A metal-defect dual-active-site hydrogenation catalyst, its preparation method and application
By preparing a metal-defect dual-active-site hydrogenation catalyst, the synergistic effect of oxygen vacancies and metal clusters was utilized to solve the problems of catalyst size control and activity in the hydrogenation reaction of nitroaromatics, realizing a highly efficient hydrogenation reaction at room temperature and pressure, exhibiting high activity, selectivity and stability.
Patent Information
- Application Number
- CN202611149284.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-31
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2046-07-31
AI Technical Summary
Existing catalysts for the hydrogenation of nitroaromatics suffer from problems such as difficulty in controlling the size and dispersion of metal clusters, formation of large particles, low oxygen vacancy concentration, insignificant synergistic effect, and low catalytic activity at room temperature and pressure.
A metal-defect dual-active-site hydrogenation catalyst was prepared by calcining a metal oxide support, combined with impregnation and mild hydrogen reduction treatment. The catalyst utilizes the synergistic effect of oxygen vacancies and metal clusters to form a stable active structure of metal-Ov-metal oxide, achieving fully exposed metal clusters and single-atom dispersion.
The efficient and selective hydrogenation reaction of nitroaromatics was achieved at near-ambient temperature and pressure. The catalyst exhibits high activity, good selectivity, and strong stability. Furthermore, the preparation process is simple and low-cost, making it suitable for large-scale production.
Smart Images

Figure CN122665602B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of catalyst technology, and relates to a hydrogenation catalyst, particularly a metal-defect dual-active-site hydrogenation catalyst, its preparation method, and its application. Background Technology
[0002] Aromatic amines are important organic chemical intermediates, widely used in dyes, pharmaceuticals, pesticides, and rubber additives. Catalytic hydrogenation of nitroaromatics is the main industrial method for preparing aromatic amines, offering advantages such as high atom economy and environmental friendliness. Currently, commonly used industrial catalysts include supported metal catalysts such as Pd, Pt, and Ni. However, the preparation of traditional supported metal catalysts relies on high-temperature conditions (typically ≥500℃), making it difficult to precisely control the distribution of active sites. Metals tend to agglomerate, forming low-activity particles, resulting in problems such as low specific surface area and few exposed active sites. Furthermore, these catalysts typically require high-temperature and high-pressure reactions, leading to high energy consumption and safety hazards.
[0003] In recent years, cluster catalysts have exhibited excellent activity and selectivity in catalytic reactions due to their unique electronic and geometric structures. Fully exposed cluster catalysts refer to catalysts where all metal atoms are exposed on the surface, with no bulk atoms. Their metal atom utilization rate is close to 100%, providing abundant unsaturated coordination active sites, making them particularly suitable for selective hydrogenation reactions. Variable-valence metal oxides have advantages such as good chemical stability, low cost, and strong metal-metal interactions. Defect-rich supports contain a large number of oxygen vacancies, which can not only participate in the reaction as active sites and regulate hydrogen spillover, but also stabilize metal clusters through strong metal-support interactions (SMSI), preventing their aggregation during the reaction.
[0004] However, the catalysts reported so far still have some problems: First, the size and dispersion of metal clusters are difficult to control precisely, and large particles are easily formed; second, the oxygen vacancy concentration is low, and the synergistic effect with metal clusters is not obvious; third, the catalytic activity is low at room temperature and pressure, which is difficult to meet the needs of industrial applications.
[0005] Therefore, how to develop a highly active, highly selective, and highly stable catalyst for hydrogenation of nitroaromatics at ambient temperature and pressure is an urgent problem to be solved in this field. Summary of the Invention
[0006] To address the shortcomings of existing technologies, the present invention aims to provide a metal-defect dual-active-site hydrogenation catalyst, its preparation method, and its applications. The preparation method of the metal-defect dual-active-site hydrogenation catalyst provided in this invention, through the synergistic effect of oxygen vacancies and fully exposed metal clusters and single atoms, enables highly efficient and selective hydrogenation of nitroaromatics at near-ambient temperature and pressure. This achieves a complete process from preparation to application under near-ambient temperature and pressure conditions. Furthermore, this metal-defect dual-active-site hydrogenation catalyst exhibits advantages such as high activity, good selectivity, and strong stability.
[0007] To achieve this objective, the present invention employs the following technical solution:
[0008] In a first aspect, the present invention provides a method for preparing a metal-defect dual-active-site hydrogenation catalyst, the method comprising the following steps:
[0009] The metal oxide support is calcined to obtain a metal oxide support containing oxygen vacancies; the metal component precursor, solvent and the metal oxide support containing oxygen vacancies are mixed and subjected to impregnation treatment and hydrogen reduction treatment to obtain the metal-defect dual active site hydrogenation catalyst; the temperature of the hydrogen reduction treatment is 10℃~40℃.
[0010] For example, in this invention, the temperature of the hydrogen reduction treatment can be 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, or 40°C, etc.
[0011] In this invention, by calcining the metal oxide support, abundant oxygen vacancies (Ov) can be generated on the metal oxide support; by loading the metal component precursor by impregnation and subjecting it to mild (room temperature, 10℃~40℃) hydrogen reduction treatment, and by utilizing the interaction between the metal and the support and the anchoring effect of oxygen vacancies on the metal component, the metal component can exist on the metal oxide support containing oxygen vacancies in the form of uniformly sized, highly dispersed, fully exposed metal clusters and single atoms.
[0012] Among them, mild hydrogen reduction treatment can not only promote the transformation of metal component oxides into fully exposed metal clusters and single atoms, inducing high dispersion of metal components, but also promote the dynamic migration of oxygen vacancies on metal oxide supports, forming a stable active structure of metal-Ov-metal oxide, thereby constructing a catalytic system with strong metal-support interaction and metal-oxygen vacancy synergistic effect, and thus significantly improving the activity, selectivity and stability of this metal-defect dual active site hydrogenation catalyst for the hydrogenation reaction of nitroaromatics.
[0013] Furthermore, the preparation method provided by this invention is simple and has low preparation cost, which is conducive to large-scale production.
[0014] It should be noted that in this invention, "full exposure" means that the surface exposure rate of the metal components' atoms is ≥90%.
[0015] As a preferred embodiment of the present invention, the metal oxide support includes any one or a combination of at least two of TiO2, CeO2, ZrO2, WO3, Fe2O3, Co3O4, MoO3, MnO2 or CuO. Typical but non-limiting combinations include combinations of TiO2 and CeO2, combinations of ZrO2 and WO3, combinations of Fe2O3 and Co3O4, combinations of WO3 and MoO3, combinations of MnO2 and CuO, combinations of TiO2, CeO2 and ZrO2, combinations of WO3, Fe2O3 and Co3O4, combinations of MoO3, MnO2 and CuO, etc., preferably anatase phase TiO2.
[0016] In this invention, when the metal oxide support is anatase TiO2, its high specific surface area and numerous surface defects are beneficial to the loading of metal components and the catalytic reaction.
[0017] As one embodiment of the present invention, the metal component precursor includes any one or a combination of at least two of chlorates, chlorides, nitrates, sulfates or molybdates containing metal components. Typical but non-limiting combinations include combinations of chlorates and chlorides, combinations of nitrates and sulfates, combinations of sulfates and molybdates, combinations of chlorates, chlorides and nitrates, combinations of nitrates, sulfates and molybdates, etc.
[0018] As one embodiment of the present invention, the metal component includes any one or a combination of at least two of Pt, Pd, Au, Ag, Ru, Ni, Rh, Cu, Co, Fe, Zn or Mo. Typical but non-limiting combinations include combinations of Pt and Pd, Ag and Ru, Ni and Rh, Cu and Co, Fe and Zn, Zn and Mo, Pt, Pd, Au and Ag, Ru, Ni and Rh, Cu, Co, Fe and Zn, etc., preferably Pd.
[0019] In this invention, when the metal component is Pd, the strong metal-support interaction between Pd and reducible oxides such as TiO2 and CeO2 can effectively anchor Pd metal clusters, inhibiting agglomeration and sintering during the reaction and maintaining stable hydrogen dissociation activity over a long period. Simultaneously, Pd has an extremely low adsorption and dissociation energy barrier for H2 molecules (theoretically calculated to be only 0.1 eV), allowing for rapid decomposition of H2 into active hydrogen at room temperature and pressure without high-temperature activation. The resulting overflow hydrogen can continuously reduce the support surface, stabilizing the oxygen vacancy concentration and preventing the oxygen vacancy from being oxidized and deactivated during the reaction, thus forming a positive synergistic cycle of oxygen vacancy regeneration.
[0020] As one embodiment of the present invention, the solvent includes any one or a combination of at least two of water, ethanol, ethylene glycol or isopropanol. Typical but non-limiting combinations include combinations of water and ethanol, combinations of ethylene glycol and isopropanol, combinations of water, ethanol and ethylene glycol, combinations of ethanol, ethylene glycol and isopropanol, combinations of water, ethanol, ethylene glycol and isopropanol, etc., preferably water.
[0021] As a preferred embodiment of the present invention, the method for preparing the metal oxide support includes: mixing a precursor salt and an alkaline solution, and carrying out a hydrothermal reaction to obtain the metal oxide support.
[0022] As one embodiment of the present invention, the precursor salt includes any one or a combination of at least two of the chloride, nitrate, sulfate or alkoxide containing the metal element in the metal oxide support. Typical but non-limiting combinations include combinations of chloride and nitrate, combinations of sulfate and alkoxide, combinations of chloride, nitrate and sulfate, combinations of nitrate, sulfate and alkoxide, and combinations of chloride, nitrate, sulfate and alkoxide, etc.
[0023] As one embodiment of the present invention, the alkaline solution includes any one or a combination of at least two of sodium hydroxide solution, sodium carbonate solution, or sodium bicarbonate solution. Typical but non-limiting combinations include combinations of sodium hydroxide solution and sodium carbonate solution, combinations of sodium carbonate solution and sodium bicarbonate solution, combinations of sodium hydroxide solution and sodium bicarbonate solution, combinations of sodium hydroxide solution, sodium carbonate solution, and sodium bicarbonate solution, etc., preferably sodium hydroxide solution.
[0024] In one embodiment of the present invention, the temperature of the hydrothermal reaction is 100℃~200℃, and the time of the hydrothermal reaction is 12h~24h.
[0025] For example, the temperature of the hydrothermal reaction can be 100℃, 120℃, 150℃, 180℃ or 200℃, etc., and the time of the hydrothermal reaction can be 12h, 15h, 18h, 21h or 24h, etc.
[0026] As a preferred embodiment of the present invention, the calcination atmosphere includes hydrogen or a nitrogen-hydrogen mixture.
[0027] As one embodiment of the present invention, the volume fraction of hydrogen in the nitrogen-hydrogen mixture is 10 vol.% to 100 vol.%, but not 100 vol.%. For example, it can be 10 vol.%, 20 vol.%, 30 vol.%, 40 vol.%, 50 vol.%, 60 vol.%, 70 vol.%, 80 vol.%, 90 vol.%, or 99 vol.%.
[0028] In one embodiment of the present invention, the calcination temperature is 200℃~1000℃, preferably 300℃~600℃, the calcination time is 1h~6h, and the calcination heating rate is 2℃ / min~10℃ / min.
[0029] For example, the calcination temperature can be 200℃, 250℃, 300℃, 350℃, 400℃, 450℃, 500℃, 550℃, 600℃, 650℃, 700℃, 750℃, 800℃, 850℃, 900℃, 950℃, or 1000℃, etc., the calcination time can be 1h, 2h, 3h, 4h, 5h, or 6h, etc., and the calcination heating rate can be 2℃ / min, 3℃ / min, 4℃ / min, 5℃ / min, 6℃ / min, 7℃ / min, 8℃ / min, 9℃ / min, or 10℃ / min, etc.
[0030] As a preferred embodiment of the present invention, the mixing temperature is 10℃~40℃ and the mixing time is 20min~40min.
[0031] For example, the mixing temperature can be 10°C, 15°C, 20°C, 25°C, 30°C, 35°C or 40°C, etc., and the mixing time can be 20 min, 25 min, 30 min, 35 min or 40 min, etc.
[0032] In one embodiment of the present invention, the mixing is performed under ultrasonic conditions.
[0033] In one embodiment of the present invention, the temperature of the impregnation treatment is 10°C to 40°C, and the time of the impregnation treatment is 4h to 8h.
[0034] For example, the temperature of the impregnation treatment can be 10°C, 15°C, 20°C, 25°C, 30°C, 35°C or 40°C, etc., and the time of the impregnation treatment can be 4h, 5h, 6h, 7h or 8h, etc.
[0035] In one embodiment of the present invention, the impregnation treatment is carried out under stirring conditions.
[0036] As one embodiment of the present invention, the atmosphere for the hydrogen reduction treatment includes hydrogen or a nitrogen-hydrogen mixture.
[0037] As one embodiment of the present invention, the volume fraction of hydrogen in the nitrogen-hydrogen mixture is 10 vol.% to 100 vol.%, but not 100 vol.%. For example, it can be 10 vol.%, 20 vol.%, 30 vol.%, 40 vol.%, 50 vol.%, 60 vol.%, 70 vol.%, 80 vol.%, 90 vol.%, or 99 vol.%.
[0038] As one embodiment of the present invention, the temperature of the hydrogen reduction treatment is 20°C to 30°C, for example, it can be 20°C, 22°C, 25°C, 28°C or 30°C.
[0039] As one embodiment of the present invention, the hydrogen reduction treatment time is 0.5h to 5h, for example, it can be 0.5h, 1h, 2h, 3h, 4h or 5h, preferably 3h to 5h.
[0040] As a preferred embodiment of the present invention, the preparation method includes the following steps:
[0041] (1) Mix the precursor salt and alkaline solution and carry out a hydrothermal reaction at 100℃~200℃ for 12h~24h to obtain the metal oxide support; calcine the metal oxide support in an atmosphere of hydrogen or nitrogen-hydrogen mixture at a heating rate of 2℃ / min~10℃ / min to 200℃~1000℃ for 1h~6h to obtain a metal oxide support containing oxygen vacancies.
[0042] (2) The metal component precursor, solvent and the metal oxide support containing oxygen vacancies are mixed under ultrasonic conditions at 10℃~40℃ for 20min~40min; then impregnated under stirring conditions at 10℃~40℃ for 4h~8h; finally, hydrogen reduction treatment is carried out at 10℃~40℃ for 0.5h~5h in an atmosphere of hydrogen or nitrogen-hydrogen mixture to obtain the metal-defect dual active site hydrogenation catalyst.
[0043] In a second aspect, the present invention provides a metal-defect dual-active-site hydrogenation catalyst, wherein the metal-defect dual-active-site hydrogenation catalyst is prepared by the preparation method described in the first aspect; the metal-defect dual-active-site hydrogenation catalyst comprises a metal oxide support containing oxygen vacancies and a metal component supported on the surface of the metal oxide support containing oxygen vacancies; the metal component exists in the form of fully exposed metal clusters and single atoms.
[0044] The metal-defect dual-active-site hydrogenation catalyst provided by this invention features a metal component highly dispersed on the surface of a metal oxide support containing oxygen vacancies, in the form of fully exposed metal clusters and single atoms. This significantly improves the atomic utilization rate of the metal component and substantially increases the number of active sites. Simultaneously, the abundant oxygen vacancies on the metal oxide support surface can strongly interact with the metal clusters, not only stabilizing the clusters and preventing their aggregation during impregnation, hydrogen reduction, and catalytic reactions, but also modulating the electronic structure of the metal component, enhancing its adsorption and activation capacity for hydrogen and nitroaromatics. Furthermore, the oxygen vacancies themselves can also serve as active sites, participating in the activation and hydrogenation process of nitroaromatics, thus forming a synergistic catalytic effect with the metal clusters. Therefore, the metal-defect dual-active-site hydrogenation catalyst provided by this invention can significantly reduce the reaction energy barrier of nitroaromatic hydrogenation, enabling the hydrogenation reaction of nitroaromatics to proceed at ambient temperature and pressure, and possesses advantages such as high activity, good selectivity, and strong stability.
[0045] As a preferred embodiment of the present invention, based on the total mass of the metal-defect dual-active-site hydrogenation catalyst being 100%, the loading of the metal component is 0.5% to 3%, for example, it can be 0.5%, 1%, 1.5%, 2%, 2.5% or 3%, preferably 1% to 2.5%.
[0046] In this invention, based on the total mass of the metal-defect dual-active-site hydrogenation catalyst being 100%, the loading of the metal component should be controlled at 0.1% to 5%. If the loading is too low, the number of active palladium sites will be too low, leading to a decrease in hydrogen dissociation efficiency. If the loading is too high, it will cause Pd agglomeration and excessive occupation of oxygen vacancies. The decrease in the number of oxygen vacancies will reduce the catalyst's ability to adsorb and activate nitrobenzene and its ability to desorb water, thereby affecting the hydrogenation activity.
[0047] In one embodiment of the present invention, the average particle size of the metal clusters in the metal component is 0.5 nm to 5 nm, for example, it can be 0.5 nm, 1 nm, 2 nm, 3 nm, 4 nm or 5 nm, etc.
[0048] Thirdly, the present invention provides an application of the metal-defect dual-active-site hydrogenation catalyst as described in the second aspect, wherein the metal-defect dual-active-site hydrogenation catalyst is applied to the hydrogenation reaction of nitroaromatics.
[0049] As a preferred embodiment of the present invention, the nitroaromatic hydrocarbon includes any one or a combination of at least two of nitrobenzene, p-nitrophenol, or 2,4-dinitrotoluene.
[0050] As one embodiment of the present invention, the hydrogenation reaction of the nitroaromatic hydrocarbon is carried out at a temperature of 10°C to 40°C, for example, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C or 40°C.
[0051] And / or, in the hydrogenation reaction of the nitroaromatic hydrocarbon, the pressure of hydrogen is 0.1 MPa to 1.5 MPa, for example, it can be 0.1 MPa, 0.5 MPa, 0.8 MPa, 1 MPa, 1.2 MPa or 1.5 MPa, etc.
[0052] In one embodiment of the present invention, in the hydrogenation reaction of the nitroaromatic hydrocarbon, the mass of the metal-defect dual-active-site hydrogenation catalyst is 2% to 6% of the mass of the nitroaromatic hydrocarbon, for example, it can be 2%, 3%, 4%, 5% or 6%, etc.
[0053] The numerical range described in this invention includes not only the point values listed above, but also any point values within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific point values included in the range.
[0054] Compared with the prior art, the present invention has the following beneficial effects:
[0055] (1) This invention generates abundant oxygen vacancies on the metal oxide support by calcining it. By loading the metal component precursor via impregnation and subjecting it to mild (room temperature, 10℃~40℃) hydrogen reduction treatment, and utilizing the metal-support interaction and the anchoring effect of oxygen vacancies on the metal component, the metal component can exist on the oxygen-vacancy-containing metal oxide support in the form of uniformly sized, highly dispersed, fully exposed metal clusters and single atoms. The mild hydrogen reduction treatment not only promotes the transformation of the metal component oxide into fully exposed metal clusters and single atoms, inducing high dispersion of the metal component, but also promotes the dynamic migration of oxygen vacancies on the metal oxide support, forming a stable active structure of metal-Ov-metal oxide. This constructs a catalytic system with strong metal-support interaction and synergistic metal-oxygen vacancy effects, significantly improving the activity, selectivity, and stability of this metal-defect dual-active-site hydrogenation catalyst for the hydrogenation reaction of nitroaromatics. Furthermore, the preparation method provided by this invention is simple and low-cost, which is beneficial for large-scale production.
[0056] (2) The metal-defect dual-active-site hydrogenation catalyst provided by this invention has a metal component that is highly dispersed on the surface of a metal oxide support containing oxygen vacancies in the form of fully exposed metal clusters and single atoms, which greatly improves the atomic utilization rate of the metal component and significantly increases the number of active sites. At the same time, the abundant oxygen vacancies on the surface of the metal oxide support can interact strongly with the metal clusters, which can not only stabilize the clusters and prevent them from agglomerating during impregnation, hydrogen reduction and catalytic reactions, but also regulate the electronic structure of the metal component and enhance its adsorption and activation ability for hydrogen and nitroaromatics. In addition, the oxygen vacancies themselves can also serve as active sites to participate in the activation and hydrogenation process of nitroaromatics, thereby forming a synergistic catalytic effect with the metal clusters. Therefore, the metal-defect dual-active-site hydrogenation catalyst provided by this invention can significantly reduce the reaction energy barrier of the hydrogenation reaction of nitroaromatics, enabling the hydrogenation reaction of nitroaromatics to be carried out at room temperature and pressure, and has the advantages of high activity, good selectivity and strong stability. Attached Figure Description
[0057] Figure 1 This is a SEM image of the metal-defect dual-active-site hydrogenation catalyst prepared in Example 1 of this invention.
[0058] Figure 2 This is a TEM image of the metal-defect dual-active-site hydrogenation catalyst prepared in Example 1 of this invention.
[0059] Figure 3 This is a spherical aberration-corrected transmission electron microscope image of the metal-defect dual-active-site hydrogenation catalyst prepared in Example 1 of this invention.
[0060] Figure 4 This is a Raman comparison diagram of the metal-defect dual-active-site hydrogenation catalysts prepared in Example 1 and Comparative Example 1 of this invention.
[0061] Figure 5 These are XRD comparison images of the metal-defect dual-active-site hydrogenation catalysts prepared in Examples 1, 5, 6 and Comparative Example 2 of this invention.
[0062] Figure 6 This is a comparison diagram of the EPR of the metal-defect dual-active-site hydrogenation catalysts prepared in Examples 1, 6 and 9 of this invention. Detailed Implementation
[0063] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.
[0064] The scope of this invention can be defined by lower and upper limits. The selected lower and upper limits define the boundaries of a specific range. The range defined in this way can be defined by the inclusion or exclusion of endpoints. Any endpoint can be independently selected for inclusion or exclusion, and all lower and upper limits can be arbitrarily combined to form new ranges. That is, any lower limit can be combined with any upper limit to form an effective range. For example, if the ranges of 60~120 and 80~110 are listed for specific parameters, it should be understood that the ranges of 60~110 and 80~120 also fall within the scope of this invention. In addition, if the minimum range values 1 and 2 are listed, and the maximum range values 3, 4 and 5 are also listed, then all ranges of 1~3, 1~4, 1~5, 2~3, 2~4 and 2~5 fall within the scope of this invention. In this invention, the numerical range "a~b" represents a shortened representation of any combination of real numbers between a and b, where a and b are both real numbers. For example, the numerical range "0~5" means that all real numbers between 0 and 5 have been fully listed in this document, and "0~5" is only a shortened representation of this set of numerical combinations. When a parameter is expressed as an integer ≥2, it is equivalent to listing positive integers that meet the requirements, such as 2, 3, 4, 5, 6, 7, 8, 9, 10, etc. When a parameter is expressed as an integer selected from "2~10", it is equivalent to listing any integer among 2, 3, 4, 5, 6, 7, 8, 9, and 10.
[0065] Unless otherwise specified, the term "at least two combinations" in this invention refers to a quantity greater than or equal to 2. For example, "any one or at least two combinations" means that any one of the listed items can be selected, or a combination of at least two of the listed items formed in a manner that does not conflict and enables the implementation of this invention.
[0066] In this invention, unless otherwise specified, the feature or solution corresponding to "and / or" covers any one of two or more related listed items, as well as any and all combinations of the related listed items. These arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. For example, "A and / or B" represents a set consisting of A, B, and combinations of A and B. "Including A and / or B" can be understood, depending on the context of the statement, as including A, including B, or simultaneously including both A and B. In this invention, "optional" means that the corresponding feature, component, step, or solution is not essential, i.e., selected from either "present" or "absent" parallel solutions. If multiple "optional" limitations appear in a technical solution, unless otherwise specified and without technical conflict or mutual constraint, each "optional" limitation is independent and does not affect the others.
[0067] In this invention, technical features or solutions described using open-ended terms such as "comprising" or "including" do not exclude additional non-conflicting elements beyond the listed elements unless otherwise specified. They are considered to disclose both closed-ended features or solutions consisting solely of the listed elements and open-ended features or solutions that may include additional non-conflicting elements beyond the listed elements. For example, if A includes a1, a2, and a3, unless otherwise specified, this means that A may consist only of a1, a2, and a3, or it may include other non-conflicting elements based on a1, a2, and a3. This corresponds to the disclosure of technical solutions such as "A consists of a1, a2, and a3," "A is selected from a1, a2, and a3," and "A not only includes a1, a2, and a3, but may also include other non-conflicting elements."
[0068] All embodiments and optional embodiments of the present invention, unless otherwise specified and without technical conflict, can be combined to form new technical solutions, and such combinations fall within the scope of the present invention. The term "embodiment" as used in this invention means that a specific feature, structure, or characteristic described in connection with an embodiment can be included in at least one embodiment or implementation of the present invention. The appearance of this phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment mutually exclusive with other embodiments. Those skilled in the art can explicitly and implicitly understand that the embodiments described in this invention can be combined with other embodiments without technical conflict.
[0069] In this invention, the ordinal numbers “first,” “second,” “third,” and “fourth” used in expressions such as “first aspect,” “second aspect,” “third aspect,” and “fourth aspect” are used for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor should they be construed as implicitly indicating the importance or quantity of the indicated technical features. They serve only as a non-exhaustive enumeration and do not constitute a closed limitation on quantity.
[0070] In this invention, the order in which the steps are written in the methods described in each embodiment does not imply a strict execution order. The actual execution order of each step should be determined based on its function and possible internal logic. Unless otherwise specified, all steps of this invention can be executed in the order they are written, or in any order without technical conflict. For example, if the method includes steps (a) and (b), it means that the method may include steps (a) and (b) executed sequentially, or it may include steps (b) and (a) executed sequentially. If the method also includes step (c), then step (c) can be added to the method in any order without conflict, including but not limited to the execution order of steps (a), (b), and (c), steps (a), (c), and (b), steps (c), (a), and (b), etc.
[0071] Example 1
[0072] This embodiment provides a method for preparing a metal-defect dual-active-site hydrogenation catalyst, comprising the following steps:
[0073] (1) 10 mL of tetrabutyl titanate was slowly added dropwise to 100 mL of 1 mol / L sodium hydroxide solution. After stirring and mixing at 20 °C for 30 min, the mixture was transferred to a 150 mL polytetrafluoroethylene-lined hydrothermal reactor and subjected to hydrothermal reaction at 180 °C for 24 h. After the hydrothermal reaction was completed and the mixture was naturally cooled to room temperature, it was centrifuged and washed alternately with deionized water and ethanol until the filtrate was neutral. The filtrate was then vacuum dried for 12 h to obtain TiO2 support.
[0074] (2) The TiO2 support was placed in a tube furnace and hydrogen gas was introduced (flow rate 20 mL / min). The temperature was increased to 500℃ at a heating rate of 5℃ / min and kept at the temperature for 2 hours. After natural cooling to room temperature, TiO2 support containing oxygen vacancies was obtained.
[0075] (3) Disperse 1g of TiO2 support containing oxygen vacancies in 2mL of deionized water, add chloropalladium acid solution (1mL, 0.188mol / L), mix at 20℃ for 30min under ultrasonic conditions, then impregnate at 20℃ for 6h under stirring conditions, and vacuum dry for 12h after impregnation. The obtained solid is ground and placed in a tube furnace, and 10vol.% nitrogen-hydrogen mixed gas (flow rate 80mL / min) is introduced and hydrogen reduction treatment is carried out at 20℃ for 3h to obtain metal-defect dual active site hydrogenation catalyst.
[0076] The metal-defect dual-active-site hydrogenation catalyst prepared by the method provided in this embodiment includes a TiO2 support containing oxygen vacancies and palladium supported on its surface. The palladium exists in the form of fully exposed metal clusters and single atoms. Based on the total mass of the metal-defect dual-active-site hydrogenation catalyst being 100%, the palladium loading is 2%, denoted as 2% Pd / TiO2-Ov catalyst.
[0077] Figure 1 This is a SEM image of the metal-defect dual-active-site hydrogenation catalyst prepared in this embodiment. As can be seen from the image, the TiO2 support is composed of a large number of densely packed nano-sized particles with gaps between the aggregates, exhibiting a loose and porous powder aggregate morphology. No obvious palladium particles were observed on the surface of the TiO2 support, indicating that palladium is highly dispersed on the surface of the TiO2 support.
[0078] Figure 2 and Figure 3The images show a TEM image and an aberration-corrected transmission electron microscope image of the metal-defect dual-active-site hydrogenation catalyst prepared in this embodiment. The images clearly show that palladium exists as uniformly sized (average particle size approximately 1 nm) palladium clusters and single palladium atoms, with all palladium atoms exposed on the surface and not forming a bulk structure, confirming the successful preparation of fully exposed metal clusters and single atoms.
[0079] Example 2
[0080] This embodiment provides a method for preparing a metal-defect dual-active-site hydrogenation catalyst, comprising the following steps:
[0081] (1) 30g of cerium nitrate hexahydrate was slowly added dropwise to 100mL of 1mol / L sodium carbonate solution. After stirring and mixing at 20℃ for 30min, the mixture was transferred to a 150mL polytetrafluoroethylene-lined hydrothermal reactor and subjected to hydrothermal reaction at 200℃ for 12h. After the hydrothermal reaction was completed and the mixture was naturally cooled to room temperature, it was centrifuged and washed alternately with deionized water and ethanol until the filtrate was neutral. The filtrate was then vacuum dried for 12h to obtain CeO2 support.
[0082] (2) The CeO2 support was placed in a tube furnace and a 10 vol.% nitrogen-hydrogen mixture was introduced (flow rate 60 mL / min). The temperature was increased to 200°C at a heating rate of 2°C / min and kept at that temperature for 6 hours. After naturally cooling to room temperature, the CeO2 support containing oxygen vacancies was obtained.
[0083] (3) 1 g of CeO2 support containing oxygen vacancies was dispersed in 2 mL of deionized water, and 1 mL of chloroplatinic acid solution (0.0094 mol / L) was added. The mixture was stirred at 10 °C for 40 min, and then impregnated at 10 °C for 8 h under stirring. After impregnation, the mixture was vacuum dried for 12 h. The resulting solid was ground and placed in a tube furnace. 50 vol.% nitrogen-hydrogen mixed gas (flow rate 40 mL / min) was introduced and hydrogen reduction was performed at 10 °C for 5 h to obtain a metal-defect dual active site hydrogenation catalyst.
[0084] The metal-defect dual-active-site hydrogenation catalyst prepared by the method provided in this embodiment includes a CeO2 support containing oxygen vacancies and platinum supported on its surface. The platinum exists in the form of fully exposed metal clusters and single atoms. Based on the total mass of the metal-defect dual-active-site hydrogenation catalyst being 100%, the platinum loading is 1%, denoted as 0.1% Pt / CeO2-Ov catalyst.
[0085] Example 3
[0086] This embodiment provides a method for preparing a metal-defect dual-active-site hydrogenation catalyst, comprising the following steps:
[0087] (1) 15g sodium tungstate was slowly added dropwise to 100mL of 1mol / L sodium bicarbonate solution. After stirring and mixing at 20℃ for 30min, the mixture was transferred to a 150mL polytetrafluoroethylene-lined hydrothermal reactor and subjected to hydrothermal reaction at 100℃ for 18h. After the hydrothermal reaction was completed and the mixture was naturally cooled to room temperature, it was centrifuged and washed alternately with deionized water and ethanol until the filtrate was neutral. The filtrate was then vacuum dried for 12h to obtain WO3 support.
[0088] (2) Place the WO3 support in a tube furnace, introduce 80 vol.% nitrogen-hydrogen mixed gas (flow rate 30 mL / min), heat to 1000℃ at a heating rate of 10℃ / min and keep it at that temperature for 1 h, and then cool naturally to room temperature to obtain the WO3 support containing oxygen vacancies.
[0089] (3) Disperse 1g of WO3 support containing oxygen vacancies in 2mL of deionized water, add ruthenium trichloride solution (1mL, 0.47mol / L), mix at 40℃ for 20min under ultrasonic conditions, then impregnate at 40℃ for 4h under stirring conditions, and vacuum dry for 12h after impregnation. The obtained solid is ground and placed in a tube furnace, hydrogen gas is introduced (flow rate 20mL / min), and hydrogen reduction treatment is carried out at 40℃ for 0.5h to obtain a metal-defect dual active site hydrogenation catalyst.
[0090] The metal-defect dual-active-site hydrogenation catalyst prepared by the method provided in this embodiment includes a WO3 support containing oxygen vacancies and ruthenium supported on its surface. The ruthenium exists in the form of fully exposed metal clusters and single atoms. Based on the total mass of the metal-defect dual-active-site hydrogenation catalyst being 100%, the ruthenium loading is 5%, denoted as 5%Ru / WO3-Ov catalyst.
[0091] Example 4
[0092] This embodiment provides a method for preparing a metal-defect dual-active-site hydrogenation catalyst. Except for keeping the volume of the chloroplatinic acid solution unchanged in step (3) and adjusting the concentration to 0.0094 mol / L, everything else is the same as in Example 1.
[0093] The metal-defect dual-active-site hydrogenation catalyst prepared by the method provided in this embodiment is the same as that in Example 1, except that the total mass of the metal-defect dual-active-site hydrogenation catalyst is 100% and the palladium loading is 0.1%.
[0094] Example 5
[0095] This embodiment provides a method for preparing a metal-defect dual-active-site hydrogenation catalyst. Except for keeping the volume of the chloroplatinic acid solution unchanged in step (3) and adjusting the concentration to 0.047 mol / L, everything else is the same as in Example 1.
[0096] The metal-defect dual-active-site hydrogenation catalyst prepared by the method provided in this embodiment is the same as that in Example 1, except that the total mass of the metal-defect dual-active-site hydrogenation catalyst is 100% and the palladium loading is 0.5%.
[0097] Example 6
[0098] This embodiment provides a method for preparing a metal-defect dual-active-site hydrogenation catalyst. Except for keeping the volume of the chloroplatinic acid solution unchanged in step (3) and adjusting the concentration to 0.094 mol / L, everything else is the same as in Example 1.
[0099] The metal-defect dual-active-site hydrogenation catalyst prepared by the method provided in this embodiment is the same as that in Example 1, except that the total mass of the metal-defect dual-active-site hydrogenation catalyst is 100% and the palladium loading is 1%.
[0100] Example 7
[0101] This embodiment provides a method for preparing a metal-defect dual-active-site hydrogenation catalyst. Except for keeping the volume of the chloroplatinic acid solution unchanged in step (3) and adjusting the concentration to 0.141 mol / L, everything else is the same as in Example 1.
[0102] The metal-defect dual-active-site hydrogenation catalyst prepared by the method provided in this embodiment is the same as that in Example 1, except that the total mass of the metal-defect dual-active-site hydrogenation catalyst is 100% and the palladium loading is 1.5%.
[0103] Example 8
[0104] This embodiment provides a method for preparing a metal-defect dual-active-site hydrogenation catalyst. Except for keeping the volume of the chloroplatinic acid solution unchanged in step (3) and adjusting the concentration to 0.0235 mol / L, everything else is the same as in Example 1.
[0105] The metal-defect dual-active-site hydrogenation catalyst prepared by the method provided in this embodiment is the same as that in Example 1, except that the total mass of the metal-defect dual-active-site hydrogenation catalyst is 100% and the palladium loading is 2.5%.
[0106] Example 9
[0107] This embodiment provides a method for preparing a metal-defect dual-active-site hydrogenation catalyst. Except for keeping the volume of the chloroplatinic acid solution unchanged in step (3) and adjusting the concentration to 0.0282 mol / L, everything else is the same as in Example 1.
[0108] The metal-defect dual-active-site hydrogenation catalyst prepared by the method provided in this embodiment is the same as that in Example 1, except that the total mass of the metal-defect dual-active-site hydrogenation catalyst is 100% and the palladium loading is 3%.
[0109] Example 10
[0110] This embodiment provides a method for preparing a metal-defect dual-active-site hydrogenation catalyst. Except for keeping the volume of the chloroplatinic acid solution unchanged in step (3) and adjusting the concentration to 0.47 mol / L, everything else is the same as in Example 1.
[0111] The metal-defect dual-active-site hydrogenation catalyst prepared by the method provided in this embodiment is the same as that in Example 1, except that the total mass of the metal-defect dual-active-site hydrogenation catalyst is 100% and the palladium loading is 5%.
[0112] Comparative Example 1
[0113] This comparative example provides a method for preparing a metal-defect dual-active-site hydrogenation catalyst, which is the same as in Example 1 except that step (2) does not involve hydrogen calcination.
[0114] The metal-defect dual-active-site hydrogenation catalyst prepared by the method provided in this comparative example is the same as that in Example 1, except that the number of oxygen vacancies on the TiO2 support surface is much smaller than that in Example 1.
[0115] Figure 4 This is a Raman comparison diagram of the metal-defect dual-active-site hydrogenation catalysts prepared in Example 1 and Comparative Example 1. As can be seen from the diagram, the yellow area (100 cm⁻¹)... -1 ~180cm -1 The peak intensity is related to the intrinsic vibrations of Ti-O lattice stretching / bending, representing a complete and defect-free TiO2 lattice framework; the peak intensity reflects the intrinsic signal of a complete crystal. The green region (580 cm⁻¹) -1 ~650cm -1 The peak () is a characteristic peak of oxygen vacancy-induced defects. After the lattice lacks O, local Ti... 3+The Raman peak caused by this defect is directly proportional to the oxygen vacancy concentration within the material due to lattice distortion. The ratio of the defect peak intensity to the intrinsic lattice peak intensity can be used to semi-quantitatively compare the number of oxygen vacancies: Example 1 > Comparative Example 1. This indicates that the metal-defect dual-active-site hydrogenation catalyst prepared in Example 1 has a higher density of oxygen vacancies, proving that the hydrogen calcination treatment successfully introduced more lattice oxygen defects into the TiO2 support.
[0116] Comparative Example 2
[0117] This comparative example provides a method for preparing a metal-defect dual-active-site hydrogenation catalyst. Except for adjusting the temperature of hydrogen reduction treatment in step (3) to 500°C, all other steps are the same as in Example 1.
[0118] The metal-defect dual-active-site hydrogenation catalyst prepared by the method provided in this comparative example is the same as that in Example 1, except that the palladium supported on the surface of the TiO2 support containing oxygen vacancies exists in the form of aggregated metal clusters.
[0119] Figure 5 These are XRD comparison images of the metal-defect dual-active-site hydrogenation catalysts prepared in Examples 1, 5, 6, and Comparative Example 2. As can be seen from the images, the metal-defect dual-active-site hydrogenation catalysts prepared in Examples 1, 5, and 6 only showed characteristic diffraction peaks on the TiO2 support, without any characteristic diffraction peaks of palladium. However, in Comparative Example 2, characteristic diffraction peaks of palladium were clearly observed. This further confirms that hydrogen reduction at room temperature can achieve a high degree of palladium dispersion on the TiO2 support surface.
[0120] Figure 6 This is a comparison of the EPR of the metal-defect dual-active-site hydrogenation catalysts prepared in Examples 1, 6, and 9. As can be seen from the figures, the metal-defect dual-active-site hydrogenation catalysts prepared in Examples 1, 6, and 9 show a significant signal peak at g=2.003, confirming the presence of oxygen vacancies on the catalyst surface, with Example 1 exhibiting the highest number of oxygen vacancies.
[0121] The metal-defect dual-active-site hydrogenation catalysts prepared in Examples 1-10 and Comparative Examples 1-2 were used for the hydrogenation reaction of nitroaromatics. Taking nitrobenzene as an example, the hydrogenation reaction of nitroaromatics was carried out for 15 min at a reaction temperature of 20°C, a hydrogen pressure of 0.15 MPa or 1.5 MPa, and a mass of 2% or 6% of the mass of nitrobenzene. The conversion rate of nitrobenzene, the selectivity of aniline, and the space-time yield were tested.
[0122] The test results are shown in Table 1.
[0123]
[0124] As can be seen from Table 1, the metal-defect dual-active-site hydrogenation catalysts prepared in Examples 1 to 3 exhibit excellent catalytic activity and selectivity in the selective hydrogenation reaction of nitrobenzene, specifically manifested as high nitrobenzene conversion, high aniline selectivity, and high space-time yield.
[0125] Examples 1 and 4-10 investigated the effect of metal component loading on the catalytic performance of a metal-defect dual-active-site hydrogenation catalyst. It can be seen that both excessively low and excessively high metal component loading lead to a decrease in nitrobenzene conversion, aniline selectivity, and space-time yield. This is because: if the metal component loading is too low, the number of active palladium sites is too low, resulting in reduced hydrogen dissociation efficiency; if the metal component loading is too high, Pd aggregation occurs, excessively occupying oxygen vacancies. The decrease in the number of oxygen vacancies reduces the catalyst's ability to adsorb and activate nitrobenzene and its ability to desorb water, thus affecting the hydrogenation activity.
[0126] The comparison between Example 1 and Comparative Example 1 shows that the oxygen vacancies on the TiO2 support play a key role in improving the catalytic performance of the metal-defect dual-active-site hydrogenation catalyst, and the synergistic effect of oxygen vacancies and palladium clusters can significantly enhance the hydrogenation performance of the catalyst.
[0127] The comparison between Example 1 and Comparative Example 2 shows that the mild hydrogen reduction treatment promotes the transformation of the metal component oxide into fully exposed metal clusters and single atoms, induces high dispersion of the metal component, and promotes the dynamic migration of oxygen vacancies on the metal oxide support, forming a stable active structure of metal-Ov-metal oxide. This constructs a catalytic system with strong metal-support interaction and metal-oxygen vacancy synergistic effect, which plays a key role in improving the catalytic performance of the metal-defect dual active site hydrogenation catalyst.
[0128] In summary, this invention, through calcination of the metal oxide support, generates abundant oxygen vacancies. By loading the metal component precursor via impregnation followed by mild (room temperature, 10℃~40℃) hydrogen reduction treatment, and utilizing the metal-support interaction and the anchoring effect of oxygen vacancies on the metal component, the metal component exists on the oxygen-vacancy-containing metal oxide support in the form of uniformly sized, highly dispersed, fully exposed metal clusters and single atoms. The mild hydrogen reduction treatment not only promotes the transformation of the metal component oxide into fully exposed metal clusters and single atoms, inducing high dispersion of the metal component, but also promotes the dynamic migration of oxygen vacancies on the metal oxide support, forming a stable active structure of metal-Ov-metal oxide. This constructs a catalytic system with strong metal-support interaction and a synergistic effect of metal-oxygen vacancies, significantly improving the activity, selectivity, and stability of this metal-defect dual-active-site hydrogenation catalyst for the hydrogenation reaction of nitroaromatics. Furthermore, the preparation method provided by this invention is simple and low-cost, which is beneficial for large-scale production.
[0129] The metal-defect dual-active-site hydrogenation catalyst provided by this invention features a metal component highly dispersed on the surface of a metal oxide support containing oxygen vacancies, in the form of fully exposed metal clusters and single atoms. This significantly improves the atomic utilization rate of the metal component and substantially increases the number of active sites. Simultaneously, the abundant oxygen vacancies on the metal oxide support surface can strongly interact with the metal clusters, not only stabilizing the clusters and preventing their aggregation during impregnation, hydrogen reduction, and catalytic reactions, but also modulating the electronic structure of the metal component, enhancing its adsorption and activation capacity for hydrogen and nitroaromatics. Furthermore, the oxygen vacancies themselves can also serve as active sites, participating in the activation and hydrogenation process of nitroaromatics, thus forming a synergistic catalytic effect with the metal clusters. Therefore, the metal-defect dual-active-site hydrogenation catalyst provided by this invention can significantly reduce the reaction energy barrier of nitroaromatic hydrogenation, enabling the hydrogenation reaction of nitroaromatics to proceed at ambient temperature and pressure, and possesses advantages such as high activity, good selectivity, and strong stability.
[0130] The applicant declares that the above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.
Claims
1. A process for the preparation of a metal-defect bi-active site hydrogenation catalyst, characterized in that, The preparation method includes the following steps: The metal oxide support is calcined to obtain a metal oxide support containing oxygen vacancies. The calcination atmosphere includes hydrogen or a nitrogen-hydrogen mixture; The metal component precursor, solvent, and the metal oxide support containing oxygen vacancies are mixed and subjected to impregnation and hydrogen reduction treatment to obtain the metal-defect dual-active-site hydrogenation catalyst. The temperature for the hydrogen reduction process is 10℃~40℃.
2. The production method according to claim 1, characterized by, The metal oxide support includes TiO2 and / or CeO2; And / or, the metal component precursor includes chloropalladium acid and / or chloroplatinic acid; And / or, the solvent includes any one or a combination of at least two of water, ethanol, ethylene glycol or isopropanol.
3. The preparation method according to claim 2, characterized in that, The preparation method of the metal oxide support includes: mixing precursor salt and alkaline solution, and carrying out a hydrothermal reaction to obtain the metal oxide support; And / or, the precursor salt includes tetrabutyl titanate and / or cerium nitrate hexahydrate; And / or, the alkaline solution includes any one or a combination of at least two of sodium hydroxide solution, sodium carbonate solution, or sodium bicarbonate solution; And / or, the temperature of the hydrothermal reaction is 100℃~200℃, and the time of the hydrothermal reaction is 12h~24h.
4. The method of claim 1, wherein, In the calcination atmosphere, the volume fraction of hydrogen in the nitrogen-hydrogen mixture is 10 vol.% to 100 vol.%, but not 100 vol.%. And / or, the calcination temperature is 200℃~1000℃, the calcination time is 1h~6h, and the calcination heating rate is 2℃ / min~10℃ / min.
5. The preparation method according to claim 1, characterized in that, The mixing temperature is 10℃~40℃, and the mixing time is 20min~40min; And / or, the mixing is performed under ultrasonic conditions; And / or, the temperature of the impregnation treatment is 10℃~40℃, and the time of the impregnation treatment is 4h~8h; And / or, the impregnation treatment is carried out under stirring conditions; And / or, the atmosphere for the hydrogen reduction treatment includes hydrogen or a nitrogen-hydrogen mixture; And / or, in the atmosphere of the hydrogen reduction treatment, the volume fraction of hydrogen in the nitrogen-hydrogen mixture is 10 vol.% to 100 vol.%, but not 100 vol.%. And / or, the hydrogen reduction treatment time is 0.5h to 5h.
6. The method of claim 1, wherein, The preparation method includes the following steps: (1) Mix the precursor salt and alkaline solution and carry out a hydrothermal reaction at 100℃~200℃ for 12h~24h to obtain the metal oxide support; calcine the metal oxide support in an atmosphere of hydrogen or nitrogen-hydrogen mixture at a heating rate of 2℃ / min~10℃ / min to 200℃~1000℃ for 1h~6h to obtain a metal oxide support containing oxygen vacancies. (2) The metal component precursor, solvent and the metal oxide support containing oxygen vacancies are mixed under ultrasonic conditions at 10℃~40℃ for 20min~40min; then impregnated under stirring conditions at 10℃~40℃ for 4h~8h; finally, hydrogen reduction treatment is carried out at 10℃~40℃ for 0.5h~5h in an atmosphere of hydrogen or nitrogen-hydrogen mixture to obtain the metal-defect dual active site hydrogenation catalyst.
7. A metal-defect dual-active-site hydrogenation catalyst, characterized in that, The metal-defect dual-active-site hydrogenation catalyst is prepared by the preparation method according to any one of claims 1 to 6; The metal-defect dual-active-site hydrogenation catalyst comprises a metal oxide support containing oxygen vacancies and a metal component supported on the surface of the metal oxide support containing oxygen vacancies. The metal components exist in the form of fully exposed metal clusters and single atoms.
8. A metal-defect dual-active-site hydrogenation catalyst as described in claim 7, characterized in that, Based on the total mass of the metal-defect dual-active-site hydrogenation catalyst being 100%, the loading of the metal component is 0.5% to 3%; And / or, in the metal component, the average particle size of the metal clusters is 0.5 nm to 5 nm.
9. The application of a metal-defect dual-active-site hydrogenation catalyst as described in claim 7 or 8, characterized in that, The metal-defect dual-active-site hydrogenation catalyst is applied to the hydrogenation reaction of nitroaromatics.
10. An application as described in claim 9, characterized in that, The nitroaromatic hydrocarbon includes any one or a combination of at least two of nitrobenzene, p-nitrophenol, or 2,4-dinitrotoluene; And / or, in the hydrogenation reaction of the nitroaromatic hydrocarbon, the reaction temperature is 10℃~40℃; And / or, in the hydrogenation reaction of the nitroaromatic hydrocarbon, the pressure of hydrogen gas is in the range of 0.1 MPa to 1.5 MPa; And / or, in the hydrogenation reaction of the nitroaromatic hydrocarbon, the mass of the metal-defect dual-active-site hydrogenation catalyst is 2% to 6% of the mass of the nitroaromatic hydrocarbon.
Citation Information
Patent Citations
Titanium dioxide supported ruthenium metal catalyst as well as preparation method and application thereof
CN115282956A
Palladium-based catalyst for catalytic hydrogenation of nitroaromatic compound as well as preparation method and application of palladium-based catalyst