A nanoparticle-induced sodium ion solid electrolyte, its preparation method and application

By introducing Na2MCl5 nanoparticles into NaTaCl6 and utilizing the electrostatic induction effect of chlorine vacancies on their surface, the amorphization of chloride solid electrolyte was achieved, improving sodium ion conductivity and battery performance, solving the problem of low sodium ion conductivity, and making it suitable for all-solid-state sodium ion batteries.

CN122659285BActive Publication Date: 2026-11-17NINGBO ORIENTAL UNIVERSITY OF TECHNOLOGY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611114656.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-07-27
Publication Date
2026-11-17
Estimated Expiration
2046-07-27

AI Technical Summary

Technical Problem

Existing chloride solid electrolytes have low sodium-ion conductivity, which makes it difficult to meet the application requirements of high-performance all-solid-state sodium-ion batteries.

Method used

A nanoparticle-induced strategy was adopted, in which Na2MCl5 nanoparticles with orthorhombic crystal system Pnma space group were introduced into NaTaCl6. The electrostatic induction effect of chlorine vacancies on their surface was utilized to promote the amorphization of NaTaCl6, form continuous sodium ion migration channels, and improve the sodium ion conductivity of the material.

Benefits of technology

It significantly improves the sodium ion conductivity of chloride solid electrolyte to 8.4 mS·cm-1, reduces interfacial impedance, and enhances the cycle stability, rate performance, and safety performance of the battery, meeting the needs of practical applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122659285B_ABST
    Figure CN122659285B_ABST
Patent Text Reader

Abstract

This invention discloses a nanoparticle-induced sodium ion solid electrolyte, its preparation method, and its application, belonging to the field of solid electrolyte technology. The general formula of the solid electrolyte is xNa₂MCl₅–(1–x)NaTaCl₆, where M is a lanthanide element, and 0 < x ≤ 0.35. The Na₂MCl₅ has an orthorhombic crystal system. Pnma The nanoparticles possess a space-group crystal structure and abundant surface chloride vacancies. The NaTaCl6 host phase exhibits an amorphous structure under the induction of Na2MCl5. This invention enhances the solid-phase migration ability of sodium ions through the electrostatic interaction between Na2MCl5 and NaTaCl6. This solid electrolyte is prepared via mechanochemical synthesis and exhibits high sodium ion conductivity, reaching up to 8.4 mS·cm at room temperature. ‑1 It exhibits excellent mechanical properties and interfacial electrochemical stability. This material can be applied in all-solid-state sodium-ion batteries, effectively improving the battery's cycle performance and rate performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of solid electrolyte technology, specifically relating to a nanoparticle-induced sodium ion solid electrolyte, its preparation method, and its application. Background Technology

[0002] Sodium-ion batteries, as an important alternative to lithium-ion batteries, are particularly suitable for large-scale energy storage and low-cost power systems. Compared to lithium, sodium is hundreds of times more abundant in the Earth's crust, with rich and stable resources and a more cost-effective raw material. Furthermore, sodium's chemical properties are similar to lithium, with its standard electrode potential only about 0.3 V higher, giving sodium-ion batteries continued application potential in terms of theoretical energy density. In recent years, with the rapid growth in demand for renewable energy generation and distributed energy storage, sodium-ion batteries have shown broad application prospects in areas such as grid peak shaving, home energy storage, and low-speed electric vehicles. In particular, the introduction of the solid-state battery concept has driven research on sodium-ion solid electrolytes to become a key focus in this field. The development of sodium-ion solid electrolytes with high ionic conductivity, high electrode interface stability, and excellent chemical stability has become an important issue in improving the overall performance of sodium-ion batteries.

[0003] Inorganic sodium ion solid electrolytes are currently mainly classified into three major systems: oxides, sulfides, and chlorides. Among them, oxide solid electrolytes, such as NASICON-type (Sodium Na Super-Ionic Conductor) or β-Al₂O₃, possess excellent chemical stability and high mechanical strength, but their room temperature ionic conductivity is typically only 10⁻⁶. -4 -10 - 3 S·cm -1 However, they also suffer from high sintering temperatures and high interfacial impedance. Sulfide solid electrolytes (such as Na3PS4 and Na3SbS4) can achieve room temperature conductivity of up to 10. -3 -10 -2 S·cm -1 However, its poor air stability and electrochemical compatibility with high-potential cathodes limit its application. In recent years, chloride solid electrolytes (such as Na3YCl6 and Na2ZrCl6) have emerged, possessing both good chemical stability and mechanical properties, and have become a research hotspot. Compared with traditional sulfide solid electrolytes, chloride systems exhibit significantly reduced sensitivity to moisture and oxygen, while also demonstrating a wider electrochemical window under high-voltage cathode conditions, effectively suppressing interfacial side reactions, thus showing potential advantages in high-energy-density all-solid-state sodium-ion batteries. Furthermore, chloride solid electrolytes typically have lower electronic conductivity, which helps reduce self-discharge and improve battery safety.

[0004] However, due to the large radius of sodium ions (1.02 Å), their migration barrier in solid crystal lattices is typically high, resulting in the overall sodium ion conductivity of existing chloride systems remaining lower than that of similar sulfide solid electrolytes, necessitating further improvements in their ion transport performance. From a crystal structure perspective, traditional chloride electrolytes are mostly highly ordered crystal structures, with limited sodium ion diffusion paths and a lack of continuous, low-barrier migration channels, which to some extent restricts their ion transport performance.

[0005] To address the aforementioned issues, researchers have attempted to optimize the structure and performance of chloride electrolytes through various strategies. For example, they have manipulated lattice parameters and defect concentrations through cation doping (e.g., introducing multivalent metal ions) to increase sodium ion vacancies and lower migration barriers; introduced structural disorder by constructing solid solutions or multi-component systems to improve the continuity of ion diffusion channels; and enhanced the overall ion conductivity of materials through nanostructuring or interface engineering. Furthermore, amorphization strategies have been considered an important approach to improving sodium ion conductivity in recent years. The lack of long-range order in amorphous structures provides a more isotropic ion migration environment, thereby lowering the ion diffusion barrier. Although some studies have achieved rapid sodium ion conduction through amorphization, such as amorphization achieved through long-term high-energy ball milling (NaTaCl6) and amorphization achieved through anion exchange (Na2O2-TaCl5), the overall methods remain relatively limited. The preparation process is complex and lacks controllability, and the resulting materials still exhibit low ion conductivity, making it difficult to meet the practical application requirements of high-performance solid-state batteries.

[0006] Therefore, it is urgent to propose new methods, mechanisms or control strategies at the material design level to achieve the amorphization of sodium-ion solid electrolytes, thereby significantly improving sodium-ion mobility, which is of great significance for promoting the development of high-performance all-solid-state sodium-ion batteries. Summary of the Invention

[0007] The purpose of this invention is to overcome the shortcomings of the prior art and provide a nanoparticle-induced sodium ion solid electrolyte, its preparation method and application, so as to solve the technical problem of low sodium ion conductivity in the prior art chloride solid electrolyte system.

[0008] To achieve the above objectives, the present invention employs the following technical solution: The first aspect of this invention discloses a nanoparticle-induced sodium ion solid electrolyte, wherein the general formula of the sodium ion solid electrolyte is: x Na2MCl5–(1- x NaTaCl6, where M is a lanthanide element, 0 < x ≤0.35; the Na2MCl5 has an orthorhombic crystal system. PnmaNanoparticles with a space group crystal structure, and the surface of Na2MCl5 nanoparticles has chlorine vacancies; NaTaCl6 exhibits an amorphous structure under the electrostatic induction of the Na2MCl5 nanoparticles.

[0009] Preferably, M is any one of Eu, Gd, Tb, Dy, or Ho.

[0010] Preferably, the Na2MCl5 nanoparticles are uniformly dispersed and embedded in the NaTaCl6.

[0011] Preferably, the size of the Na2MCl5 nanoparticles is ≤100nm.

[0012] Preferably, the sodium ion solid electrolyte, after being cold-pressed at room temperature, has a sodium ion conductivity of 0.5 mS·cm. -1 -10 mS·cm -1 .

[0013] A second aspect of this invention discloses a method for preparing the above-mentioned nanoparticle-induced sodium ion solid electrolyte, comprising the following steps: S1, sodium chloride, lanthanide chloride and tantalum chloride are mixed according to the stoichiometric ratio of the general formula of sodium ion solid electrolyte to obtain a mixture; S2, the mixture is subjected to mechanochemical synthesis under an inert gas atmosphere or vacuum conditions to obtain the solid electrolyte.

[0014] Preferably, in S1, the lanthanide chloride is selected from any one of europium chloride, gadolinium chloride, terbium chloride, dysprosium chloride, or holmium chloride.

[0015] Preferably, in S2, the mechanochemical synthesis is performed by ball milling, with a ball milling speed of 500 rpm to 800 rpm and a ball milling time of 0.5 h to 60 h.

[0016] Preferably, the ball milling speed is 600 rpm and the ball milling time is 27 h.

[0017] The third aspect of the present invention discloses the application of the nanoparticle-induced sodium-ion solid electrolyte described in any of the above claims in an all-solid-state sodium-ion battery, wherein the sodium-ion solid electrolyte serves as the positive electrode electrolyte in the all-solid-state sodium-ion battery.

[0018] Compared with the prior art, the present invention has the following beneficial effects: This invention discloses an amorphous sodium ion solid electrolyte induced by lanthanide nanoparticles, wherein the solid electrolyte is selected from those with orthorhombic crystal systems. Pnma(P represents the primitive lattice, n represents the n-type glide plane along the a-axis, m represents the mirror plane along the b-axis, and a represents the a-type glide plane along the c-axis) The lanthanide sodium chloride Na₂MCl₅ of space group, where M is a lanthanide element, has... Pnma Lanthanide sodium chlorides in space group NaTaCl6 are nanoparticles rich in chloride vacancies on their surface. By introducing a small amount of these lanthanide chloride nanoparticles into NaTaCl6, the electrostatic interaction between the chloride vacancies on their surface and the host crystalline NaTaCl6 phase can effectively induce local structural distortion, weaken the interaction between charge carriers and the anion framework, and thus promote the amorphous transformation of the host NaTaCl6 phase. This significantly improves the sodium ion conductivity of the material, enabling it to achieve a sodium ion conductivity of up to 8.4 mS·cm in chloride solid electrolyte systems. -1 This material effectively reduces interfacial impedance. Simultaneously, it exhibits excellent interfacial electrochemical stability, effectively suppressing interfacial side reactions, thereby significantly improving the battery's cycle stability, rate performance, and safety performance. This material meets practical application requirements, possesses significant application value and promising industrialization prospects, and is expected to further expand the application of all-solid-state sodium-ion batteries in high-energy-density energy storage.

[0019] This invention also discloses a method for preparing nanoparticle-induced sodium ion solid electrolyte. Through a high-energy mechanochemical synthesis process, lanthanide nanoparticles rich in surface chloride vacancies can be spontaneously formed. The obtained nanoparticle-induced sodium ion solid electrolyte has excellent mechanical properties. Under low molding pressure conditions, a dense structure can be obtained by cold pressing of powder while maintaining high sodium ion conductivity. Attached Figure Description

[0020] Figure 1 The X-ray diffraction phase analysis diagrams of the sodium ion solid electrolytes 0.2Na2GdCl5–0.8NaTaCl6 and 0.2Na2TbCl5–0.8NaTaCl6 obtained in Examples 1 and 2 of this invention are shown. Figure 2 This is a scanning electron microscope image of the 0.2Na2GdCl5–0.8NaTaCl6 sodium ion solid electrolyte obtained in Example 1 of this invention; Figure 3 This is the AC impedance diagram of the 0.2Na2GdCl5–0.8NaTaCl6 sodium ion solid electrolyte obtained in Example 1 of this invention; Figure 4 This is the AC impedance diagram of the 0.2Na2TbCl5–0.8NaTaCl6 sodium ion solid electrolyte obtained in Example 2 of the present invention; Figure 5This is the AC impedance diagram of the 0.2Na2DyCl5–0.8NaTaCl6 sodium ion solid electrolyte obtained in Example 3 of the present invention; Figure 6 This is the AC impedance diagram of the 0.2Na2HoCl5–0.8NaTaCl6 sodium ion solid electrolyte obtained in Example 4 of this invention; Figure 7 This is the AC impedance diagram of the 0.2Na2EuCl5–0.8NaTaCl6 sodium ion solid electrolyte obtained in Example 5 of the present invention; Figure 8 This is the AC impedance diagram of the 0.15Na2GdCl5–0.85NaTaCl6 sodium ion solid electrolyte obtained in Example 6 of the present invention; Figure 9 This is the AC impedance diagram of the 0.25Na2GdCl5–0.75NaTaCl6 sodium ion solid electrolyte obtained in Example 7 of the present invention; Figure 10 This is the AC impedance diagram of the 0.35Na2GdCl5–0.65NaTaCl6 sodium ion solid electrolyte obtained in Example 8 of the present invention; Figure 11 This is the AC impedance diagram of the 0.2Na2CeCl5–0.8NaTaCl6 sodium ion solid electrolyte obtained in Comparative Example 1 of this invention; Figure 12 This is the AC impedance diagram of the 0.2Na2LuCl5–0.8NaTaCl6 sodium ion solid electrolyte obtained in Comparative Example 2 of this invention; Figure 13 This is a graph showing the long-cycle performance of the all-solid-state sodium-ion battery obtained in Application Example 1 of this invention; Figure 14 This is a rate performance diagram of the all-solid-state sodium-ion battery obtained in Application Example 1 of the present invention. Detailed Implementation

[0021] The present invention will now be described in further detail with reference to the accompanying drawings: To enable those skilled in the art to understand the features and effects of the present invention, the terms and expressions mentioned in the specification are explained and defined in general below. Unless otherwise specified, all technical and scientific terms used herein have the ordinary meaning understood by those skilled in the art regarding the present invention, and in case of conflict, the definitions in this specification shall prevail.

[0022] In this article, unless otherwise specified, “contains,” “includes,” “containing,” “has,” or similar terms cover the meanings of “composed of” and “mainly composed of,” for example, “A contains a” covers the meanings of “A contains a and others” and “A contains only a.”

[0023] The present invention will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be understood that after reading the teachings of this invention, those skilled in the art can make various alterations or modifications to the invention.

[0024] The following examples use instruments and equipment conventional in the art. Experimental methods in the following examples, unless otherwise specified, are generally performed under conventional conditions or as recommended by the manufacturer. All raw materials used in the following examples are conventional commercially available products with specifications conventional in the art. In this specification and the following examples, unless otherwise specified, "%" refers to weight percentage, "parts" refers to parts by weight, and "ratio" refers to weight proportion.

[0025] In sodium-ion solid electrolyte systems, sulfide solid electrolytes are widely considered a core candidate system for sodium-ion all-solid-state batteries due to their excellent ion conductivity. However, sulfide solid electrolytes have significant inherent drawbacks: their chemical stability is poor, and they readily react with moisture and oxygen in air, leading to deliquescence failure and the potential release of toxic and harmful gases such as hydrogen sulfide, severely limiting their practical applications. In contrast, chloride solid electrolytes share some similarities with sulfide systems in terms of crystal structure and ion conduction mechanism, while exhibiting superior overall performance in terms of air stability and electrochemical stability, thus attracting increasing attention. However, chloride solid electrolytes still face a key performance bottleneck: their intrinsic sodium-ion conductivity is relatively low, typically around 10 at room temperature. -6 -10 - 4 S·cm -1 Even with optimization through component control and other means, the conductivity of chloride solid electrolytes still falls short of the levels of sulfide systems. These issues directly result in high ohmic impedance in the battery system, limited rate performance, and charge / discharge efficiency that fails to meet practical application requirements. This, to some extent, restricts the application, promotion, and industrialization of chloride solid electrolytes in sodium-ion all-solid-state batteries.

[0026] Based on this, the first aspect of the present invention discloses a nanoparticle-induced sodium ion solid electrolyte, wherein the general formula of the sodium ion solid electrolyte is: x Na2MCl5–(1- x NaTaCl6, where M is a lanthanide element, 0 < x ≤0.35; the Na2MCl5 has an orthorhombic crystal system. PnmaThe nanoparticles have a space group crystal structure, and the surface of the Na2MCl5 nanoparticles has chlorine vacancies; NaTaCl6 exhibits an amorphous structure under the electrostatic induction of the Na2MCl5 nanoparticles.

[0027] In this invention, Na₂MCl₅ nanoparticles with abundant surface chlorine vacancies are introduced as an induction source. The strong localized electrostatic field generated by their surface charge directly acts on the adjacent NaTaCl₆ lattice, weakening the Na₂MCl₅ lattice. + With Cl - Coulomb interactions between the framework elements induce a transformation of NaTaCl6 from a long-range ordered crystal to a short-range ordered amorphous structure. This amorphization eliminates grain boundary resistance and anisotropic diffusion barriers found in traditional crystalline materials, constructing continuous sodium ion migration channels and significantly improving the overall ionic conductivity of the material. Simultaneously, 0 < 0 < 0. x A content range of ≤0.35% ensures sufficient induction strength while avoiding disruption of the amorphous network's coherence due to excessive crystalline phase. This electrostatic induction significantly enhances the sodium-ion conductivity of the material, enabling the sodium-ion conductivity of this chloride solid electrolyte to reach a maximum of 8.4 mS·cm. -1 Among them, amorphous structure refers to a material whose internal atomic or molecular arrangement lacks three-dimensional long-range order, but may have short-range ordered structure.

[0028] In some embodiments, 0.15 ≤ x ≤0.35.

[0029] In some embodiments, M is one of the lanthanide elements europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), and holmium (Ho); by limiting M to five specific lanthanide elements, it is ensured that an orthorhombic crystal system can be formed. Pnma Nanoparticles with a space group crystal structure.

[0030] In some embodiments, the morphology of the resulting amorphous sodium ion solid electrolyte material is not limited and may be granular, sheet-like, or other forms. Regardless of the form, the Na2MCl5 nanoparticles are uniformly dispersed and embedded in the NaTaCl6.

[0031] Furthermore, the size of the Na2MCl5 nanoparticles is ≤100 nm. By controlling the size of the Na2MCl5 nanoparticles within the range of ≤100 nm, the specific surface area of ​​the material is significantly increased, thereby providing a higher density of surface chloride vacancies per unit mass.

[0032] In a specific example x Na2MCl5–(1- xNaTaCl6 is 0.2Na2MCl5–0.8NaTaCl6. NaTaCl6 is granular with a particle size ranging from 200µm to 2mm. Nanoscale Na2MCl5 nanoparticles can be uniformly attached to the outer surface of NaTaCl6 and embedded therein.

[0033] In some embodiments, the sodium ion conductivity of the powder material after room temperature cold pressing is 0.5 mS·cm. -1 -10 mS·cm -1 Furthermore, it is 0.54 mS·cm -1 –8.4 mS·cm -1 This conductivity range covers the measured data of all embodiments of the present invention, proving that the technical solution can still achieve high ion conduction performance that meets the low ohmic impedance requirements of all-solid-state batteries under simple processing conditions that do not require high-temperature sintering.

[0034] A second aspect of this invention discloses a method for preparing the aforementioned nanoparticle-induced sodium-ion solid electrolyte. This method employs a high-energy mechanochemical synthesis approach, reacting precursors sodium chloride (NaCl), lanthanide chloride (MCl3), and tantalum chloride (TaCl5) according to the stoichiometric ratio of the general formula. The specific preparation method includes the following steps: S1, Sodium chloride, lanthanide chloride and tantalum chloride are mixed according to the stoichiometric ratio of the general formula to obtain a mixture; S2, the mixture is subjected to mechanochemical synthesis under an inert gas atmosphere or vacuum conditions to obtain the solid electrolyte.

[0035] In the above process, mechanochemical synthesis is carried out under an inert gas or vacuum environment. The intense collision and shear forces generated by high-energy ball milling simultaneously drive the solid-phase reaction to generate Na2MCl5 nanoparticles and induce the formation of chlorine vacancies on their surface in situ. At the same time, the high-energy input directly breaks the long-range order of NaTaCl6 and transforms it into an amorphous structure under the guidance of the electrostatic field of Na2MCl5 nanoparticles. This one-step process avoids the decomposition or impurity introduction caused by traditional high-temperature heat treatment, and realizes the synergistic control of the generated nanoparticles and the amorphization of the main body. The process is simple and the product has high purity.

[0036] In some embodiments, in S1, the lanthanide chloride (MCl3) is selected from europium chloride (EuCl3), gadolinium chloride (GdCl3), terbium chloride (TbCl3), dysprosium chloride (DyCl3), and holmium chloride (HoCl3). By specifying the precursor lanthanide chloride, it is ensured that it can be completely converted into the corresponding lanthanide chloride during the mechanochemical synthesis reaction. PnmaThe Na2MCl5 phase of the space group, and these precursors have moderate reactivity and thermodynamic stability.

[0037] In some embodiments, the mechanochemical synthesis method is ball milling, wherein the ball milling speed is 500–800 rpm and the ball milling time is 0.5 h–60 h. By controlling the ball milling speed and time within this range, sufficient kinetic energy input is provided to drive the solid-state reaction and amorphous transformation, while avoiding local overheating due to excessive speed or grain coarsening due to excessive time. This broad parameter window takes into account the adaptability to different equipment conditions and raw material batches, ensuring that products with ideal nanostructures and amorphous characteristics can be obtained under different cumulative energy inputs.

[0038] In a specific example, the preparation process involves placing a mixture of sodium chloride (NaCl), gadolinium chloride (GdCl3), and tantalum chloride (TaCl5) in a ball mill jar at a specific molar ratio. Using a planetary ball mill or similar apparatus, the raw material powders collide and undergo a mechanochemical reaction within the jar. The milling speed is 600 rpm, and the reaction time is 27 hours, yielding the target product. The raw material powders can be stored in a vacuum or under inert gas protection, such as nitrogen, argon, or helium. This example produces a sodium-ion solid electrolyte with optimal size distribution and surface chloride vacancy density induced by nanoparticles, while achieving an optimal balance in the amorphization of NaTaCl6, thus producing a solid electrolyte material with the highest ionic conductivity.

[0039] A third aspect of the present invention discloses the application of the above-mentioned nanoparticle-induced sodium-ion solid electrolyte, which can be used in all-solid-state sodium-ion batteries. The all-solid-state sodium-ion battery includes a positive electrode, a negative electrode, and a solid electrolyte layer disposed between the positive and negative electrodes.

[0040] The positive electrode comprises positive electrode active material particles, carbon black particles and positive electrode electrolyte in a mass ratio of 4:2:4. The positive electrode electrolyte is the above-mentioned nanoparticle-induced sodium ion solid electrolyte particles. For example, the positive electrode active material particles are Na3V2(PO4)3.

[0041] The negative electrode is the active material, such as metallic materials or carbon materials. Among them, metallic materials can be elemental metals or alloys.

[0042] The solid electrolyte layer is divided into a positive electrode side solid electrolyte layer and a negative electrode side solid electrolyte layer. The positive electrode side solid electrolyte layer is the aforementioned nanoparticle-induced sodium ion solid electrolyte, and the negative electrode side solid electrolyte layer is a sulfide solid electrolyte, such as Na3PS4, Na3SbS4, etc.

[0043] In application, this solid electrolyte is used in the positive electrode of an all-solid-state sodium-ion battery. It utilizes its excellent ionic conductivity and electronic insulation to serve as the ionic conductive framework for the positive electrode active material. Its amorphous structure facilitates the insertion and extraction of the positive electrode active material and interfacial ion exchange, effectively reducing the interfacial impedance on the positive electrode side, thereby significantly improving the cycle stability and rate performance of the battery.

[0044] Preferably, the positive electrode active material is Na3V2(PO4)3; Preferably, the negative electrode active material is Na. 15 Sn4 alloy; Preferably, the electrolyte layer on the negative electrode side is a Na3PS4 sulfide solid electrolyte; Preferably, the electrolyte layer on the positive electrode side is a 0.2Na2GdCl5–0.8NaTaCl6 chloride electrolyte.

[0045] The following description, in conjunction with specific embodiments, provides further details.

[0046] Example 1 This embodiment provides a nanoparticle-induced sodium-ion solid electrolyte for all-solid-state sodium-ion batteries, with a composition of 0.2Na₂GdCl₅–0.8NaTaCl₆. The specific preparation method is as follows: Commercially available sodium chloride (NaCl), gadolinium chloride (GdCl3), and tantalum chloride (TaCl5) were mixed uniformly in an argon-protected glove box at a stoichiometric ratio of 6:1:4. (The last sentence appears to be incomplete and possibly refers to a different topic.) x Na2MCl5–(1- x In the case of NaTaCl6 where M=Gd and x=0.2, 1g of the mixed powder was placed in a 100mL zirconium dioxide ball mill jar, and 60g of grinding beads were added accordingly. After sealing the jar, it was ball milled at 600 rpm for 27 h. Subsequently, the jar was transferred to a glove box, and the product inside was scraped off to obtain 0.2Na2GdCl5–0.8NaTaCl6 sodium ion solid electrolyte.

[0047] X-ray diffraction phase analysis was performed on the obtained 0.2Na₂GdCl₅–0.8NaTaCl₆ sodium ion solid electrolyte material, and the results are as follows: Figure 1 As shown. Analysis results indicate that the obtained solid electrolyte material contains only diffraction peaks of Na₂GdCl₅ lanthanide chloride nanoparticles, corresponding to an orthorhombic crystal system. Pnma The space group, while the NaTaCl6 main phase maintains an amorphous state.

[0048] Scanning electron microscopy analysis was performed on the obtained 0.2Na₂GdCl₅–0.8NaTaCl₆ sodium ion solid electrolyte, and the results are as follows: Figure 2 As shown in the figure. The analysis results show that the solid electrolyte exhibits obvious composite structure characteristics: the Na2GdCl5 lanthanide chloride nanoparticles are uniform, with a size of about 50 nm, and are dispersed and embedded in the NaTaCl6 amorphous matrix, forming a composite morphology of nanoparticles and amorphous matrix.

[0049] Electrochemical impedance spectroscopy was performed on the obtained 0.2Na₂GdCl₅–0.8NaTaCl₆ sodium ion solid electrolyte material, and the results are as follows: Figure 3 And as shown in Table 1. The analytical results show that the cold-pressed ionic conductivity of its powder is 8.4 mS·cm. -1 .

[0050] Example 2 This embodiment provides a nanoparticle-induced sodium-ion solid electrolyte for all-solid-state sodium-ion batteries, the composition of which is 0.2Na2TbCl5–0.8NaTaCl6.

[0051] Except for changing the raw materials to sodium chloride (NaCl), terbium chloride (TbCl3), and tantalum chloride (TaCl5), the other procedures are the same as in Example 1, corresponding to... x Na2MCl5–(1- x In the case of NaTaCl6 with M=Tb and x=0.2, the resulting 0.2Na₂TbCl₅–0.8NaTaCl₆ sodium ion solid electrolyte still exhibits an orthorhombic crystal system, where the Na₂TbCl₅ lanthanide chloride nanoparticles remain. Pnma The structure of space groups ( Figure 1 Similar to Example 1, the cold-pressed powder ionic conductivity is 4.9 mS·cm, as shown in Table 1. -1 Electrochemical impedance spectroscopy, such as Figure 4 As shown.

[0052] Example 3 This embodiment provides a nanoparticle-induced sodium-ion solid electrolyte for all-solid-state sodium-ion batteries, the composition of which is 0.2Na2DyCl5–0.8NaTaCl6.

[0053] Except for changing the raw materials to sodium chloride (NaCl), dysprosium chloride (DyCl3), and tantalum chloride (TaCl5), the other procedures are the same as in Example 1, corresponding to... x Na2MCl5–(1- x The case of NaTaCl6 with M=Dy and x=0.2. The cold-pressed ionic conductivity of the obtained 0.2Na2DyCl5–0.8NaTaCl6 sodium ion solid electrolyte powder is shown in Table 1, which is 1.0 mS·cm. -1 Electrochemical impedance spectroscopy, such as Figure 5 As shown.

[0054] Example 4 This embodiment provides a nanoparticle-induced sodium-ion solid electrolyte for all-solid-state sodium-ion batteries, the composition of which is 0.2Na2HoCl5–0.8NaTaCl6.

[0055] Except for changing the raw materials to sodium chloride (NaCl), holmium chloride (HoCl3), and tantalum chloride (TaCl5), the other procedures are the same as in Example 1, corresponding to... x Na2MCl5–(1- x The case of NaTaCl6 with M=Ho and x=0.2. The cold-pressed ionic conductivity of the obtained 0.2Na2HoCl5–0.8NaTaCl6 sodium ion solid electrolyte powder is shown in Table 1, which is 1.2 mS·cm. -1 Electrochemical impedance spectroscopy, such as Figure 6 As shown.

[0056] Example 5 This embodiment provides a nanoparticle-induced sodium-ion solid electrolyte for all-solid-state sodium-ion batteries, the composition of which is 0.2Na2EuCl5–0.8NaTaCl6.

[0057] Except for changing the raw materials to sodium chloride (NaCl), europium chloride (EuCl3), and tantalum chloride (TaCl5), the other procedures are the same as in Example 1, corresponding to... x Na2MCl5–(1- x The case of NaTaCl6 with M=Eu and x=0.2. The cold-pressed ionic conductivity of the obtained 0.2Na2EuCl5–0.8NaTaCl6 sodium ion solid electrolyte powder is shown in Table 1, which is 0.54 mS·cm. -1 Electrochemical impedance spectroscopy, such as Figure 7 As shown.

[0058] Example 6 This embodiment provides a nanoparticle-induced sodium-ion solid electrolyte for all-solid-state sodium-ion batteries, the composition of which is 0.15Na2GdCl5–0.85NaTaCl6.

[0059] Except for changing the ball milling time to 20 hours and the stoichiometric ratio of sodium chloride (NaCl), gadolinium chloride (GdCl3), and tantalum chloride (TaCl5) to 23:3:17, the other procedures are the same as in Example 1, corresponding to... x Na2MCl5–(1- xThe case of NaTaCl6 with M=Gd and x=0.15 is shown in Table 1. The cold-pressed ionic conductivity of the obtained 0.15Na2GdCl5–0.85NaTaCl6 sodium ion solid electrolyte powder is 2.2 mS·cm. -1 Electrochemical impedance spectroscopy, such as Figure 8 As shown.

[0060] Example 7 This embodiment provides a nanoparticle-induced sodium-ion solid electrolyte for all-solid-state sodium-ion batteries, the composition of which is 0.25Na2GdCl5–0.75NaTaCl6.

[0061] Except for changing the ball milling time to 20 hours and the stoichiometric ratio of sodium chloride (NaCl), gadolinium chloride (GdCl3), and tantalum chloride (TaCl5) to 5:1:3, the other procedures are the same as in Example 1, corresponding to... x Na2MCl5–(1- x The case of NaTaCl6 with M=Gd and x=0.25 is shown in Table 1. The cold-pressed ionic conductivity of the obtained 0.25Na2GdCl5–0.75NaTaCl6 sodium ion solid electrolyte powder is 2.4 mS·cm. -1 Electrochemical impedance spectroscopy, such as Figure 9 As shown.

[0062] Example 8 This embodiment provides a nanoparticle-induced sodium-ion solid electrolyte for all-solid-state sodium-ion batteries, the composition of which is 0.35Na2GdCl5–0.65NaTaCl6.

[0063] Except for changing the ball milling time to 20 hours and the stoichiometric ratio of sodium chloride (NaCl), gadolinium chloride (GdCl3), and tantalum chloride (TaCl5) to 27:7:13, the other procedures are the same as in Example 1, corresponding to... x Na2MCl5–(1- x The case of NaTaCl6 with M=Gd and x=0.35 is shown in Table 1. The cold-pressed ionic conductivity of the obtained 0.35Na2GdCl5–0.65NaTaCl6 sodium ion solid electrolyte powder is 0.9 mS·cm. -1 Electrochemical impedance spectroscopy, such as Figure 10 As shown.

[0064] Example 9 In this embodiment, the ball milling speed is 500 rpm, the ball milling time is 60 h, and the remaining procedures are the same as in Embodiment 1.

[0065] Example 10 In this embodiment, the ball milling speed is 800 rpm, the ball milling time is 0.5 h, and the remaining procedure steps are the same as in Embodiment 1.

[0066] Comparative Example 1 Using the same procedures as in Example 1, the raw materials were changed to sodium chloride (NaCl), cerium chloride (CeCl3), and tantalum chloride (TaCl5) to obtain a 0.2Na2CeCl5–0.8NaTaCl6 sodium ion solid electrolyte. The molar mass ratio of NaCl, CeCl3, and TaCl5 was maintained at 6:1:4. Comparative Example 1 and the electrochemical impedance spectroscopy method were the same as in Examples 1-8. The cold-pressed ionic conductivity of the powder, as shown in Table 1, was 0.07 mS·cm. -1 Electrochemical impedance spectroscopy, such as Figure 11 As shown.

[0067] Comparative Example 2 Using the same procedures as in Example 1, the raw materials were changed to sodium chloride (NaCl), lutetium chloride (LuCl3), and tantalum chloride (TaCl5) to obtain a 0.2Na2LuCl5–0.8NaTaCl6 sodium ion solid electrolyte. The molar ratio of NaCl, LuCl3, and TaCl5 was maintained at 6:1:4. Comparative Example 2 and the electrochemical impedance spectroscopy test methods were the same as in Examples 1-8. The cold-pressed ionic conductivity of the powder, as shown in Table 1, was 0.16 mS·cm. -1 Electrochemical impedance spectroscopy, such as Figure 12 As shown.

[0068] Application Example 1 The sodium-ion solid electrolyte induced by the 0.2Na2GdCl5–0.8NaTaCl6 nanoparticles obtained in Example 1 was assembled into an all-solid-state sodium-ion battery using a mold assembly method in a glove box under argon atmosphere. The positive electrode was prepared by uniformly mixing Na3V2(PO4)3, carbon black, and 0.2Na2GdCl5–0.8NaTaCl6 in a mass fraction of 4:2:4; the negative electrode was Na... 15 Sn4 alloy; the solid electrolyte layer on the positive electrode side is 0.2Na2GdCl5–0.8NaTaCl6; the solid electrolyte layer on the negative electrode side is Na3PS4. The electrochemical charge-discharge performance of the all-solid-state sodium-ion battery was tested at room temperature. Figure 13 The battery's long-cycle performance at room temperature is shown, where hollow rhombuses represent coulombic efficiency, hollow circles represent charge specific capacity, and solid circles represent discharge specific capacity. Figure 14The results show its rate performance at room temperature, with the lines from dark to light representing 0.1C, 0.5C, 1C, 2C, and 3C, respectively. The experimental results demonstrate that the nanoparticle-induced sodium-ion solid electrolyte material described in this invention can achieve stable operation of all-solid-state sodium-ion batteries at room temperature, providing a feasible solution for expanding the applicable material systems for all-solid-state batteries.

[0069] Table 1. Statistics on the cold-pressed sodium ion conductivity of solid electrolytes prepared in Examples 1-8 and Comparative Examples 1-2

[0070] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A nanoparticle-induced sodium ion solid electrolyte, characterized in that, The general formula of the sodium ion solid electrolyte is: x Na2MCl5–(1- x NaTaCl6, where M is a lanthanide element, 0 < x ≤0.35; the Na2MCl5 has an orthorhombic crystal system. Pnma The nanoparticles have a space group crystal structure and have chlorine vacancies on their surface; M is any one of Eu, Gd, Tb, Dy or Ho, and the size of the Na2MCl5 nanoparticles is ≤100nm. NaTaCl6 exhibits an amorphous structure under the electrostatic induction of the Na2MCl5 nanoparticles.

2. The nanoparticle-induced sodium ion solid electrolyte according to claim 1, characterized in that, The Na2MCl5 nanoparticles are uniformly dispersed and embedded in the NaTaCl6.

3. The nanoparticle-induced sodium ion solid electrolyte according to claim 1, characterized in that, The sodium ion solid electrolyte, after being cold-pressed at room temperature, has a sodium ion conductivity of 0.5 mS·cm. -1 -10 mS·cm -1 .

4. A method for preparing a nanoparticle-induced sodium ion solid electrolyte as described in claim 1, characterized in that, Includes the following steps: S1, sodium chloride, lanthanide chloride and tantalum chloride are mixed according to the stoichiometric ratio of the general formula of sodium ion solid electrolyte to obtain a mixture; S2, the mixture is subjected to mechanochemical synthesis under an inert gas atmosphere or vacuum conditions to obtain the solid electrolyte.

5. The method for preparing nanoparticle-induced sodium ion solid electrolyte according to claim 4, characterized in that, In S1, the lanthanide chloride is selected from any one of europium chloride, gadolinium chloride, terbium chloride, dysprosium chloride, or holmium chloride.

6. The method for preparing nanoparticle-induced sodium ion solid electrolyte according to claim 4, characterized in that, In S2, the mechanochemical synthesis is carried out by ball milling, with a ball milling speed of 500 rpm to 800 rpm and a ball milling time of 0.5 h to 60 h.

7. The method for preparing nanoparticle-induced sodium ion solid electrolyte according to claim 6, characterized in that, The ball milling speed is 600 rpm, and the ball milling time is 27 h.

8. The application of the nanoparticle-induced sodium-ion solid electrolyte as described in any one of claims 1-3 in an all-solid-state sodium-ion battery, characterized in that, The sodium-ion solid electrolyte serves as the positive electrode electrolyte in an all-solid-state sodium-ion battery.

Citation Information

Patent Citations

  • Halide-based sodium ion solid electrolyte as well as preparation method and application thereof

    CN115566259A

  • High-capacity sulfide positive electrode material, preparation method and application thereof, and sodium ion battery

    CN116632229A