN116495866A