A method for detecting lead and cadmium in grains and oils using screen-printed electrodes based on MWCNTs / NiO NPs doped carbon paste.

By incorporating MWCNTs and NiO NPs into conductive carbon paste and fabricating electrodes using a one-step screen printing process, the problems of cumbersome electrode fabrication processes and poor reproducibility in existing electrodes are solved. This enables highly sensitive detection of Pb2+ and Cd2+, making it suitable for rapid on-site detection of heavy metals in grains and oils.

CN122651830BActive Publication Date: 2026-11-17NANJING UNIV OF FINANCE & ECONOMICS
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611132409.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-07-29
Publication Date
2026-11-17
Estimated Expiration
2046-07-29

AI Technical Summary

Technical Problem

Existing screen-printed electrodes for electrochemical detection of heavy metals generally suffer from problems such as cumbersome preparation processes, poor electrode reproducibility, easy detachment of modified layers, and low utilization of nanomaterials. At the same time, functional catalytic materials are easily encapsulated and deactivated by resin when doped into carbon paste, making it difficult to achieve one-step printing preparation for efficient detection of lead and cadmium in grains and oils.

Method used

Multi-walled carbon nanotubes (MWCNTs) and nano-nickel oxide (NiO NPs) were doped into conductive carbon paste in the form of pre-dispersions. After homogenization by three-roll milling, a working electrode (MWCNTs/NiO-SPCE) without secondary modification was prepared by one-step screen printing process. Pb2+ and Cd2+ were detected by differential pulse anodic stripping voltammetry (DPASV).

Benefits of technology

High-sensitivity detection of Pb2+ and Cd2+ was achieved, with detection limits of 0.5 μg/L and 0.77 μg/L, respectively. The intra-batch relative standard deviation (RSD) was 2.1%, and the inter-batch RSD was 2.1%. It was successfully applied to the determination of trace Pb2+ and Cd2+ in actual grain and oil samples, overcoming the shortcomings of traditional methods and providing a new path for the large-scale, low-cost production of high-performance heavy metal electrochemical sensors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122651830B_ABST
    Figure CN122651830B_ABST
Patent Text Reader

Abstract

This invention discloses a method for detecting lead and cadmium in grains and oils using a screen-printed electrode based on MWCNTs / NiO NPs-doped carbon paste, belonging to the fields of electrochemical sensors and food safety detection technology. This invention incorporates multi-walled carbon nanotubes and nano-nickel oxide into a conductive carbon paste in the form of a pre-dispersion. The paste is then homogenized using a three-roll mill to obtain a modified conductive carbon paste, and a working electrode requiring no secondary modification is prepared using a one-step screen printing process. The working electrode of this invention can be used to simultaneously detect Pb. 2+ and Cd 2+ The detection limits were 0.5 μg / L and 0.77 μg / L, respectively; and the intra-batch relative standard deviation of the working electrode was 92%, with an inter-batch RSD of 2.1%. Furthermore, the preparation method of the working electrode in this invention is simple, reproducible, and suitable for mass production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for detecting lead and cadmium in grains and oils using a screen-printed electrode based on MWCNTs / NiO NPs doped carbon paste, belonging to the fields of electrochemical sensors and food safety detection technology. Background Technology

[0002] Lead (Pb) and cadmium (Cd) are two of the most concerning heavy metal elements in environmental monitoring due to their high toxicity, recalcitrant nature, and bioaccumulation. While traditional atomic absorption spectrometry (AAS) and inductively coupled plasma mass spectrometry (ICP-MS) are sensitive and accurate, their expensive instruments, complex operation, and cumbersome pretreatment processes make them unsuitable for rapid on-site detection and emergency monitoring.

[0003] Electrochemical stripping voltammetry has become one of the most promising technologies for rapid on-site detection of trace heavy metals in water due to its high sensitivity, good selectivity, portable instrumentation, and low cost. Screen-printed electrodes (SPEs) are compact (typical substrate size approximately 12.5 mm × 30 mm), requiring only 50-100 μL of sample per measurement. Their low cost, allowing for single-use without cleaning, makes them particularly suitable for portable on-site detection devices.

[0004] To improve the detection sensitivity of screen-printed carbon electrodes (SPCEs) for heavy metal ions, researchers typically employ a "post-modification" strategy, which involves drop-coating a functional nanomaterial modification layer onto the surface of the pre-printed bare carbon working electrode. Commonly used functional materials include: multi-walled carbon nanotubes (MWCNTs), which significantly enhance the electron transport rate on the electrode surface due to their high conductivity, large specific surface area, and excellent chemical stability; and nickel oxide (NiO), a p-type semiconductor metal oxide, which has been proven effective against Pb. 2+ The anodic dissolution reaction exhibits good electrocatalytic activity; chitosan (CS) is rich in amino and hydroxyl groups, which can complex heavy metal ions to achieve pre-enrichment, while also having good film-forming properties and nanomaterial dispersion ability.

[0005] However, the "post-modification" strategy has several inherent shortcomings: (1) It requires two steps: first, screen printing bare electrodes and curing them, then drop coating and secondary drying, which takes a long time; (2) Drop coating relies on manual operation, and the droplet size and spreading uniformity are difficult to control precisely, resulting in unsatisfactory reproducibility between electrodes; (3) The modification layer is only physically adsorbed onto the electrode surface and is easily detached during the stirring and enrichment process; (4) There is leakage or wall-mounted loss of the modification solution, resulting in low utilization of nanomaterials.

[0006] The technical approach of pre-doping functional nanomaterials into conductive carbon paste and directly forming modified working electrodes through a one-step screen printing process can theoretically fundamentally solve the above problems. Furthermore, catalytically active materials (such as NiO) may be encapsulated in the resin matrix of the carbon paste and lose their activity.

[0007] Therefore, how to pre-dope functional nanomaterials into conductive carbon paste and directly form a modified working electrode through one-step screen printing for the detection of lead and cadmium in grains and oils is an urgent problem to be solved. Summary of the Invention

[0008] [Technical Issues] Existing screen-printed electrodes for electrochemical detection of heavy metals generally employ post-modification processes, which have drawbacks such as cumbersome preparation procedures, poor electrode reproducibility, easy detachment of the modification layer, and low utilization rate of nanomaterials. In addition, functional catalytic materials are easily encapsulated and deactivated by resin when doped into carbon paste, making it difficult to achieve one-step printing preparation of modified screen-printed carbon electrodes that can efficiently detect lead and cadmium in grains and oils.

[0009] [Technical Solution] To address the aforementioned problems, this invention provides a method for detecting lead and cadmium in grains and oils using a screen-printed electrode based on MWCNTs / NiO NPs-doped carbon paste. Specifically, this invention incorporates multi-walled carbon nanotubes (MWCNTs) and nano-nickel oxide (NiO NPs) into a conductive carbon paste in a pre-dispersion form. The paste is then homogenized using a three-roll mill to obtain a modified conductive carbon paste. A working electrode (MWCNTs / NiO-SPCE) requiring no secondary modification is then fabricated using a one-step screen printing process. The working electrode (MWCNTs / NiO-SPCE) of this invention can be used to simultaneously detect Pb. 2+ and Cd 2+ The detection limits (S / N=3) were 0.5 μg / L and 0.77 μg / L, respectively, which were approximately 2.9 times and 3.2 times lower than those of the undoped bare carbon paste electrode. Furthermore, the intra-batch relative standard deviation (RSD) of the working electrode was 92% (n=7), and the inter-batch RSD was 2.1% (n=5). In addition, the preparation method of the working electrode in this invention is simple, reproducible, and can be mass-produced, and it has been successfully applied to trace Pb in actual grain and oil samples. 2+ and Cd 2+ The determination.

[0010] The first objective of this invention is to provide a method for preparing a screen-printed electrode of MWCNTs / NiO NPs doped carbon paste, comprising the following steps: (1) Add terpineol to MWCNTs powder and mix evenly to obtain a mixture; then, sonicate the mixture at 15-20℃ to obtain pre-dispersion A; (2) Add terpineol to NiO powder and mix evenly to obtain a mixture; then, sonicate the mixture at 15-20℃ to obtain pre-dispersion B; (3) Mix and grind predispersant A and predispersant B to obtain a nanomaterial predispersed composite; (4) Add the pre-dispersed nanomaterial composite to the conductive carbon slurry and stir evenly to obtain a coarse slurry; (5) Grind the coarse slurry until the fineness is ≤15 μm, then degas it to obtain MWCNTs / NiO NPs doped carbon slurry; (6) Print MWCNTs / NiO NPs doped carbon paste on the surface of a bare electrode without a working electrode, and then cure it in a gradient to obtain a screen-printed electrode with MWCNTs / NiO NPs doped carbon paste. The mass ratio of MWCNTs powder, NiO powder, and conductive carbon paste is 2-3:1:100.

[0011] In one embodiment of the present invention, the MWCNTs powder in step (1) has a tube diameter of 20-40 nm and a length of 5-15 μm.

[0012] In one embodiment of the present invention, the mass ratio of MWCNTs powder to terpineol in step (1) is 2-3:3-4.5.

[0013] In one embodiment of the present invention, terpineol is added in two parts in step (1), with the mass ratio of the first and second additions being 2:1.

[0014] In one embodiment of the present invention, the mixing in step (1) can be carried out by stirring with a glass rod or by stirring with a stirrer.

[0015] In one embodiment of the present invention, the ultrasonic treatment in step (1) has a power of 200-300W and a time of 50-70min.

[0016] In one embodiment of the present invention, the particle size of the NiO powder in step (2) is <50 nm.

[0017] In one embodiment of the present invention, the mass ratio of NiO powder to terpineol in step (2) is 1-2:2.

[0018] In one embodiment of the present invention, the mixing in step (2) can be carried out by stirring with a glass rod or by stirring with a stirrer.

[0019] In one embodiment of the present invention, the ultrasonic treatment power in step (2) is 200-300W and the time is 20-40min.

[0020] In one embodiment of the present invention, the grinding time in step (3) is 10-30 min.

[0021] In one embodiment of the present invention, the endpoint of grinding in step (3) is determined as follows: the material is a uniform black paste, a small amount is picked up with a glass rod and applied to white paper, and no obvious color stripes or particle spots are observed under light.

[0022] In one embodiment of the present invention, the nanomaterial pre-dispersed composite is added in three parts in step (4), with the mass ratio of the first, second and third additions being 3:3:2. After each addition, the mixture is stirred for 3-10 minutes.

[0023] In one embodiment of the present invention, after all the nanomaterial pre-dispersed composite is added in step (4), stirring is continued for 10-20 minutes.

[0024] In one embodiment of the present invention, the grinding in step (5) is carried out using a three-roll mill, with the speed ratio of the feed roller, intermediate roller and discharge roller set to 1:2:4.

[0025] In one embodiment of the present invention, the grinding is performed 2-4 times in step (5).

[0026] In one embodiment of the present invention, the grinding endpoint in step (5) is a fineness of ≤15 μm.

[0027] In one embodiment of the present invention, degassing in step (5) is vacuum degassing, specifically by evacuating to -0.08 MPa and holding for 10 min.

[0028] In one embodiment of the present invention, the bare electrode without a working electrode in step (6) is prepared according to conventional processes, except that it does not have a working electrode.

[0029] In one embodiment of the present invention, the thickness of the MWCNTs / NiO NPs doped carbon paste brushed onto the surface of the bare electrode without a working electrode in step (6) is 11-13 mm.

[0030] In one embodiment of the present invention, the gradient curing in step (6) is to cure at 60°C for 10 min, then at 80°C for 15 min, then at 120°C for 30 min, and then naturally cool.

[0031] In one embodiment of the present invention, after the electrodes are prepared in step (6), they are placed one by one into an antistatic self-sealing bag, a small packet of silica gel desiccant is added, and the bag is sealed and stored in a refrigerator at 4°C; the shelf life is 30 days.

[0032] The second objective of this invention is to prepare a screen-printed electrode of MWCNTs / NiO NPs doped carbon paste using the method described herein.

[0033] The third objective of this invention is to provide a method for detecting lead and cadmium in grains and oils using a screen-printed electrode based on MWCNTs / NiO NPs-doped carbon paste, comprising the following steps: The raw materials are pretreated to obtain the solution to be tested; DPASV was measured using a screen-printed electrode made of MWCNTs / NiO NPs-doped carbon paste, and Pb was recorded. 2+ and Cd 2+ The concentration of Pb in the raw material was calculated by substituting the dissolution peak current into the regression equation of the standard curve, subtracting the reagent blank, and then multiplying by the corresponding dilution factor. 2+ and Cd 2+ The content of.

[0034] In one embodiment of the present invention, the raw materials are one or more of wheat flour, rice, and soybean oil.

[0035] In one embodiment of the present invention, Pb is detected. 2+ The standard curve regression equation is Ipa = 53c + 0.25, where Ipa is the peak current of the DPV (μA), and c is the heavy metal Pb. 2+ Concentration (μg / L), R 2 It is 0.968.

[0036] In one embodiment of the present invention, Cd is detected. 2+ The standard curve regression equation is Ipa = 28.8c +0.12, where Ipa is the peak DPV current (μA) and c is the heavy metal Cd. 2+ Concentration (μg / L), R 2 It is 0.997.

[0037] The fourth objective of this invention is the application of the screen-printed electrode of MWCNTs / NiO NPs doped with carbon paste described in this invention in the field of food testing.

[0038] [Beneficial Effects] (1) This invention is the first to successfully incorporate multi-walled carbon nanotubes and nano-nickel oxide into conductive carbon paste in the form of a pre-dispersion, and to prepare a working electrode that does not require secondary modification using a one-step screen printing process.

[0039] (2) The MWCNTs / NiO NPs doped carbon paste used in this invention maximizes the synergistic effect of functional materials while maintaining the printability and conductivity of the carbon paste.

[0040] (3) In this invention, MWCNTs and NiO need to be pre-dispersed into pastes with terpineol as the medium, then combined and ground, and added to carbon slurry in batches. Then, they are homogenized by three-roll milling (roller gap 25, 15, 8 μm, 3 times) with a fineness ≤15 μm.

[0041] (4) The P2-SPCE prepared in this invention is effective against Pb 2+ and Cd 2+ The DPASV dissolution peak current was 2.9 times and 3.2 times that of bare carbon paste SPCE; the detection limits were 0.5 μg / L and 0.77 μg / L, respectively (S / N=3).

[0042] (5) The intra-batch RSD of P2-SPCE prepared by the present invention is 2.1% (n=7) and the inter-batch RSD is 92% (n=5), which is superior to the manual drop-coating modification method.

[0043] (6) The P2-SPCE prepared in this invention was successfully used for the detection of rice, edible oil and wheat flour, with a recovery rate of 94.6%-103.5%, which is consistent with the results of ICP-MS.

[0044] (7) The present invention adopts the MWCNTs / NiO doped conductive carbon paste and one-step screen printing technology route, which effectively overcomes the defects of traditional "post-modification" method such as low preparation efficiency, poor batch consistency and weak bonding of functional materials, and provides a practical new path for the large-scale and low-cost production of high-performance heavy metal electrochemical sensors. Attached Figure Description

[0045] Figure 1 Electrode pairs with different MWCNTs / NiO contents for Pb 2+ and Cd 2+ Comparison chart of DPASV responses.

[0046] Figure 2 The diagram shows a comparison of the DPASV responses of Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3.

[0047] Figure 3 This is a SEM image of the electrode from Example 1.

[0048] Figure 4 This is a SEM image of the electrode in Comparative Example 1.

[0049] Figure 5 The CV curves of the NiO-MWCNTs / SPCE electrode are shown at different scan rates (0.01, 0.02, 0.03, 0.04, 0.05 V / s).

[0050] Figure 6The graph shows the correlation between the peak currents of the oxidation and reduction peaks and the scan rate in the CV curves of the NiO-MWCNTs / SPCE electrode at different scan rates (0.01, 0.02, 0.03, 0.04, 0.05 V / s). Detailed Implementation

[0051] The preferred embodiments of the present invention are described below. It should be understood that the embodiments are for better explanation of the present invention and are not intended to limit the present invention.

[0052] Test method: 1. Film thickness measurement The thickness of the working electrode layer was determined using a profilometer (Dektak XT).

[0053] Measurement parameters: stylus pressure 3 mg, scan length 2 mm, scan speed 0.05 mm / s. Three electrodes were taken for each formulation, and each electrode was scanned once at three different locations (near center, near edge, and near edge), and the average value of 9 scans was taken.

[0054] 2. Sheet resistance measurement The sheet resistance of the cured working electrode layer was measured using a four-probe sheet resistance meter (ST2258C). The four-probe probe was gently pressed vertically into the center of the circular film surface of the working electrode. The reading was recorded after stabilization, and the unit is 65 Ω / mm. 2 Five electrodes were tested for each formulation, and the average value was taken.

[0055] 3. SEM surface morphology observation The microstructure of the working electrode surface after curing carbon pastes with different formulations was observed using a field emission scanning electron microscope (Hitachi SU8010). The electrode sheet was attached to the sample stage with conductive carbon adhesive, with an accelerating voltage of 5 kV, a working distance of 8-10 mm, and magnifications of 5000× and 20000×. The dispersion state of MWCNTs and the distribution of NiO particles in the carbon layer were observed in detail.

[0056] 4. Electrochemical performance characterization All electrochemical tests were performed on an electrochemical workstation using SPCE’s own three-electrode system (working electrode: MWCNTs / NiO doped carbon layer; reference electrode: Ag / AgCl printed layer; counter electrode: carbon layer).

[0057] (1) Cyclic voltammetry (CV) characterization A solution containing 5.0 mmol / L K3[Fe(CN)6] and 0.1 mol / L KCl was used as the probe electrolyte.

[0058] Scan range: -0.2 V to +0.7 V (vs. printed Ag / AgCl reference electrode); Scan rate: 50 mV / s; Sampling interval: 1 mV.

[0059] Record the anode peak current (Ipa), cathode peak current (Ipc), anode peak potential (Epa), and cathode peak potential (Epc), and calculate the peak potential difference ΔEp = Epa - Epc. The smaller ΔEp and the larger Ipa, the better the electrochemical reversibility and electron transport rate of the electrode.

[0060] (2) Electrochemical impedance spectroscopy (EIS) characterization Electrolytes are the same as (1); Frequency range: 0.1 Hz to 100 kHz; AC disturbance amplitude: 5 mV; Bias voltage: Open circuit potential (OCP, approximately +0.22 V).

[0061] The Nyquist plot was fitted with an equivalent circuit using ZView software (Randles equivalent circuit: Rs + (Rct / / CPE) + W) to obtain parameters such as solution resistance (Rs) and charge transfer resistance (Rct). The smaller the Rct value, the faster the charge transfer rate at the electrode / solution interface.

[0062] (3) Calculation of the effective active area of ​​the electrode CV curves were measured at different scan rates (10, 20, 50, 80, 100, 150, 200 mV / s) in solutions containing 5.0 mmol / L K3[Fe(CN)6] and 0.1 mol / L KCl.

[0063] According to the Randles-Sevcik equation (25℃):

[0064] In the formula: Ipa is the anode peak current (A), n=1 ([Fe(CN)6] 3- / 4- (This is a single-electron reaction), D = 7.6 × 10⁻⁶ -6 cm 2 / s([Fe(CN)6] 3- The diffusion coefficient in 0.1 mol / L KCl is C = 5.0 × 10⁻⁶. -6 mol / cm 3 v is the scan rate (V / s). Using Ipa to represent v 1 / 2 Plot the graph and calculate the effective active area Aeff (cm) from the slope. 2 ).

[0065] 5. DPASV Detection Method for Heavy Metals (1) Detection conditions Pb was analyzed using differential pulsed anodic stripping voltammetry (DPASV). 2+ and Cd 2+ Simultaneous detection.

[0066] The specific parameter settings are shown in Table 1 below: Table 1

[0067] The electrolyte solution was a 0.1 mol / L NaAc-HAc buffer solution (pH 5.0).

[0068] The tests were conducted at room temperature (25±2°C).

[0069] (2) Measurement Operation Procedure (a) Sample addition: Accurately pipette 80 μL of the test solution (0.1 mol / L NaAc-HAc buffer solution adjusted to pH 5.0) and drop it onto the three-electrode junction area of ​​the SPCE. Visually confirm that the droplet completely covers the working electrode, reference electrode, and counter electrode.

[0070] (b) Enrichment (electrodeposition): In the workstation software, start the chronoamperometry mode, set the potential to -1.2 V and the time to 120 s. Click "Start" and simultaneously start the magnetic stirring. At this stage, the Pb in the solution... 2+ and Cd 2+ On the surface of the working electrode, it is reduced to elemental metal and enriched in the doped carbon layer:

[0071]

[0072] The high conductivity provided by MWCNTs ensures rapid electron transport; the active sites of NiO promote metal nucleation and deposition.

[0073] (c) Equilibrium: After the enrichment timer finishes, stirring is automatically stopped, and the mixture is allowed to stand for 10 seconds. This stage allows the solution on the electrode surface to return to a static state, eliminating the interference of convection on subsequent dissolution signals.

[0074] (d) DPV anodic dissolution scan: The workstation automatically switches to DPV mode and scans from -1.0 V to -0.3 V according to "(1) Detection Condition". A 50 mV pulse is superimposed on each potential step. The current is sampled before the pulse is applied and before the pulse ends. The curve of the difference (ΔI) versus potential (E) is recorded.

[0075] When the scan potential reaches Cd 0 The oxidation potential (approximately -0.79 V vs. Ag / AgCl) and Pb 0 At an oxidation potential of approximately -0.56 V, the enriched metals are oxidized and dissolved, resulting in sharp characteristic dissolution peaks:

[0076]

[0077] (e) Data reading: After the scan is complete, use the "Peak Analysis" function in the PSTrace software to automatically identify the peak potential and peak height. Record Pb. 2+ (approximately -0.56 V) and Cd 2+ The peak current value Ipa (μA) is approximately -0.79 V.

[0078] (f) Cleaning and disposal: After the assay, the SPCE was placed in blank buffer and washed with stirring at +0.3 V for 60 s to completely dissolve any residual metals. The SPCE is a disposable electrode and should not be reused in principle; the washing step is only performed when repeatability testing (multiple assays with the same electrode) is required. For grain and oil sample testing, a new electrode is used for each sample.

[0079] (3) Establishment of the standard curve Pb was diluted with 0.1 mol / L NaAc-HAc buffer (pH 5.0). 2+ and Cd 2+ Standard stock solution, prepare a series of mixed standard solutions (Pb) 2+ and Cd 2+ (Same concentration), see Table 2 for details: Table 2

[0080] Following the steps in “(2) Determination Procedure”, the DPASV curves of each standard solution were measured sequentially from low to high concentration, with each concentration measured in parallel three times (using a new electrode each time). A linear regression was performed with the peak current Ipa (μA) as the ordinate and the concentration c (μg / L) as the abscissa to obtain the standard curve equation Ipa = k·c + b and the correlation coefficient R.2 .

[0081] (4) Calculation of detection limit Eleven DPASV assays were performed consecutively using a blank solution (S0, 0 μg / L) to obtain 11 Pb samples. 2+ and Cd 2+ Dissolution peak current values ​​(all close to zero, representing baseline noise).

[0082] Calculate the standard deviation σ of the blank peak current.

[0083] Calculate the detection limit using the following formula:

[0084] In the formula: σ is the standard deviation of 11 blank measurements, and k is the slope of the standard curve (sensitivity, μA·L / μg).

[0085] The raw materials used in the embodiments and their purchase sources are shown in Table 3: Table 3

[0086] The method for preparing a bare electrode without a working electrode is as follows: (1) Preparation of special printing screen: An aluminum alloy mesh frame with an outer frame size of 300 mm × 200 mm is selected, and polyester wire mesh is stretched on the surface of the mesh frame; Only a 200-mesh screen was used to prepare the printing stencil for the silver conductor layer and the insulating layer. The screen diameter was 50 μm, the mesh opening was 77 μm, and the tension of the screen was adjusted to 22±2 N / cm.

[0087] Autotype Plus 8000 diazo photosensitive emulsion was coated onto the screen using a grooving method, with two coats on the printing side and one coat on the ink side. After each coating operation, the screen was dried in a 40 ℃ constant temperature oven for 15 min, ultimately controlling the dry film thickness of the photosensitive emulsion to 12 μm. After the emulsion was completely dry, a special film with a suitable bare electrode without a working electrode was attached, and the screen was exposed for 60 s using a UV exposure device with a wavelength of 365 nm and an energy density of 5 mW / cm². The exposed screen was then rinsed and developed with 40 ℃ warm water for 90 s to remove the photosensitive emulsion from unexposed areas, forming a stencil printing pattern. After development, the screen was dried in a 40 ℃ oven for 30 min. Qualified printing screens with clear pattern edges and no mesh blockage were inspected and selected for later use.

[0088] (2) Structured design of electrode patterns: The SPCE used adopts a classic three-electrode coplanar layout, and the design dimensions are as follows: Working electrode (WE): Circular, 3.0 mm in diameter, with an area of ​​approximately 7.07 mm². 2 ; Reference electrode (RE): rectangular, 1.5 mm × 5.0 mm, located to the left of the working electrode, with a spacing of 0.8 mm; Counter electrode (CE): Arc-shaped, surrounding the right side of the working electrode, with an area of ​​approximately 12 mm². 2 Spacing 0.8 mm; Silver wires: Three independent wires connect WE, RE, and CE to three contacts on the bottom of the substrate (each 1.0 mm wide), with a contact spacing of 2.54 mm; Substrate dimensions: 30.0 mm long × 12.5 mm wide.

[0089] (3) Pretreatment of PET substrate: A4-sized PET film with a thickness of 0.188 mm was selected as the electrode carrier substrate. The film was uniformly cut into rectangular pieces of 30.0 mm × 12.5 mm using a cutting device. Using a lint-free cloth soaked in anhydrous ethanol, the printing surface of each PET substrate was wiped one by one to thoroughly remove dust, oil and other impurities from the substrate surface. After cleaning, the substrates were neatly placed in a petri dish and dried in a 60 ℃ constant temperature oven for 10 min. After being removed, they were allowed to cool naturally to room temperature for later use.

[0090] (4) Silver wire screen printing and curing: Install and fix the 200-mesh special screen prepared in step (1) on the screen printing equipment. calibrate the distance between the screen and the substrate using a micrometer, controlling the mesh distance to 2.0 mm. Weigh 3 g of ten strips of 826H conductive silver paste and place them at the starting end of the screen squeegee. Use a back-inking blade at a 15° angle to complete a single dampening operation, ensuring the conductive silver paste evenly fills the screen's perforated mesh openings, without penetrating the mesh.

[0091] Precisely position the pretreated PET substrate in the vacuum adsorption area of ​​the printing table, turn on the vacuum pump to adsorb and fix the substrate, and ensure that the contact end of the substrate faces the operating side. Select a polyurethane squeegee with a hardness of 70 Shore A and an intact, undamaged blade, and make the squeegee form a 65° angle with the screen plane, and complete the squeegee printing in one go at a constant speed of 50±5 mm / s. The squeegee printing pressure is such that the conductive silver paste completely penetrates the mesh, and the printed silver conductor pattern is continuous, uniform, and without broken lines, overflow, or diffusion defects.

[0092] After printing, slowly lift the screen, peel off and remove the substrate, place the substrate horizontally in the oven, and cure at 120 ℃ for 15 min; after curing, allow it to cool naturally to room temperature. (5) Printing and curing of the reference electrode layer: Replace the special reference electrode printing screen and adjust the screen distance of the printing equipment to 2.0 mm; weigh about 1 g of GwentC61003D silver chloride / silver reference electrode special slurry, and stir it for 2 min with a clean glass rod to ensure that the internal components of the slurry are mixed evenly and to eliminate precipitation and agglomeration. Complete the pattern printing by referring to the silver wire printing process in step (4). During the printing process, accurately align the preset area of ​​the substrate to ensure that the placement of the reference electrode meets the design standards. After the printing operation is completed, place the substrate stably in the constant temperature oven, set the curing temperature to 80 ℃ and the holding time to 10 min. After curing, take out the substrate and let it cool naturally to room temperature for later use.

[0093] (6) Printing and curing of the insulating layer: Replace the 200-mesh insulating layer printing screen with a screen spacing of 1.5 mm. Take 2 g of SD-301 UV-curable insulating ink and place it at the screen feed end. Use a polyurethane squeegee to unidirectionally squeegee at a 45° angle and a constant speed of 60 mm / s to ensure the insulating ink completely covers all conductive silver wire areas on the substrate surface. During printing, precise alignment and masking are performed, exposing only the pre-set 6 mm × 10 mm rectangular electrode working surface and three external contact points on the bottom of the substrate. The remaining wire areas are completely covered by the insulating ink. Immediately after each printing pass, UV curing is performed by placing the substrate under a 365 nm UV-LED curing light source, controlling the irradiation distance to 5 cm and the light source power to 50 mW / cm. 2 The surface is continuously irradiated and cured for 40 seconds. After curing, the state of the insulation layer is checked by touch. The surface is considered qualified if it is completely dry, non-sticky, and not sticky to the touch, thus obtaining a bare screen-printed electrode without the working electrode.

[0094] In the examples, the operations without a specific temperature refer to room temperature (25±2℃), and the stirring speed without a specific value are all for the purpose of uniform mixing.

[0095] Example 1 A method for preparing a screen-printed electrode of MWCNTs / NiO NPs doped carbon paste includes the following steps: (1) Accurately weigh 2.00 g of MWCNTs powder and place it in a clean 25 mL stoppered glass bottle; use a micropipette to add 2.0 g of terpineol and stir slowly with a glass rod for 2 min to fully wet the MWCNTs with terpineol; then add the remaining 1.0 g of terpineol and continue stirring for 3 min; after stirring, the MWCNTs should be a black, moist paste with no flying dry powder; Place the glass bottle in a CNC ultrasonic cleaner, maintain the water temperature at 20℃, set the ultrasonic power to 250 W, and the total ultrasonic time to 60 min, using intermittent mode: pause for 5 min every 20 min of ultrasonic cleaning, check and replenish ice during the interval; after ultrasonic cleaning, MWCNTs should be a uniform, glossy, black, viscous paste (similar to "wet mud"), with no dry powder particles or flocculent agglomerates visible to the naked eye; remove the glass bottle, wipe the outer wall dry, and label it as pre-dispersion A; (2) Accurately weigh 1.00 g of nano NiO powder and place it in a 10 mL clean glass bottle with a stopper; add 2.0 g of terpineol (twice the mass of NiO), and stir with a glass rod for 3 min until uniform; then sonicate (power 250 W, water temperature maintained at 20℃) for 30 min (continuous sonication); after sonication, NiO should be a uniform gray-green viscous paste; this is recorded as pre-dispersion B. (3) Transfer all of the pre-dispersion A and pre-dispersion B into an agate mortar with an inner diameter of 120 mm, and grind them in a circular motion for 15 min with a pestle; during the grinding process, use the pestle to scrape the material adhering to the wall of the mortar back to the central area. Grinding endpoint judgment: The material is a uniform black paste. A small amount is picked up with a glass rod and spread on white paper. When observed under light, there are no obvious color streaks or particle spots. The resulting material is denoted as a pre-dispersed nanomaterial composite (total mass 8.0 g). (4) Weigh 100.00 g of ten JF-818 commercial conductive carbon pastes and place them in a 250 mL beaker; stir the carbon paste with a glass rod for 2 min to make it uniform (because the solvent may settle slightly during the storage of the carbon paste). The pre-dispersed nanomaterial composite (8.0 g) obtained in step (3) was added to the carbon slurry in three portions: First time: Add 3.0 g of nanomaterial pre-dispersed composite to the center of the carbon slurry surface, and stir with a glass rod in a figure-eight motion for 5 min to make the pre-dispersed composite be coated and fused by the carbon slurry; Second time: Add 3.0 g and stir for 5 minutes; Third time: Add 2.0 g and stir for 5 minutes; After all the ingredients are added, continue stirring for 15 minutes; at this point, the slurry will be a uniform black color, and you will obtain a coarsely mixed slurry. (5) Transfer the coarse slurry to the feed hopper of the three-roll mill. The speed ratio of the three rollers (feed roller, intermediate roller, and discharge roller) of the three-roll mill is set to 1:2:4, and all are operated at room temperature (25±2℃). Grind sequentially according to the parameters in Table 4: Table 4

[0096] After each grinding pass, scrape the slurry from the discharge roller with a stainless steel spatula to check its uniformity and measure its fineness. After the third grinding pass, use a scraper fineness meter to determine the fineness according to GB / T 1724-2019 "Determination of Grinding Fineness of Paints, Varnishes and Printing Inks": Place approximately 0.5 g of slurry at the deepest end of the groove of the scraper fineness meter, scrape the entire groove at a uniform speed with a scraper, and observe the scale markings of continuous particle scratches in the groove under light within 3 seconds. Acceptable standard: Fineness ≤ 15 μm.

[0097] After testing, the fineness was found to be 11μm.

[0098] The ground slurry was transferred to a clean 100 mL brown glass bottle, placed open in a vacuum desiccator, and evacuated to -0.08 MPa for 10 min to remove air bubbles introduced during the grinding process. After degassing, the bottle was sealed and stored at room temperature (25°C) away from light to obtain MWCNTs / NiO NPs doped carbon slurry. (6) Install a 250-mesh carbon paste working electrode layer screen on the surface of the bare electrode without a working electrode, and adjust the screen distance to 2.0 mm; take 2 g of MWCNTs / NiO NPs doped carbon paste on the screen; first, wet the screen once; using the silver conductor pattern as a positioning reference, make the working electrode layer screen pattern and the end of the silver conductor precisely aligned (error < 0.2 mm), with the squeegee angle at 65° and the speed at 40 mm / s, and squeegee once at a uniform speed; then perform gradient curing, and the curing process is shown in Table 5 below: Table 5

[0099] After curing, visually inspect the working electrode layer: it should be a uniform gray-black matte film, free of cracks, bubbles, and pinholes; thus obtaining a screen-printed electrode with MWCNTs / NiO NPs doped carbon paste. Storage method: Place each item individually into an anti-static self-sealing bag, add a small packet of silica gel desiccant, seal, and store in a refrigerator at 4℃. Shelf life is 30 days.

[0100] Example 2 The amounts of MWCNTs powder, NiO, and terpineol in Example 1 were adjusted as shown in Table 6 below: Table 6

[0101] Everything else remained the same as in Example 1, resulting in the modified electrode.

[0102] The modified electrodes were subjected to performance tests, and the test results are shown in Table 7 below: (1) Physical performance testing: Table 7 Physical properties of carbon pastes with different formulations

[0103] As can be seen from Table 7: Viscosity: The viscosity of the carbon paste increases monotonically with increasing MWCNTs and NiO content. MWCNTs have a high specific surface area (approximately 200 m²). 2 The addition of P5 (6.0% addition) gives it extremely strong liquid absorption capacity, but the flow resistance of the carbon paste increases significantly with high addition levels. The viscosity of P5 (35,400 mPa·s) is close to the upper limit of screen printing (generally, >40,000 mPa·s is difficult to pass through the screen), and in actual printing, P5 has been found to cause screen clogging and incomplete patterns. The viscosity of P2 (3.0% addition) is 22,300 mPa·s, which is about 21% higher than that of P0, but is still within the ideal printing viscosity range for 250 mesh screens.

[0104] Sheet resistance: The sheet resistance of the original carbon paste P0 is 28 Ω / □; the sheet resistance of P2 (3.0% added, MWCNTs:NiO=2:1) ​​is 65 Ω / □, approximately 2.3 times that of P0, still within an acceptable range (target ≤150 Ω / □, to ensure no impact on DPASV electron transport). The sheet resistance of P5 increases sharply to 198 Ω / □, indicating that excessive nanomaterials (especially semiconductor NiO) excessively disrupt the direct contact between carbon particles, severely damaging the conductive pathway.

[0105] Printability: P0-P2 have excellent printability, with clear and sharp patterns; P3 and P4 are still acceptable; P5 shows a tendency to clog the screen (large MWCNTs in the carbon paste partially clog the 250 mesh), making it unsuitable for actual production.

[0106] Overall evaluation: The P2 formulation (total addition 3.0 wt%, MWCNTs:NiO=2:1) ​​achieved the best balance between conductivity, printability and nanomaterial content, and was selected as the optimal formulation for all subsequent experiments.

[0107] (2) Electrochemical performance characterization The results are shown in Table 8: Table 8. Electrodes with different formulations in [Fe(CN)6] 3- / 4- CV and EIS parameters in the probe

[0108] As can be seen from Table 8: The P0 electrode has ΔEp = 385 mV and Rct = 915 Ω, indicating that the electrochemical reversibility of the bare carbon paste electrode is generally poor.

[0109] The ΔEp of the P2 electrode decreased to 252 mV, a reduction of 55.3%; Rct decreased to 428 Ω, only 19.5% of that of P0; and the effective active area Aeff reached 0.128 cm². 2 It is 2.05 times that of P0. The "bridging" conductive network of MWCNTs and the electrocatalytic synergistic effect of NiO significantly improve the electrochemical performance of the electrode.

[0110] P3 (4.0%, MWCNTs:NiO=3:1) is very close to P2 in CV and EIS data (Ipa is slightly higher and Rct is slightly lower), but its overall cost performance is not as good as P2.

[0111] The performance of P4 (MWCNTs:NiO=1:1) is significantly worse than that of P2 and P3, which confirms that when the proportion of NiO is too high, its semiconductor properties actually weaken the overall conductivity.

[0112] Due to severe aggregation of nanomaterials, P5's performance indicators are even worse than P1's.

[0113] In a concentration of 10 μg / L Pb 2+ and 10 μg / L Cd 2+ Electrochemical performance was tested in a mixed standard solution, and the results are as follows: Figure 5 The CV curves of the NiO-MWCNTs / SPCE electrode are shown at different scan rates (0.01, 0.02, 0.03, 0.04, 0.05 V / s). From... Figure 5 It can be seen that the currents of both the oxidation and reduction peaks increase significantly with increasing scan rate, indicating that the electrode exhibits good electrochemical response at high scan rates. This is consistent with the typical characteristics of diffusion-controlled electrode processes.

[0114] Figure 6 The graph shows the correlation between the peak currents of the oxidation and reduction peaks and the scan rate in the CV curves of the NiO-MWCNTs / SPCE electrode at different scan rates (0.01, 0.02, 0.03, 0.04, 0.05 V / s). Figure 6 It can be seen that the peak currents of the oxidation and reduction peaks exhibit a highly linear relationship with the scan rate, and their fitting equations are y = 5.64194 - 7.78071x and y = -2.95394 + 6.97096x (R²). 2 =0.98765 and R 2 =0.99689). This good linear relationship indicates that the peak current is mainly controlled by the diffusion process.

[0115] Based on the Randles-Sevcik equation, the peak current Ip under diffusion-controlled conditions is proportional to the square root of the scan rate v: Ip = k√v; where Ip is the peak current (μA); k is a constant; and v is the scan rate (mV / s). The linear fit in the experimental results is highly consistent with this theoretical model. As the scan rate increases, the diffusion layer thickness decreases, allowing reactants to reach the electrode surface more quickly, leading to a significant increase in peak current. However, at higher scan rates, the positions of the oxidation and reduction peaks show slight shifts. This is generally attributed to the diffusion layer failing to establish sufficiently under high scan rate conditions, resulting in changes in the reactant concentration gradient and thus affecting the kinetic response of the electrochemical process. This shift reflects a mismatch between the diffusion layer thickness and the scan rate, further demonstrating the diffusion-controlled nature of this electrode process.

[0116] Therefore, the NiO-MWCNTs / SPCE electrode exhibits typical diffusion-controlled behavior in cyclic voltammetry. Experimental results validate the applicability of the Randles-Sevcik theoretical model, demonstrating the electrode's potential for high-sensitivity electrochemical detection.

[0117] (3) DPASV detection performance In a concentration of 10 μg / L Pb 2+ and 10 μg / L Cd 2+ In the mixed standard solution, the DPASV response of each electrode formulation was compared, and the results are shown in Table 9. Table 9. Electrode formulations for Pb 2+ and Cd 2+ Comparison of DPASV response (c=10 μg / L each, n=3)

[0118] As can be seen from Table 9: Sensitivity: P2-SPCE to Pb 2+ and Cd 2+ The dissolution peak currents were 53 μA and 28.8 μA, respectively, which are 2.9 times and 3.2 times that of PO-SPCE (bare carbon paste). This improvement is attributed to the synergistic effect of the highly efficient conductive network constructed by MWCNTs and the electrocatalytic active sites provided by NiO.

[0119] Peak potential: Pb of P2-SPCE 2+ and Cd 2+ The dissolution peak potentials shifted positively by approximately 40 mV and 50 mV (relative to P0), respectively, indicating that the electrocatalytic effect of NiO reduced the activation overpotential of the dissolution reaction.

[0120] Two-peak separation: Pb² +Peak (-0.56V) and Cd² + The potential difference at the peak (-0.75V) is 190 mV, with complete baseline separation, enabling accurate quantification of two ions simultaneously in the same scan.

[0121] P2 vs P3: P3's peak current is slightly higher than P2's, but the improvement is limited. Considering that P3 has higher sheet resistance and reduced printability, P2 has a better overall cost performance.

[0122] (4) Standard curve and detection limit P2-SPCE for different concentrations of Pb 2+ and Cd 2+ The DPASV determination results of the mixed standard solution are shown in Table 10.

[0123] Table 10

[0124] (5) Performance comparison with existing literature on doped / modified SPCEs is shown in Table 11: Table 11

[0125] Note: Serial number 1 comes from the literature (Injang U, Noyrod P, Siangproh W, et al. Determination of trace heavy metals in herbs by sequential injection analysis-anodic stripping voltammetry using screen-printed carbon nanotube selectrodes. Analytica Chimica Acta, 2010, 668(1): 54–60.). Number 2 comes from the literature (Ramalingam M, Ponnusamy VK, Sangilimuthu S N. Graphitic carbon nitride nanomaterials-based electrochemical sensing interfaces for monitoring heavy metal ions in aqueous environments. Chemosphere, 2023, 323: 138212.). Number 3 is from the literature (Li Jinxia. Fabrication and application research of graphene-doped carbon printed array electrodes [D]. Ningxia University, 2014.). As can be seen from Table 11, P2-SPCE is significantly better than existing post-drop-coated modified SPCE and single graphene-doped SPCE in terms of detection limit.

[0126] Example 3 The reproducibility and stability tests of P2-SPCE in Example 1 are as follows: (1) Intra-batch reproducibility: Using the same P2-SPCE tablet, for samples containing 10 μg / L Pb 2+ and 10 μg / L Cd 2+ The mixed standard solution was measured seven times consecutively (after each measurement, the solution was washed at +0.3 V for 60 s).

[0127] The test results are as follows: 7 times Pb 2+ The peak current RSD is 2.1%, Cd 2+ The result was 2.5%, indicating excellent repeatability of the electrode.

[0128] (2) Batch-to-batch reproducibility: Using the same batch of P2-doped carbon paste, five SPCEs were printed using the same process, and the content of 10 μg / L Pb was measured. 2+ and 10 μg / L Cd 2+ A mixed standard solution.

[0129] The test results are as follows: Pb between 5 electrodes 2+ The peak current RSD is 3%, Cd 2+ The RSD was 3.5%, which is significantly better than the manual drip coating method (the inter-batch RSD of the drip coating method reported in the literature is usually between 5% and 10%), demonstrating the advantage of the screen printing doping route in terms of batch consistency.

[0130] (3) Long-term stability: P2-SPCE was sealed and stored in a desiccator at 4℃. It was removed on days 1, 7, 15, and 30, and the content of 10 μg / L Pb was determined. 2+ and 10 μg / L Cd 2+ A mixed standard solution.

[0131] The test results are as follows: On day 30, Pb 2+ and Cd 2+ The response currents retained 92% and 95% of their initial values, respectively. MWCNTs and NiO embedded in the carbon paste resin matrix were effectively protected, exhibiting better stability than surface-coated modified layers, which typically decreased to 70%-80% after 30 days.

[0132] Example 4 A method for detecting lead and cadmium in grains and oils using a screen-printed electrode based on MWCNTs / NiO NPs doped carbon paste includes the following steps: (1) Raw material pretreatment: Accurately weigh 1.000 g (accurate to 0.1 mg) of sample (soybean oil) and place it in a 50 mL centrifuge tube. Add 5.0 mL of n-hexane (chromatographic grade) to dissolve the oil. Then add 5.0 mL of 1.0 mol / L HNO3 solution, vortex for 5 min, and then sonicate for 20 min. Centrifuge at 4000 rpm for 10 min, carefully transfer the lower acidic aqueous phase to a 10 mL volumetric flask; add 3.0 mL of 1.0 mol / L HNO3 to the upper oil phase and repeat the extraction once more, combining the two acidic aqueous phases. Adjust the pH to approximately 5.0 with 5.0 mol / L NaOH solution, add 1.0 mL of 1.0 mol / L NaAc-HAc buffer (pH 5.0), and bring the volume to 10 mL with ultrapure water to obtain the test sample; simultaneously prepare a complete reagent blank.

[0133] Weigh 2.90 g (accurate to 0.01 g) of anhydrous sodium acetate, add 2.7 mL of glacial acetic acid, dissolve in 10% nitric acid aqueous solution, and bring the volume to 100 mL to obtain the extract; weigh 0.30 g of pulverized sample (wheat flour or rice ground through an 80-mesh sieve) into a 2 mL stoppered centrifuge tube, add 1.5 mL of the extract, vortex for 3 min, centrifuge at 7000 r / min for 3 min, and take the supernatant as the sample to be tested.

[0134] (2) Perform DPASV determination on the sample to be tested. Each sample solution is measured in parallel 3 times (using a new electrode each time), and record the Pb. 2+ and Cd 2+ The dissolution peak current was used to calculate the concentration by substituting it into the standard curve regression equation in Table 10. After subtracting the reagent blank, the concentration was multiplied by the corresponding dilution factor to obtain the Pb concentration in the raw material. 2+ and Cd 2+ The content of.

[0135] Simultaneously, ICP-MS was used to compare and determine the same digestion / extraction solutions; ICP-MS conditions: RF power 1550 W, carrier gas (Ar) flow rate 1.05 L / min, collision cell mode (He), internal standard elements. 209 Bi (used for Pb) 2+ ) and 115In (for Cd) 2 + ).

[0136] (3) Add Pb to the sample digestion / extraction solution with the measured background value at three concentration levels: low (equivalent to 0.05 mg / kg in the sample), medium (0.20 mg / kg), and high (0.50 mg / kg). 2+ and Cd 2+ Spiking recovery experiments were conducted using mixed standard solutions, with each spiking level measured in triplicate.

[0137] The test results are shown in Table 12 below: Table 12 Pb in grain and oil samples 2+ and Cd 2+ The measurement results (n=3)

[0138] As can be seen from Table 12, the above results are all lower than the limits for Pb in cereals and their products specified in the current national food safety standard "Limits of Contaminants in Food" (GB 2762-2022). 2+ Limit (0.2 mg / kg) and Cd 2+ Limits (0.2 mg / kg for rice, 0.1 mg / kg for wheat flour). Pb in edible oil samples. 2+ and Cd 2+ All were below the method detection limit.

[0139] The results of P2-SPCE determination were not significantly different from those of ICP-MS (paired t-test, p>0.05), and the relative deviations of the two methods were both less than 10%, indicating that the method of this application has good accuracy in the determination of grain and oil matrices.

[0140] Pb 2+ The spiked recoveries ranged from 94.6% to 103.5%, and Cd... 2+ The spiked recoveries ranged from 92.7% to 100.8%, all within the acceptable range of 80%-120% specified in GB / T 27404-2008 "Laboratory Quality Control Standard for Physicochemical Testing of Food", and were concentrated between 92% and 104%, indicating that P2-SPCE effectively targets Pb in complex matrices of grains and oils. 2+ and Cd 2+ The measurement has excellent accuracy.

[0141] Comparing the recovery rates of grain samples (solid digestion) and edible oil samples (liquid-liquid extraction), no significant matrix inhibition or enhancement effects were found.

[0142] Taking rice samples as an example, the single-sample determination time of the method in Example 1 (P2-SPCE / DPASV) is approximately 15 minutes (including approximately 25 minutes of pretreatment), while the ICP-MS method requires approximately 2 hours for pretreatment and determination. The cost of the P2-SPCE instrument (portable electrochemical workstation) is approximately 50,000 yuan, and that of ICP-MS is approximately 1.5 million yuan. Therefore, Example 1 has significant advantages in terms of detection cost, ease of operation, and field applicability, and is expected to serve as a method for detecting Pb in grains and oils. 2+ and Cd 2+ Alternative technologies for rapid screening and on-site monitoring.

[0143] Comparative Example 1 The nano-NiO powder in Example 1 was omitted, and the amount of MWCNTs powder was adjusted to 3g, while other aspects remained the same as in Example 1, to obtain the electrode.

[0144] Comparative Example 2 In Example 1, the nano-NiO powder was changed to iron oxide powder, while other aspects remained the same as in Example 1, to obtain the electrode.

[0145] Comparative Example 3 Steps (1) and (2) of Example 1 are omitted. 2.00 g of MWCNTs powder, 1.00 g of nano NiO powder and 5 g of terpineol are directly mixed and ground according to step (3). The rest is the same as in Example 1 to obtain the electrode.

[0146] The obtained electrodes were subjected to performance testing, and the test results are as follows: Figure 2 This is a comparison chart of the DPASV responses of Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3. From... Figure 2 It can be seen that the electrochemical response of Example 1 is the best.

[0147] Figure 3 This is a SEM image of the electrode from Example 1. Figure 4 This is a SEM image of the electrode in Comparative Example 1. From... Figure 3 and Figure 4 It can be seen that the MWCNTs / NiO NPs-doped carbon paste used in Example 1 exhibits better conductive network continuity. A good interpenetrating structure is formed between conductive materials of different dimensions. This synergistic effect effectively reduces contact resistance, thus its conductivity is superior to the carbon paste of Comparative Example 1.

[0148] Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Anyone skilled in the art can make various modifications and alterations without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be determined by the claims.

Claims

1. A method for detecting lead and cadmium in grain and oil based on MWCNTs / NiO NPs doped carbon paste screen-printed electrode, characterized in that, Includes the following steps: The raw materials are pretreated to obtain the solution to be tested; The MWCNTs / NiO NPs doped carbon paste screen-printed electrode is used for DPASV determination of the test solution, and the Pb 2+ and Cd 2+ dissolution peak current is recorded. The concentration is calculated by substituting the standard curve regression equation, deducting the reagent blank, and multiplying the corresponding dilution multiple to obtain the content of Pb 2+ and Cd 2+ in the raw material; The method for preparing screen-printed electrodes of MWCNTs / NiO NPs doped carbon paste includes the following steps: (1) Add terpineol to MWCNTs powder and mix evenly to obtain a mixture; then, sonicate the mixture at 15-20℃ to obtain pre-dispersion A; wherein the mass ratio of MWCNTs powder to terpineol is 2-3:3-4.5; (2) Add terpineol to NiO powder and mix evenly to obtain a mixture; then, sonicate the mixture at 15-20℃ to obtain pre-dispersion B; wherein the mass ratio of NiO powder to terpineol is 1-2:2; (3) Mix and grind predispersant A and predispersant B to obtain a nanomaterial predispersed composite; (4) Add the pre-dispersed nanomaterial composite to the conductive carbon slurry and stir evenly to obtain a coarse slurry; (5) Grind the coarse slurry until the fineness is ≤15 μm, then degas it to obtain MWCNTs / NiO NPs doped carbon slurry; wherein, the grinding is carried out by a three-roll mill, and the speed ratio of the feed roller, the intermediate roller and the discharge roller is set to 1:2:4; (6) Print MWCNTs / NiO NPs doped carbon paste on the surface of a bare electrode without a working electrode, and then cure it in a gradient to obtain a screen-printed electrode with MWCNTs / NiO NPs doped carbon paste. The mass ratio of MWCNTs powder, NiO powder and conductive carbon paste is 2-3:1:

100.

2. The method according to claim 1, characterized in that, In step (1), terpineol is added in two parts, with a mass ratio of 2:1 between the first and second additions.

3. The method according to claim 1, characterized in that, In step (4), the pre-dispersed nanomaterial composite is added in three parts, with the mass ratio of the first, second and third additions being 3:3:

2. After each addition, the mixture is stirred for 3-10 minutes.

4. The method according to claim 1, characterized in that, In step (1), the ultrasonic treatment power is 200-300W and the time is 50-70min.

5. The method according to claim 1, characterized in that, In step (2), the ultrasonic treatment power is 200-300W and the time is 20-40min.

6. The method according to claim 1, characterized in that, In step (6), the gradient curing process involves curing at 60°C for 10 minutes, then at 80°C for 15 minutes, and at 120°C for 30 minutes, followed by natural cooling.

7. The method according to claim 1, characterized in that, In step (6), the thickness of the MWCNTs / NiO NPs doped carbon paste on the surface of the bare electrode without a working electrode is 11-13 mm.

Citation Information

Patent Citations

  • Method for preparing non-enzyme glucose sensor based on silk-screen printing

    CN104713929A