A method and apparatus for the co-recovery of valuable metals by magnetohydrodynamic vortex enhancement in copper slag, including aggregation and sedimentation, and lead-zinc co-recovery.
By applying current and magnetic field to the copper slag melt to form a magnetohydrodynamic vortex flow field, combined with multi-stage condensation, the problem of high residual valuable metals in copper slag is solved, realizing efficient lead-zinc co-recovery and resource utilization of copper slag.
Patent Information
- Application Number
- CN202611191394.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-07
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2046-08-07
AI Technical Summary
Existing copper slag depletion technologies suffer from problems such as high residual value of metal elements, long depletion time, high energy consumption, and complex flue gas treatment, making it difficult to achieve efficient recycling.
By introducing an electric current and applying a magnetic field into the copper slag melt, a magnetohydrodynamic vortex flow field is formed, which promotes the sedimentation and volatilization of valuable metal components. By combining the coupling of multi-mode magnetic field and current, the aggregation and sedimentation of valuable metals are achieved, and lead and zinc components are recovered using a multi-stage condensation device.
It improved the recovery rate of valuable metals, reduced the content of valuable metals in tailings, realized the reduction and resource utilization of copper slag, and improved the volatilization recovery efficiency of lead and zinc.
Smart Images

Figure CN122727552B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metallurgical technology, and in particular to a method and apparatus for the co-recovery of valuable metals by strengthening the aggregation and sedimentation of copper slag using magnetohydrodynamic vortex. Background Technology
[0002] Copper slag is a solid waste generated during the pyrometallurgical smelting of copper, characterized by its large output, large storage area, and high environmental risk. Copper slag contains various valuable metals such as copper, iron, lead, zinc, cobalt, nickel, gold, and silver, possessing high resource utilization value. With increasingly stringent requirements for the comprehensive utilization of mineral resources and stricter environmental policies in my country, achieving efficient recovery of valuable metals from copper slag has become an important direction in the field of metallurgical solid waste resource utilization. Technologies for recovering valuable metals from copper slag mainly include pyrometallurgical depletion and hydrometallurgical extraction. Pyrometallurgical depletion is a mature process with a large processing capacity, capable of enriching and separating valuable metals such as copper and iron under high-temperature molten conditions, but it suffers from high energy consumption, high flue gas treatment pressure, and relatively low separation efficiency. Hydrometallurgical extraction can selectively leach valuable metals at lower temperatures, but it has drawbacks such as high reagent consumption, long process flow, and complex wastewater and waste residue treatment.
[0003] Domestic researchers have conducted extensive research on the comprehensive utilization of copper slag. For example, Wei Yonggang et al. invented "A method for low-carbon deep depletion of copper slag, application number CN202210122753.4". The copper slag depletion method includes the following steps: molten copper slag produced by copper pyrometallurgy is directly introduced into a reduction depletion furnace and heated to a specified temperature. Biomass carbon and slag-forming agent are added to the copper slag in a certain proportion and kept at a specified temperature for a certain time, so that the copper and iron oxides in the copper slag are fully reduced to metallic copper and iron to form a copper-iron alloy. After the metal phase in the slag aggregates and settles, it separates from the slag phase. The upper layer is molten slag, and the lower layer of molten metal is discharged from the bottom of the reduction depletion furnace to obtain the copper-iron alloy.
[0004] Wu Long et al. invented "A method for copper slag depletion, application number CN202111455979.8". This method adds a tubular smelting device between the copper smelting equipment and the storage tank. The liquid copper slag is slowly flowed down by gravity. Oxidizing gas and reducing gas are blown into the bottom of the tubular smelting device. A gas burner is added to the top of the device to heat the copper slag. A powder injection device can be added to the top to inject carbon powder into the fluid and control the reduction conditions of valuable metals.
[0005] The invention of Zhang Ting'an et al., “A method for preparing copper-chromium wear-resistant cast iron by reduction of molten depleted copper slag, application number CN201910391175.2”, includes the following steps: (1) depleting molten copper slag at a temperature of 1200-1250℃; discharging the remaining slag from the matte as raw material melt; or using the depleted molten copper slag as raw material melt; (2) heating to 1400-1450℃, stirring with a stirring paddle to form a molten pool with centrifugal vortex in the reduction furnace; (3) blowing a reducing agent to carry out eddy current reduction smelting; discharging the slag; (4) adding ferrochrome alloy for tempering smelting, casting, and obtaining copper-chromium wear-resistant cast iron.
[0006] Although the above methods can deplete copper slag, they still have problems such as a high content of valuable metal elements in the depleted copper slag and a long depletion time. Summary of the Invention
[0007] The purpose of this invention is to provide a method and apparatus for enhancing the aggregation and sedimentation of valuable metals in copper slag using magnetohydrodynamic vortex and for the co-recovery of lead and zinc, thereby reducing the content of valuable metals in depleted slag and improving the recovery rate of valuable metals.
[0008] The objective of this invention can be achieved through the following technical solution: a method for the co-recovery of valuable metals by magnetohydrodynamic vortex enhancement in copper slag, including the following steps: S1: Current is passed into the copper slag melt in the molten pool and a magnetic field is applied. The Lorentz force generated by the coupling of the current and the magnetic field has a component force that promotes the flow of the copper slag melt. A magnetohydrodynamic vortex flow field is formed in the copper slag melt. The valuable metal components in the copper slag melt settle and form a bottom valuable metal enriched phase. The lead and zinc components volatilize to form lead and zinc flue gas. S2: Collect the bottom valuable metal enriched phase and tailings separately, and perform staged condensation on the lead-zinc-containing flue gas generated during the treatment process to obtain lead-enriched products and zinc-enriched products.
[0009] Preferably, in step S1, the solid copper slag is pretreated and then heated and melted, or the hot copper slag is directly introduced into the molten pool to form a conductive copper slag melt.
[0010] More preferably, the particle size of the solid copper slag after crushing, screening and drying pretreatment is 80-200 mesh, and the melting temperature of the copper slag is 1200-1400℃; or the temperature of the hot copper slag when it is introduced into the molten pool is 1200-1400℃.
[0011] More preferably, the copper slag is derived from slag produced during flash smelting, oxygen-enriched bottom-blown smelting, side-blown smelting, converter blowing, or depletion treatment; wherein the typical ranges of Cu, Fe, Pb, and Zn by mass fraction are 1%–5%, 35%–50%, 0.5%–3%, and 3%–10%, respectively, and the typical contents of Au and Ag are 0.1–2 g / t and 20–150 g / t, respectively, and may contain one or more associated elements of Co and Ni.
[0012] Preferably, the temperature of the copper slag melt in step S1 is maintained at 1100-1400℃ during the treatment process, and the treatment time is 10-120 min.
[0013] More preferably, the temperature of the copper slag melt in step S1 is maintained at 1200-1350℃ during the treatment process, and the treatment time is 30-120 min.
[0014] Preferably, additives are added to the copper slag melt in step S1 to adjust the viscosity, alkalinity and fluidity of the slag phase.
[0015] More preferably, the additive includes one or more of calcium oxide, limestone, silicon dioxide, and calcium-containing composite flux.
[0016] More preferably, the amount of the additive added is 1% to 15% of the mass of the copper slag.
[0017] In this invention, the additives are used to reduce the viscosity of the slag phase, adjust the basicity of the slag phase, and improve the aggregation and settling conditions of valuable metal components.
[0018] Preferably, the valuable metal component includes one or more of the following: copper-containing metal phase, copper matte phase, iron-containing metal phase, copper-iron alloy phase, and associated phases containing nickel, cobalt, gold, or silver.
[0019] More preferably, the valuable metal component includes copper and iron.
[0020] Preferably, the lead-zinc-containing flue gas passes through at least two condensation zones in sequence, wherein the temperature of the first condensation zone is 800-1000℃ and is used to capture lead-enriched products; the temperature of the second condensation zone is 400-600℃ and is used to capture zinc-enriched products.
[0021] More preferably, the lead-zinc-containing flue gas passes through three condensation zones in sequence, wherein the third condensation zone is a terminal collection zone with a temperature not exceeding 100°C, used to collect residual dust that was not condensed in the first two stages.
[0022] More preferably, the three-stage condensation zones are connected in series along the flue gas flow direction and each is equipped with an independent temperature detection and control unit; the first-stage condensation zone adopts a high-temperature heat preservation condensation section, the second-stage condensation zone adopts a medium-temperature condensation section, and the third-stage condensation zone adopts a filtration and collection section after natural cooling or water cooling. The condensation products of each stage are collected, weighed, and subjected to component analysis.
[0023] In this invention, the lead volatilization recovery rate and zinc volatilization recovery rate are calculated as the ratio of the recovery amount of the corresponding elements in each stage of condensation products and residual dust to the total amount of the corresponding elements in the original copper slag.
[0024] Preferably, the magnetic field described in step S1 is a multi-mode magnetic field.
[0025] Preferably, step S1 specifically includes the following steps: S11: Current is passed into the copper slag melt in the molten pool and a first magnetic field is applied through the multi-mode magnetic field generating component. The Lorentz force generated by the coupling of the current and the first magnetic field has a component force that promotes the flow of the copper slag melt. A magnetohydrodynamic vortex flow field is formed in the copper slag melt, which promotes the collision, aggregation and enrichment of valuable metal components dispersed in the copper slag melt, and enhances the volatilization of lead and zinc components from the interior of the copper slag melt to the gas-liquid interface. S12: Switch the multi-mode magnetic field generating component to apply the second magnetic field, and simultaneously reduce the current intensity and magnetic field intensity to weaken the circumferential flow and shearing in the copper slag melt, forming a low-flow-rate sedimentation and enrichment area in the lower part of the molten pool, so that the aggregated valuable metal components settle under the action of density difference and form a bottom valuable metal enriched phase. The magnetic induction intensity of the second magnetic field and the magnetic field gradient formed in the sedimentation enrichment region are both smaller than those of the first magnetic field.
[0026] In this invention, a magnetic field with adjustable direction, intensity, gradient, effective area, and excitation timing is applied to the copper slag melt through a multi-mode magnetic field generating component, so that the current and magnetic field are coupled to generate Lorentz force.
[0027] In this invention, step S11 involves controlling the multi-mode magnetic field generating component to operate in a first magnetic field mode. The first magnetic field is preferably a composite magnetic field with a radial magnetic induction intensity component, primarily acting on the vortex-promoting region in the upper part of the molten pool. The first magnetic field couples with a composite current having axial and radial components, generating a large circumferential Lorentz force component and a Lorentz force component that promotes radial or axial circulation of the melt. This causes the copper slag melt to form rotating flow, radial circulating flow, vertical circulating flow, or a combination thereof, thereby enhancing the mixing of the copper slag melt with additives, promoting the collision, aggregation, and enrichment of valuable metal components such as copper, and strengthening the mass transfer and volatilization of lead and zinc components from the melt interior to the gas-liquid interface. Step S12 switches the multi-mode magnetic field generating component to the second magnetic field mode and simultaneously reduces the current intensity and magnetic field intensity. The second magnetic field is preferably a composite magnetic field with a dominant axial magnetic induction intensity component and a low magnetic induction intensity. The radial magnetic induction intensity component, the magnetic field gradient at the bottom of the molten pool, and the corresponding circumferential Lorentz force component in the second magnetic field mode are all smaller than those in the first magnetic field mode, thereby weakening the circumferential flow and shearing of the melt and forming a low-velocity, low-shear sedimentation enrichment region at the bottom of the molten pool, so that the aggregated valuable metal components settle stably under the action of density difference.
[0028] In this invention, the first magnetic field mode is used to form a flow field with a large circumferential velocity or strong circulating flow in the vortex agglomeration region, and to promote the volatilization and mass transfer of lead and zinc; the second magnetic field mode forms a low velocity and low shear flow field in the sedimentation enrichment region by reducing the radial magnetic induction intensity component and the corresponding circumferential Lorentz force component, and by reducing the current intensity and magnetic field intensity.
[0029] More preferably, the first magnetic field and the second magnetic field include at least one of an axial magnetic field, a radial magnetic field, a transverse magnetic field, an inclined magnetic field, a rotating magnetic field, and a composite magnetic field formed by superimposing at least two of them.
[0030] More preferably, at least two of the magnetic field direction, magnetic field strength, magnetic field gradient, magnetic field area of action, and excitation timing of the first magnetic field and the second magnetic field are different.
[0031] More preferably, the first magnetic field is a composite magnetic field with a radial magnetic induction intensity component, which mainly covers the upper part of the molten pool and has a large magnetic induction intensity and magnetic field gradient; the second magnetic field is a composite magnetic field with an axial magnetic induction intensity component as the main component and a low magnetic induction intensity, whose radial magnetic induction intensity component and the circumferential Lorentz force component generated under the corresponding current conditions are both smaller than the first magnetic field mode, and the magnetic field mainly acts on the upper part or the periphery of the molten pool, and forms a sedimentation enrichment area with a small magnetic field intensity and Lorentz force in the lower part of the molten pool.
[0032] More preferably, steps S11 and S12 are both performed under inert gas protection, a weakly reducing atmosphere, or an atmosphere with controllable oxygen potential, with the oxygen partial pressure controlled at 10. -10 ~10 -4 Pa.
[0033] Preferably, the current intensity in step S1 is 150 to 350 A.
[0034] Preferably, the magnetic induction intensity of the magnetic field in step S1 is 1.0 to 20 T.
[0035] In this invention, step S2 discharges and collects the bottom valuable metal enriched phase and the upper tailings, respectively, and performs graded condensation and capture on the lead-zinc-containing flue gas generated during the treatment process to obtain lead-enriched products, zinc-enriched products and residual dust, thereby achieving the synergistic recovery of valuable metal components and lead-zinc components in copper slag.
[0036] A device for the magnetohydrodynamic vortex-enhanced aggregation and sedimentation of valuable metals in copper slag and the co-recovery of lead and zinc, used to implement the above method, comprising: A melt processing furnace for carrying copper slag melt is provided with a copper slag inlet, a tail slag outlet, a valuable metal enriched phase outlet and a flue gas outlet, and the copper slag melt is placed in the molten pool of the melt processing furnace body. Heating components used to heat copper slag to a molten state and maintain the temperature of the molten copper slag; An electrode assembly for generating an electric current in a copper slag melt includes a first electrode and a second electrode connected to a DC power supply assembly. A multi-mode magnetic field generating component for applying a magnetic field to copper slag melt includes at least two independently adjustable electromagnet units. By changing the on / off state, excitation current direction, and excitation current intensity of each electromagnet unit, at least two magnetic field modes with different magnetic field directions, magnetic field intensities, or magnetic field spatial distributions can be selectively formed. The control component is connected to the DC power supply component and the multi-mode magnetic field generating component respectively, and is used to control the current flowing into the copper slag molten material, and to control the formation and switching of different magnetic field modes; Atmosphere control components are used to regulate the reaction atmosphere inside the melt processing furnace; The flue gas condensation and collection assembly is connected to the flue gas outlet and includes a high-temperature heat preservation condensation section, a medium-temperature condensation section and an end-of-line filtration and collection section connected in series along the flue gas flow direction. These sections are used to collect lead-enriched products, zinc-enriched products and residual dust, respectively.
[0037] Preferably, the magnetic field directions of the at least two electromagnet units are arranged parallel, intersecting or orthogonal to each other, and each electromagnet unit is connected to an independent excitation power supply to form an axial magnetic field, a radial magnetic field, a transverse magnetic field, an inclined magnetic field, a rotating magnetic field or a composite magnetic field.
[0038] Preferably, the first electrode extends into the copper slag melt from the top of the melt treatment furnace at a position offset from the center line of the furnace body, and the second electrode is set at the bottom or side wall of the melt treatment furnace, and the horizontal projections of the two electrodes do not overlap.
[0039] Preferably, the first and second electrodes are arranged in a non-aligned staggered manner to form a composite current with both axial and radial components in the copper slag melt. This composite current can be coupled with radial, axial, or composite magnetic fields respectively to obtain circumferential, radial, or axial Lorentz force components, thereby improving the tunability of different magnetohydrodynamic flow field modes.
[0040] More preferably, the horizontal misalignment distance between the first electrode and the second electrode is 10% to 30% of the inner diameter of the molten pool.
[0041] Preferably, the molten pool of the melt processing furnace includes a vortex agglomeration region and a sedimentation enrichment region from top to bottom. The two regions are not separated by a solid partition, but are dynamically formed by the spatial differences in the range of magnetic field action, Lorentz force intensity and melt flow rate.
[0042] More preferably, the vortex agglomeration region is the upper 2 / 3 of the molten pool, and the sedimentation enrichment region is the lower 1 / 3 of the molten pool.
[0043] In this invention, under the first magnetic field mode, the multi-mode magnetic field generating component makes the Lorentz force intensity in the vortex agglomeration region greater than the Lorentz force intensity in the sedimentation enrichment region; under the second magnetic field mode, the current intensity and magnetic field intensity are reduced simultaneously, further reducing the flow velocity and shear strength in the sedimentation enrichment region.
[0044] In this invention, the first magnetic field mode and the second magnetic field mode are operated sequentially according to a preset time sequence, or switched according to the melt flow state, the aggregation state of valuable metal components and the volatilization state of lead and zinc.
[0045] Preferably, the control component is configured to execute the agglomeration control stage and the settling control stage sequentially according to a preset timing sequence; in the agglomeration control stage, a first magnetic field mode is formed to promote the rotation or circulation of the copper slag melt; in the settling control stage, the control component switches to a second magnetic field mode and simultaneously reduces the magnetic field strength and current strength; according to the adjustment needs of the magnetic field spatial distribution, the excitation of some electromagnet units used to form the radial magnetic induction intensity component can be stopped or reduced to reduce the corresponding circumferential Lorentz force component.
[0046] Preferably, the atmosphere control component includes an air inlet pipe connected to the melt processing furnace.
[0047] Compared with the prior art, the present invention has the following technical advantages: 1) In this invention, the rotating or circulating flow formed by the coupling of current and the first magnetic field mode can improve the uniformity of the temperature field and composition field of the molten pool, strengthen the reaction between copper slag and additives, reduce the viscosity of slag phase, and reduce insufficient depletion caused by local temperature or composition inhomogeneity.
[0048] 2) This invention can achieve phased control of the melt flow field without mechanical stirring, improve the separation efficiency of valuable metals and the recovery rate of lead and zinc volatilization, reduce the residual valuable metals in the tailings, and realize the reduction, harmlessness and resource utilization of copper slag.
[0049] 3) This invention utilizes a multi-modal magnetic field with adjustable direction, intensity, gradient, and timing of action to couple with melt current, constructing different magnetohydrodynamic flow fields according to different processing stages, thereby achieving phased control of melt mixing, droplet coalescence, lead-zinc volatilization mass transfer, and valuable metal sedimentation processes, solving the problem that a single fixed flow field cannot simultaneously achieve both enhanced mixing and stable sedimentation.
[0050] 4) The magnetohydrodynamic vortex flow field of the present invention can increase the collision probability between dispersed valuable metal droplets or particles, and promote the agglomeration and growth of valuable metal components such as copper; by switching to the second magnetic field mode and simultaneously reducing the current intensity and magnetic field intensity, the shearing and re-entraining effect of the melt can be weakened, promoting the sedimentation and enrichment of the agglomerated valuable metal components to the bottom of the molten pool, and reducing the residual valuable metal in the tailings.
[0051] 5) The multimodal magnetohydrodynamic flow field of the present invention can continuously update the gas-liquid interface of the melt, shorten the mass transfer distance of lead and zinc components from the interior of the melt to the surface, and improve the volatilization and removal efficiency of lead and zinc; combined with a multi-stage gradient condensation device, lead-enriched products and zinc-enriched products can be obtained respectively.
[0052] 6) This invention eliminates the need to place the mechanical stirring components in a high-temperature corrosive melt for extended periods, thereby reducing mechanical wear and equipment maintenance costs. Furthermore, it can adapt to the treatment of copper slag with different compositions, phases, and temperature conditions by adjusting the operating modes of the current and magnetic field.
[0053] 7) This invention achieves the synergistic recovery of valuable metal components such as copper and lead-zinc components in copper slag, which is beneficial to reducing the valuable metal content in tailings and realizing the reduction, harmlessness and high-value resource utilization of copper slag.
[0054] 8) Under the specific implementation conditions of this invention, the copper content in the treated tailings is not higher than 0.35 wt%, the copper recovery rate is not lower than 95%, the lead volatilization recovery rate is not lower than 70%, the zinc volatilization recovery rate is not lower than 85%, and the valuable metal components such as copper are enriched and recovered in the enriched phase at the bottom of the molten pool. Attached Figure Description
[0055] Figure 1This is a schematic diagram of the structure of the copper slag magnetofluid vortex-enhanced valuable metal aggregation and sedimentation and lead-zinc co-recovery device of the present invention. In the diagram: 1-melt processing furnace, 11-copper slag inlet, 12-tail slag outlet, 13-valuable metal enriched phase outlet, 14-flue gas outlet, 2-heating assembly, 3-electrode assembly, 31-first electrode, 32-second electrode, 4-multimode magnetic field generating assembly, 5-control assembly, 6-temperature detection element, 7-insulation assembly, 8-air inlet pipe. Detailed Implementation
[0056] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments. These embodiments are based on the technical solution of the present invention and provide detailed implementation methods and specific operating procedures. However, the scope of protection of the present invention is not limited to the following embodiments.
[0057] Unless otherwise specified, the reagents, methods, instruments, and equipment used in this invention are conventional in the art. Unless otherwise specified, the reagents and materials used in the following examples are all commercially available.
[0058] The copper slag used in the following comparative examples and embodiments was taken from the depleted slag of copper pyrometallurgical furnace, wherein the mass fractions of Cu, Fe, Pb and Zn were 3.2 wt%, 44 wt%, 1.6 wt% and 7 wt%, respectively, and the contents of Au and Ag were 0.5 g / t and 83 g / t, respectively.
[0059] A device for the co-recovery of valuable metals by magnetohydrodynamic vortex enhancement in copper slag, involving aggregation and sedimentation, and co-recovery of lead and zinc, has the following structure: Figure 1 As shown, it includes: The system includes a multi-mode magnetic field generating component 4, a copper slag inlet 11, a temperature detection element 6, a first electrode 31, an air inlet pipe 8, a flue gas outlet 14, a tail slag outlet 12, a valuable metal enriched phase outlet 13, a heating component 2, a melt processing furnace 1, a second electrode 32, a heat preservation component 7, and a control component 5.
[0060] The furnace body of the melt processing furnace 1 is used to contain copper slag melt and is equipped with a heat preservation component 7. The furnace body is also equipped with a temperature detection element 6, a first electrode 31, an air inlet pipe 8, and a flue gas outlet 14. The detection end of the temperature detection element 6 extends into the furnace body to detect the temperature of the copper slag melt in real time. The air inlet pipe 8 is connected to the interior of the furnace body and is used to introduce inert gas, weak reducing gas, or process gas for controlling oxygen potential into the furnace. The flue gas outlet 14 is connected to the subsequent lead-zinc flue gas condensation and collection component to discharge the lead-zinc containing flue gas generated during the processing.
[0061] The side wall of the melt processing furnace 1 is provided with a copper slag inlet 11, a tail slag outlet 12, and a valuable metal enriched phase outlet 13. The copper slag inlet 11 is used to add solid pretreated copper slag into the furnace or to introduce hot copper slag; the tail slag outlet 12 is located above the valuable metal enriched phase outlet 13 and is used to discharge the treated upper tail slag; the valuable metal enriched phase outlet 13 is located near the bottom of the furnace and is used to discharge the copper-containing and other valuable metal enriched phase that has settled and accumulated at the bottom of the furnace.
[0062] Heating component 2 is installed on the furnace body to heat the copper slag to a molten state and maintain the processing temperature of the molten copper slag. Insulation component 7 is installed on the outside and top of the furnace body to reduce heat loss from the furnace body and maintain a stable temperature inside the furnace.
[0063] The first electrode 31 extends into the copper slag melt from the top of the furnace body, offset from the centerline. The second electrode 32 is located at the bottom of the furnace body and contacts the copper slag melt. The horizontal projections of the first electrode 31 and the second electrode 32 do not coincide. Preferably, the horizontal misalignment distance between the two electrodes is 10% to 30% of the inner diameter of the molten pool; the following embodiment uses an offset distance of approximately 20%. This non-directly aligned arrangement allows the current to have both axial and radial components as it flows from the first electrode 31 to the second electrode 32, facilitating coupling with magnetic fields in different directions and forming a circumferential Lorentz force component as well as a Lorentz force component that promotes radial or axial circulation of the melt. The first electrode 31 and the second electrode 32 are electrically connected to an external DC power supply assembly, and their polarities can be determined or switched according to process requirements to adjust the current direction and current distribution in the copper slag melt.
[0064] The multimodal magnetic field generating component 4 is located on the outside of the furnace body and includes at least two sets of electromagnet units arranged opposite each other. The control component 5 is electrically connected to the multimodal magnetic field generating component 4 and is used to adjust the on / off state of each electromagnet unit, the direction of the excitation current, the intensity of the excitation current, and the timing of the excitation action, so that the multimodal magnetic field generating component 4 can selectively generate magnetic field working modes with different directions, intensities, gradients, and action methods.
[0065] After the first electrode 31 and the second electrode 32 introduce a composite current into the copper slag melt, the composite current couples with the magnetic field generated by the multi-mode magnetic field generating component 4, causing the conductive copper slag melt to be subjected to a Lorentz force. By adjusting the direction, intensity, gradient, area of action, and excitation timing of the magnetic field through the control component 5, the direction and magnitude of the Lorentz force can be changed, thereby forming different magnetohydrodynamic flow states in the copper slag melt. Figure 1 The rotating arrows in the diagram are used to indicate one type of vortex flow state and are not used to define the specific flow direction of the melt.
[0066] During the process, the molten pool dynamically forms a vortex agglomeration zone and a sedimentation enrichment zone from top to bottom. Based on the effective height of the molten pool, the vortex agglomeration zone is preferably located in the upper 2 / 3 of the range, and the sedimentation enrichment zone is preferably located in the lower 1 / 3 of the range. The two zones are not separated by solid partitions, but are formed by the coverage of the magnetic field, the intensity of the Lorentz force, and the difference in melt flow velocity.
[0067] During the polymerization stage, the control component 5 controls the multi-mode magnetic field generating component 4 to operate in the first magnetic field mode. The first magnetic field mode is preferably a composite magnetic field with a radial magnetic induction intensity component. The magnetic field mainly covers the vortex polymerization region in the upper part of the molten pool. This magnetic field couples with the composite current to generate a large circumferential Lorentz force component and a Lorentz force component that promotes radial or axial circulation of the melt. This causes the copper slag melt to form a rotating or circulating flow, enhances the heat and mass transfer inside the melt and the mixing reaction between the copper slag and the additives, increases the collision frequency between dispersed valuable metal droplets or particles, promotes the aggregation and growth of valuable metal components such as copper, and enhances the migration and volatilization of lead and zinc components from the interior of the melt to the gas-liquid interface.
[0068] During the settling stage, control component 5 controls the multi-mode magnetic field generating component 4 to switch to the second magnetic field mode, and simultaneously reduces the current intensity and magnetic field intensity. The second magnetic field mode is preferably a composite magnetic field with a dominant axial magnetic induction intensity component and a relatively low magnetic induction intensity. By stopping or reducing the excitation current of part of the electromagnet unit used to generate the radial magnetic induction intensity component, the radial magnetic induction intensity component, the magnetic field gradient at the bottom of the molten pool, and the corresponding circumferential Lorentz force component in the second magnetic field mode are reduced, thereby reducing the circumferential flow velocity and flow shear intensity at the bottom of the molten pool, forming a low-velocity settling and enrichment region. This allows the aggregated valuable metal components to settle stably to the bottom of the furnace under the action of density difference and form a valuable metal enriched phase. After the treatment is completed, the bottom enriched phase is discharged through the valuable metal enriched phase outlet 13, the upper tailings are discharged through the tailings outlet 12, and the lead-zinc containing flue gas is transported to the subsequent flue gas condensation and collection component through the flue gas outlet 14.
[0069] The specific number, installation position, and magnetic field combination of the multi-mode magnetic field generating components 4 can be adjusted according to the size of the furnace body, the physical properties of the copper slag melt, and the processing target. As long as the control component 5 can form at least two magnetic field working modes with different magnetic field directions, magnetic field strengths, magnetic field distributions, or excitation timings, it belongs to the multi-mode magnetic field generating components 4 described in this invention.
[0070] The flue gas condensation and collection assembly comprises a first-stage high-temperature insulated condensation section, a second-stage medium-temperature condensation section, and a third-stage end-of-line filtration and collection section connected in series along the flue gas flow direction. The first-stage high-temperature insulated condensation section is equipped with independent heating and insulation devices, with the temperature controlled at 800–1000℃; the second-stage medium-temperature condensation section is equipped with independent temperature control and cooling devices, with the temperature controlled at 400–600℃; the third-stage end-of-line filtration and collection section is located after the flue gas has been naturally cooled or water-cooled, with an inlet temperature not exceeding 100℃.
[0071] The first-stage high-temperature condensation section, the second-stage medium-temperature condensation section, and the third-stage terminal filtration and collection section are each equipped with detachable collection containers or dust collection components to collect lead-enriched products, zinc-enriched products, and residual dust, respectively. After treatment, the products at each stage are weighed and the Pb and Zn contents are determined, and the lead volatilization recovery rate and zinc volatilization recovery rate are calculated accordingly.
[0072] The following detailed description is based on specific embodiments.
[0073] Comparative Example 1 (No current, no magnetic field, no additives) 1. Weigh 20 kg of copper slag material that has been crushed, screened and dried, and load it into the furnace body of melt processing furnace 1. Seal the furnace body and check the airtightness of the device.
[0074] 2. Turn on heating component 2 and raise the furnace temperature to 1300℃ at a heating rate of 10℃ / min to completely melt the copper slag material into copper slag melt, and hold the temperature for 10 minutes to allow the melt temperature to stabilize.
[0075] 3. Maintain the temperature of the copper slag melt at 1250℃, do not pass current to the first electrode 31 and the second electrode 32, do not start the multimode magnetic field generating component 4, and do not add additives. Let it stand for 60 minutes to allow the dispersed valuable metal droplets or particles in the copper slag melt to naturally aggregate and settle under the action of density difference.
[0076] 4. After treatment, heating is stopped. The valuable metal enriched phase formed at the bottom of the furnace is first discharged through the valuable metal enriched phase outlet 13, and then the upper tailings are discharged through the tailings outlet 12. The tailings are sampled and tested after cooling. The lead- and zinc-containing flue gas generated during the treatment process is sequentially introduced through the flue gas outlet 14 into the first-stage high-temperature heat preservation and condensation section at a temperature of 900±50℃, the second-stage medium-temperature condensation section at a temperature of 500±50℃, and the third-stage end-filter collection section with an inlet temperature not exceeding 100℃, to collect the lead enriched products, zinc enriched products, and residual dust, respectively. The products at each stage are weighed and subjected to Pb and Zn composition analysis.
[0077] The experimental results showed that the copper content in the tailings was 1.82 wt%, with a copper recovery rate of 43.13%; the lead volatilization recovery rate was 49.35%, and the zinc volatilization recovery rate was 58.72%. The agglomeration and sedimentation of fine valuable metal droplets in the copper slag melt were insufficient, and the tailings still contained a large amount of fine copper-containing components.
[0078] Comparative Example 2 (current applied, no magnetic field, no additives) 1. Weigh 20 kg of pretreated copper slag material and load it into the furnace body of melt treatment furnace 1. Seal the furnace body and check the airtightness of the device.
[0079] 2. High-purity argon gas is introduced into the furnace through inlet pipe 8 to replace the furnace atmosphere, and the oxygen partial pressure inside the furnace is controlled to 10. -6 Pa; turn on heating component 2 and raise the furnace temperature to 1300℃ at a heating rate of 10℃ / min to completely melt the copper slag material, and hold the temperature for 10 min.
[0080] 3. Maintain the temperature of the copper slag melt at 1250℃, turn on the DC power supply component, and pass a DC current of 250 A into the copper slag melt through the first electrode 31 and the second electrode 32; do not start the multimode magnetic field generating component 4, do not add any additives, and keep it at the temperature for 60 min.
[0081] 4. After treatment, power supply and heating are stopped. The bottom valuable metal enriched phase is collected through the valuable metal enriched phase outlet 13, and the upper tailings are discharged through the tailings outlet 12. The lead-zinc containing flue gas is treated under the three-stage gradient condensation conditions described in Comparative Example 1, and the lead enrichment product, zinc enrichment product, and residual dust are collected respectively.
[0082] The experimental results showed that the copper content in the tailings was 1.15 wt%, with a copper recovery rate of 64.06%; the lead volatilization recovery rate was 52.68%, and the zinc volatilization recovery rate was 61.29%. The Joule heating generated by the current improved the local temperature distribution of the melt, and the aggregation and sedimentation effect of valuable metal components was better than that of Comparative Example 1, but there was still obvious entrainment of copper-containing components in the tailings.
[0083] Example 1 (Current coupled with first magnetic field mode, no additives) 1. Weigh 20 kg of pretreated copper slag material and load it into the furnace body of melt treatment furnace 1. Seal the furnace body and check the airtightness of the device.
[0084] 2. High-purity argon gas is introduced into the furnace through inlet pipe 8 to replace the atmosphere inside the furnace, thereby controlling the oxygen partial pressure inside the furnace to 10. -6 Pa; turn on heating component 2 and raise the furnace temperature to 1300℃ at a heating rate of 10℃ / min to completely melt the copper slag material, and hold the temperature for 10 min.
[0085] 3. Maintain the temperature of the copper slag melt at 1250℃ and turn on the DC power supply component. The first electrode 31 and the second electrode 32 are arranged in a non-directly opposite manner with a horizontal offset distance of approximately 20% of the inner diameter of the molten pool. A DC current of 250 A is passed into the copper slag melt through the two electrodes, forming a composite current with both axial and radial components in the melt. Simultaneously, the multi-mode magnetic field generating component 4 is controlled by the control component 5 to operate in the first magnetic field mode, applying a composite magnetic field with a magnetic induction intensity of 10 T, having a radial magnetic induction intensity component, and mainly covering approximately 2 / 3 of the vortex agglomeration region in the upper part of the molten pool. This causes the composite current to couple with the first magnetic field, generating a circumferential Lorentz force component, forming a magnetohydrodynamic vortex flow field in the copper slag melt. The measured vortex rotation speed of the melt is approximately 500 r / min. No additives are added, and the temperature is maintained for 60 min.
[0086] 4. After treatment, power supply, excitation, and heating are stopped. The bottom valuable metal enriched phase is first discharged through the valuable metal enriched phase outlet 13, and then the upper tailings are discharged through the tailings outlet 12. The lead-zinc containing flue gas is treated under the three-stage gradient condensation conditions described in Comparative Example 1, and the lead enrichment product, zinc enrichment product, and residual flue dust are collected separately.
[0087] Experimental results show that the copper content in the tailings is 0.30 wt%, with a copper recovery rate of 91.00%; the lead volatilization recovery rate is 68.72%, and the zinc volatilization recovery rate is 82.36%. The magnetohydrodynamic vortex formed by the coupling of current and the first magnetic field mode improves the degree of melt mixing and temperature uniformity, promotes the collision and coalescence of dispersed copper-containing droplets, and improves the mass transfer efficiency of lead and zinc components from the melt interior to the gas-liquid interface.
[0088] Example 2 (Collateral treatment of current, first magnetic field mode and CaO additive) 1. Weigh 20 kg of pretreated copper slag material and load it into the furnace body of melt treatment furnace 1. Seal the furnace body and check the airtightness of the device.
[0089] 2. High-purity argon gas is introduced into the furnace through inlet pipe 8 to replace the atmosphere inside the furnace, thereby controlling the oxygen partial pressure inside the furnace to 10. -6 Pa; turn on heating component 2 and raise the furnace temperature to 1300℃ at a heating rate of 10℃ / min to completely melt the copper slag material, and hold the temperature for 10 min.
[0090] 3. Add CaO additive, accounting for 5% of the copper slag mass, to the copper slag melt. The first electrode 31 and the second electrode 32 are arranged in a non-directly opposite manner with a horizontal offset distance of approximately 20% of the inner diameter of the molten pool. Turn on the DC power supply component and the multi-mode magnetic field generator 4, and pass a DC current of 250 A into the copper slag melt through the two electrodes. A composite first magnetic field with a magnetic induction intensity of 10 T, having a radial magnetic induction intensity component, and mainly acting on the upper vortex agglomeration region of the molten pool, is applied through the control component 5. This magnetic field couples with the composite current to generate a circumferential Lorentz force component and form a magnetohydrodynamic vortex flow field. The copper slag melt and CaO additive are premixed for 5 minutes using the magnetohydrodynamic vortex to ensure uniform dispersion of the additive in the melt.
[0091] 4. Maintain the temperature of the copper slag melt at 1250℃, continue to maintain the current intensity of 250 A and the magnetic induction intensity of the first magnetic field mode at 10 T, so that the vortex rotation speed of the melt is stabilized at about 500 r / min, and hold for 60 min to promote the collision and aggregation of valuable metal components and enhance the volatilization mass transfer of lead and zinc components.
[0092] 5. After treatment, power supply, excitation, and heating are stopped. The bottom valuable metal enriched phase is first discharged through the valuable metal enriched phase outlet 13, and then the upper tailings are discharged through the tailings outlet 12. The lead-zinc containing flue gas is treated under the three-stage gradient condensation conditions described in Comparative Example 1, and the lead enrichment product, zinc enrichment product, and residual flue dust are collected separately.
[0093] The experimental results show that the copper content in the tailings is 0.22 wt%, with a copper recovery rate of 95.14%; the lead volatilization recovery rate is 73.56%, and the zinc volatilization recovery rate is 87.24%. CaO additives can adjust the slag phase composition and reduce slag viscosity. Combined with the mixing and agglomeration effects of magnetohydrodynamic vortices, this improves the coalescence and settling efficiency of valuable metal droplets and further enhances the volatilization recovery rate of lead and zinc components.
[0094] Example 3 (Multimodal Magnetic Field Staged Control Group) 1. Weigh 20 kg of pretreated copper slag material and load it evenly into the furnace body of melt treatment furnace 1. Seal the furnace body and check the airtightness of the device.
[0095] 2. High-purity argon gas is introduced into the furnace through inlet pipe 8 to replace the atmosphere inside the furnace, thereby controlling the oxygen partial pressure inside the furnace to 10. -6 Pa; turn on heating component 2 and raise the furnace temperature to 1300℃ at a heating rate of 10℃ / min, so that the copper slag material is completely melted to form copper slag melt, and hold the temperature for 10 min to stabilize the melt temperature.
[0096] 3. Add CaO additives, accounting for 5% of the copper slag mass, to the copper slag melt. The first electrode 31 and the second electrode 32 are arranged in a non-directly opposite staggered manner, with a horizontal offset distance of approximately 20% of the inner diameter of the molten pool. Turn on the DC power supply component and pass a DC current of 250 A into the copper slag melt through the first electrode 31 and the second electrode 32, so that the current in the copper slag melt has both axial and radial components. At the same time, the control component 5 controls the multi-mode magnetic field generating component 4 to operate in the first magnetic field mode. In the first magnetic field mode, the electromagnet units located at different positions in the furnace body are activated according to the first excitation combination, and the on / off state, excitation current direction, and excitation current intensity of each electromagnet unit are adjusted respectively to form a composite magnetic field containing a radial magnetic induction intensity component, with the magnetic induction intensity set to 10 T. The first magnetic field mainly covers the upper two-thirds of the vortex agglomeration region in the molten pool, and gradually weakens from this region to the lower part of the molten pool. This causes the composite current to couple with the first magnetic field to generate a large circumferential Lorentz force component and a Lorentz force component that promotes radial or axial circulation of the melt, forming a magnetohydrodynamic vortex flow field in the copper slag melt that combines rotating flow and circulating flow.
[0097] 4. The copper slag melt and CaO additive were premixed for 5 min using the first magnetic field mode to ensure uniform dispersion of the additive. Then, the temperature of the copper slag melt was maintained at 1250℃, the current intensity was maintained at 250 A and the magnetic induction intensity was maintained at 10 T, and the mixture was treated in the first magnetic field mode for 40 min to enhance melt mixing, promote the collision and aggregation of valuable metal droplets or particles containing copper, and enhance the mass transfer and volatilization of lead and zinc components from the melt interior to the gas-liquid interface.
[0098] 5. After the first stage of processing, the control component 5 switches each electromagnet unit from the first excitation combination to the second excitation combination, shuts down or reduces the excitation current of some electromagnet units used to enhance the radial magnetic induction intensity component, and adjusts the direction of the excitation current of the remaining electromagnet units. The multimode magnetic field generating component 4 is switched to the second magnetic field mode dominated by the axial magnetic induction intensity component. At the same time, the current intensity is reduced from 250 A to 150 A, and the magnetic induction intensity is reduced from 10 T to 2 T. Processing continues for 20 min. The second magnetic field mainly acts on the upper part and periphery of the molten pool. Its radial magnetic induction intensity component and the magnetic field gradient in the lower part of the molten pool are both smaller than those in the first magnetic field mode, which reduces the corresponding circumferential Lorentz force component and forms a low-velocity, low-shear sedimentation enrichment region in about 1 / 3 of the lower part of the molten pool. This reduces the breakage, redispersion, and re-entrainment of the aggregated valuable metal droplets, allowing the aggregated valuable metal components to settle stably to the bottom of the furnace under the action of density difference and form a valuable metal enriched phase.
[0099] In this embodiment, the first magnetic field mode and the second magnetic field mode differ not only in magnetic induction intensity but also in magnetic field direction, magnetic field gradient, main area of action, and excitation combination. The first magnetic field mode forms a composite magnetic field containing a radial magnetic induction intensity component through the first excitation combination, which couples with the composite current to generate a large circumferential Lorentz force component and a Lorentz force component that promotes melt circulation. This is mainly used to enhance melt rotation, circulation, and collision and coalescence of valuable metal components. The second magnetic field mode, by switching to the second excitation combination, reduces the radial magnetic induction intensity component, the magnetic field gradient at the bottom of the molten pool, and the corresponding circumferential Lorentz force component. This is mainly used to weaken melt shear and disturbance, providing stable settling conditions for the coalesced valuable metal components.
[0100] 6. After treatment, power supply, excitation, and heating are stopped. The bottom valuable metal enriched phase is first discharged through the valuable metal enriched phase outlet 13, and then the upper tailings are discharged through the tailings outlet 12. The lead-zinc containing flue gas is discharged through the flue gas outlet 14 and treated according to the three-stage gradient condensation conditions described in Comparative Example 1. The lead enriched product, zinc enriched product, and residual dust are collected separately.
[0101] The experimental results showed that the copper content in the tailings was 0.19 wt%, with a copper recovery rate of 97.26%; the lead volatilization recovery rate was 75.63%, and the zinc volatilization recovery rate was 89.12%. Compared with the continuous treatment method using the first magnetic field mode in Example 2, under the same total treatment time, this example enhanced the collisional aggregation of valuable metal components and the lead-zinc volatilization mass transfer using the first magnetic field mode, and switched to the second magnetic field mode in the later stage of treatment, reducing the current intensity and magnetic induction intensity. This resulted in a reduction of the copper content in the tailings from 0.22 wt% to 0.19 wt%, a relative reduction of approximately 13.64%; an increase in copper recovery rate from 95.14% to 97.26%, an increase of 2.12 percentage points; an increase in lead volatilization recovery rate from 73.56% to 75.63%, an increase of 2.07 percentage points; and an increase in zinc volatilization recovery rate from 87.24% to 89.12%, an increase of 1.88 percentage points. The above results indicate that multimodal magnetic field staged control can take into account melt mixing, droplet collision and aggregation, and lead-zinc volatilization mass transfer under strong flow field conditions in the early stage, as well as the stable sedimentation of valuable metal enriched phase under weak flow field conditions in the later stage. This reduces the breakage, redispersion, and re-entrainment of aggregated valuable metal droplets, thereby further reducing copper residue in tailings and improving the overall recovery effect of copper and lead-zinc components.
[0102] The above description of the embodiments is provided to enable those skilled in the art to understand and use the invention. It will be apparent to those skilled in the art that various modifications can be made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above embodiments, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the invention should be within the protection scope of the present invention.
Claims
1. A method for the magnetohydrodynamic vortex-enhanced aggregation and sedimentation of valuable metals in copper slag and the co-recovery of lead and zinc, characterized in that, Includes the following steps: S1: Current is passed into the copper slag melt in the molten pool and a magnetic field is applied. The Lorentz force generated by the coupling of the current and the magnetic field has a component force that promotes the flow of the copper slag melt. A magnetohydrodynamic vortex flow field is formed in the copper slag melt. The valuable metal components in the copper slag melt settle and form a bottom valuable metal enriched phase. The lead and zinc components volatilize to form lead and zinc flue gas. S2: Collect the bottom valuable metal enriched phase and tailings separately, and perform staged condensation on the lead-zinc-containing flue gas generated during the process to obtain lead-enriched products and zinc-enriched products. Additives are added to the copper slag melt in step S1 to adjust the viscosity, basicity and fluidity of the slag phase; The additives include one or more of calcium oxide, limestone, silicon dioxide, and calcium-containing composite flux; The amount of the additive added is 1% to 15% of the mass of the copper slag; Step S1 specifically includes the following steps: S11: Current is passed into the copper slag melt in the molten pool and a first magnetic field is applied through the multi-mode magnetic field generating component. The Lorentz force generated by the coupling of the current and the first magnetic field has a component force that promotes the flow of the copper slag melt. A magnetohydrodynamic vortex flow field is formed in the copper slag melt, which promotes the collision, aggregation and enrichment of valuable metal components dispersed in the copper slag melt, and enhances the volatilization of lead and zinc components from the interior of the copper slag melt to the gas-liquid interface. S12: Switch the multi-mode magnetic field generating component to apply the second magnetic field, and simultaneously reduce the current intensity and magnetic field intensity to weaken the circumferential flow and shearing in the copper slag melt, forming a low-flow-rate sedimentation and enrichment area in the lower part of the molten pool, so that the aggregated valuable metal components settle under the action of density difference and form a bottom valuable metal enriched phase. The magnetic induction intensity of the second magnetic field and the magnetic field gradient formed in the sedimentation enrichment region are both smaller than those of the first magnetic field; The first magnetic field and the second magnetic field include at least one of the following: axial magnetic field, radial magnetic field, transverse magnetic field, tilting magnetic field, rotating magnetic field, and a composite magnetic field formed by superposition of at least two of them; At least two of the following are different between the first and second magnetic fields: magnetic field direction, magnetic field strength, magnetic field gradient, magnetic field region of action, and excitation timing. The first magnetic field has a radial magnetic induction intensity component and mainly acts on the vortex agglomeration region in the upper part of the molten pool, causing it to couple with the melt current to generate a large circumferential Lorentz force component; the radial magnetic induction intensity component and the corresponding circumferential Lorentz force component in the second magnetic field mode are smaller than those in the first magnetic field mode, so that a low-velocity sedimentation and enrichment region is formed in the lower part of the molten pool. The method is implemented using a device for enhanced aggregation and sedimentation of valuable metals in copper slag magnetohydrodynamic vortex and co-recovery of lead and zinc. The device includes: The melt processing furnace (1) used to carry copper slag melt is provided with a copper slag inlet (11), a tail slag outlet (12), a valuable metal enriched phase outlet (13) and a flue gas outlet (14). The copper slag melt is placed in the molten pool of the furnace body of the melt processing furnace (1). The furnace body of the melt processing furnace (1) is used to contain copper slag melt, and it is equipped with heat preservation components (7). Heating components (2) are used to heat copper slag to a molten state and maintain the temperature of the copper slag melt. An electrode assembly (3) for generating current in copper slag melt includes a first electrode (31) and a second electrode (32) connected to a DC power supply assembly. The multi-mode magnetic field generating component (4) for applying a magnetic field to copper slag melt includes at least two independently adjustable electromagnet units. By changing the on / off state, excitation current direction and excitation current intensity of each electromagnet unit, at least two magnetic field modes with different magnetic field directions, magnetic field intensities or magnetic field spatial distributions can be selectively formed. The control component (5) is connected to the DC power supply component and the multi-mode magnetic field generating component (4) respectively, and is used to control the current flowing into the copper slag melt, and to control the formation and switching of different magnetic field modes; Atmosphere control components are used to regulate the reaction atmosphere inside the melt processing furnace (1); The flue gas condensation and collection assembly is connected to the flue gas outlet (14) and is used to perform graded condensation of lead- and zinc-containing flue gas and collect lead-enriched products and zinc-enriched products respectively. The magnetic field directions of the at least two electromagnet units are arranged parallel, intersecting or orthogonal to each other, and each electromagnet unit is connected to an independent excitation power supply to form an axial magnetic field, radial magnetic field, transverse magnetic field, tilting magnetic field, rotating magnetic field or composite magnetic field. The first electrode (31) extends into the copper slag melt from the top of the melt treatment furnace (1) at a position offset from the center line of the furnace body, and the second electrode (32) is set at the bottom or side wall of the melt treatment furnace (1), and the horizontal projections of the first electrode (31) and the second electrode (32) do not coincide. The first electrode (31) and the second electrode (32) form a composite current with both axial and radial components in the copper slag melt.
2. The method for enhanced aggregation and sedimentation of valuable metals in copper slag using magnetohydrodynamic vortex technology and for the co-recovery of lead and zinc according to claim 1, characterized in that, The valuable metal components include one or more of the following: copper-containing metal phase, copper-matte phase, iron-containing metal phase, copper-iron alloy phase, and associated phases containing nickel, cobalt, gold, or silver.
3. The method for enhanced aggregation and sedimentation of valuable metals in copper slag using magnetohydrodynamic vortex technology and for the co-recovery of lead and zinc according to claim 1, characterized in that... The lead- and zinc-containing flue gas passes through at least two condensation zones in sequence. The temperature of the first condensation zone is 800–1000°C, which is used to capture lead-enriched products. The temperature of the second condensation zone is 400–600°C, which is used to capture zinc-enriched products.
4. The method for enhanced aggregation and sedimentation of valuable metals in copper slag using magnetohydrodynamic vortex technology and for the co-recovery of lead and zinc according to claim 1, characterized in that... Steps S11 and S12 are both performed under inert gas protection, a weakly reducing atmosphere, or an atmosphere with controllable oxygen potential, with the oxygen partial pressure controlled at 10. -10 ~10 -4 Pa.
5. The method for enhanced aggregation and sedimentation of valuable metals in copper slag using magnetohydrodynamic vortex technology and for the co-recovery of lead and zinc according to claim 1, characterized in that... The temperature of the copper slag melt in step S1 is 1100-1400℃, and the processing time is 10-120 min; The current intensity in step S1 is 150–350 A; The magnetic induction intensity of the magnetic field in step S1 is 1.0 to 20 T.
6. The method for enhanced aggregation and sedimentation of valuable metals in copper slag using magnetohydrodynamic vortex technology and for the co-recovery of lead and zinc according to claim 1, characterized in that, The melt pool of the melt processing furnace (1) includes a vortex agglomeration region and a sedimentation enrichment region from top to bottom. The two regions are dynamically formed by the spatial distribution of the magnetic field and the flow velocity difference, and no solid partition is set. The multi-mode magnetic field generating component (4) makes the Lorentz force intensity in the vortex agglomeration region greater than the Lorentz force intensity in the sedimentation enrichment region in the first magnetic field mode, and simultaneously reduces the current intensity and magnetic field intensity in the second magnetic field mode to form a low-velocity, low-shear flow field in the sedimentation enrichment region.
Citation Information
Patent Citations
A method for preparing copper-chromium wear-resistant cast iron by reduction of molten, depleted copper slag
CN110004352B
A method for copper slag depletion
CN114150157B
Method for low-carbon deep dilution of copper slag
CN115011806A
Method for reducing and separating lead and zinc from lead smelting slag
CN122428132A