High-ductility concrete and carbon fiber cloth composite reinforcement method

By coating the surface of autoclaved aerated concrete (AAC) panels with a thermally activated latent interfacial penetrating reinforcing agent and spraying high-ductility concrete to form an ECC layer, and then bonding carbon fiber cloth along the stress direction, combined with an anchoring structure, the problems of low flexural strength and brittleness of AAC panels are solved. This achieves efficient panel reinforcement and ductile failure mode, and is suitable for the reinforcement of existing buildings.

CN122589241BActive Publication Date: 2026-11-17JIANGXI CHINA COAL BRIDGE ENGINEERING TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202610749159.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-05-28
Publication Date
2026-11-17
Estimated Expiration
2046-05-28

AI Technical Summary

Technical Problem

Autoclaved aerated concrete (AAC) panels have low flexural strength and significant brittleness, making it difficult to effectively reinforce them with existing technologies. In particular, reinforcement cannot be implemented on panels that have already been installed or are in existing buildings, and there is a lack of technical solutions for synergistic reinforcement with continuous carbon fiber cloth external bonding technology and high-ductility concrete.

Method used

By coating the surface of autoclaved aerated concrete (AAC) panels with a thermally activated latent interfacial penetration enhancer, spraying high-ductility concrete to form an ECC layer, and attaching carbon fiber cloth along the stress direction, combined with an anchoring structure, a multi-layer composite reinforcement structure is formed. The curing reaction of the impregnating adhesive triggers the penetration enhancement of the interfacial agent, forming an interfacial transition zone of mechanical interlocking and chemical bonding.

Benefits of technology

It significantly improves the flexural strength of autoclaved aerated concrete (AAC) panels, changes the failure mode to ductile bending, inhibits end peeling of carbon fiber cloth, enhances material utilization and durability, and is suitable for reinforcement of factory-made and installed panels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122589241B_ABST
    Figure CN122589241B_ABST
Patent Text Reader

Abstract

This invention relates to a method for reinforcing autoclaved aerated concrete (AAC) slabs with a composite of high-ductility concrete and carbon fiber cloth, belonging to the field of building structure reinforcement technology. The method includes: roughening the surface of the slab and coating it with an interface agent containing a heat-activated latent penetrating reinforcing agent; spraying high-ductility concrete in two layers; after the first layer has initially set, bonding the carbon fiber cloth; utilizing the exothermic curing reaction of the impregnating adhesive to trigger the bidirectional penetration and curing of the latent penetrating reinforcing agent in the interface agent, forming an interface-reinforced transition zone between the slab and the high-ductility concrete; then setting up an anchoring structure, spraying a second layer of high-ductility concrete to cover the carbon fiber cloth, and curing. This invention constructs a dual dynamic linkage mechanism between process steps, transforming the exothermic curing process into a driving force for actively strengthening the interface, and optimizing the stress transmission path through interface reinforcement to suppress end peeling of the carbon fiber cloth, thereby significantly improving the flexural bearing capacity of the reinforced slab and changing the failure mode from brittle fracture to ductile progressive failure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of building structure reinforcement technology, specifically a composite reinforcement method using high-ductility concrete and carbon fiber cloth. Background Technology

[0002] Autoclaved aerated concrete (AAC) panels are lightweight, porous panels made primarily from siliceous and calcareous materials such as cement, lime, and silica sand, with aluminum powder foaming agent added, and cured under high temperature and pressure steam. These panels possess advantages such as low density, excellent thermal insulation, and outstanding fire resistance, and are widely used in interior and exterior wall panels and floor slab systems of prefabricated buildings. However, the porous structure of AAC panels inherently results in low flexural strength and significant brittleness. The panels are highly susceptible to cracking and even fracture during handling, hoisting, and installation. When used as floor slabs, they deform significantly under concentrated loads with no obvious warning signs before failure, limiting their application in scenarios involving high mechanical loads. Therefore, effectively reinforcing AAC panels, especially improving their flexural strength and mitigating their brittle failure mode, has been a long-standing technical need in this field.

[0003] Currently, reinforcement methods for autoclaved aerated concrete (AAC) panels mainly focus on the panel production stage. A typical approach involves incorporating short carbon fiber strands during slurry preparation, dispersing these strands as reinforcement components within the panel matrix. While this method can improve the panel's intrinsic strength to some extent, its reinforcement effect is limited by the uniformity of the short fiber dispersion in the slurry. The fiber dosage is constrained by the gasification process and slurry flowability, making further improvements difficult. Furthermore, because the short fibers are randomly distributed without directionality within the matrix, they cannot provide targeted reinforcement to specific stress areas of the panel, resulting in low material utilization. More importantly, this internal incorporation method is only applicable to the panel manufacturing stage and cannot be used to reinforce AAC panels that have already been manufactured, installed, or are already in existing buildings, significantly limiting its applicability. In addition, there is currently no technical solution that combines continuous carbon fiber fabric external bonding technology with high-ductility concrete for the reinforcement of AAC panels, representing a clear technological gap in this field. Summary of the Invention

[0004] To address the problems of the prior art, this invention provides a method for composite reinforcement of high-ductility concrete and carbon fiber cloth.

[0005] To solve the above-mentioned technical problems, the present invention is achieved through the following technical solution: Firstly, a method for reinforcing autoclaved aerated concrete (AAC) panels using a composite reinforcement of high-ductility concrete and carbon fiber cloth, comprising the following steps: S1: Roughen the surface of the autoclaved aerated concrete (AAC) slab to be reinforced, and then coat it with an interface agent containing a thermally activated latent interface penetration enhancer to seal the pores on the surface of the AAC slab and form an interface layer with thermally responsive characteristics. S2: High-ductility concrete is sprayed onto the surface coated with the interface agent to form a first ECC layer, wherein the spraying thickness of the first ECC layer is 50% to 70% of the total design thickness of the ECC layer; S3: After the first ECC layer has initially set, at least one layer of carbon fiber cloth is bonded to the surface of the first ECC layer along the stress direction of the autoclaved aerated concrete slab using an impregnating adhesive that can generate heat of curing reaction, to form a CFRP reinforcement layer. S4: Anchoring structures are provided at both ends of the longitudinal direction of the carbon fiber cloth; S5: After the carbon fiber cloth is pasted and surface dry, a second ECC layer is sprayed to completely cover the carbon fiber cloth. The spraying thickness of the second ECC layer is 30% to 50% of the total design thickness of the ECC. The first ECC layer and the second ECC layer together constitute an ECC reinforcement layer with a total design thickness of 15 to 30 mm. S6: Curing the composite reinforcement layer after spraying; In step S3, the heat released during the curing reaction of the impregnating adhesive is conducted to the interface layer formed in step S1, triggering the latent interface penetration enhancer to penetrate and cure bidirectionally into the autoclaved aerated concrete (AAC) substrate and the first ECC layer, forming a reinforced transition zone with mechanical interlocking and chemical bonding; and... The formation of the enhanced transition zone enhances the interfacial stiffness and bond strength between the autoclaved aerated concrete (AAC) panel and the first ECC layer, thereby optimizing the stress transfer path from the CFRP reinforcement layer to the substrate under stress and suppressing stress concentration and peeling failure at the ends of the CFRP reinforcement layer.

[0006] In one specific embodiment of the first aspect, in step S1, the thermally activated latent interfacial penetration enhancer is a nano-silica sol encapsulated by a thermosensitive polymer or a latent epoxy curing agent, with a thermal activation temperature of 40–70°C; the main component of the interfacial agent is a diluted solution of acrylate copolymer emulsion and water in a mass ratio of 1:2 to 1:4, and the coating amount is 0.15–0.30 kg / m³. 2 .

[0007] In one specific embodiment of the first aspect, in steps S2 and S5, the high-ductility concrete comprises, by weight parts: 80-120 parts cement, 100-150 parts grade I fly ash, 80-100 parts silica sand, 0.10-0.15 parts thickener, 1.0-5.0 parts polycarboxylate superplasticizer, water, with a water-cement ratio of 0.30-0.45, and polyvinyl alcohol fiber, wherein the volume content of the polyvinyl alcohol fiber is 1.5%-2.5%.

[0008] In one specific embodiment of the first aspect, in step S3, the carbon fiber cloth has a tensile strength ≥3400MPa, an elastic modulus ≥230GPa, and a unit area mass of 200~300g / m². 2 The number of layers is 1 to 3; the impregnating adhesive that generates curing heat is a two-component solvent-free epoxy resin impregnating adhesive, the mass ratio of component A to component B is 2:1 to 4:1, the peak temperature of the exothermic curing reaction is 50 to 70°C, the bond strength after curing is ≥2.5MPa, and the adhesive content of the carbon fiber cloth is controlled at 35% to 45%; when laying multiple layers of carbon fiber cloth, the adjacent two layers of carbon fiber cloth are bonded with the impregnating adhesive, and the overlap length between layers is not less than 150mm.

[0009] In one specific embodiment of the first aspect, in step S4, the anchoring structure is selected from any of the following forms: ECC covering anchoring, wherein the end of the carbon fiber cloth is extended and completely wrapped by the second ECC layer, and the anchoring length is not less than 150 mm; corrugated toothed plate mechanical anchoring, wherein a corrugated toothed steel anchoring plate is provided at the end of the carbon fiber cloth, the anchoring plate is embedded in the first ECC layer, the carbon fiber cloth is fastened by the tooth groove of the corrugated toothed plate and then covered and sealed by the second ECC layer, the tooth depth of the corrugated toothed plate is 5-10 mm, and the tooth spacing is 10-20 mm; or U-shaped folded wrapping anchoring, wherein the carbon fiber cloth is folded along the width direction at the edge of the autoclaved aerated concrete slab to form a U-shaped wrapping, and the folding width is not less than 1 / 2 of the slab thickness.

[0010] In one specific embodiment of the first aspect, in step S1, the roughening treatment makes the surface roughness reach 0.5 to 1.5 mm; in step S2, the spraying pressure of the first ECC layer is 0.3 to 0.6 MPa, and the spraying distance is 0.4 to 0.8 m.

[0011] In one specific embodiment of the first aspect, in step S6, the curing conditions are: a temperature of 15-30°C and a relative humidity of ≥90% for a period of not less than 7 days, or sealing curing is performed by spraying a curing agent.

[0012] In one specific embodiment of the first aspect, the autoclaved aerated concrete slab is an ALC floor slab or an ALC wall panel.

[0013] Secondly, an autoclaved aerated concrete (AAC) panel, reinforced by a composite reinforcement method of high-ductility concrete and carbon fiber cloth, comprises, from the inside out: Autoclaved aerated concrete (AAC) panel substrate; The interface-enhanced transition zone is formed by the bidirectional penetration and curing of the latent penetration enhancer in the interface agent after being activated by heat. This zone simultaneously forms a mechanical interlock and chemical bond with the substrate and the outer ECC layer. First ECC layer; The CFRP reinforcement layer is bonded to the first ECC layer by an impregnating adhesive and arranged along the stress direction, and includes at least one layer of carbon fiber cloth; The second ECC layer completely covers the CFRP enhancement layer; The CFRP reinforcement layer has anchoring structures at both ends in the longitudinal direction, and the first ECC layer and the second ECC layer together form an ECC reinforcement layer with a total thickness of 15 to 30 mm.

[0014] In one specific embodiment of the second aspect, the flexural bearing capacity of the reinforced slab is increased by 150% to 250% compared with the unreinforced autoclaved aerated concrete slab of the same specification, the failure mode is ductile bending failure, and there is no peeling at the CFRP end during failure.

[0015] The beneficial effects of this invention are as follows: 1. This invention constructs a dual dynamic linkage mechanism of "thermo-chemical-mechanical" between process steps by pre-setting a thermally activated latent penetrating reinforcing agent in the interface agent and using the heat release during the curing of the carbon fiber cloth impregnating adhesive as a trigger signal. In the first linkage, the heat released by the curing reaction of the impregnating adhesive is conducted to the interface agent layer through the first layer of high-ductility concrete, triggering the thermal response release of the latent penetrating reinforcing agent. The nanoscale active components, under the influence of concentration gradient and capillary action, penetrate bidirectionally along the pores of the autoclaved aerated concrete slab and the capillaries of the high-ductility concrete, reacting with the hydration products of the substrate to form an interface reinforcement transition zone with both mechanical interlocking and chemical bonding effects. This transition zone eliminates the abrupt stiffness change interface between the substrate and the reinforcement layer in traditional reinforcement processes, achieving a gradual gradient change in material composition and a smooth transition in mechanical properties. In the second layer of linkage, the formation of the interface-enhanced transition zone improves the interfacial stiffness and overall bonding integrity between the substrate and the high-ductility concrete layer. It optimizes the stress transfer path from the carbon fiber reinforcement layer to the substrate when the component is under stress, effectively reducing the shear stress concentration in the end region of the carbon fiber cloth, and suppressing the most common end-debonding failure mode in carbon fiber cloth reinforcement from a mechanical mechanism perspective. The two linkages are coupled with each other, transforming the originally passively stacked reinforcement layer structure into an active system with self-reinforcing and self-optimizing capabilities.

[0016] 2. This invention achieves directional reinforcement and systemic protection of autoclaved aerated concrete (AAC) panels through a multi-level synergistic structure consisting of an AAC panel substrate, a thermally responsive interface-reinforced transition zone, a first layer of high-ductility concrete, a carbon fiber reinforcement layer, a second layer of high-ductility concrete, and end anchoring structures. The carbon fiber fabric is laid directionally along the stress direction of the panel, fully utilizing the high tensile strength of continuous fibers to provide efficient directional reinforcement to the tension zone. The strain hardening characteristics and multi-crack mechanism of the high-ductility concrete layer dissipate energy through the development of dense micro-cracks during stress, endowing the reinforced component with significant ductile deformation capacity and damage tolerance, transforming the inherent brittle fracture mode of AAC panels into a ductile progressive failure mode. Simultaneously, the two layers of high-ductility concrete provide full protection for the carbon fiber fabric, isolating it from external environmental erosion of the carbon fiber fabric and impregnating adhesive. Its low permeability and self-healing crack properties further enhance the durability of the reinforcement system under long-term service conditions. The synergistic effect of the end anchoring structure and the interface reinforcement transition zone ensures the coordinated work of the carbon fiber cloth and the substrate from both end constraint and interface bonding dimensions, thus guaranteeing the full utilization of the high-strength properties of the carbon fiber cloth. Furthermore, the method of this invention is not limited by the production stage of autoclaved aerated concrete (AAC) panels and can be applied to the reinforcement of factory-made panels, panels before installation, and panels already installed in existing buildings, demonstrating strong construction adaptability. Attached Figure Description

[0017] Figure 1 This is a schematic diagram illustrating the principle of the dual dynamic linkage mechanism of the present invention. Detailed Implementation

[0018] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0019] like Figure 1 The method of composite reinforcement of high ductility concrete and carbon fiber cloth is shown.

[0020] I. This invention abandons the existing approach of treating each reinforcing layer as a passively stacked structure, and for the first time introduces a dual dynamic linkage mechanism of "thermo-chemical-mechanical" in the ECC-CFRP composite reinforcement system. Specifically, the heat of reaction released during the curing process of the carbon fiber cloth impregnating adhesive is used as a trigger signal to activate the latent penetrating reinforcing agent embedded in the interface agent, allowing it to actively penetrate and cure into the substrates on both sides (ALC board and the first ECC layer), thus strengthening the originally weakest "ALC board-ECC" interface at both physical and chemical levels. This strengthening of the interface further optimizes the stress transmission path of the entire reinforcement system, effectively suppressing the peeling damage at the ends of the carbon fiber cloth, thereby achieving a positive feedback loop and systematic synergistic effect between process steps.

[0021] To make the objectives, technical solutions, and advantages of the present invention clearer, the technical solutions of the present invention will be clearly and completely described below in conjunction with specific embodiments.

[0022] II. Raw material preparation and requirements.

[0023] 1. Autoclaved aerated concrete (ALC) panels.

[0024] The autoclaved aerated concrete (AAC) panels to be reinforced are standard industrially produced ALC panels with a dry density of 400–700 kg / m³. 3 The thickness is 75-200mm. Before reinforcement, the surface of the board should be free of obvious oil stains, release agent residue, and loose peeling layers.

[0025] 2. Interface agent components.

[0026] Interface agents consist of basic components and functional components: Basic components: a dilution of acrylate copolymer emulsion and water, with a mass ratio of 1:2 to 1:4, preferably 1:3. The acrylate copolymer emulsion is a commercially available architectural interface treatment emulsion (such as BASF Acronal series), with a solid content of 45% to 55%, and its main function is to seal the pores on the surface of ALC boards and provide basic adhesion.

[0027] Functional Component – ​​Thermally Activated Latent Penetration Enhancer: This component comprises nano-silica sol encapsulated by a thermosensitive polymer. The nano-silica sol has a solid content of 30% and an average particle size of 8–15 nm. The encapsulating material is a temperature-responsive polymer (such as poly(N-isopropylacrylamide) or its copolymers), with a designed lower critical solution temperature (LCST) of 45–55 °C. Encapsulation is performed via in-situ polymerization or spray drying to form core-shell microcapsules with an average particle size of 5–20 μm. When the ambient temperature reaches the LCST, the polymer shell undergoes a phase transition, shrinking or rupturing to release the core nano-silica sol.

[0028] Formulation ratio: The amount of thermally activated latent penetration enhancer is 5% to 15% of the mass of the interface agent base component, preferably 10%.

[0029] 3. High ductility concrete (ECC) components.

[0030] High-ductility concrete comprises the following components by weight: Cement (P·O 42.5 ordinary Portland cement): 100 parts; Grade 1 fly ash (fineness ≤12% residue on 45μm sieve, water requirement ≤95%): 120 parts; Silica sand (fineness modulus 1.8–2.2, maximum particle size 0.3 mm): 90 parts; Thickener (hydroxypropyl methylcellulose, viscosity 100000 mPa·s): 0.12 parts; Polycarboxylate superplasticizer (water reduction rate ≥30%): 3.0 parts; Water: Water-to-binder ratio 0.38; Polyvinyl alcohol (PVA) fiber: volume fraction 2.0%, fiber length 12mm, diameter 39μm, tensile strength 1600MPa, elastic modulus 40GPa (such as Japanese Kuraray RECS15 type). This mix design is based on micromechanical design principles to ensure that the ECC exhibits strain hardening and multi-crack characteristics. Its 28-day ultimate tensile strain is ≥3.5%, its 28-day compressive strength is 45–55 MPa, and the crack width can be controlled within 80 μm.

[0031] 4. Carbon fiber reinforced polymer (CFRP) cloth.

[0032] Tensile strength: ≥3400MPa; Elastic modulus: ≥230 GPa; Mass per unit area: 300g / m² 2 ; Calculated thickness: 0.167 mm; Elongation: ≥1.6%.

[0033] 5. Impregnating adhesive.

[0034] The impregnating adhesive is a two-component solvent-free epoxy resin impregnating adhesive. Component A is epoxy resin (bisphenol A type), and component B is a modified amine curing agent. The mass ratio of component A to component B is 3:1. The pot life of this impregnating adhesive at 25℃ is 40-60 minutes, the peak temperature of the exothermic curing reaction is 55-65℃ (measured under adhesive layer thickness of 0.5-1.0 mm), and the bond strength after curing is ≥2.5 MPa (concrete failure mode).

[0035] III. Specific Implementation Steps Step (1): ALC board surface interface treatment Input: Autoclaved aerated concrete (ALC) panels to be reinforced, in either finished or installed condition.

[0036] Procedure: First, the surface of the ALC board to be reinforced is roughened. Use a wire brush or sandblasting process to remove surface dust, release agent residue, and loose layers. The surface roughness (Rz) after roughening should reach 0.5–1.5 mm to increase the mechanical interlocking area. After treatment, blow away surface dust with compressed air.

[0037] Then, an interface agent containing a heat-activated latent penetration enhancer is applied. After uniformly mixing the base component and functional component of the interface agent in a specific ratio, it is evenly applied to the roughened ALC board surface using a roller or brush. The coating amount is 0.15–0.30 kg / m². 2 0.20 kg / m 2 When applying the coating, ensure that the surface is evenly covered and there are no missed areas.

[0038] Output: An interface agent layer with sealed surface pores and thermally responsive properties. This interface agent layer remains stable and inert at room temperature (below 25°C), and the latent penetration enhancer is perfectly encapsulated by the polymer shell, preventing penetration reaction.

[0039] Process principle explanation: Roughening treatment increases the micro-roughness of the ALC board surface, increasing the mechanical bonding area between the subsequent ECC layer and the substrate. The acrylic copolymer emulsion interface agent can penetrate into the pores 50-200 μm deep on the surface of the ALC board, forming a continuous polymer film on the pore surface and sealing the highly absorbent channels of the ALC board. This prevents the ALC board from absorbing water from the ECC slurry too quickly during subsequent ECC spraying, thus preventing an imbalance in the water-cement ratio at the interface. On the other hand, it provides an inert base layer for subsequent heat-triggered penetration enhancement. The latent penetration enhancer is uniformly dispersed in the interface agent in the form of microcapsules. It does not participate in the reaction during room temperature curing and is in a "dormant" state, waiting for the thermal signal to trigger in step (3).

[0040] Step (2): Spray the first layer of high-ductility concrete (ECC) Input: ALC plate after step (1) is completed and the interface agent layer is dry.

[0041] Procedure: Weigh each component according to the aforementioned ECC mix proportion. First, add the dry materials such as cement, fly ash, silica sand, and thickener to a forced mixer and dry mix for 2 minutes to ensure thorough mixing. Then, add water and polycarboxylate superplasticizer, and continue mixing for 3 minutes until the slurry is uniform and the fluidity reaches 160-200 mm (jump test). Finally, add PVA fibers and mix for 2 minutes until the fibers are evenly dispersed and there is no clumping.

[0042] The prepared ECC slurry is sprayed onto the ALC board surface to be reinforced using a wet spraying machine. The spraying parameters are: spraying pressure 0.3–0.6 MPa, preferably 0.4 MPa; spraying distance 0.4–0.8 m, preferably 0.6 m. Spraying is performed in multiple layers, with each layer controlled to a thickness of 3–5 mm, and multiple layers are stacked until the designed thickness is achieved.

[0043] The thickness of the first ECC layer is 50% to 70% of the total designed ECC thickness. When the total designed ECC thickness is 20mm, the thickness of the first ECC layer is 12mm (60%).

[0044] Output: The first ECC layer, with a thickness of 50% to 70% of the total design thickness, has a smooth surface and forms a preliminary bond with the ALC board through an interface agent layer.

[0045] Process principle explanation: Wet spraying process is adopted. Under the impetus of compressed air, ECC slurry impacts the surface of ALC board at a certain speed. The cement paste in the slurry can be embedded in the micro-pits formed by surface roughening, forming a preliminary mechanical interlock. Layered spraying can avoid slurry sagging and uneven fiber distribution caused by excessive thickness of a single spray. The thickness ratio of the first ECC layer (50%~70%) is of key significance: if it is too thin, it cannot provide enough flexible base layer to accommodate stress deformation; if it is too thick, the heat released by the curing of the impregnating adhesive in step (3) will be too much attenuated and affect the efficiency of thermal triggering. The thickness ratio of 50%~70% can ensure that the length of the heat conduction path is moderate, while ensuring the structural function of the ECC layer.

[0046] After spraying, allow the first ECC layer to stand at ambient temperature (15–30°C) to enter the initial setting state. The criterion for initial setting is: lightly pressing the surface with a finger leaves no obvious indentation, but the ECC still remains moist and chemically active (approximately 2–4 hours, depending on ambient temperature). In this state, the ECC matrix has completed the initial hydration reaction and has a certain shape retention ability, but it still contains a large number of unhydrated cement particles and free water. The pH value of the pore solution is approximately 12.5–13.0, enabling it to subsequently receive infiltrated substances and undergo chemical reactions.

[0047] Step (3): Apply carbon fiber reinforced polymer (CFRP) cloth – dynamic linkage triggering step Input: the first ECC layer formed in step (2) (initial setting state), and the interface agent layer containing latent permeability enhancer formed in step (1) (thermal isoelectric signal waiting to be triggered state).

[0048] Procedure: After the first ECC layer has initially set, the carbon fiber cloth is bonded to the surface of the first ECC layer along the stress direction (longitudinal direction) of the ALC plate using impregnating adhesive. The specific bonding process is as follows: First, a layer of impregnating adhesive is evenly applied to the surface of the first ECC layer as a primer, with a coating amount of 0.3–0.5 kg / m². 2 Then, lay the carbon fiber cloth flat on the base coat and roll it with a roller along the fiber direction to fully impregnate the carbon fiber cloth and remove air bubbles; finally, apply another layer of top coat to the surface of the carbon fiber cloth, with a coating amount of 0.2-0.4 kg / m². 2 The process ensures the carbon fiber cloth is fully impregnated. The adhesive content of the carbon fiber cloth is controlled at 35%–45%. One to three layers are laid, with an overlap length of no less than 150 mm between layers in multi-layer laying.

[0049] Dynamic linkage triggering process (the following processes occur synchronously during this step): After the carbon fiber cloth is pasted, the impregnating adhesive begins to cure. The curing reaction of the two-component epoxy resin is an exothermic reaction. Under the conditions of an adhesive layer thickness of 0.5-1.0 mm and an ambient temperature of 25°C, the peak temperature of the exothermic curing reaction can reach 55-65°C, and the duration of the temperature above 50°C is about 30-60 minutes.

[0050] The heat of curing is conducted through the first ECC layer to the interface agent layer formed in step (1). The response temperature of the thermosensitive polymer encapsulating the nano-silica sol microcapsules in the interface agent layer is 45-55°C, which precisely matches the peak exothermic temperature of the impregnating adhesive (55-65°C). When the local temperature of the interface agent layer reaches the response temperature of the microcapsules, the polymer shell undergoes a phase change, shrinks, or ruptures, releasing the nano-silica sol encapsulated inside.

[0051] After the nano-silica sol is released, due to the large number of capillary pores and moisture in both the ALC substrate and the first ECC layer, the nano-silica sol undergoes the following bidirectional permeation behavior driven by the concentration gradient and capillary action: Penetration into the ALC plate: Nano-sized silica sol (particle size 8-15 nm) penetrates inward along the pores (pore size tens to hundreds of micrometers) on the surface of the ALC plate, reaching a penetration depth of 0.5-2.0 mm. After entering the pores of the ALC plate, the active SiO2 in the nano-sized silica sol reacts with the hydration product Ca(OH)2 in the ALC plate to form CSH (hydrated calcium silicate) gel, creating chemically bonded micro-nails and wedges within the pores of the ALC plate.

[0052] Penetration towards the first ECC layer: Nano-silica sol penetrates outward along the capillaries of the ECC layer, and works together with the hydration products of unhydrated cement particles in the ECC and the pozzolanic reaction products of fly ash to further fill and compact the capillary pores of the ECC layer, thereby enhancing the density and strength of the ECC layer.

[0053] This bidirectional penetration and curing process forms an interface-reinforced transition zone with a thickness of 1–3 mm at the interface. This transition zone is not a sharp boundary, but rather a functional layer with a gradual gradient in material composition and mechanical properties from the ALC substrate to the ECC layer. Its gradient characteristics are as follows: on the ALC side, it is dominated by a mechanically interlocked structure formed by CSH gel filling the pores of the ALC; in the middle region, it is dominated by an organic-inorganic interpenetrating network formed by the interface agent acrylate polymer film and the penetrated and cured nano-SiO2; and on the ECC side, it is dominated by a dense reinforcing layer formed by the dense filling of ECC capillaries.

[0054] Output: (1) CFRP reinforcement layer - carbon fiber cloth is firmly bonded to the surface of the first ECC layer by the cured impregnating adhesive; (2) Interface reinforcement transition zone - an reinforcement transition zone with a thickness of 1 to 3 mm is formed between the ALC plate and the first ECC layer, which has the dual functions of mechanical interlocking and chemical bonding.

[0055] The first closed loop of the dual linkage is completed: the heat released by the curing of the impregnating adhesive in step (3) (which was originally an unfavorable factor that could accelerate the uneven hydration of ECC) is transformed into a positive driving force that triggers the release of the latent penetration enhancer in step (1), actively strengthening the weakest interface of "ALC board - first layer ECC".

[0056] Step (4): Anchoring treatment of carbon fiber cloth ends Input: The CFRP-reinforced sheet material after step (3) is completed.

[0057] Procedure: Anchoring structures are installed at both ends of the carbon fiber cloth in the longitudinal direction. The anchoring structures can take one of the following three forms or a combination thereof: Form A – ECC Cover Anchoring: The end of the carbon fiber cloth extends to the non-stressed area of ​​the ALC plate (such as at the plate support or within 1 / 8 to 1 / 6 of the span), and is completely wrapped by the second ECC layer in step (5) to form a grip-type anchoring. The anchoring length is not less than 150 mm, preferably 180 to 250 mm. The end of the carbon fiber cloth transitions smoothly to the surface of the first ECC layer without wrinkles or warping.

[0058] Form B – Corrugated Toothed Plate Mechanical Anchoring: A corrugated toothed steel anchoring plate (1.5–2.0 mm thick, Q235 material) is installed at the end of the carbon fiber cloth. The tooth depth of the corrugated toothed plate is 5–10 mm, the tooth spacing is 10–20 mm, and the plate width is the same as the width of the carbon fiber cloth. The anchoring plate is embedded in the first ECC layer (positioning grooves can be pre-embedded before the first ECC layer initially sets). After the carbon fiber cloth is tightened by winding back and forth through the tooth grooves of the corrugated toothed plate, it is covered and sealed by the second ECC layer. The bending path of the corrugated teeth can convert the longitudinal tensile force on the carbon fiber cloth into oblique compressive stress on the ECC on both sides of the tooth groove, effectively anchoring the carbon fiber cloth.

[0059] Form C – U-shaped Fold-over Anchoring: When reinforcing an ALC wall panel, the carbon fiber cloth is folded over along the width direction at the edge of the panel (both ends in the width direction) to form a U-shaped wrap. The fold width is not less than 1 / 2 of the panel thickness, preferably 60% to 80% of the panel thickness. The bending radius of the carbon fiber cloth at the fold is not less than 20mm to avoid fiber breakage. The ends of the folded carbon fiber cloth are covered and wrapped by a second ECC layer.

[0060] Output: The carbon fiber cloth ends are anchored to provide end constraints for subsequent stress.

[0061] Process principle explanation: The primary failure mode of carbon fiber cloth reinforced structural components is end peeling failure—during the stress process, the tensile stress borne by the carbon fiber cloth is transmitted to the substrate through the interface, forming stress concentration at the end of the carbon fiber cloth, causing the carbon fiber cloth to gradually peel off from the substrate starting from the end. Setting an end anchoring structure can effectively suppress the occurrence of peeling. In particular, in this invention, since an interface-enhanced transition zone has been formed through dynamic linkage in step (3), the stiffness and bonding strength of the first interface have been fundamentally improved, the stress transmission path is more uniform, and the degree of shear stress concentration at the end of the carbon fiber cloth has been reduced. Therefore, the design requirements of the anchoring structure can be reduced accordingly, and the anchoring length or the scale of the anchoring device can be reduced.

[0062] Step (5): Spray the second layer of high-ductility concrete (ECC) Input: After steps (3) and (4) are completed, the carbon fiber cloth has been pasted and the anchoring structure has been set.

[0063] Operation: After the carbon fiber cloth is pasted and the impregnating adhesive is surface dry (approximately 4-6 hours after pasting, when it is no longer sticky to the touch), spray the second layer of high-ductility concrete. The mix proportion and mixing process of ECC are the same as in step (2). The second layer of ECC completely covers the carbon fiber cloth and anchoring structure, and the spray thickness is 30%-50% of the total design thickness of ECC. When the total design thickness of ECC is 20mm, the spray thickness of the second layer of ECC is 8mm (40%).

[0064] The first ECC layer and the second ECC layer together constitute an ECC reinforcement layer with a total design thickness of 15-30mm.

[0065] Output: The carbon fiber cloth is completely covered and wrapped by the second ECC layer, and the total thickness of the ECC reinforcement layer reaches the design value.

[0066] Process principle explanation: The second ECC layer has multiple functions: (1) As a protective layer, it isolates the carbon fiber cloth from the external environment and prevents the carbon fiber cloth from being directly affected by adverse factors such as ultraviolet aging, mechanical scratches, and high temperature from fire; (2) As an additional force transmission layer, it participates in the stress transmission when the component is under stress and forms a double constraint on the carbon fiber cloth together with the first ECC layer; (3) As an anchoring cover layer, it forms a closed enclosure for the anchoring structure set in step (4) to ensure the long-term reliable operation of the anchoring structure; (4) When under stress, the second ECC layer also plays the role of multi-crack characteristics and participates in energy dissipation and ductility contribution.

[0067] The 30% to 50% thickness ratio design takes into account the following factors: the main function of the second layer of ECC is protection and coverage, rather than the main structural load-bearing body, so its thickness can be less than that of the first layer; however, if it is too thin (<5mm), it may not be able to effectively exert the multi-slit cracking characteristics due to the limited fiber distribution, and the durability of the protective layer is insufficient.

[0068] Step (6): Maintenance Input: The complete reinforced plate after step (5) is completed.

[0069] Operation: Curing the composite reinforcement layer after spraying. One of the following curing methods can be used: (1) Cover with plastic film and wet cure for no less than 7 days under the conditions of temperature 15~30℃ and relative humidity ≥90%; (2) Spray curing agent (such as acrylic film-forming curing agent) for sealing curing.

[0070] During the curing period, the boards should be protected from vibration, impact and concentrated loads.

[0071] Output: The ECC layer reaches the design strength, and the entire reinforcement system forms a stable composite stress structure.

[0072] Process Principle Explanation: The high ductility and multi-crack characteristics of ECC rely on appropriate interfacial bonding between the fiber and the cement matrix, which is highly sensitive to curing conditions. Sufficient water curing ensures complete cement hydration and the pozzolanic reaction of fly ash, forming a dense hydration product matrix. Simultaneously, it ensures appropriate chemical and frictional bonding between the PVA fibers and the matrix—neither too strong (leading to fiber breakage rather than pull-out, resulting in loss of ductility) nor too weak (leading to easy fiber pull-out and insufficient strength). A 7-day curing period ensures that ECC reaches over 70% of its 28-day strength, and crack width control is essentially achieved.

[0073] IV. Summary of the Logical Chain of the Dynamic Linkage Mechanism The dual dynamic linkage mechanism of this invention: First thermally triggered penetration enhancement closed loop: Step (3) impregnation adhesive curing releases heat (heat source); heat conduction passes through the first layer of ECC; triggers the latent penetration enhancer in the interface agent in step (1) (thermal response release); nano silica sol penetrates bidirectionally into ALC plate and ECC; volcanic ash reaction occurs to generate CSH gel; forming an interface enhancement transition zone of mechanical interlocking and chemical bonding; effect: the bonding strength of ALC plate-ECC interface is greatly improved.

[0074] Second mechanical feedback optimization closed loop: interface enhancement transition zone is formed; stiffness transition from ALC plate to ECC layer is smoother and more uniform; stress transmission path is optimized when under stress; the degree of shear stress concentration at the end of CFRP reinforcement layer in step (3) is reduced; CFRP end peeling was effectively suppressed; the effect was that the CFRP strength utilization rate was further improved and the system ductility was enhanced.

[0075] This dual linkage transforms the reinforcement system from a passive superposition of functional layers into an active system with self-reinforcing and self-optimizing capabilities.

[0076] V. Examples The technical solution and beneficial effects of the present invention will be further described below with reference to a specific embodiment. It should be understood that this embodiment is only used to explain the present invention and is not intended to limit the scope of the present invention.

[0077] Example 1: ALC floor slab reinforcement (1) Parameters of the slab to be reinforced: A certain autoclaved aerated concrete (ALC) floor slab, with dimensions of 3000mm (length) × 600mm (width) × 150mm (thickness) and a dry density of 520kg / m³. 3 The device has an internal steel mesh (φ5@150 bidirectional), and the measured bending capacity is 6.8kN (four-point bending, span 2.7m). The failure mode is brittle fracture with a single crack at mid-span, and the mid-span failure deflection is 4.5mm.

[0078] (2) Preparation of interface agent: Acronal S400 (BASF) and water were mixed at a mass ratio of 1:3 and stirred evenly as the basic component of the interface agent. Thermosensitive polymer-encapsulated nano-silica sol microcapsules (self-made, nano-silica sol solid content 30%, microcapsule average particle size 10μm, response temperature 50℃) were added as the functional component at 10% of the mass of the basic component and stirred evenly to obtain an interface agent containing a heat-activated latent penetration enhancer.

[0079] (3) ECC preparation: Weigh the ECC components (per cubic meter) according to the following proportions: Cement (P·O 42.5): 350 kg; Grade 1 fly ash: 420 kg; Silica sand (fineness modulus 2.0): 315 kg; Hydroxypropyl methylcellulose: 0.42 kg; Polycarboxylate superplasticizer: 10.5 kg; Water: Water-to-binder ratio 0.38; PVA fiber (Kuraray RECS15): 26kg (volume content 2.0%).

[0080] (4) Reinforcement construction: Construct according to steps (1) to (6) in the aforementioned specific implementation method: Step (1): Grind the bottom surface of the ALC board with a wire brush to a roughness of 0.8mm, and apply an interface agent at a rate of 0.20kg / m. 2 Let it stand until it is surface dry (about 45 minutes).

[0081] Step (2): Wet spray the first layer of ECC, spray pressure 0.4MPa, spray distance 0.6m, thickness 12mm (60% of the total design thickness of 20mm), and let stand until initial setting (about 3 hours).

[0082] Step (3): Lay a layer of carbon fiber cloth (Toray UT70-30, tensile strength 3450MPa, elastic modulus 240GPa, unit area mass 300g / m²). 2 The adhesive was laid along the entire longitudinal length of the board. The ratio of impregnating adhesive A:B was 3:1, with the adhesive content controlled at approximately 40%. After bonding, the temperature change during the curing process of the impregnating adhesive was observed—a thermocouple was embedded at the interface between the adhesive layer and the first ECC layer, and the peak temperature was measured to be 58℃, lasting for approximately 45 minutes. Simultaneously, a temperature sensor embedded in the interface agent layer was used to measure the peak temperature of the interface agent layer, which was 51℃, confirming that the microcapsule response temperature had been reached.

[0083] Step (4): Extend the carbon fiber cloth 180mm into the support at both ends to serve as the ECC covering anchor section.

[0084] Step (5): After the carbon fiber cloth is pasted and surface dry (about 5 hours), wet spray the second layer of ECC with a thickness of 8mm (40% of the total design thickness), and the total thickness of ECC is 20mm.

[0085] Step (6): Cover with plastic film and water for 7 days at room temperature (about 20°C).

[0086] (5) Effect verification: After the reinforcement is completed, a four-point bending test is carried out on the reinforced plate (span 2.7m, loading point 0.9m from the support), and it is compared with the unreinforced ALC plate of the same specification.

[0087] ; The damage development process observed during the experiment is as follows: When loaded to about 8kN, the first microcrack (about 30μm wide) began to appear in the tensile zone of the first ECC layer. When loaded to the range of 10 to 14 kN, multiple parallel micro-cracks (crack spacing of about 3 to 8 mm) appeared in the ECC layer, exhibiting a typical multi-crack cracking mode, with the crack width controlled within 60 μm. When the load exceeds 15kN, the CFRP begins to bear the main tensile stress, and the strain increases linearly with the load. When loaded to 18.9 kN, the CFRP underwent progressive fracture in the mid-span region. No end peeling occurred during the entire process, and the cracks were mostly closed after unloading.

[0088] (6) Comparative example: A common interface agent (only acrylic emulsion dilution) without thermally activated latent penetration enhancer was used for reinforcement construction according to the same steps and parameters, and a four-point bending test under the same conditions was carried out.

[0089] ; Comparative results show that under ordinary interface agent conditions, due to the lack of an interface-reinforced transition zone formed by thermally triggered penetration enhancement, the bonding strength and stiffness of the ALC-ECC interface are insufficient. During stress, some areas of the interface experience bonding failure, leading to slight peeling at the CFRP ends and limiting the full utilization of CFRP strength. In contrast, the interface-reinforced transition zone formed by the dual dynamic linkage mechanism in this embodiment effectively avoids interface bonding failure, ensuring the synergistic work between CFRP and the substrate, and fully realizing the reinforcement effect.

[0090] This embodiment verifies the effectiveness of the method of the present invention for strengthening ALC floor slabs. By triggering the latent penetrating reinforcing agent in the interface agent in step (1) through the exothermic curing of the impregnating adhesive in step (3), an interface-enhanced transition zone is formed between the ALC slab and the ECC layer. This enhanced transition zone optimizes the stress transmission path, effectively inhibits CFRP end peeling, and increases the flexural bearing capacity of the reinforced slab by 178%. The failure mode changes from brittle fracture to ductile failure, achieving the design objective of a dual dynamic linkage mechanism.

[0091] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A method for reinforcing autoclaved aerated concrete (AAC) slabs with a composite of high-ductility concrete and carbon fiber fabric, characterized in that, Includes the following steps: S1: Roughen the surface of the autoclaved aerated concrete (AAC) slab to be reinforced, and then coat it with an interface agent containing a thermally activated latent interface penetration enhancer to seal the pores on the surface of the AAC slab and form an interface layer with thermally responsive characteristics. The thermally activated latent interfacial penetration enhancer is a nano-silica sol encapsulated by a thermosensitive polymer or a latent epoxy curing agent. S2: High-ductility concrete is sprayed onto the surface coated with the interface agent to form a first ECC layer, wherein the spraying thickness of the first ECC layer is 50% to 70% of the total design thickness of the ECC layer; S3: After the first ECC layer has initially set, at least one layer of carbon fiber cloth is bonded to the surface of the first ECC layer along the stress direction of the autoclaved aerated concrete slab using an impregnating adhesive that can generate heat of curing reaction, to form a CFRP reinforcement layer. S4: Anchoring structures are provided at both ends of the longitudinal direction of the carbon fiber cloth; S5: After the carbon fiber cloth is pasted and surface dry, a second ECC layer is sprayed to completely cover the carbon fiber cloth. The spraying thickness of the second ECC layer is 30% to 50% of the total design thickness of the ECC. The first ECC layer and the second ECC layer together constitute an ECC reinforcement layer with a total design thickness of 15 to 30 mm. S6: Curing the composite reinforcement layer after spraying; In step S3, the heat released by the curing reaction of the impregnating adhesive is conducted to the interface layer formed in step S1, triggering the latent interface penetration enhancer to penetrate and cure bidirectionally into the autoclaved aerated concrete board substrate and the first ECC layer, forming a reinforced transition zone of mechanical interlocking and chemical bonding. and, The formation of the enhanced transition zone enhances the interfacial stiffness and bond strength between the autoclaved aerated concrete (AAC) panel and the first ECC layer, thereby optimizing the stress transfer path from the CFRP reinforcement layer to the substrate under stress and suppressing stress concentration and peeling failure at the ends of the CFRP reinforcement layer.

2. The method according to claim 1, characterized in that, In step S1, the thermal activation temperature of the thermally activated latent interfacial penetration enhancer is 40–70°C; the main component of the interfacial agent is a diluted solution of acrylate copolymer emulsion and water, with a mass ratio of 1:2 to 1:4, and the coating amount is 0.15–0.30 kg / m². 2 .

3. The method according to claim 1, characterized in that, In steps S2 and S5, the high-ductility concrete comprises, by weight parts: 80-120 parts cement, 100-150 parts grade I fly ash, 80-100 parts silica sand, 0.10-0.15 parts thickener, 1.0-5.0 parts polycarboxylate superplasticizer, water, with a water-cement ratio of 0.30-0.45, and polyvinyl alcohol fiber, wherein the volume content of the polyvinyl alcohol fiber is 1.5%-2.5%.

4. The method according to claim 1, characterized in that, In step S3, the carbon fiber cloth has a tensile strength ≥3400MPa, an elastic modulus ≥230GPa, and a unit area mass of 200~300g / m². 2 The number of layers is 1 to 3; the impregnating adhesive that generates curing heat is a two-component solvent-free epoxy resin impregnating adhesive, the mass ratio of component A to component B is 2:1 to 4:1, the peak temperature of the exothermic curing reaction is 50 to 70°C, the bond strength after curing is ≥2.5MPa, and the adhesive content of the carbon fiber cloth is controlled at 35% to 45%; when laying multiple layers of carbon fiber cloth, the adjacent two layers of carbon fiber cloth are bonded with the impregnating adhesive, and the overlap length between layers is not less than 150mm.

5. The method according to claim 1, characterized in that, In step S4, the anchoring structure is selected from any of the following forms: ECC covering anchoring, wherein the end of the carbon fiber cloth is extended and completely wrapped by the second ECC layer, and the anchoring length is not less than 150 mm; corrugated toothed plate mechanical anchoring, wherein a corrugated toothed steel anchoring plate is provided at the end of the carbon fiber cloth, the anchoring plate is embedded in the first ECC layer, the carbon fiber cloth is fastened by the tooth groove of the corrugated toothed plate and then covered and sealed by the second ECC layer, the tooth depth of the corrugated toothed plate is 5-10 mm, and the tooth spacing is 10-20 mm; or U-shaped folded wrapping anchoring, wherein the carbon fiber cloth is folded along the width direction at the edge of the autoclaved aerated concrete slab to form a U-shaped wrapping, and the folding width is not less than 1 / 2 of the slab thickness.

6. The method according to claim 1, characterized in that, In step S1, the roughening treatment makes the surface roughness reach 0.5 to 1.5 mm; in step S2, the spraying pressure of the first ECC layer is 0.3 to 0.6 MPa, and the spraying distance is 0.4 to 0.8 m.

7. The method according to claim 1, characterized in that, In step S6, the curing conditions are: a temperature of 15-30°C and a relative humidity of ≥90% for at least 7 days, or sealing curing is performed by spraying a curing agent.

8. The method according to any one of claims 1 to 7, characterized in that, The autoclaved aerated concrete (AAC) slab is either an ALC floor slab or an ALC wall panel.

9. An autoclaved aerated concrete (AAC) slab, characterized in that, The reinforcement obtained by the method described in any one of claims 1 to 8 comprises, from the inside out: Autoclaved aerated concrete (AAC) panel substrate; The interface-enhanced transition zone is formed by the bidirectional penetration and curing of the latent penetration enhancer in the interface agent after being activated by heat. This zone simultaneously forms a mechanical interlock and chemical bond with the substrate and the outer ECC layer. First ECC layer; The CFRP reinforcement layer is bonded to the first ECC layer by an impregnating adhesive and arranged along the stress direction, and includes at least one layer of carbon fiber cloth; The second ECC layer completely covers the CFRP enhancement layer; The CFRP reinforcement layer has anchoring structures at both ends in the longitudinal direction, and the first ECC layer and the second ECC layer together form an ECC reinforcement layer with a total thickness of 15 to 30 mm.

10. The autoclaved aerated concrete slab according to claim 9, characterized in that, The flexural bearing capacity of the reinforced slab is increased by 150% to 250% compared with the unreinforced autoclaved aerated concrete slab of the same specification. The failure mode is ductile bending failure, and there is no peeling at the ends of the CFRP during failure.

Citation Information

Patent Citations

  • Treatment method for improving adhesive force of interfaces of new and old concrete

    CN111188492A

  • Two-way reinforcement of a damaged reinforced concrete plate through FRP / high-ductility high-permeability concrete and preparation method

    CN112482817A