A method for deep purification of sodium sulfate from industrial solid waste
By employing processes such as alkaline precipitation, sulfide co-precipitation, and chelate resin deep adsorption, combined with activated carbon adsorption, ozone oxidation, and ion exchange, the problem of removing heavy metals and impurities from industrial solid waste sodium sulfate has been solved, enabling high-value reuse and environmentally friendly sodium sulfate product production.
Patent Information
- Application Number
- CN202611141088.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-30
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2046-07-30
AI Technical Summary
Existing technologies cannot effectively remove heavy metals and other impurities from industrial solid waste sodium sulfate, making it unable to meet the usage requirements of the plastic filler, detergent, glass manufacturing, papermaking and textile printing and dyeing industries, and large-scale stockpiling causes environmental pollution and resource waste.
Heavy metals were removed by a method of alkaline precipitation-sulfurization co-precipitation-chelation resin deep adsorption, combined with activated carbon adsorption, ozone oxidation, stripping deammoniation and ion exchange processes, and finally sodium sulfate was purified by MVR evaporation crystallization.
This technology enables the high-value reuse of sodium sulfate, an industrial solid waste, with product quality reaching or even exceeding that of sodium sulfate mined from mines. It eliminates the risk of heavy metal pollution, maintains the physical and chemical properties of the product, and achieves resource conservation and environmental benefits.
Smart Images

Figure CN122646875B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of industrial solid waste resource utilization technology, specifically to a process for deep purification of industrial solid waste sodium sulfate to remove heavy metals and other impurities, making it meet the reuse requirements of industries such as plastic fillers, detergents, glass manufacturing, papermaking, and textile printing and dyeing. Background Technology
[0002] (I) Composition and hazards of impurities in industrial solid waste sodium sulfate In existing lithium-ion battery ternary cathode material precursor production processes, sulfate systems (such as nickel sulfate, cobalt sulfate, and manganese sulfate) are typically used as metal raw materials. The core reaction formula in the co-precipitation reaction stage is: M 2+ SO4+ 2NaOH → M(OH)2↓ + Na2SO4 In this reaction system, M represents metal ions such as nickel (Ni), cobalt (Co), and manganese (Mn). The generated M(OH)₂ is a water-insoluble precipitate, which can be collected as a precursor product through a solid-liquid separation process. Na₂SO₄, however, remains largely in the mother liquor as a soluble byproduct. With continuous recycling and concentration of the mother liquor, high-salt wastewater or waste salt rich in sodium sulfate is eventually formed. Since the metal ions carried in the raw materials cannot be completely utilized or removed by the precursor precipitation, the byproduct sodium sulfate inevitably contains various heavy metal impurities.
[0003] Based on the analysis of sodium sulfate produced as a byproduct by several domestic lithium battery manufacturers, the types and contents of residual impurities are as follows: (1) Heavy metal ions: Nickel (Ni 2+ The content is usually between 5-50 mg / kg, and the cobalt (Co) content is... 2+ The content is 3-30 mg / kg, manganese (Mn) 2+ The content is 5-80 mg / kg. Trace amounts of copper (Cu) may also be present in the ternary system. 2+ ), iron (Fe) 2+ ), aluminum (Al) 3+ The content varies from 1 to 20 mg / kg.
[0004] (2) Alkaline earth metals: calcium (Ca 2+ The content is usually between 100-800 mg / kg, magnesium (Mg) 2+ The content is between 50-500 mg / kg, mainly from the residue in the lime milk precipitation pretreatment process and the associated components in the raw materials.
[0005] (3) Chloride ions (Cl) -The content is between 500-5000 mg / kg, which comes from the use of hydrochloric acid and the introduction of washing water during the production process.
[0006] (4) Organic matter (COD): The content is between 100-1000 mg / kg, which comes from the residue of organic reagents such as extractants and chelating agents.
[0007] (5) Ammonia nitrogen (NH4) + The content is between 50-500 mg / kg, which comes from the residue of ammonia water used as a precipitant in the synthesis of precursors.
[0008] (6) Moisture content: 0.5-3.0%, which affects the storage stability of the product and its performance in downstream applications.
[0009] The hazards posed by these impurities are multifaceted. Heavy metals such as nickel, cobalt, and manganese exhibit bioaccumulation and persistent toxicity. If they enter downstream applications along with sodium sulfate, they will be released into plastics and glass products over a long period, causing secondary pollution. According to the "Identification Standard for Hazardous Waste: Leaching Toxicity Identification" (GB 5085.3-2007), the leaching toxicity limit for nickel is 5 mg / L, and for cobalt, it is 5 mg / L. If the heavy metal content in the byproduct sodium sulfate exceeds the limit and is not properly treated, the concentration of heavy metals in the leachate may exceed hazardous waste standards after leaching by rainwater during storage, thus being classified as hazardous waste. This would bring huge disposal costs and legal risks to enterprises, especially as the metals could enter rivers and lakes or seep into the ground, causing serious environmental pollution. This large amount of sodium sulfate, a byproduct inevitably produced with the main reaction, is the fundamental chemical source of the current industry's pressure on solid waste storage and the pain points in resource utilization.
[0010] (ii) Overproduction and Stockpiling Pollution The synthesis reaction of ternary precursors dictates that each ton of precursor will inevitably produce approximately 1.46-1.67 tons of sodium sulfate. Taking the NCM523 precursor as an example, the theoretical yield is approximately 1.46 tons of sodium sulfate per ton of precursor. Adding the sodium sulfate in the washing water and mother liquor, the actual co-production ratio in the industry is between 1:1.5 and 1:1.7.
[0011] my country's lithium battery production capacity has expanded rapidly in recent years. Based solely on publicly disclosed project data, the annual production of sodium sulfate as a byproduct of the national lithium battery industry is conservatively estimated to exceed 1.5 million tons. With the continued expansion of lithium battery production capacity, the pressure to comply with regulations regarding its disposal is becoming increasingly severe.
[0012] Such a massive output far exceeds the absorption capacity of downstream industries. The traditional downstream markets for industrial-grade sodium sulfate (anhydrous sodium sulfate)—filler, dyeing, glass, and detergent industries—have relatively stable annual demand and cannot absorb the million-ton-level new supply from the lithium battery industry in the short term. Large quantities of by-product sodium sulfate can only be stored in factory warehouses or temporary storage yards, leading to environmental risks including: (1) Heavy metal leaching pollution: When stored sodium sulfate is leached by rainwater, the residual nickel, cobalt and manganese heavy metal ions will seep into the soil and groundwater, causing persistent pollution.
[0013] (2) Soil salinization: Sodium sulfate is a highly soluble salt. Large-scale accumulation or diffusion with rainwater will significantly increase the salt and sulfate content of the surrounding soil, damage the soil structure, and inhibit plant growth.
[0014] (3) Water pollution: When sodium sulfate leachate flows into surface water bodies, it will increase the salinity of the water, disrupt the osmotic pressure balance of aquatic organisms, and cause fish and benthic organisms to die.
[0015] (4) Land and capital occupation: The large amount of stockpiling not only occupies valuable industrial land, but also requires continuous investment in the construction and maintenance of anti-seepage and dust control facilities.
[0016] (III) The problem of product duplication and resource waste in mining sodium sulfate and by-product sodium sulfate. my country is one of the major producers of natural sodium sulfate (anhydrous sodium sulfate), with natural sodium sulfate deposits or salt lake resources distributed in Yuncheng Salt Lake in Shanxi, Meishan in Sichuan, Hengyang in Hunan, Inner Mongolia, and other places. The existing annual production capacity of sodium sulfate produced through mining and chemical synthesis in China can already meet the demand of traditional downstream markets.
[0017] Before the large-scale influx of industrial solid waste sodium sulfate into the market, the supply and demand of sodium sulfate from mines was basically in balance with downstream demand. However, with the explosive growth of the lithium battery industry, the annual increase of more than 1.5 million tons of by-product sodium sulfate has impacted the existing market structure. (1) Product duplication: Natural sodium sulfate mined from mines and sodium sulfate from industrial solid waste both have the chemical composition of Na2SO4 and are targeted at the same downstream customers. The two are in direct competition at the product level, resulting in redundant capacity construction.
[0018] (2) Waste of resources: On the one hand, mining companies continue to mine sodium sulfate, consuming non-renewable mineral resources; on the other hand, a large amount of sodium sulfate produced by lithium battery companies is stockpiled or even abandoned due to substandard quality or lack of disposal channels. This situation of "mining on one hand and abandoning on the other" is a huge waste of social resources.
[0019] (3) Environmental superposition effect: Mining sodium sulfate will generate environmental problems such as mine wastewater, tailings slag, and destruction of surface vegetation; the stockpiling of industrial solid waste sodium sulfate will also cause heavy metal leaching and salinization problems. The simultaneous operation of two production lines will increase the environmental burden many times over.
[0020] (4) Vicious price competition: In order to reduce storage costs, by-product sodium sulfate often enters the market at extremely low prices or even by subsidizing transportation costs, squeezing the profit margins of mining companies and disrupting the normal market order.
[0021] Therefore, if industrial solid waste sodium sulfate can be deeply purified to achieve a quality that meets or even exceeds that of sodium sulfate mined from mines, thus realizing "replacing ore with waste", it will not only solve the solid waste disposal problem of lithium battery companies, but also reduce the consumption of natural mineral resources, achieving dual environmental benefits. Summary of the Invention
[0022] The technical problem to be solved by the present invention is to provide a method for deep purification of industrial solid waste sodium sulfate, which removes heavy metal ions, alkaline earth metals, chloride ions, organic matter and ammonia nitrogen impurities to the level that meets the requirements of the plastic filling industry, detergent industry, glass manufacturing industry, papermaking industry and textile printing and dyeing industry without changing the product's color, transparency and physical and chemical properties, thereby realizing the high-value reuse of industrial solid waste sodium sulfate.
[0023] To solve the above-mentioned technical problems, the technical solution of the present invention is as follows: A method for deep purification of sodium sulfate from industrial solid waste includes the following steps: S1, Dissolution and Pretreatment The raw material, crude anhydrous sodium sulfate from industrial solid waste, is dissolved in deionized water to prepare a sodium sulfate solution with a concentration of 200-280 g / L. The solution is heated to 60-80°C to ensure complete dissolution. Sodium hydroxide is added to the solution to adjust the pH to 10.5-11.5, so that the residual heavy metal ions of nickel, cobalt, manganese, copper, iron, and aluminum can form hydroxide precipitates under alkaline conditions. The reaction time is controlled at 30-60 minutes, and the temperature is maintained at 60-80°C.
[0024] Sodium sulfide is added as a co-precipitant during the heavy metal precipitation stage. The optimal dosage of sodium sulfide is 1.05-1.20 times the theoretical stoichiometry to further reduce the residual amount of heavy metal ions. The solubility of sulfide precipitates formed by the reaction of sodium sulfide with heavy metal ions is much lower than that of hydroxide precipitates, which can reduce the content of nickel, cobalt, and manganese to even lower levels.
[0025] After multiple reactions, when the heavy metal content reaches a certain concentration, solid-liquid separation is carried out by plate and frame filter or precision filter (filtration accuracy ≤1μm). The filter residue (heavy metal hydroxide and sulfide precipitates) is collected and handed over to a qualified unit to recover the valuable metals.
[0026] S2, Deep calcium and magnesium removal Cool the filtrate from step S1 to 40-55°C, add sodium carbonate solution, preferably 1.1-1.3 times the theoretical stoichiometry, and react for 20-40 minutes to precipitate the residual calcium ions into calcium carbonate; then add sodium hydroxide to adjust the pH to 12.0-12.5 to precipitate the magnesium ions into magnesium hydroxide.
[0027] After the reaction is complete, a second precision filtration (filtration accuracy ≤1μm) is performed to remove calcium carbonate and magnesium hydroxide precipitates. This step can reduce the calcium content to ≤50 mg / kg and the magnesium content to ≤30 mg / kg.
[0028] Following chemical precipitation, a primary ion exchange process is introduced, preferably using chelating cation exchange resins (such as aminophosphonic acid resins or iminodiacetic acid resins) to further adsorb residual trace amounts of calcium, magnesium, and heavy metal ions. The operating flow rate of the ion exchange column is preferably controlled at 5-15 BV / h (bed volume / hour), which can reduce the total calcium and magnesium content in the effluent to ≤10 mg / kg.
[0029] S3. Removal of organic matter and decolorization The solution treated in step S2 is passed through an activated carbon adsorption column. Coconut shell-based granular activated carbon is preferred (iodine value ≥1000 mg / g, methylene blue value ≥180 mg / g), with a flow rate controlled at 3-8 BV / h. Activated carbon effectively adsorbs residual organic extractants, chelating agent residues, and colored substances in the solution, reducing the solution color to below 10 Hazen.
[0030] An ozone oxidation process is connected in series after the activated carbon adsorption column. Ozone is introduced into the solution at a dosage of 5-15 mg / L for a contact time of 10-20 minutes to oxidize and decompose residual recalcitrant organic matter, while simultaneously eliminating any potentially present ferrous ions (Fe2+). 2+ ) is oxidized to trivalent iron (Fe) 3+ This allows for subsequent removal. The ozone-oxidized solution then undergoes a first-stage precision filtration (0.45μm) to remove trace amounts of flocculents produced during ozone oxidation.
[0031] S4, deamination The solution treated in step S3 is adjusted to pH 11.0-12.0 and then fed into a stripping ammonia removal tower. The tower temperature is controlled at 95-105°C, and the steam-to-liquid mass ratio is controlled at 0.15-0.30. Under alkaline high-temperature conditions, ammonium ions (NH4+) in the solution...+ The ammonia gas is converted into free ammonia (NH3), which is carried away by steam and escapes from the top of the column. The ammonia-containing gas at the top of the column is then condensed and recovered or absorbed by sulfuric acid to produce ammonia water or ammonium sulfate as byproducts.
[0032] The ammonia nitrogen content in the solution after ammonia removal can be reduced to ≤10 mg / kg. The effluent from the bottom of the ammonia removal tower is a purified sodium sulfate solution with low ammonia nitrogen and low heavy metal content.
[0033] S5, dechlorination The solution after deammoniation in step S4 is passed through an anion exchange resin column, preferably a quaternary ammonium type strong basic anion exchange resin with high selectivity for chloride ions. The resin is then used to process chloride ions. - Its preferential exchange capacity removes chloride ions from the solution, while simultaneously removing sulfate ions (SO42-). 2- Because of its divalent nature, it has a stronger affinity for resin and will not be lost in large quantities through exchange.
[0034] The ion exchange column is operated at a flow rate of 6-17 BV / h, and the chloride ion content in the effluent can be reduced to ≤100 mg / kg. Once the resin is saturated, it is regenerated using a 4-10% sodium chloride solution.
[0035] For raw materials with low chloride ion content (<1000 mg / kg), this step can be omitted, and the chloride ion content in the product can be naturally reduced through the salt separation effect during the subsequent evaporation and crystallization process.
[0036] S6, MVR evaporation crystallization and drying The purified solution, after ammonia or chlorine removal, is fed into an MVR (Mechanical Vapor Recompression) evaporation crystallization system. The evaporation temperature is controlled at 85-105°C, and the operating pressure of the evaporation system is atmospheric pressure or slightly positive pressure. During the evaporation process, sodium sulfate gradually reaches supersaturation and crystallizes out due to the characteristic that its solubility changes with temperature.
[0037] The secondary steam generated by evaporation and crystallization is pressurized and heated by a compressor and then recycled as a heat source. The steam compression ratio is controlled at 1.3-1.8 and the evaporation concentration ratio is controlled at 2.5-4.0 times.
[0038] Because sodium chloride has a higher solubility than sodium sulfate at high temperatures, and the solubility of sodium chloride is less affected by temperature, sodium sulfate precipitates preferentially during the evaporation and crystallization process, while most of the sodium chloride remains in the mother liquor, thus achieving the separate crystallization of sodium sulfate and sodium chloride.
[0039] The crystallized slurry is centrifuged to obtain wet sodium sulfate crystals. The mother liquor is returned to the evaporation system for further concentration or a small amount of high-salt mother liquor is discharged for separate treatment. The wet sodium sulfate is dried in a fluidized bed dryer or rotary dryer with hot air at 120-180°C until the moisture content is ≤0.1%.
[0040] The dried anhydrous sodium sulfate is graded by a vibrating screen, with the particle size controlled between 0.2-1.0 mm to remove excessively fine powder and excessively large particles, thus obtaining purified anhydrous sodium sulfate product. After passing the graded product inspection, it is packaged and stored.
[0041] Compared with the prior art, the present invention has at least the following beneficial effects: (1) Achieving "replacing ore with waste" and saving mineral resources. The industrial solid waste sodium sulfate purified by the method of this invention has reached or even exceeded the Class I superior grade standard of GB / T 6009-2014, and can directly replace sodium sulfate mined from mines. For every ton of sodium sulfate replaced, the mining of 1 ton of natural sodium sulfate is reduced, thus saving non-renewable mineral resources.
[0042] (2) Elimination of heavy metal pollution risks. This invention utilizes a three-stage heavy metal removal process involving alkaline precipitation, sulfide co-precipitation, and deep adsorption with chelating resin to reduce the contents of nickel, cobalt, and manganese to below 1 mg / kg, 1 mg / kg, and 2 mg / kg, respectively, far below the limits set by the "Identification Standard for Hazardous Waste - Leaching Toxicity Identification" (GB 5085.3-2007). The purified product no longer possesses hazardous characteristics and can be managed and circulated as a general industrial product, significantly reducing the environmental compliance costs for enterprises.
[0043] (3) Maintaining the physical and chemical properties of the product. The process design of this invention fully considers the requirements of downstream industries for the color, transparency, and whiteness of sodium sulfate products. Through the synergistic effect of three stages—activated carbon adsorption decolorization, ozone oxidation decolorization, and fractional crystallization—the final product has a whiteness ≥90%, a color ≤5 Hazen, and a 10% aqueous solution transparency ≥95%, which is indistinguishable from the superior grade sodium sulfate mined from mines in terms of appearance and performance, thus meeting the strict requirements of the plastic filler industry for the whiteness and transparency of fillers.
[0044] (4) Full-process resource recovery and comprehensive utilization of by-products. The by-products generated in multiple stages of the process of this invention all have recycling value: the heavy metal precipitation filter residue contains valuable metals such as nickel, cobalt, and manganese, which can be handed over to hydrometallurgical enterprises for recycling; the ammonia water or ammonium sulfate recovered in the stripping and deammoniation process can be used as chemical raw materials or fertilizers; the mother liquor of evaporation and crystallization contains sodium chloride, which can be further crystallized and recovered for use as industrial salt. The entire process realizes full utilization of materials and no waste discharge.
[0045] (5) Low energy consumption and economic feasibility. MVR evaporation crystallization technology utilizes a secondary steam compression cycle, which saves 50-70% energy compared to traditional multi-effect evaporation. Combined with the pretreatment stage operating at a lower temperature and the optimization of the freeze crystallization-assisted salt separation process, the energy consumption per unit product of the overall process is controlled within a reasonable range, giving the purified product a cost advantage in the market compared to mineral sodium sulfate. Attached Figure Description
[0046] The following figures are intended only to illustrate and explain the present invention and do not limit the scope of the invention. Wherein: Figure 1 This is a schematic diagram of the process flow of the present invention. Detailed Implementation
[0047] The present invention will be further described below with reference to the accompanying drawings and embodiments. In the following detailed description, only certain exemplary embodiments of the invention are described by way of illustration. Undoubtedly, those skilled in the art will recognize that various modifications can be made to the described embodiments without departing from the spirit and scope of the invention. Therefore, the drawings and description are illustrative in nature and not intended to limit the scope of the claims.
[0048] Example 1 Using crude anhydrous sodium sulfate, a byproduct of a ternary precursor production enterprise, as raw material, its original specifications are as follows: Na₂SO₄ content 96.5%, Ni content 35 mg / kg, Co content 22 mg / kg, Mn content 58 mg / kg, Ca content 650 mg / kg, Mg content 380 mg / kg, Cl content 96.5%, Ni content 35 mg / kg, Co content 22 mg / kg, Mn content 58 mg / kg, Ca content 650 mg / kg, Mg content 380 mg / kg, Cl content 380 mg / kg, Cl content 35 mg / kg, Ca content 35 mg / kg, Mg ... - Content 2800 mg / kg, Fe content 80 mg / kg, COD 560 mg / kg, ammonia nitrogen 280 mg / kg, moisture 1.8%, whiteness 72%, color 85 Hazen.
[0049] refer to Figure 1 The method for further purification of the above-mentioned crude anhydrous sodium sulfate includes the following steps: S1. Take 1000 kg of the crude sodium sulfate and add deionized water to prepare a solution with a concentration of 240 g / L. Heat to 70°C. Add 30% sodium hydroxide solution to adjust the pH to 11.0, and simultaneously add sodium sulfide (1.10 times the theoretical amount). Stir the reaction for 45 minutes. After the reaction is complete, filter by plate and frame filter press and collect the filtrate. Analyze the filtrate: Ni 3.2 mg / kg, Co 2.1 mg / kg, Mn 4.8 mg / kg, Fe 1.5 mg / kg.
[0050] S2. Cool the filtrate to 50°C, add sodium carbonate (1.20 times the theoretical amount), react for 30 minutes, then add sodium hydroxide to adjust the pH to 12.2, and react for another 20 minutes. After precision filtration, the concentrations are: Ca 38 mg / kg, Mg 22 mg / kg. The filtrate is then passed through an aminophosphonic acid chelating resin column (flow rate 10 BV / h), and the effluent concentration is: Total Ca + Mg 8 mg / kg.
[0051] S3. The filtrate is passed through a coconut shell activated carbon adsorption column (iodine value 1050 mg / g, flow rate 5 BV / h), then oxidized with ozone (dosage 10 mg / L, contact time 15 minutes), and finally filtered through a 0.45 μm precision filter. Detection: COD 15 mg / kg, color 3 Hazen.
[0052] S4. Adjust the pH of the filtrate to 11.5 and introduce it into the stripping ammonia removal tower. The tower temperature is 100°C, and the vapor-liquid ratio is 0.20. The bottom effluent test result shows an ammonia nitrogen level of 6 mg / kg.
[0053] S5. After ammonia removal, the solution is passed through a quaternary ammonium strong base anion exchange resin column (flow rate 10 BV / h), and the Cl⁻ content in the effluent is 65 mg / kg.
[0054] S6. The purified solution is fed into the MVR evaporation crystallization system at an evaporation temperature of 95°C, a compression ratio of 1.5, and a concentration ratio of 3.0. After centrifugation, the wet product is dried in a fluidized bed dryer at 150°C.
[0055] S7. After the dried product is graded by a vibrating screen, the test results are as follows: Na₂SO₄ 99.5%, Fe 0.001%, Ca+Mg 0.01%, Cl₂ - 0.1%, moisture 0.06%, Ni 0.5 mg / kg, Co 0.4 mg / kg, Mn 1.0 mg / kg, whiteness 93%, chroma 3 Hazen, transparency 97%.
[0056] The product appears as white, uniform crystalline particles, with no visible difference in color, transparency, or feel compared to commercially available high-quality mineral sodium sulfate.
[0057] Example 2 Using crude sodium sulfate, a byproduct of a wet recycling plant of waste ternary lithium batteries, as raw material, its original specifications are as follows: Na₂SO₄ content 95.8%, Ni content 42 mg / kg, Co content 28 mg / kg, Mn content 75 mg / kg, Ca content 520 mg / kg, Mg content 290 mg / kg, Cl ... - Content 800 mg / kg, Fe content 65 mg / kg, COD 380 mg / kg, ammonia nitrogen 150 mg / kg, moisture 2.1%, whiteness 68%.
[0058] The same process flow as in Example 1 was adopted, with the following parameter adjustments: In step S1, the pH was adjusted to 11.2, and the sodium sulfide dosage was 1.15 times the theoretical amount; in step S2, the sodium carbonate dosage was 1.15 times the theoretical amount; in step S3, the ozone dosage was 12 mg / L; in step S4, the deammoniation tower temperature was 102°C; in step S5, due to the raw material Cl... -The concentration is relatively low (800 mg / kg), omitting the independent dechlorination step and relying on the salt separation effect of evaporation and crystallization to reduce Cl. - .
[0059] Final purified product test results: Na₂SO₄ 99.5%, Fe 0.001%, Ca+Mg 0.005%, Cl - 0.06%, moisture 0.04%, Ni 0.8 mg / kg, Co 0.7 mg / kg, Mn 1.5 mg / kg, whiteness 92%, color 4 Hazen, transparency 96%.
[0060] Example 3 Sodium sulfate, a byproduct of the evaporation and crystallization of a lithium precipitation mother liquor, was used as raw material. Its original specifications were: Na₂SO₄ content 97.2%, Ni content 8 mg / kg, Co content 5 mg / kg, Mn content 12 mg / kg, Ca content 180 mg / kg, Mg content 95 mg / kg, Cl content... - Content 4200 mg / kg, Fe content 25 mg / kg, COD 220 mg / kg, ammonia nitrogen 420 mg / kg, moisture 1.5%, whiteness 78%.
[0061] The characteristic of this raw material is Cl. - The ammonia nitrogen content is relatively high, while the heavy metal content is relatively low. Process adjustments: In step S1, the pH is adjusted to 10.8, and the sodium sulfide dosage is reduced to 1.05 times the theoretical amount (low heavy metal content); in step S4, the ammonia removal tower temperature is increased to 105°C, and the vapor-liquid ratio is increased to 0.25 (high ammonia nitrogen content); step S5 retains an independent dechlorination process (Cl...). - (High), the flow rate of the anion exchange resin column was reduced to 8 BV / h to increase the contact time.
[0062] Final purified product test results: Na₂SO₄ 99.5%, Fe 0.0009%, Ca+Mg 0.004%, Cl - 0.03%, moisture 0.04%, Ni 0.3 mg / kg, Co 0.2 mg / kg, Mn 0.8 mg / kg, whiteness 94%, color 2 Hazen, transparency 98%.
[0063] The above description is merely an illustrative embodiment of the present invention and is not intended to limit the scope of the invention. Any equivalent changes and modifications made by those skilled in the art without departing from the concept and principles of the present invention should fall within the scope of protection of the present invention.
Claims
1. A method for deep purification of industrial solid waste sodium sulfate, wherein the industrial solid waste sodium sulfate is solid waste generated in the production process of lithium battery ternary cathode material precursors; characterized in that, Includes the following steps: S1, Dissolution and Pretreatment The raw material, crude anhydrous sodium sulfate from industrial solid waste, is dissolved in deionized water to prepare a sodium sulfate solution with a concentration of 200-280 g / L. The solution is heated to 60-80°C, and sodium hydroxide is added to adjust the pH to 10.5-11.5 so that heavy metal ions can form hydroxide precipitates. Sodium sulfide is added as a co-precipitant so that heavy metal ions can form sulfide precipitates. After reacting for 30-60 minutes, solid-liquid separation is performed to remove heavy metal hydroxide and sulfide precipitates. S2, Deep calcium and magnesium removal The filtrate from step S1 is cooled to 40-55°C, sodium carbonate is added to cause calcium ions to precipitate as calcium carbonate, and sodium hydroxide is added to adjust the pH to 12.0-12.5 to cause magnesium ions to precipitate as magnesium hydroxide. After filtering to remove calcium carbonate and magnesium hydroxide precipitates, the filtrate is passed through a chelating cation exchange resin to further remove residual calcium, magnesium and heavy metal ions. S3. Removal of organic matter and decolorization The solution after step S2 is first passed through an activated carbon adsorption column to remove residual organic extractants, chelating agents, and colored substances. Then, ozone is introduced into the solution to oxidize and decompose the residual recalcitrant organic matter and oxidize any ferrous ions that may be present to ferric ions for subsequent removal. The ozone-oxidized solution is then filtered to remove trace amounts of flocculents produced by ozone oxidation. S4, deamination The pH of the solution after step S3 is adjusted to 11.0-12.0, and stripping is performed at 95-105°C to remove ammonia nitrogen. S5, dechlorination If the chloride ion content in the raw material is ≥1000mg / kg, the solution after deammoniation in step S4 will be passed through an anion exchange resin column to remove chloride ions. If the chloride ion content in the raw material is <1000mg / kg, this step can be omitted; S6, MVR evaporation crystallization and drying The solution after deammoniation or dechlorination is fed into an MVR evaporation crystallization system and evaporated and crystallized at 85-105°C. Separate crystallization is achieved by utilizing the difference in solubility between sodium sulfate and sodium chloride. The crystallized slurry is then centrifuged and dried to obtain purified anhydrous sodium sulfate product.
2. The method for deep purification of industrial solid waste sodium sulfate as described in claim 1, characterized in that: In step S1, the amount of sodium sulfide added is 1.05-1.20 times the theoretical stoichiometry.
3. The method for deep purification of industrial solid waste sodium sulfate as described in claim 1, characterized in that: In step S2, the amount of sodium carbonate added is 1.1-1.3 times the theoretical stoichiometry.
4. The method for deep purification of industrial solid waste sodium sulfate as described in claim 1, characterized in that: In step S2, the chelating cation exchange resin is an aminophosphonic acid type resin or an iminodiacetic acid type resin, and the operating flow rate is 5-15 BV / h.
5. The method for deep purification of industrial solid waste sodium sulfate as described in claim 1, characterized in that: In step S3, the activated carbon is coconut shell-based granular activated carbon with an iodine value ≥1000 mg / g and a flow rate controlled at 3-8 BV / h.
6. The method for deep purification of industrial solid waste sodium sulfate as described in claim 1, characterized in that: In step S3, the ozone dosage is 5-15 mg / L, and the contact time is 10-20 minutes.
7. The method for deep purification of industrial solid waste sodium sulfate as described in claim 1, characterized in that: In step S4, the mass ratio of steam to liquid in the stripping and ammonia removal process is 0.15-0.
30.
8. The method for deep purification of industrial solid waste sodium sulfate as described in claim 1, characterized in that: In step S5, the anion exchange resin is a quaternary ammonium type strong basic anion exchange resin, and the operating flow rate is 8-15 BV / h.
9. The method for deep purification of industrial solid waste sodium sulfate as described in claim 1, characterized in that: In step S6, the vapor compression ratio of MVR evaporation crystallization is 1.3-1.8, and the evaporation concentration ratio is 2.5-4.0 times.
10. The method for deep purification of industrial solid waste sodium sulfate as described in any one of claims 1 to 9, characterized in that: In step S1, solid-liquid separation is performed using plate and frame filter press or a precision filter with a filtration accuracy of ≤1μm; in step S2, filtration is performed using a precision filter with a filtration accuracy of ≤1μm.
Citation Information
Patent Citations
Material recovery method of wastewater containing high-concentration ammonia-nitrogen and heavy metal ions and treatment system
CN103466870A
Method for recovering sodium sulfate from desulfurization and denitrification waste water