Al-Mg alloys and their preparation methods
By adding TCB seed particles and controlling the Fe/Mn ratio in Al-Mg alloys to form a three-dimensional network structure and refine the grains, the problem of insufficient hardness in Al-Mg alloys is solved, and a significant improvement in high hardness and wear resistance is achieved, making it suitable for tire molds.
Patent Information
- Application Number
- CN202610614776.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-05-07
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2046-05-07
AI Technical Summary
Existing Al-Mg alloys lack sufficient hardness in the tire mold field, leading to increased sulfidation corrosion, surface wear, and cavity damage, making it difficult to meet the comprehensive requirements of high hardness, high wear resistance, good machinability, and reasonable economy.
By adding C-doped TiB2 and B-doped TiC seed particles to Al-Mg alloys and controlling the mass ratio of Fe to Mn to be 1.8-2.2:1, a three-dimensional interconnected intermetallic compound network structure is formed. Combined with the compositional gradient of Ti and Zr, the α-Al grains are refined and the matrix hardness of the alloy is improved.
It significantly improves the Brinell hardness of Al-Mg alloys to 65-82 HBW, enhances crack resistance and overall mechanical properties, and meets the high hardness and wear resistance requirements of tire molds.
Smart Images

Figure CN122189449B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metallic materials, specifically designing an Al-Mg alloy and its preparation method. Background Technology
[0002] Al-Mg alloys are among the most widely used series of aluminum alloys, possessing advantages such as high thermal conductivity, good machinability, large coefficient of thermal expansion, corrosion resistance, and good surface finish, thus being widely used in rubber molds. These molds are typically cast directly, significantly reducing mold manufacturing costs and processing cycles.
[0003] Although Al-Mg alloys are widely used in the field of tire molds, the Brinell hardness of commercially available conventional aluminum-magnesium alloy tire molds is generally in the range of 50-60 HBW. Their inherent insufficient hardness can lead to increased mold sulfidation corrosion, surface wear and cavity damage, casting defects that reduce precision, and other problems, which seriously restrict the service life of the molds and the quality of tire manufacturing.
[0004] To address the problem of insufficient hardness in Al-Mg alloys, those skilled in the art have made various attempts, mainly including compositional microalloying, surface treatment strengthening, and deformation strengthening, but these technical solutions all have their own limitations.
[0005] Microalloying significantly increases material costs, offers limited improvement in hardness, and often comes at the cost of alloy plasticity, leading to decreased hardness and cracking. Surface nano-sizing only improves surface properties and cannot fundamentally enhance the hardness of the alloy matrix. During long-term service, the surface nanocrystalline layer is prone to degradation, resulting in decreased wear resistance and a decline in the overall performance of the mold. Most importantly, the industrial application of surface nano-sizing technology to large tire molds still faces considerable challenges. The hardness increase from deformation strengthening is limited by the degree of work hardening, and annealing significantly reduces the hardness increment gained from deformation. Furthermore, the recovery and recrystallization processes lead to a decrease in the mechanical properties of the alloy. For large-sized, complex tire molds, the overall deformation strengthening process is extremely difficult to implement and cannot be widely promoted and applied in production.
[0006] In summary, although there are various methods in the existing technology to improve the hardness of Al-Mg alloys, they are either limited by high cost, limited by the extent of hardness improvement, or have failed to solve the fundamental problem that they can only improve the surface properties while the hardness of the matrix is insufficient. Therefore, it is difficult to simultaneously meet the comprehensive requirements of tire molds for high hardness, high wear resistance, good machinability, and reasonable economy. Summary of the Invention
[0007] This invention develops an Al-Mg alloy that significantly improves hardness at the matrix level and its preparation method.
[0008] According to one aspect of the present invention, an Al-Mg alloy is provided, the Al-Mg alloy comprising the following components by mass percentage: Mg 4.5~6.5%, Fe 0.10~0.30%, Mn 0.05~0.15%, and TCB seed particles 0.005~0.03%, wherein the TCB seed particles are at least one of C-doped TiB2 and B-doped TiC, and wherein the mass ratio of Fe to Mn in the Al-Mg alloy is 1.8-2.2:1.
[0009] Optionally, the Al-Mg alloy includes an intermetallic compound phase, which includes Al3Mg2 and Al6(Fe, Mn).
[0010] Optionally, the Al-Mg alloy further includes α-Al grains and grain boundaries located between adjacent α-Al grains, wherein the intermetallic compound phase forms a three-dimensional interconnected network structure at the grain boundaries.
[0011] Optionally, the Al-Mg alloy further includes the following components by mass percentage: Ti 0.12~0.25%, Zr 0.02~0.10%, Si <0.2%, other impurity elements ≤0.05% individually, total ≤0.15%, with the balance being Al.
[0012] Optionally, the average size of the α-Al grains is 50 μm to 150 μm.
[0013] Optionally, the Al-Mg alloy forms a compositional gradient from the center of the α-Al grain to the grain boundary, in which the mass ratio of Ti to Zr decreases sequentially.
[0014] Optionally, the Brinell hardness value of the Al-Mg alloy is 65-82 HBW.
[0015] According to another aspect of the present invention, a method for preparing the Al-Mg alloy as described above is provided, the method comprising: (1) melting pure aluminum and adjusting the temperature of the aluminum melt to 760°C to 800°C; (2) adding Al-Fe master alloy, Al-Mn master alloy and Al-TCB seed alloy to the aluminum melt and dissolving them, wherein the content of TCB seed particles in the Al-TCB seed alloy is 0.5wt% to 3wt%; (3) adjusting the melt temperature to 730°C to 760°C, adding pure magnesium and dissolving it; (4) casting to obtain the Al-Mg alloy.
[0016] Optionally, in step (2), Al-Ti master alloy and Al-Zr master alloy are added to the aluminum melt and dissolved.
[0017] Optionally, the preparation method further includes a step of refining the melt after step (3) and before step (4).
[0018] According to the present invention, by controlling the Mg content, adding TCB seed particles and controlling their content, adding Fe and Mn and controlling their content, and the mass ratio of Fe to Mn, the hardness of Al-Mg alloys with the same Mg content can be significantly improved. Attached Figure Description
[0019] Figure 1 The Al-Mg alloys of Example 2 and Comparative Example 2, wherein, Figure 1 (a) shows the fine-grained microstructure of the Al-Mg alloy in Example 2. Figure 1 (b) shows the continuous or semi-continuous grain boundary network structure composed of Al3Mg2 and Al6(Fe, Mn) phases in Example 2. Figure 1 (c) shows the fine-grained microstructure of the Al-Mg alloy in Comparative Example 2. Figure 1 (d) represents the continuous or semi-continuous grain boundary network structure composed of Al3Mg2 and Al6(Fe, Mn) phases in Comparative Example 2. Detailed Implementation
[0020] The following detailed embodiments are provided to aid the reader in gaining a comprehensive understanding of the products and methods described herein. However, after understanding this disclosure, various changes, modifications, and equivalents of the products and methods described herein will become clear. For example, the order of steps in the methods described herein is merely illustrative and is not limited to the order set forth herein, but may be changed as will become clear after understanding this disclosure, except for steps that must occur in a specific order. Furthermore, for clarity and conciseness, descriptions of features known in the art may be omitted.
[0021] The features described herein may be implemented in different forms and should not be construed as limited to the examples described herein. Rather, the examples described herein are provided only to illustrate some of the many feasible ways in which the products and methods described herein may be understood upon understanding the contents of this disclosure.
[0022] Unless otherwise defined, all terms used herein (including technical and scientific terms) shall have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure pertains upon understanding this disclosure. Unless expressly defined herein, terms such as those defined in a general dictionary shall be interpreted as having the same meaning as in this disclosure and shall not be interpreted in an idealized or overly formalistic manner.
[0023] It should also be understood that the terms “comprising / including” or “having” as used throughout the specification indicate the presence of the said ingredient, step, or operation, but do not exclude the presence or addition of one or more other ingredients. Therefore, unless explicitly stated to the contrary, the words “comprising,” “including,” or “having” will be understood to imply the inclusion of the said ingredient, step, or operation but do not exclude any other ingredient, step, or operation.
[0024] Al-Mg alloys The Al-Mg alloy according to an embodiment of the present invention comprises the following components by mass percentage: Mg 4.5~6.5%, Fe 0.10~0.30%, Mn 0.05~0.15%, and TCB seed particles 0.005~0.03%, wherein the TCB seed particles can be at least one of C-doped TiB2 and B-doped TiC, and wherein the mass ratio of Fe to Mn in the Al-Mg alloy is 1.8-2.2:1.
[0025] In the Al-Mg alloy according to an embodiment of the present invention, a portion of Mg is dissolved in the Al matrix, while the other portion forms an intermetallic compound phase (Al3Mg2 compound phase) due to a non-equilibrium solidification eutectic reaction.
[0026] Al-Mg alloys may include α-Al grains and grain boundaries located between adjacent α-Al grains, with Al3Mg2 compound phases distributed on the grain boundaries. Compared to Mg dissolved in the Al matrix, the Al3Mg2 compound phase distributed on the grain boundaries provides a greater strengthening effect.
[0027] According to embodiments of the present invention, in a 100wt% Al-Mg alloy, the Mg content can be 4.5~6.5wt%. The Mg content plays a crucial role in the hardness of the Al-Mg alloy. When the Mg content in a 100wt% Al-Mg alloy is less than 4.5wt%, the Mg content is too low, and most of the Mg is dissolved in the matrix, making it difficult to form the Al3Mg2 compound phase that plays a strengthening role, resulting in insufficient hardness and strength of the alloy. Furthermore, when the Mg content in a 100wt% Al-Mg alloy is greater than 6.5%, the excessively high Mg content leads to overly coarse Al3Mg2 compound phases at the grain boundaries, making the alloy brittle, prone to cracking or fracture, and resulting in poor service performance.
[0028] In the Al-Mg alloy according to an embodiment of the present invention, Fe and Mn form intermetallic compound phases (Al6(Fe,Mn) compound phases) distributed on the grain boundaries, which together with Al3Mg2 compounds form a three-dimensional interconnected network structure, for example, forming a continuous or semi-continuous network structure to strengthen the alloy.
[0029] According to embodiments of the present invention, based on a 100wt% Al-Mg alloy, the Fe content can be 0.10–0.30wt%, and the Mn content can be 0.05–0.15wt%. When the Fe content is less than 0.10wt% or the Mn content is less than 0.05wt% based on a 100wt% Al-Mg alloy, the Mn or Fe content is too low, resulting in insufficient hardening effect. When the Fe content is greater than 0.30wt% or the Mn content is greater than 0.15wt% based on a 100wt% Al-Mg alloy, the Fe or Mn content is too high, leading to poor alloy plasticity and increased brittleness.
[0030] According to an embodiment of the present invention, the mass ratio of Fe to Mn in the Al-Mg alloy is 1.8-2.2:1. This is to allow Mn to better modify the Fe phase, so that Al... 13 The transformation of the Fe4 phase into the Al6(Fe, Mn) phase involves both an increase in the phase's mass fraction and an improvement in its morphology, changing from sharp, needle-like structures to short, rod-like ones. If the Fe / Mn mass ratio is less than 1.8, the excessive Mn content will cause the Al6(Fe, Mn) phase to become blocky, making it difficult to form a network structure with Al3Mg2 compounds at grain boundaries. If the Fe / Mn mass ratio is greater than 2.2, the excessive Fe content will prevent sufficient Mn modification, resulting in the formation of more sharp, needle-like Al6(Fe, Mn) phases. 13 Fe4 phase. This type of hard phase not only makes it difficult to form a continuous or semi-continuous reinforcing network structure with Al3Mg2 compounds at the grain boundaries, but also becomes a stress concentration source during the stress process, which reduces the plasticity and toughness of the alloy and increases the tendency to crack, thereby weakening its comprehensive mechanical properties and service reliability.
[0031] The Al-Mg alloy according to embodiments of the present invention may further include TCB seed particles. The TCB seed particles may be at least one of C-doped TiB2 and B-doped TiC. That is, the TCB seed particles may be only C-doped TiB2, or only B-doped TiC, or may include both C-doped TiB2 and B-doped TiC.
[0032] TCB seed particles can serve as nucleation substrates for α-Al, refining the grains, which significantly improves the hardness of Al-Mg alloys. Furthermore, after grain refinement, there are more grain boundary networks per unit area, and the network structure formed by the Al3Mg2 and Al6(Fe, Mn) phases is more compact, thereby further improving the alloy properties. According to embodiments of the present invention, the average size of the α-Al grains can be from 50 μm to 150 μm. The average size of the α-Al grains can refer to the average size of at least ten grains.
[0033] According to embodiments of the present invention, based on a 100wt% Al-Mg alloy, the content of TCB seed particles can be 0.005~0.03wt%. When the content of TCB seed particles is less than 0.005wt% based on a 100wt% Al-Mg alloy, it is difficult to sufficiently refine α-Al and effectively improve the hardness of the Al-Mg alloy. When the content of TCB seed particles exceeds 0.03wt% based on a 100wt% Al-Mg alloy, the effect of grain refinement no longer improves.
[0034] In existing technologies, the hardness of Al-Mg alloys with conventional compositions often struggles to exceed 60 HBW. Increasing the Mg content can improve the hardness, but the increase is limited and insufficient to meet industrial requirements.
[0035] According to embodiments of the present invention, by adding TCB seed particles, Fe, and Mn while simultaneously controlling the content of TCB seed particles and the mass ratio of Fe to Mn, synergistic optimization of grain refinement and grain boundary strengthening network can be achieved in Al-Mg alloys, resulting in a significant increase in hardness at the same Mg content. Specifically, TCB seed particles act as a nucleation substrate for α-Al, effectively promoting α-Al grain refinement and thus improving alloy hardness. Simultaneously, after grain refinement, there are more grain boundary networks per unit area, and the network structure formed by Al3Mg2 and Al6(Fe, Mn) phases is more compact, effectively improving alloy hardness. Furthermore, the mass ratio of Fe to Mn of 1.8-2.2:1 allows the Fe phase to fully metamorphose into the Al6(Fe, Mn) phase, avoiding the formation of sharp, needle-like Al phases. 13 The Fe4 phase is modified to a short rod-like morphology, allowing it to co-construct a continuous or semi-continuous three-dimensional strengthening network structure with Al3Mg2 compounds at the grain boundaries. Through synergistic regulation of TCB seed particles and the mass ratio of Fe to Mn, the alloy's hardness can be significantly improved, along with its resistance to cracking and fracture during service, thereby enhancing its overall mechanical properties and reliability.
[0036] According to embodiments of the present invention, the Al-Mg alloy may further include the following components by mass percentage: Ti 0.12~0.25%, Zr 0.02~0.10%, Si <0.2%, other impurity elements ≤0.05% individually, total ≤0.15%, with the balance being Al.
[0037] In Al-Mg alloys, Ti assists TCB seed particles in refining the matrix grains, strengthens through solid solution, and can also form hard TiAl3 particles. All of these factors combined strengthen and harden the alloy.
[0038] According to an embodiment of the present invention, based on a 100wt% Al-Mg alloy, the Ti content is 0.12~0.25wt% to fully strengthen and harden the alloy.
[0039] When the Ti content is less than 0.12wt% in an Al-Mg alloy with a content of 100wt%, the amount of Ti added is insufficient to fully exert its promoting effect on grain refinement, and it is also difficult to form a sufficient amount of hard TiAl3 particles. Therefore, the effect of assisting TCB seed particles in refining α-Al grains and solid solution strengthening is limited, resulting in insufficient improvement in the hardness of the alloy.
[0040] When the Ti content is greater than 0.25 wt% in a 100 wt% Al-Mg alloy, the excess Ti will form too many coarse TiAl3 hard particles during solidification, which will become stress concentration sources when subjected to stress, reducing the plasticity and toughness of the alloy.
[0041] In Al-Mg alloys, Zr mainly plays a role in solid solution strengthening. According to embodiments of the present invention, based on a 100wt% Al-Mg alloy, the Zr content can be 0.02~0.10wt% to fully exert the role of solid solution strengthening.
[0042] According to embodiments of the present invention, adding a small amount of Si can help improve hardness, but if the Si content is greater than or equal to 0.2 wt% based on a 100 wt% Al-Mg alloy, it will lead to alloy brittleness. Therefore, based on a 100 wt% Al-Mg alloy, the Si content is less than 0.2 wt%.
[0043] According to an embodiment of the present invention, based on a 100wt% Al-Mg alloy, other impurity elements are individually ≤0.05wt% and in total ≤0.15wt%.
[0044] According to embodiments of the present invention, an Al-Mg alloy exhibits a compositional gradient with a decreasing Ti / Zr mass ratio from the center of the α-Al grain to the grain boundary. This is because the solute redistribution coefficient of Ti / Zr in aluminum alloys is greater than 1, so the concentration is highest at the first solidification site (grain center), and decreases as the grain grows to the grain boundary.
[0045] According to embodiments of the present invention, the Brinell hardness value of Al-Mg alloys can be 65-82 HBW.
[0046] As described above, according to the present invention, by adding TCB seed particles, Fe and Mn and simultaneously controlling the content of TCB seed particles and the mass ratio of Fe to Mn, the hardness of Al-Mg alloys can be significantly improved at the matrix level.
[0047] Preparation methods of Al-Mg alloys The preparation method of Al-Mg alloy according to an embodiment of the present invention may include: (1) melting pure aluminum and adjusting the temperature of the aluminum melt to 760°C to 800°C; (2) adding Al-Fe master alloy, Al-Mn master alloy and Al-TCB seed alloy to the aluminum melt and dissolving them, wherein the content of TCB seed particles in the Al-TCB seed alloy is 0.5% to 3%; (3) adjusting the melt temperature to 730°C to 760°C, adding pure magnesium and dissolving it; (4) casting to obtain Al-Mg alloy.
[0048] The following will describe in detail each step of the preparation method of Al-Mg alloys.
[0049] First, pure aluminum can be melted and the temperature of the molten aluminum can be adjusted to 760℃~800℃. For example, pure aluminum can be added to a smelting furnace for melting.
[0050] Then, Al-Fe master alloy, Al-Mn master alloy, and Al-TCB seed alloy are added to the above-mentioned aluminum melt and dissolved. If the aluminum melt temperature is below 760℃, the Al-Fe, Al-Mn, and Al-TCB seed alloys may not dissolve sufficiently, affecting the homogenization of Fe and Mn elements and the dispersion effect of TCB seed particles, thereby weakening the synergistic effect of grain refinement and grain boundary strengthening network. If the melt temperature is above 800℃, the excessively high temperature will exacerbate the melt's gas absorption and oxidation tendency. Therefore, in step (2), the melt temperature should be controlled within the range of 760℃ to 800℃ to ensure that each master alloy and seed particle is fully dissolved and maintains a good dispersion state.
[0051] According to embodiments of the present invention, the content of TCB seed particles in the Al-TCB seed alloy can be 0.5wt% to 3wt%. The TCB seed particles can be at least one of C-doped TiB2 and B-doped TiC.
[0052] According to an embodiment of the present invention, in step (2), Al-Ti master alloy and Al-Zr master alloy may be added to the aluminum melt and dissolved.
[0053] Next, adjust the melt temperature to 730℃~760℃, add pure magnesium and dissolve it. If the melt temperature is less than 730℃, the pure magnesium may not dissolve sufficiently, resulting in uneven distribution of Mg in the ingot, weakening the solid solution strengthening effect of Mg in the matrix and its promoting effect on the formation of Al3Mg2 strengthening phase, thus affecting the hardness and strength improvement of the alloy. In addition, a lower temperature will prolong the melt holding time, increasing the risk of melt gas absorption and oxidation, which is not conducive to obtaining a uniform and stable Al-Mg alloy. If the melt temperature is higher than 760℃, it may cause Mg to burn off. Therefore, in step (3), the melt temperature should be controlled within the range of 730℃~760℃ to ensure sufficient dissolution while avoiding burn-off.
[0054] In step (4), the melt is poured to obtain an Al-Mg alloy.
[0055] The method for preparing Al-Mg alloys according to embodiments of the present invention may further include a step of refining the melt after step (3) and before step (4). That is, the melt is refined and then cast. The present invention may use refining processes of Al-Mg alloys known in the art without any limitation. As an example, the refining temperature may be 720°C to 750°C, and the refining time may be 15 min to 30 min. As an example, refining may be carried out by adding a refining agent to the melt, or by introducing argon gas into the melt, or by using a combined refining process with both a refining agent and argon gas.
[0056] Examples and Comparative Examples Prepare the raw materials required for the Al-Mg alloys of the examples and comparative examples according to the mass ratios shown in Table 1 below: pure aluminum, pure magnesium, Al-Fe master alloy, Al-Mn master alloy, Al-Ti master alloy, Al-Zr master alloy, and Al-TCB seed alloy. The content of TCB seed alloy in the Al-TCB seed alloy is 1.0%.
[0057] Add pure aluminum to the melting furnace, heat and melt it, and adjust the melt temperature to 760℃~800℃. Add Al-Fe master alloy, Al-Mn master alloy, Al-Ti master alloy, Al-Zr master alloy, and Al-TCB seed alloy. After they are completely dissolved, adjust the melt temperature to 730℃~760℃ and add pure magnesium.
[0058] Add 0.2% (by mass) of sodium-free refining agent to the melt, and simultaneously introduce argon gas (flow rate 1.0 L / min) for compound refining. The refining temperature is 740℃, and the refining time is 15 min. Then cast to obtain an Al-Mg alloy.
[0059] The microstructure of Al-Mg alloys was observed using an optical microscope, and the size of α-Al grains was measured. For example, the size of α-Al grains could be the average size of 10 grains.
[0060] Hardness testing was conducted according to GB / T 231.1-2018 standard. The surface of the Al-Mg alloy sample was polished and then the hardness was tested. The average Brinell hardness at ten points was taken as the HBW Brinell hardness of the Al-Mg alloy.
[0061] Table 1
[0062] Referring to Table 1, in Examples 1 to 4, based on a 100wt% Al-Mg alloy, the Mg content ranged from 4.5 to 6.5wt%, the Fe content ranged from 0.10 to 0.30wt%, the Mn content ranged from 0.05 to 0.15wt%, the Fe / Mn mass ratio was 1.8-2.2, and the TCB seed particle content ranged from 0.005 to 0.03wt%. Therefore, the average grain size ranged from 50μm to 150μm, and the hardness ranged from 65 to 82 HBW. Furthermore, in Examples 1 to 4, based on a 100wt% Al-Mg alloy, the Ti content ranged from 0.12 to 0.25wt%, the Zr content ranged from 0.02 to 0.10wt%, and the Si content was less than 0.2wt%.
[0063] The contents of Mg, Fe, Mn, Ti, Zr, and Si in Comparative Examples 1, 2, 3, and 4 were the same as those in Examples 1, 2, 3, and 4, respectively. The difference was that TCB seed particles were not added in Comparative Examples 1, 2, 3, and 4. Compared with Comparative Example 1, the hardness of Example 1 increased from 60 HBW to 67 HBW after the addition of TCB seed particles, an increase of approximately 11.7%; compared with Comparative Example 2, the hardness of Example 2 increased from 64 HBW to 73 HBW after the addition of TCB seed particles, an increase of approximately 14.1%; compared with Comparative Example 3, the hardness of Example 3 increased from 66 HBW to 78 HBW, an increase of approximately 18.2%; and compared with Comparative Example 4, the hardness of Example 4 increased from 69 HBW to 80 HBW, an increase of approximately 15.9%.
[0064] The above results indicate that, under the same composition ratio, Comparative Examples 1-4 without added TCB seed particles lack heterogeneous nucleation sites, resulting in larger α-Al grain sizes and a looser, coarser network structure formed by the Al3Mg2 and Al6(Fe, Mn) phases, leading to lower hardness. However, after adding an appropriate amount of TCB seed particles, the grains are significantly refined (as shown in Table 1, the grain size of Example 1 decreased from 265 μm in Comparative Example 1 to 105 μm, the grain size of Example 2 decreased from 271 μm in Comparative Example 2 to 89 μm, the grain size of Example 3 decreased from 310 μm in Comparative Example 3 to 72 μm, and the grain size of Example 4 decreased from 295 μm in Comparative Example 4 to 55 μm), with more grain boundary networks per unit area and a denser network structure formed by the Al3Mg2 and Al6(Fe, Mn) phases, effectively improving the alloy hardness.
[0065] Figure 1 The Al-Mg alloys of Example 2 and Comparative Example 2, wherein, Figure 1 (a) shows the fine-grained microstructure of the Al-Mg alloy in Example 2. Figure 1 (b) shows the continuous or semi-continuous grain boundary network structure composed of Al3Mg2 and Al6(Fe, Mn) phases in Example 2. Figure 1 (c) shows the fine-grained microstructure of the Al-Mg alloy in Comparative Example 2. Figure 1 (d) represents the continuous or semi-continuous grain boundary network structure composed of Al3Mg2 and Al6(Fe, Mn) phases in Comparative Example 2. Figure 1 As shown in (c) and (d), without the addition of TCB seed particles, the α-Al grain size is relatively large, and the network structure formed by the Al3Mg2 and Al6(Fe, Mn) phases is relatively loose and coarse. In contrast, as Figure 1 As shown in (a) and (b), with the addition of an appropriate amount of TCB seed particles, the grains are significantly refined, there are more grain boundary meshes per unit area, and the network structure formed by Al3Mg2 and Al6(Fe, Mn) phases is more compact.
[0066] In Comparative Example 5, the contents of Mg, Ti, and Si were outside the scope of this invention, and no Zr or TCB seed particles were added, resulting in a lower hardness of 53 HBW. Compared to Comparative Example 5, Comparative Example 6 added TCB seed particles, which improved the hardness, but it was still less than 60 HBW. This indicates that the TCB seed particles work synergistically with the composition of the Al-Mg alloy to improve hardness.
[0067] Furthermore, Examples 5, 6, 7, and 8 differed from Example 1 only in the Fe content, i.e., the Fe / Mn mass ratio was adjusted. In Example 5, the Fe / Mn mass ratio was 2.2, and in Example 6, it was 1.8, maintaining relatively high hardness values of 66 HBW and 68 HBW, respectively. In Comparative Example 7, the Fe / Mn mass ratio was 2.6, and in Comparative Example 8, it was 1.4, resulting in hardness values decreasing to 62 HBW and 61 HBW, respectively. This demonstrates that even with the addition of TCB seed particles, a significant decrease in hardness occurs when the Fe / Mn mass ratio is outside the 1.8 to 2.2 range of this invention. Therefore, TCB seed particles need to work synergistically with the Fe / Mn mass ratio to improve hardness.
[0068] As described above, according to the present invention, by controlling the Mg content, adding TCB seed particles and controlling their content, adding Fe and Mn and controlling their content, and the mass ratio of Fe to Mn, the hardness of Al-Mg alloys with the same Mg content can be significantly improved.
[0069] Furthermore, according to the Al-Mg alloy of the present invention, by simultaneously adding Ti and Zr and controlling their addition amounts, it is beneficial to improve the hardness of the Al-Mg alloy.
[0070] The Al-Mg alloy of the present invention has high hardness, simple preparation process, and high technical reliability, and has important engineering significance and broad application prospects.
[0071] While this disclosure has been described in conjunction with what is now considered to be actual embodiments, it should be understood that the invention is not limited to the disclosed embodiments. Rather, it is intended to cover various variations and equivalents that are included within the spirit and scope of the appended claims.
Claims
1. An Al-Mg alloy, characterized in that, The Al-Mg alloy comprises the following components by mass percentage: Mg 4.5~6.5%, Fe 0.10~0.30%, Mn 0.05~0.15%, TCB seed particles 0.005~0.03%, Ti 0.12~0.25%, Zr 0.02~0.10%, Si <0.2%, balance Al. The TCB seed particles are at least one of C-doped TiB2 and B-doped TiC. In the Al-Mg alloy, the mass ratio of Fe to Mn (Fe / Mn) is 1.8-2.2:
1. The Al-Mg alloy comprises an intermetallic compound phase, which includes Al3Mg2 and Al6(Fe, Mn). The Al-Mg alloy further includes α-Al grains and grain boundaries located between adjacent α-Al grains, wherein the intermetallic compound phase forms a three-dimensional interconnected network structure at the grain boundaries.
2. The Al-Mg alloy according to claim 1, characterized in that, In the Al-Mg alloy, the individual impurity elements are ≤0.05%, and the total is ≤0.15%.
3. The Al-Mg alloy according to claim 1, characterized in that, The average size of the α-Al grains is 50 μm to 150 μm.
4. The Al-Mg alloy according to claim 1, characterized in that, The Al-Mg alloy forms a compositional gradient from the center of the α-Al grains to the grain boundaries, with the Ti / Zr mass ratio decreasing sequentially.
5. The Al-Mg alloy according to claim 1, characterized in that, The Brinell hardness value of the Al-Mg alloy is 65-82 HBW.
6. A method for preparing an Al-Mg alloy according to any one of claims 1 to 5, characterized in that, The preparation method includes: (1) Melt pure aluminum and adjust the temperature of the molten aluminum to 760℃~800℃; (2) Add Al-Fe master alloy, Al-Mn master alloy, Al-Ti master alloy, Al-Zr master alloy and Al-TCB seed alloy to the aluminum melt and dissolve them, wherein the content of TCB seed particles in the Al-TCB seed alloy is 0.5wt%~3wt%; (3) Adjust the melt temperature to 730℃~760℃, add pure magnesium and dissolve it; (4) Casting to obtain the Al-Mg alloy.
7. The method for preparing Al-Mg alloys according to claim 6, characterized in that, The preparation method further includes a step of refining the melt after step (3) and before step (4).
Citation Information
Patent Citations
Heat-resistant high-strength piston aluminum alloy and preparation method thereof
CN118756018A
Aluminum alloy sheet for forming
JP2007077486A