A mineral fire retardant powder based on endothermic decomposition synergy and its preparation method

By combining mineral groups A and B with staggered decomposition temperatures, and combining them with group C to catalyze char formation and smoke suppression, the problems of concentrated heat absorption and decomposition and loose residues in inorganic mineral fire retardant powder during fires are solved. This achieves continuous heat absorption and dense barrier properties over a wide temperature range, improves fire resistance and smoke suppression performance, and ensures the stability of the preparation process.

CN122772589BActive Publication Date: 2026-11-17LIAONING DIER IND CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611249212.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-08-18
Publication Date
2026-11-17
Estimated Expiration
2046-08-18

AI Technical Summary

Technical Problem

Existing inorganic mineral fire retardant powders absorb heat and decompose within a narrow temperature range during fires, losing their cooling effect. The decomposition residues are loose and difficult to form a continuous and dense barrier layer, resulting in insufficient flame retardant and smoke suppression properties. Furthermore, the preparation process is unstable.

Method used

A composite granule is prepared by using a group consisting of aluminum hydroxide, boehmite, hydromagnesia, and calcium magnesium carbonate, with staggered decomposition temperatures, combined with a group consisting of sepiolite, fluorophlogopite, and aluminum dihydrogen phosphate (Group B) to form a ceramic barrier layer, and adding a group consisting of zinc hydroxystannate, zinc molybdate, and zinc borate (Group C) to catalyze the formation of carbon for smoke suppression. The granules are then produced through in-situ deposition and spray drying.

Benefits of technology

It enables continuous heat absorption over a wide temperature range, forming a dense barrier layer that enhances fire resistance and smoke suppression while maintaining material stability during the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122772589B_ABST
    Figure CN122772589B_ABST
Patent Text Reader

Abstract

This invention discloses a mineral fire retardant powder based on endothermic decomposition synergy and its preparation method, belonging to the technical field of inorganic mineral fire retardant materials. The fire retardant powder of this invention consists of an endothermic decomposition group A, a ceramicized barrier group B, a catalytic charring and smoke suppression group C, and other components. Group A is composed of aluminum hydroxide, boehmite, magnesia, and calcium magnesium carbonate, whose decomposition temperature zones are staggered. In preparation, group A is first tightly graded, then zinc hydroxystannate is deposited in situ on the particle surface and a silanized layer is grafted onto it. After being mixed with group B and the remaining groups to form a slurry, it is spray-dried and granulated using a closed-loop control of the outlet gas temperature, and then sieved to obtain composite particles. When exposed to fire, the fire retardant powder of this invention continuously absorbs heat and cools down over a wide temperature range. The decomposed oxides are sintered into a dense ceramicized barrier layer via phosphate. Group C catalyzes the early formation of the barrier layer and suppresses smoke. The synergistic effects of each group are simultaneously exerted within the micro-regions of the particles, resulting in continuous thermal protection, dense barrier, and suppressed smoke.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of inorganic mineral fire-retardant materials, specifically relating to a mineral fire-retardant powder based on endothermic decomposition synergy and its preparation method. Background Technology

[0002] Fire-retardant materials are used to slow down the heating of substrates, inhibit the spread of flames, and reduce the release of smoke and toxic gases in fire-prone environments. They are widely used in building structures, industrial facilities, and marine engineering equipment where high fire protection requirements are necessary. Inorganic mineral fire-retardant powders are an important type of material. Their main components are mostly mineral fillers that undergo endothermic decomposition upon heating. During decomposition, they cool down by absorbing heat, release water vapor or carbon dioxide to dilute flammable gases, and leave residues on the substrate surface to slow heat transfer. To improve flame retardancy and smoke suppression performance, existing materials often incorporate metallic compound flame retardant synergists and char-forming smoke-suppressing agents, and these components are mixed and powdered using appropriate preparation processes.

[0003] However, existing inorganic mineral fire-retardant powders are mostly based on a single heat-absorbing filler. Their heat absorption and decomposition are concentrated in a narrow temperature range. Once the fire temperature rises beyond this range, they lose their continuous cooling effect and cannot provide stable thermal protection throughout the entire fire process. At the same time, the residues left after the decomposition of a single filler are mostly loose oxide powders with poor adhesion, making it difficult to form a continuous and dense heat-insulating barrier layer. When exposed to fire, the residues are prone to disintegration, and heat and oxygen can still be transferred to the substrate through the loose residues, resulting in insufficient heat insulation.

[0004] In existing materials, flame retardant synergists and char-forming aids are often added in a simple mixing manner, lacking spatial tightness with the endothermic filler and its decomposition products. This makes it difficult to apply the catalytic effect precisely to the areas where the residue sinters into a shell, resulting in the formation of a dense barrier layer lagging behind the peak heat release of the fire, and the flame retardant and smoke-suppressing potential not being fully realized. Furthermore, if the components are only mechanically blended, their distribution in the final product is uneven, making it difficult to ensure that each component works synergistically within the same small area when exposed to fire.

[0005] In the preparation process, the decomposition initiation temperature of endothermic mineral fillers is often low. If the temperature control during drying and granulation is inadequate, the filler will partially decompose before powdering, and its endothermic capacity will be consumed during the preparation stage, resulting in a decrease in the fire resistance of the finished product and instability between batches. The above problems indicate that the existing technology has shortcomings in terms of endothermic temperature coverage, barrier molding of residues, in-situ catalysis of synergistic components, and protection of endothermic capacity during the preparation process. It is necessary to design a mineral fire-retardant powder and its preparation method that allows endothermic processes to continue continuously over a wide temperature range, allows residues to be sintered into a dense barrier layer, allows synergistic components to be catalyzed nearby and pre-formed, and allows the preparation process to not damage the endothermic capacity. Summary of the Invention

[0006] To address the problems existing in the background art, this invention provides a mineral fire retardant powder based on endothermic decomposition synergy, which, by weight of raw materials, is composed of group A, group B, group C, and other components; wherein:

[0007] Group A consists of 20-35 parts aluminum hydroxide, 10-20 parts boehmite, 10-20 parts hydromagnesia, and 8-15 parts calcium magnesium carbonate.

[0008] Group B consists of 5-10 parts sepiolite, 4-8 parts fluorophlogopite, and 3-6 parts aluminum dihydrogen phosphate.

[0009] Group C consists of 1.5–4 parts zinc hydroxystannate, 1–3 parts zinc molybdate, and 1.5–3 parts zinc borate;

[0010] The other components consist of 3-8 parts expanded vermiculite, 0.5-2 parts 3-aminopropyltriethoxysilane, and 0.3-1 parts sodium hexametaphosphate;

[0011] The zinc hydroxystannate of group C is partially deposited on the particle surface of aluminum hydroxide, boehmite, hydromagnesia and calcium magnesium carbonate of group A, forming a zinc hydroxystannate deposition coating layer; the particle surface also has a silanized layer formed by the hydrolysis and condensation of 3-aminopropyltriethoxysilane of the other components.

[0012] In a preferred embodiment, the mineral fire retardant powder is a composite particle with a median particle size of 20–40 μm.

[0013] In the preferred embodiment, group A consists of 26-30 parts aluminum hydroxide, 13-17 parts boehmite, 12-16 parts hydromagnesia, and 9-13 parts calcium magnesium carbonate; group B consists of 6-8 parts sepiolite, 5-7 parts fluorophlogopite, and 3-5 parts aluminum dihydrogen phosphate; group C consists of 2-4 parts zinc hydroxystannate, 1.5-2.5 parts zinc molybdate, and 2-3 parts zinc borate; and the other components consist of 4-6 parts expanded vermiculite, 0.8-1.5 parts 3-aminopropyltriethoxysilane, and 0.4-0.6 parts sodium hexametaphosphate.

[0014] This invention also provides a method for preparing mineral fire-retardant powder based on endothermic decomposition synergy, comprising the following steps:

[0015] S1, crush and classify each component of group A into multiple particle sizes, determine the blending ratio of each particle size according to the target particle size distribution curve of continuous gradation that makes the particles compact, blend them, stir and mix until uniform, and obtain heat-absorbing mineral gradation powder.

[0016] S2, the heat-absorbing mineral grade powder is dispersed in water, sodium stannate and zinc sulfate are added to generate the zinc hydroxystannate deposition coating layer of group C on the particle surface in situ, and then 3-aminopropyltriethoxysilane of the other components is added to modify the particle surface, and the deposition-coated modified particles are obtained by filtration.

[0017] S3, disperse the components of group B in water, then add zinc molybdate and zinc borate of group C, expanded vermiculite and sodium hexametaphosphate of the other components, and the deposited coated modified particles, mix at below 25°C to obtain a slurry, and carry out S4 within 30 minutes after the slurry is mixed;

[0018] S4, the slurry is atomized and fed into a spray drying tower for drying and granulation. The temperature of the outlet gas of the spray drying tower is detected by a temperature sensor and fed back to the controller. The controller adjusts the slurry feed flow rate and hot air heating power according to the deviation between the outlet gas temperature and the set value, so that the outlet gas temperature is maintained within the set range that will not cause the decomposition of group A, and composite particles are obtained.

[0019] S5, the composite particles are sieved to obtain the mineral fireproof powder.

[0020] Furthermore, S1 includes:

[0021] S11, aluminum hydroxide, boehmite, hydromagnesia and calcium magnesium carbonate of group A are respectively subjected to air jet milling and air jet classification to obtain powders of multiple particle sizes;

[0022] S12, the volumetric particle size distribution of each particle size class was determined by laser diffraction particle size analysis to obtain the upper and lower limits of particle size for each particle size class;

[0023] S13, calculate the volume fraction of each particle size according to the target particle size distribution curve, then convert the volume fraction to the mass fraction according to the density of each particle size powder, and weigh the powder of the corresponding particle size according to the mass fraction.

[0024] S14, the weighed powders of each particle size are added to a mixer and stirred. The contents of aluminum hydroxide, boehmite, hydromagnesia and calcium magnesium carbonate in different sampling points of the mixer are determined by X-ray diffraction quantitative phase analysis. The coefficient of variation of the contents of the above four components at each sampling point is calculated. Mixing is stopped when the coefficient of variation is no greater than 5%, and the endothermic mineral graded powder is obtained.

[0025] Furthermore, in S13, the target particle size distribution curve is determined by the following formula:

[0026] ;

[0027] In the formula, For particles smaller than The cumulative volume fraction of particles in the heat-absorbing mineral graded powder; Particle size; The maximum particle size in the heat-absorbing mineral graded powder; The minimum particle size of the particles in the heat-absorbing mineral graded powder; The distribution modulus is taken as 0.21 to 0.30; the first division modulus is calculated using the following formula. Volume fraction at the particle size level:

[0028] ;

[0029] In the formula, For the first The volume fraction of each particle size in the heat-absorbing mineral powder; For the first Upper limit of particle size for each particle size class; For the first Lower limit of particle size for each particle size class; and The particle size calculated by the above formula is equal to and Cumulative volume fraction at time; The number represents the particle size, ranging from 1 to... , For the total number of particles, when When equal to 1 equal ,when equal hour equal ,and Greater than 0; convert the volume fraction to the first volume fraction using the following formula. Mass fraction per particle size:

[0030] ;

[0031] In the formula, For the first Mass fraction of each particle size; For the first Density of individual particle sizes; For the first Volume fraction of each particle size; for From 1 to The sum of the products of density and volume fraction of powder particles of each particle size; For the first Density of individual particle sizes; For the first Volume fraction of each particle size; The particle size index is used for summation; based on the mass fraction of each particle size. Weigh out the powder of the appropriate particle size.

[0032] Furthermore, S2 includes:

[0033] S21, the heat-absorbing mineral grade powder is dispersed in deionized water to obtain a suspension. Sodium stannate and zinc sulfate are added to the suspension at a molar ratio of tin to zinc of 1:1. The mixture is reacted for 0.5 to 3 hours at a pH of 7.0 to 9.0 and a temperature of 25 to 60°C to allow zinc hydroxystannate to be deposited in situ on the particle surface. The amount of sodium stannate and zinc sulfate added is calculated as the mass fraction of zinc hydroxystannate in group C based on the theoretical production of zinc hydroxystannate.

[0034] S22, add pre-hydrolyzed 3-aminopropyltriethoxysilane to the suspension after depositing zinc hydroxystannate, stir to graft a silanized layer onto the particle surface, then filter and wash until the filtrate is free of white turbidity when tested with barium chloride solution, and dry at a temperature not exceeding 120°C to obtain deposited and coated modified particles.

[0035] Furthermore, S4 includes:

[0036] S41, the slurry is fed into the atomizer via a frequency conversion feed pump and atomized into droplets and then fed into the spray drying tower. Hot air heated by an electric heater is introduced into the spray drying tower to dry and granulate the droplets, and the temperature sensor is installed at the outlet of the spray drying tower.

[0037] S42, the controller acquires the outlet gas temperature detected by the temperature sensor at a sampling period of 0.5 to 10 seconds, and obtains the deviation by subtracting the set value from the outlet gas temperature;

[0038] S43, the controller calculates the increment of the speed setpoint of the variable frequency feed pump according to the deviation between the current sampling period and the two previous sampling periods using an incremental proportional-integral-derivative algorithm, and updates the speed setpoint accordingly, so that when the outlet gas temperature is higher than the set value, the speed setpoint is increased to increase the slurry feed flow rate and decrease the outlet gas temperature;

[0039] S44, the controller limits the updated speed setpoint between a preset upper speed limit and a lower speed limit, and limits the integral action of the incremental proportional-integral-derivative algorithm; when the speed setpoint reaches the upper speed limit but the outlet gas temperature is still higher than the upper limit of the set range, the controller reduces the heating power of the electric heater; when the speed setpoint reaches the lower speed limit but the outlet gas temperature is still lower than the lower limit of the set range, the controller increases the heating power of the electric heater.

[0040] S45, repeat S42 to S44 to maintain the outlet gas temperature within the set range; the set value is the target outlet gas temperature selected within the range of 85 to 115°C, the set range is the temperature range 2 to 10°C above and below the set value, and the upper limit of the set range is not higher than 115°C; the coefficient of variation of aluminum, magnesium, calcium and zinc content at different sampling points in the obtained composite particles is not greater than 10%, and the obtained composite particles do not show the characteristic peaks of oxides formed by the thermal decomposition of group A when detected by X-ray diffraction.

[0041] Furthermore, the incremental proportional-integral-differential algorithm described in S43 calculates the increment of the speed setpoint and updates the speed setpoint using the following formula:

[0042] ;

[0043] In the formula, For the first The increment of the given rotational speed value in each sampling period; For the first The given rotational speed value for each sampling period; For the first The given rotational speed value for each sampling period; , , These are the non-negative discrete proportional gain, integral gain, and differential gain calculated based on the sampling period, respectively. , , The first , No. , No. Deviation per sampling period; The sampling period number is a positive integer; the deviation is calculated using the following formula:

[0044] ;

[0045] In the formula, For the first Deviation per sampling period; For the first The outlet gas temperature detected in each sampling cycle; The setpoint; the updated speed setpoint It is limited to between the lower speed limit and the upper speed limit.

[0046] The beneficial effects achieved by this invention are as follows:

[0047] This invention combines aluminum hydroxide, boehmite, magnesia, and calcium magnesium carbonate, which have staggered decomposition temperatures, into Group A. Through close packing and gradation, the minerals are spatially adjacent, allowing their endothermic decomposition to proceed continuously and sequentially during the fire-induced heating process. The lower-temperature minerals decompose and absorb heat first, followed by higher-temperature minerals as the temperature rises. This endothermic effect occurs over a wide temperature range without interruption, allowing for continuous heat absorption and the release of water vapor and carbon dioxide to dilute flammable gases during fire. Compared to existing materials that primarily use a single endothermic filler and concentrate heat absorption in a narrow temperature range, the multi-mineral staggered combination in Group A provides thermal protection throughout the entire fire development process.

[0048] This invention incorporates a group B, consisting of sepiolite, fluorophlogopite, and aluminum dihydrogen phosphate, in addition to group A. Aluminum dihydrogen phosphate undergoes thermal condensation to form a low-melting-point mobile phase, while sepiolite and fluorophlogopite provide the fiber and lamellar framework. The refractory oxides remaining after the decomposition of group A, which are initially loose powders, are wetted and bonded by the mobile phase of group B at high temperatures, sintering them into a continuous, dense, ceramicized barrier layer. This barrier layer prevents heat and oxygen from being transferred to the substrate and keeps the residue intact, thus improving its heat insulation and structural integrity during fire exposure. This dense barrier function is not present when group A or group B exists alone; it is achieved through the combined action of group A (providing the aggregate) and group B (providing the sintered mobile phase).

[0049] This invention further incorporates group C, composed of zinc hydroxystannate, zinc molybdate, and zinc borate. The metal oxides generated upon heating possess Lewis acidity, catalyzing the formation of the mobile phase of group B and the sintering of the oxide aggregate. This allows the dense formation of the ceramicized barrier layer to occur before the peak heat release of a fire, promoting char formation of the condensed phase and suppressing the release of smoke and toxic gases. The barrier layer forms before the most intense stage of combustion, suppressing the release of heat and combustible volatiles early. The heat release reduction and smoke suppression effect of group C in a system containing groups A and B is greater than its effect when used alone, exhibiting a synergistic enhancement that is difficult to predict based on the individual effects of each component. Group A provides endothermic heat and aggregate, group B provides the sintering mobile phase, and group C catalyzes, advances formation, and suppresses smoke; the resulting fireproofing and smoke suppression effect is superior to the simple sum of the individual effects of the three components.

[0050] In the gradation preparation stage, this invention determines the blending ratio of each mineral in each particle size of group A based on the target particle size distribution curve of the continuous gradation that enables close packing of particles. Since this curve uses the maximum and minimum particle sizes as boundaries and adjusts the relative content of fine particles using the distribution modulus, it allows coarse and fine particles to fill each other, reducing porosity and thus increasing the loading of endothermic minerals per unit volume. It also ensures that minerals with different decomposition temperatures are spatially adjacent, providing a structural basis for the continuous relay of endothermic action over a wide temperature range and the close sintering of decomposition oxides. Because the densities of the minerals in group A are different, and particle size analysis yields a volume-based distribution, this invention further converts the volume fraction to a mass fraction based on the density of each particle size before weighing, correcting the deviation caused by directly using volume fraction for batching. This ensures that the designed close-packed gradation is accurately achieved in terms of mass ratio, and the batching results are repeatable. The present invention also uses the coefficient of variation of the content of the four minerals at each sampling point as a criterion for whether the mixing is in place. The smaller the coefficient of variation, the closer the composition of each part is. Thus, the uniformity of mixing is transformed into a measurable and identifiable index, ensuring that the graded powder has reached the required uniformity before entering the subsequent process, so that the above-mentioned structural basis can be stably established in batch preparation.

[0051] In the spray drying granulation stage of the preparation process, this invention uses the outlet gas temperature minus a set value as the deviation and employs an incremental proportional-integral-differential algorithm to adjust the speed of the variable frequency feed pump. The incremental algorithm calculates the increment of the speed setpoint only based on the deviation of the most recent sampling periods, without accumulating historical deviations. This results in low computational load and facilitates limiting the output and integral action. It avoids abrupt jumps when adjusting the action between the feed and hot air, and exhibits strong adaptability to fluctuations in both feed and hot air. This invention uses the feed flow rate as the primary adjustment variable, altering the evaporation heat absorption by changing the moisture entering the tower per unit time, thus providing a rapid response to the outlet gas temperature. Furthermore, it utilizes segmented adjustment of the heating power to address conditions after the feed adjustment reaches its limit, stabilizing the outlet gas temperature within a set range below the decomposition initiation temperature of group A. This prevents premature decomposition of the endothermic minerals before powder formation, ensuring that their endothermic capacity is fully preserved in the finished product, and preventing any loss of the material's endothermic properties during the preparation process. This invention also uses the coefficient of variation of the content of each element in the composite particles and whether the characteristic peaks of decomposed oxides appear in the diffraction pattern as criteria. The former characterizes the consistency of the distribution of each component in the particles, and the latter confirms that group A did not decompose during the drying process. The effect of closed-loop temperature control is transformed into verifiable uniformity and non-decomposition indicators, so that the synergistic effect of each level can be exerted synchronously in the micro-region of the composite particles with consistent composition, and the fireproof performance is stable and repeatable between batches. Temperature control improves the stability of fireproof materials. Attached Figure Description

[0052] Figure 1The graphs show a comparison of thermal decomposition endothermic effects between Example 1 and each individual endothermic mineral, where (a) is the DSC heat flow curve of each sample and (b) is a bar chart of segmented heat endothermic effects of each sample.

[0053] Figure 2 The graphs show the heat release comparison of Examples 1-3, Comparative Examples 1-6, and the matrix. (a) is a graph showing the heat release rate of Example 1, Comparative Examples 1, 2, 6, and the matrix, and (b) is a bar chart showing the peak heat release rate of each sample.

[0054] Figure 3 The chart shows the limiting oxygen index of Examples 1-3 and Comparative Examples 1-6, and the synergistic comparison chart of Group C. (a) is a bar chart of the limiting oxygen index of each sample, and (b) is a bar chart comparing the measured peak value and the summed predicted peak value of Example 1.

[0055] Figure 4 The diagrams show the preparation control and microscopic uniformity comparison of Example 1 and Comparative Examples 4 and 5. (a) is the outlet gas temperature curve of Example 1 and Comparative Example 5, and (b) is the bar chart of the endothermic enthalpy retention rate and elemental content variation coefficient of Group A of Example 1, Comparative Example 4 and Comparative Example 5.

[0056] Figure 5 This is a flowchart of a method for preparing mineral fire retardant powder based on endothermic decomposition synergy according to the present invention. Detailed Implementation

[0057] This invention relates to a mineral fire retardant powder based on endothermic decomposition synergy and its preparation method. The specific implementation method is further described below in conjunction with the composition and preparation process of the fire retardant powder.

[0058] Existing inorganic mineral fire retardant powders are mostly based on a single endothermic filler. Their endothermic decomposition is concentrated within a narrow temperature range, and they lose their cooling effect once the temperature exceeds this range. Furthermore, the decomposition residues are mostly loose oxide powders, making it difficult to form a continuous and dense barrier layer. When exposed to fire, this often results in problems such as excessive smoke, debris disintegration, and insufficient insulation. To address these shortcomings, this embodiment is designed by combining multiple minerals with staggered decomposition temperature zones into Group A, allowing the endothermic effect to continue continuously over a wider temperature range. Group B introduces phosphates, which form a low-melting-point mobile phase upon heating, enabling the oxides generated from the decomposition of Group A to be sintered and bonded into a continuous and dense ceramicized barrier layer. Group C introduces a Lewis acid-containing metal compound to catalyze and accelerate the ceramicization and charring processes while suppressing smoke. Other components improve insulation, dispersion, and interfacial bonding. All the above components are deposited in situ, surface modified, and spray-dried to produce composite particles with consistent composition, allowing the synergistic effect between the three components and other components to occur simultaneously within the micro-regions of each composite particle.

[0059] Group A is an endothermic decomposition component, composed of aluminum hydroxide, boehmite, hydromagnesia, and calcium magnesium carbonate. By mass, aluminum hydroxide comprises 20-35 parts, boehmite 10-20 parts, hydromagnesia 10-20 parts, and calcium magnesium carbonate 8-15 parts. Boehmite is monohydrated aluminum oxide with the chemical formula γ-AlOOH; hydromagnesia is hydrated basic magnesium carbonate mineral with the chemical formula Mg5(CO3)4(OH)2·4H2O; and calcium magnesium carbonate is a hendrite-type carbonate mineral with the chemical formula CaMg3(CO3)4. Its calcium-to-magnesium atomic ratio is 1:3, distinguishing it from dolomite CaMg(CO3)2, which has a calcium-to-magnesium atomic ratio of 1:1. The endothermic decomposition initiation temperatures of these four minerals are staggered sequentially. Aluminum hydroxide absorbs heat and releases water of crystallization at approximately 180–300℃ via the reaction 2Al(OH)3 → Al2O3 + 3H2O. Boehmite undergoes further dehydration at approximately 340–500℃ via the reaction 2AlOOH → Al2O3 + H2O. Magnesia hydrophora releases water of crystallization and carbon dioxide in stages at approximately 220–550℃ and completes its decomposition via the reaction Mg5(CO3)4(OH)2·4H2O → 5MgO + 4CO2 + 5H2O. Calcium magnesium carbonate releases carbon dioxide at approximately 450–650℃ via the reaction CaMg3(CO3)4 → CaO + 3MgO + 4CO2. Because the decomposition temperature zones of each mineral are sequential and partially overlap, the overall endothermic process of Group A occurs continuously within the range of approximately 180–650℃. When exposed to fire, it continuously absorbs heat, dilutes combustible gases, and releases water vapor and carbon dioxide to form a gas phase barrier, avoiding the problem of overly concentrated cooling effect and narrow temperature range of a single endothermic filler. The refractory oxides such as aluminum oxide, magnesium oxide, and calcium oxide left after the decomposition of various minerals provide aggregates for the subsequent ceramic barrier layer.

[0060] Group B is a ceramicized barrier component, composed of sepiolite, fluorophlogopite, and aluminum dihydrogen phosphate. By weight of raw materials, sepiolite comprises 5-10 parts, fluorophlogopite 4-8 parts, and aluminum dihydrogen phosphate 3-6 parts. Sepiolite is a fibrous, hydrous magnesium silicate mineral with the chemical formula Mg₄Si₆O₅. 15 (OH)₂·6H₂O, its fiber structure acts as a skeleton reinforcement and tortuous path barrier at high temperatures; fluorophlogopite is a synthetic mica with the chemical formula KMg₃(AlSi₃O₂). 10 F2, in a lamellar form, exhibits high thermal stability and extends the diffusion path of heat and oxygen. Aluminum dihydrogen phosphate, with the chemical formula Al(H2PO4)3, undergoes thermal dehydration and condensation to form a low-melting-point mobile phase of aluminum phosphate and aluminum polyphosphate. This mobile phase wets and binds the refractory oxide aggregate formed by the decomposition of group A at higher temperatures. The refractory oxides of group A are themselves loose powders, which are sintered into a continuous and dense ceramic shell by the phosphate mobile phase of group B at high temperatures. This forms a barrier layer that isolates heat and oxygen. This barrier function is produced by the combination of group A and group B, and cannot be possessed by either component alone, constituting a synergy between group A and group B.

[0061] Group C is a catalytic charring and smoke-suppressing component, composed of zinc hydroxystannate, zinc molybdate, and zinc borate. By weight of raw materials, zinc hydroxystannate comprises 1.5–4 parts, zinc molybdate 1–3 parts, and zinc borate 1.5–3 parts. The chemical formula of zinc hydroxystannate is ZnSn(OH)6, and the zinc and tin oxides produced by thermal dehydration exhibit Lewis acidity. The chemical formula of zinc molybdate is ZnMoO4. The zinc borate is hydrated zinc borate, commonly with the chemical formula 2ZnO·3B2O. 3· 3.5H₂O, upon heating, releases water of crystallization and forms a glassy borate phase. This group of metal compounds, acting as Lewis acid catalysts, lowers the initiation temperature of the ceramization and charring reactions, allowing the formation of the B-group mobile phase and the sintering of the oxide aggregate to occur earlier, constructing a barrier layer before the heat release peak. Simultaneously, elements such as tin, molybdenum, and boron promote charring of the condensed phase and inhibit the formation of flue gas and carbon monoxide. Group A provides endothermic heat and aggregate, Group B provides the sintering mobile phase, and Group C catalyzes, advances the forming process, and suppresses smoke. The combined fireproofing and smoke-suppressing effect is superior to the simple superposition of the individual effects of the three, constituting a synergistic effect between Groups A, B, and C.

[0062] The other components consist of expanded vermiculite, 3-aminopropyltriethoxysilane, and sodium hexametaphosphate. By weight of raw materials, expanded vermiculite comprises 3–8 parts, 3-aminopropyltriethoxysilane 0.5–2 parts, and sodium hexametaphosphate 0.3–1 part. Expanded vermiculite is a layered expanded silicate mineral with low thermal conductivity, serving as a lightweight insulating filler. 3-aminopropyltriethoxysilane is a silane coupling agent with the chemical formula H₂N(CH₂)₃Si(OC₂H₅)₃, which, through hydrolysis and condensation, grafts onto the particle surface to form a silanized layer, improving particle dispersibility in the aqueous phase and interfacial bonding between phases. Sodium hexametaphosphate, with the chemical formula (NaPO₃)₆, acts as a dispersant to regulate slurry rheology and inhibit particle agglomeration.

[0063] To balance heat absorption, barrier layer density, and smoke suppression effect, the amounts of the above components can be further optimized. Aluminum hydroxide is preferably 26-30 parts, boehmite is preferably 13-17 parts, magnesia is preferably 12-16 parts, calcium magnesium carbonate is preferably 9-13 parts, sepiolite is preferably 6-8 parts, fluorophlogopite is preferably 5-7 parts, aluminum dihydrogen phosphate is preferably 3-5 parts, zinc hydroxystannate is preferably 2-4 parts, zinc molybdate is preferably 1.5-2.5 parts, zinc borate is preferably 2-3 parts, expanded vermiculite is preferably 4-6 parts, 3-aminopropyltriethoxysilane is preferably 0.8-1.5 parts, and sodium hexametaphosphate is preferably 0.4-0.6 parts.

[0064] In the prepared fire-retardant powder, zinc hydroxystannate of group C exists at least partially on the surface of each mineral particle of group A in the form of particulate or film-like deposits, forming a zinc hydroxystannate deposition coating layer. The particle surface also has a silanized layer formed by the hydrolysis and condensation of 3-aminopropyltriethoxysilane. The zinc hydroxystannate, acting as a catalyst, is deposited in situ on the surface of the group A particles that generate oxide aggregate, ensuring that the catalytic effect occurs precisely in the micro-regions that require sintering into a shell. This facilitates the uniform and early formation of the ceramicized barrier layer at the particle scale. The fire-retardant powder is a composite particle, and the median particle size of the composite particles, measured by laser diffraction particle size analysis, is preferably 20–40 μm. The median particle size refers to the particle size corresponding to a cumulative volume fraction of 50%.

[0065] The aforementioned fire-retardant powder can be prepared by methods including S1 to S5. For example... Figure 5 As shown, S1 is the endothermic mineral gradation step, in which each component of group A is crushed and graded into multiple particle sizes, the blending ratio of each particle size is determined according to the target particle size distribution curve of continuous gradation that makes the particles compact and the particles are blended, and the mixture is stirred until uniform to obtain endothermic mineral gradation powder. S1 further includes S11 to S14.

[0066] In step S11, the aluminum hydroxide, boehmite, magnesia, and calcium magnesium carbonate of group A are pulverized by an air jet mill and classified by an air classifier, respectively, to obtain powders of multiple particle sizes. The air jet milling and air classification use high-speed airflow as the medium, which introduces fewer impurities and results in a narrower particle size distribution. In step S12, the volume-based particle size distribution of each particle size is determined using a laser diffraction particle size analyzer to obtain the upper and lower limits of the particle size for each particle size. The volume-based particle size distribution refers to the particle size distribution statistically weighted by particle volume.

[0067] In S13, the volume fraction of each particle size is calculated according to the target particle size distribution curve. Then, the volume fraction is converted into a mass fraction according to the density of each particle size powder, and the powder of the corresponding particle size is weighed according to the mass fraction. The target particle size distribution curve is derived from the continuous particle size distribution model proposed by Andreasen and Andersen, and is modified by Dinger and Funk by introducing a minimum particle size. Its expression is shown in the following formula.

[0068] ;

[0069] In the formula, For particles smaller than The cumulative volume fraction (%) of particles in endothermic mineral graded powder; Particle size (μm); The maximum particle size (μm) in the endothermic mineral grade powder. The minimum particle size (μm) in the endothermic mineral grade powder. The distribution modulus is dimensionless. , , They represent , , of Power of 1. Distribution modulus. It reflects the relative content of fine particles in the particle size distribution. The smaller the particle size, the higher the proportion of fine particles and the easier it is to fill the gaps. When the value is no greater than approximately 0.37, this distribution tends to achieve a higher bulk density. To balance bulk density and slurry rheology, The preferred value is 0.21 to 0.30. The close packing of particles can reduce the porosity of the graded powder, increase the amount of heat-absorbing minerals in a unit volume, and make minerals with different decomposition temperature zones spatially adjacent to each other. This allows the staggered heat absorption to continue continuously in the same micro-zone, and also allows the oxide aggregates formed after the decomposition of each mineral to be pre-arranged in a close manner, which is convenient for subsequent sintering and densification.

[0070] After obtaining the cumulative distribution from the above formula, the th The volume fraction of each particle size is the difference in cumulative distribution at the upper and lower limits of that particle size, as shown in the following formula.

[0071] ;

[0072] In the formula, For the first Volume fraction (%) of each particle size in endothermic mineral powder. For the first Upper limit of particle size (μm) for each particle size class; For the first Lower limit of particle size (μm) for each particle size class; and The particle size calculated by the above formula is equal to and Cumulative volume fraction (%) at time; The number represents the particle size, ranging from 1 to... , The total number of particles; when When equal to 1 equal ,when equal hour equal ,and Greater than 0.

[0073] Since aluminum hydroxide, boehmite, magnesia, and calcium magnesium carbonate have different densities, and laser diffraction yields a volume-based distribution, direct weighing based on volume fraction would introduce inaccuracies. Therefore, it is necessary to convert the volume fraction to a mass fraction based on density. Let the first... The volume fraction of each particle size is Density is The first unit of graded powder volume The mass of each particle size is proportional to... and The product of the masses of each particle size is proportional to the sum of the masses of each particle size. and The sum of the products, the first The mass fraction of each particle size is the ratio of the two, as shown in the following formula.

[0074] ;

[0075] In the formula, For the first Mass fraction (%) of each particle size; For the first Density of individual particle size powder (g / cm³); For the first Volume fraction (%) of each particle size; express From 1 to The sum of the products of the density and volume fraction of powder of each particle size; For the first Density of individual particle size powder (g / cm³); For the first Volume fraction (%) of each particle size; The particle size index is used for summation. After obtaining the mass fraction of each particle size using the above formula, the corresponding particle size powder is weighed accordingly.

[0076] In step S14, the weighed powders of each particle size are added to a mixer and stirred. Quantitative phase analysis is performed on sampling points at different locations within the mixer using an X-ray diffractometer. The contents of aluminum hydroxide, boehmite, hydromagnesia, and calcium magnesium carbonate at each sampling point are determined. The coefficient of variation (COP) of each of the four components at each sampling point is calculated. Mixing is stopped when the COP is no greater than the preferred limit of 5%, resulting in an endothermic mineral-grade powder. The COP is the ratio of the standard deviation to the mean of a set of data, expressed as a percentage. It measures the dispersion of component contents between sampling points; a smaller COP indicates more uniform mixing. Using the contents of each of the four minerals, rather than a single tracer component, as the homogeneity criterion avoids misjudging overall homogeneity due to the accidental uniformity of a particular mineral. Quantitative phase analysis using X-ray diffraction can be achieved using a full-spectrum fitting method or an internal standard method.

[0077] S2 is an in-situ deposition coating and surface modification step, in which endothermic mineral grade powder is dispersed in water, sodium stannate and zinc sulfate are added to generate the hydroxy zinc stannate deposition coating layer of group C in situ on the particle surface, and then 3-aminopropyltriethoxysilane is added to modify the particle surface. The particles are then filtered to obtain the deposition-coated modified particles. S2 further includes S21 and S22.

[0078] In S21, an endothermic mineral-grade powder is dispersed in deionized water to obtain a suspension. Sodium stannate and zinc sulfate are added to the suspension at a 1:1 molar ratio of tin to zinc. The reaction is carried out under neutral to weakly alkaline conditions, causing zinc hydroxystannate to deposit in situ on the particle surface. The reaction proceeds according to the formula: Na2SnO3 + ZnSO4 + 3H2O → ZnSn(OH)6 + Na2SO4. In this reaction, zinc hydroxystannate adheres to the particle surface as a deposit, while sodium sulfate dissolves in the aqueous phase. The preferred reaction conditions are pH 7.0–9.0, temperature 25–60℃, and reaction time 0.5–3 h. The amount of sodium stannate and zinc sulfate added is based on the theoretical production of zinc hydroxystannate to reach the mass fraction of zinc hydroxystannate in group C. The theoretical production amount refers to the amount of zinc hydroxystannate that should be produced by the complete reaction of the added sodium stannate and zinc sulfate according to the above reaction formula. Measuring based on the theoretical production amount avoids underestimation due to insufficient actual deposition rate. Zinc hydroxystannate, which serves as a catalyst, is generated in situ on the surface of Group A particles, placing it in close proximity to the minerals that generate oxide aggregates. This provides conditions for the early and localized catalysis of subsequent ceramicization.

[0079] In step S22, pre-hydrolyzed 3-aminopropyltriethoxysilane is added to the suspension after the deposition of zinc hydroxystannate. Stirring causes a silanization layer to be grafted onto the particle surface. The particles are then filtered, washed, and dried to obtain the deposited and coated modified particles. The ethoxy group of 3-aminopropyltriethoxysilane is first hydrolyzed in water to form silanol. The silanol then condenses with the hydroxyl groups on the particle surface to form a silicon-oxygen covalent bond, which then polymerizes to form a silanization layer. Pre-hydrolysis refers to hydrolyzing the silane in water or a water-alcohol system before adding it to the suspension to improve grafting efficiency. Washing is continued until the filtrate shows no white turbidity when tested with barium chloride solution, indicating that sulfate ions have been largely removed. This avoids the presence of soluble byproduct salts in the product. Barium chloride reacts with sulfate ions to form a white barium sulfate precipitate; therefore, the absence of white turbidity is used as a criterion for complete sulfate removal. The drying temperature is preferably no higher than 120°C, which is lower than the decomposition initiation temperature of aluminum hydroxide, preventing premature decomposition of group A during the drying process. The silanization layer and the zinc hydroxystannate deposition coating layer together improve the dispersibility and interfacial bonding of particles, and play an isolating and protective role for the carbonate minerals of Group A in subsequent mixing.

[0080] Step S3 is the slurry preparation step. The components of group B are dispersed in water, and then zinc molybdate and zinc borate from group C, expanded vermiculite and sodium hexametaphosphate from the other components, and the deposited coated modified particles are added. The mixture is then stirred at a temperature below 25°C to obtain a slurry. Step S4 is performed within 30 minutes after mixing. Aluminum dihydrogen phosphate is acidic in water. If it comes into prolonged contact with carbonate minerals such as magnesite and calcium magnesium carbonate from group A at high temperatures, a neutralization reaction may occur, releasing carbon dioxide, consuming phosphate, and thickening the slurry. Therefore, a method is adopted where group B is dispersed first, then the remaining components are added, mixed briefly at a temperature below 25°C, and spray-dried within 30 minutes to shorten the contact window between the acidic phosphate and carbonate. The deposited coating layer and silanized layer on the surface of the deposited coated modified particles also isolate the internal carbonates. The preferred solid content of the slurry is 30–55 wt%. The dispersing effect of sodium hexametaphosphate helps maintain the slurry's fluidity at this solid content.

[0081] S4 is a closed-loop temperature-controlled spray drying granulation step. The slurry is atomized and sent into the spray drying tower for drying and granulation. The temperature sensor detects the outlet gas temperature of the spray drying tower and feeds it back to the controller. The controller adjusts the slurry feed flow rate and hot air heating power according to the deviation between the outlet gas temperature and the set value, so that the outlet gas temperature is maintained within the set range that will not cause the decomposition of group A, and composite particles are obtained. S4 further includes S41 to S45.

[0082] In S41, the slurry is atomized into droplets by a variable frequency feed pump and then fed into a spray drying tower. Hot air heated by an electric heater is introduced into the spray drying tower to dry and granulate the droplets. A temperature sensor is installed at the outlet of the spray drying tower. The droplets are rapidly dehydrated and solidified into composite particles in the hot air. Multiple components in the slurry are simultaneously fixed within the same droplet, allowing components A, B, and C to coexist with other components within each composite particle. This three-level synergy occurs within the micro-regions of the particle.

[0083] In S42, the controller collects the outlet gas temperature detected by the temperature sensor with a sampling period of preferably 0.5 to 10 seconds, and obtains the deviation by subtracting the set value from the outlet gas temperature. The deviation is shown in the following formula.

[0084] ;

[0085] In the formula, For the first Deviation (°C) for each sampling period; For the first The outlet gas temperature (°C) detected in each sampling cycle; The set value (°C); This is the sampling period number, rounded to a positive integer. When the outlet gas temperature exceeds the set value... A positive value indicates a positive value, and vice versa.

[0086] In S43, the controller calculates the increment of the variable frequency feed pump's speed setpoint based on the current sampling period and the deviation between the previous two sampling periods using an incremental proportional-integral-derivative algorithm. It then updates the speed setpoint accordingly, increasing the speed setpoint and increasing the slurry feed flow rate to lower the outlet gas temperature when the outlet gas temperature exceeds the setpoint. Increasing the feed flow rate increases the amount of moisture entering the tower per unit time, leading to increased evaporation heat absorption and a decrease in outlet gas temperature. Therefore, using the feed pump speed as the primary regulating variable allows for a faster response to the outlet temperature.

[0087] The incremental proportional-integral-differential algorithm is obtained by difference from the positional discrete proportional-integral-differential algorithm. The positional algorithm is shown in the following equation.

[0088] ;

[0089] In the formula, For the first The rotational speed setpoint (r / min) for each sampling period; The proportional gain (r·min) -1 ·℃ -1 ); The integral gain (r·min) calculated over the sampling period -1 ·℃ -1 ); The differential gain calculated over the sampling period (r·min) -1 ·℃ -1 ); For the first Deviation (°C) for each sampling period; For the first Deviation (°C) for each sampling period; For the first Deviation (°C) for each sampling period; express From 0 to The sum of the deviations of each sampling period; The sampling period number is used for summation; This is the sampling period number, which is a positive integer.

[0090] In the The given rotational speed value for the sampling period is also expressed in the positional formula described above. The positional expression of the sampling period and the first sampling period Subtracting the positional expressions for each sampling period, the difference between the sums of the integral terms is exactly... After eliminating the accumulation of historical biases, the incremental algorithm is obtained as shown in the following formula.

[0091] ;

[0092] In the formula, For the first The increment of the given rotational speed value (r / min) per sampling period; , , These are the proportional gain, the integral gain calculated over the sampling period, and the differential gain (r·min). -1 ·℃ -1 All three take non-negative values; , , The first , No. , No. Deviation (°C) for each sampling period; is the sampling period number, which is a positive integer. The incremental algorithm only needs to store the deviation of the most recent three sampling periods, without accumulating historical deviations. It has a small computational load and is easy to limit. The speed setpoint is updated according to the following formula.

[0093] ;

[0094] In the formula, For the first The rotational speed setpoint (r / min) for each sampling period; For the first The rotational speed setpoint (r / min) for each sampling period; For the first The increment of the given rotational speed (r / min) per sampling period. When the deviation is... Define and , , When a non-negative value is taken, if the outlet gas temperature is too high, the deviation is positive and the increment is positive. The speed setpoint and feed flow rate increase accordingly, and the outlet gas temperature drops. The adjustment direction is consistent with that described in S43.

[0095] In S44, the controller limits the updated speed setpoint between a preset upper and lower speed limit, and limits the integral action of the incremental algorithm to suppress integral saturation. The upper and lower speed limits can be determined by the rated operating conditions of the variable frequency feed pump and the spray drying tower. When the speed setpoint reaches the upper speed limit but the outlet gas temperature is still higher than the upper limit of the set range, the controller reduces the heating power of the electric heater; when the speed setpoint reaches the lower speed limit but the outlet gas temperature is still lower than the lower limit of the set range, the controller increases the heating power of the electric heater. This split-range regulation, with feed flow rate as the primary factor and heating power as the secondary factor, can maintain a stable outlet temperature even after the feed rate regulation reaches its limits.

[0096] In step S45, steps S42 to S44 are repeated to bring the outlet gas temperature to a convergence and maintain it within the set range. The set value is preferably a target outlet gas temperature selected within the range of 85–115°C. The set range is a temperature interval of 2–10°C above and below the set value, with the upper limit not exceeding 115°C. This upper limit is lower than the decomposition initiation temperature of aluminum hydroxide, thus preventing premature decomposition of group A during the drying process and preserving its heat absorption capacity to the finished product. Each droplet undergoes a consistent drying process under the controlled outlet temperature, resulting in a consistent distribution of components in the resulting composite particles. This can be characterized by the coefficient of variation of Al, Mg, Ca, and Zn element content at different sampling points not exceeding a preferred limit of 10%. Furthermore, the absence of characteristic peaks for aluminum oxide, magnesium oxide, or calcium oxide formed by the thermal decomposition of group A in the composite particles obtained by X-ray diffraction confirms that group A has not decomposed. Considering that the outlet gas temperature is only an indirect indicator, to further ensure that the material does not undergo a thermal process exceeding the decomposition temperature, the inlet air temperature of the spray drying tower can be limited to no higher than 180°C.

[0097] In step S5, the composite particles are sieved to obtain the mineral fire-retardant powder. The sieve mesh size can be selected according to the target median particle size, so that the median particle size of the composite particles is 20-40 μm. In the above spray drying process, the spray drying tower is equipped with a temperature sensor, a controller, a variable frequency feed pump, and an electric heater. The controller is configured to execute the above incremental proportional-integral-derivative algorithm, and to compensate and adjust the heating power of the electric heater after the variable frequency feed pump reaches the preset upper or lower speed limit. This links the closed-loop control of the outlet temperature with preventing premature decomposition of group A and ensuring consistent particle composition, so that temperature control serves the performance stability of the fire-retardant material.

[0098] Group A continuously absorbs heat over a wide temperature range and provides oxide aggregates. Group B sintersulates aggregates at high temperatures to form a dense ceramicized barrier layer. Group C catalyzes and pre-ceramizes and chars the aggregates while suppressing smoke. Other components improve heat insulation, dispersion, and interface. Composite particles with consistent composition are produced through in-situ deposition, surface modification, and closed-loop temperature-controlled spray drying. This allows the three levels of synergy to work simultaneously within the micro-regions of the particles. The resulting mineral fire retardant powder provides continuous cooling, dense barrier, and suppressed smoke when exposed to fire. Furthermore, the preparation process is stable and repeatable.

[0099] Example 1: The mineral fire retardant powder of Example 1 was prepared according to the following method. In S1, 28 parts by weight of aluminum hydroxide, 15 parts by weight of boehmite, 14 parts by weight of magnesia, and 11 parts by weight of calcium magnesium carbonate were weighed as Group A. In S11, the above four minerals were subjected to air jet milling and air jet classification to obtain powders of multiple particle sizes. In S12, the volumetric particle size distribution of each particle size was determined using a laser diffraction particle size analyzer. In S13, the distribution modulus was taken... The volume fraction of each particle size was calculated based on the target particle size distribution curve, and then converted to mass fraction based on the density of each particle size. The mixture was then weighed accordingly. In S14, the mixture was stirred and the content of the four components at each sampling point was quantitatively analyzed by X-ray diffraction until the coefficient of variation was no greater than 5%, yielding an endothermic mineral grade powder. In S2, the endothermic mineral grade powder was dispersed in deionized water. In S21, sodium stannate and zinc sulfate were added at a 1:1 molar ratio of tin to zinc, and reacted at pH 8.0 and 40℃ for 1.5 h, so that the theoretical amount of zinc hydroxystannate reached 3 parts and was deposited in situ on the particle surface. In S22, 1.2 parts of pre-hydrolyzed 3-aminopropyltriethoxysilane were added to graft a silanized layer. The mixture was filtered and washed until the filtrate showed no white turbidity as detected by barium chloride. It was then dried at 110℃ to obtain the deposited and coated modified particles. In step S3, 7 parts sepiolite, 6 parts fluorophlogopite, and 4 parts aluminum dihydrogen phosphate are dispersed in water. Then, 2 parts zinc molybdate, 2.5 parts zinc borate, 5 parts expanded vermiculite, and 0.5 parts sodium hexametaphosphate are added along with the deposition-coated modified particles. The mixture is stirred at below 25°C to a slurry with a solid content of 45 wt%, and then carried out in step S4 within 30 minutes. In step S4, the slurry is atomized by a variable frequency feed pump and then enters the spray drying tower. The inlet air temperature is 170°C, and the outlet gas temperature is detected at a 2-second sampling cycle. The feed pump speed is adjusted using an incremental proportional-integral-derivative algorithm, supplemented by range-based heating power adjustment. The setpoint is 100°C, and the set range is 95–105°C, maintaining the outlet gas temperature within this range to obtain composite particles. In step S5, the particles are sieved to obtain mineral fire-retardant powder with a median particle size of 30 μm.

[0100] Example 2 differs from Example 1 in its formulation and several process parameters. By weight, it contains: 20 parts aluminum hydroxide, 10 parts boehmite, 10 parts magnesia, 8 parts calcium magnesium carbonate, 5 parts sepiolite, 4 parts fluorophlogopite, 3 parts aluminum dihydrogen phosphate, 1.5 parts zinc hydroxystannate, 1 part zinc molybdate, 1.5 parts zinc borate, 3 parts expanded vermiculite, 0.5 parts 3-aminopropyltriethoxysilane, and 0.3 parts sodium hexametaphosphate; the distribution modulus in S13... Set the value to 0.22; in step S4, set the temperature to 90°C and the temperature range to 85-95°C. The remaining steps are the same as in Example 1.

[0101] Example 3 differs from Example 1 in its formulation and several process parameters. By weight, it contains: 35 parts aluminum hydroxide, 20 parts boehmite, 20 parts magnesia, 15 parts calcium magnesium carbonate, 10 parts sepiolite, 8 parts fluorophlogopite, 6 parts aluminum dihydrogen phosphate, 4 parts zinc hydroxystannate, 3 parts zinc molybdate, 3 parts zinc borate, 8 parts expanded vermiculite, 2 parts 3-aminopropyltriethoxysilane, and 1 part sodium hexametaphosphate; the distribution modulus in S13 is... The value is set to 0.29; in S4, the set value is 110℃ and the set range is 105~115℃. The remaining steps are the same as in Example 1.

[0102] Comparative Example 1 differs from Example 1 in that the formulation does not contain Group B and Group C, S21 does not contain sodium stannate and zinc sulfate and does not form a zinc hydroxystannate deposition coating layer, S3 does not contain sepiolite, fluorophlogopite, aluminum dihydrogen phosphate, zinc molybdate and zinc borate, Group A and other components are retained, and the remaining steps are the same as in Example 1.

[0103] Comparative Example 2 differs from Example 1 in that the formulation does not contain Group C, sodium stannate and zinc sulfate are not added in S21, zinc molybdate and zinc borate are not added in S3, Groups A and B are retained along with other components, and the remaining steps are the same as in Example 1.

[0104] Comparative Example 3 differs from Example 1 in that it uses 68 parts by total mass of aluminum hydroxide instead of the four minerals in Group A. The rest of the formulation and steps are the same as in Example 1.

[0105] Comparative Example 4 has the same formulation as Example 1, except that it does not undergo in-situ deposition in S2 and spray drying in S4. Instead, the components are mechanically blended. Zinc hydroxystannate is an added commercially available powder. The resulting powder has the same composition as Example 1 but is not a composite particle.

[0106] Comparative Example 5 differs from Example 1 in that closed-loop temperature control is not applied in S4, the feed pump speed and heating power are fixed, and the outlet gas temperature is approximately 175°C and fluctuates to 195°C. The remaining steps are the same as in Example 1.

[0107] Comparative Example 6 differs from Example 1 in that its formulation does not contain Group A and Group B, but is prepared by using only 3 parts of zinc hydroxystannate, 2 parts of zinc molybdate, and 2.5 parts of zinc borate from Group C, along with other components, in accordance with the corresponding steps.

[0108] Experimental Example 1: Experimental Example 1 used thermogravimetric-differential scanning calorimetry (TGC) to investigate the endothermic behavior of Group A. Individual minerals used in Example 1—aluminum hydroxide, boehmite, magnesia, and calcium magnesium carbonate—as well as the Group A mixture prepared according to the mass fractions in Example 1, were subjected to thermogravimetric analysis and differential scanning calorimetry (DSC) under a nitrogen atmosphere at a heating rate of 10 °C / min. The heat endothermic and total endothermic enthalpy for each temperature range were obtained by integrating the heat flow curves. The results are shown in Table 1 and... Figure 1 As shown. Figure 1 (a) shows the DSC heat flow curves for each sample. Figure 1 (b) shows the segmented heat absorption of each sample in the temperature ranges of 200–300, 300–400, 400–500, 500–600, and 600–700℃.

[0109] Depend on Figure 1As can be seen in (a), the endothermic reactions of aluminum hydroxide, boehmite, hydromagnesia, and calcium magnesium carbonate are concentrated at approximately 200–340°C, 380–520°C, 220–550°C, and 450–650°C, respectively. The heat flow of each individual mineral returns to the baseline outside its temperature range, while the heat flow of group A in Example 1 remains consistently above the baseline within the range of approximately 200–650°C, without any significant gaps. Figure 1 As can be seen in (b), the four individual minerals only have significant heat absorption in one or two intervals corresponding to their respective decomposition temperature zones, while the heat absorption in the remaining intervals is close to zero. In contrast, the combination of group A in Example 1 has considerable heat absorption in all five intervals. Therefore, it can be concluded that when four minerals with staggered decomposition temperature zones are combined in a continuous gradation, the heat absorption occurs continuously throughout the entire range of the heating process without interruption.

[0110] In step S1 of this invention, the close packing gradation makes minerals with different decomposition temperatures spatially adjacent to each other. When exposed to fire, the low-temperature minerals decompose and absorb heat first, and as the temperature rises, the higher-temperature minerals decompose and absorb heat in turn. That is, the dehydration and decarburization endothermic peaks of each mineral are connected one after another and partially overlap on the temperature axis, integrating the isolated narrow endothermic peaks of each individual mineral into a wide and continuous endothermic zone.

[0111] Table 1. Thermal decomposition endothermic data for each endothermic mineral and Group A combination in Example 1:

[0112]

[0113] Experimental Example 2: Experimental Example 2 used the cone calorimeter method to investigate the heat release during the combustion process. The fire retardant powders from Examples 1-3 and Comparative Examples 1-6 were added in equal proportions to the same water-based fire retardant coating matrix, coated onto a substrate of the same specification to prepare samples, and tested at 50 kW / m². 2 The radiative flux was tested, and the heat release rate and ignition time were recorded. The results are shown in Table 2 and... Figure 2 As shown. Figure 2 (a) shows the heat release rate of the matrix versus time for Examples 1, Comparative Examples 1, 2, and 6. Figure 2 (b) shows a comparison of the peak heat release rates of Examples 1-3, Comparative Examples 1-6, and the matrix.

[0114] Depend on Figure 2 As can be seen in (a), the peak value of the matrix is ​​approximately 850 kW / m. 2 The comparative example 1, which only contains Group A, decreased to approximately 430 kW / m². 2 The comparative ratio 2, including groups A and B, further decreased to approximately 360 kW / m². 2 The comparative example 6, which only contains Group C, only decreased to approximately 800 kW / m². 2 The three-component complete Example 1 was reduced to approximately 278 kW / m³. 2 The peak is the lowest and flattest. (From...) Figure 2 As can be seen in (b), the peak values ​​of Examples 1 to 3 are all lower than those of all comparative examples.

[0115] As can be seen, Comparative Example 1 shows that Group A reduced the peak power from approximately 850 kW / m² to approximately 430 kW / m². 2 This indicates that the endothermic decomposition of Group A in this invention can dilute and remove heat, reducing heat release. Comparative Example 2 shows a further reduction in peak heat output of approximately 70 kW / m³ compared to Comparative Example 1. 2 Furthermore, the residue of Comparative Example 1 was a loose oxide, while the residue of Comparative Example 2 was a dense shell, indicating that Group B of the present invention sintered the decomposed oxide of Group A into a ceramic barrier layer, blocking heat return. This barrier peak reduction effect is not possessed by Group A alone, proving that the combination of Group A and Group B produces a new function, demonstrating the synergy between A and B. Comparative Example 6 shows that Group C alone has very little peak reduction, but after adding Group C to the system containing Group A and Group B, the peak value decreased from about 360 to about 278 kW / m. 2 The reduction in temperature is much greater than its individual effect, indicating that group C of the present invention plays a role in the system that exceeds its own independent contribution. The metal oxides generated by the heated zinc hydroxystannate, zinc molybdate and zinc borate of group C have Lewis acidity, which can catalyze the formation of the phosphate mobile phase of group B and the sintering of oxide aggregate, so that the ceramic barrier layer is densified in advance before the arrival of the heat release peak, and a significant peak reduction is obtained with a small amount of group C.

[0116] Table 2, Results of cone calorimetry test:

[0117]

[0118] Experiment 3 investigated the synergistic effect between flame retardant rating and Group C. The limiting oxygen index was measured, vertical combustion grading was performed and afterflame time was recorded, and smoke density rating was measured. Sample preparation was the same as in Experiment 2. The results are shown in Table 3 and... Figure 3 As shown. Figure 3 (a) shows a comparison of the limiting oxygen index of Examples 1-3 and Comparative Examples 1-6. Figure 3 (b) shows a comparison between the peak value of Example 1 predicted by summing the data from Comparative Example 2 and Comparative Example 6 and the measured peak value of Example 1.

[0119] Depend on Figure 3 As can be seen in (a), the limiting oxygen indices of Examples 1-3 are 33.0-34.8, all higher than those of all comparative examples, indicating that the formulations with all three components require a higher oxygen concentration to maintain combustion. Figure 3 As can be seen in (b), the peak value of Example 1, predicted by the summation contribution of group C in the A+B system, is approximately 310 kW / m³. 2 The measured value in Example 1 was approximately 278 kW / m³. 2 The actual measured value was approximately 32 kW / m lower than the sum of the predicted values. 2The summation prediction here is obtained by subtracting the difference between the peak value of the matrix and the peak value of Comparative Example 6 from the peak value of Comparative Example 2, that is, the peak reduction amount of Group C alone superimposed on the A+B system. This indicates that the peak reduction effect of Group C on the system is greater than its individual effect plus the simple sum of the system's peak reduction. The Lewis acid catalyst of Group C lowers the initiation temperature of the formation of the mobile phase of Group B and the sintering of the oxide aggregate, causing the ceramicized barrier layer to densify earlier. The barrier layer formed earlier inhibits the release of heat and combustible volatiles before the most intense stage of combustion, resulting in peak reduction and flame retardancy improvement that exceeds the summation prediction.

[0120] Table 3. Limiting oxygen index, vertical combustion rating, and smoke density:

[0121]

[0122] Experiment 4 investigated thermal insulation, preparation control, and microscopic uniformity. A coating containing fire-retardant powder was applied to a steel substrate, and the time it took for the temperature of the unexposed side to rise to 300°C under a standard flame was recorded. The thermal conductivity of the residue after high-temperature treatment was measured. The appearance temperature of the ceramic phase in the residue was determined by X-ray diffraction. The retention rate of the endothermic enthalpy of group A was characterized by the ratio of the endothermic enthalpy of group A (measured by thermogravimetric analysis) to the unheated baseline. The elemental content at different sampling points was determined by scanning electron microscopy (SEM) energy dispersive spectroscopy, and the coefficient of variation was calculated. The results are shown in Table 4. Figure 4 As shown. Figure 4 In Figure (a), the closed-loop control curve of the outlet gas temperature in Example 1, the open-loop curve of Comparative Example 5, and the reference line for the decomposition initiation temperature of aluminum hydroxide are shown. Figure 4 (b) shows a comparison of the endothermic enthalpy retention rate and elemental content variation coefficients in Group A of Examples 1, 4, and 5.

[0123] Depend on Figure 4 As can be seen in (a), the outlet gas temperature of Example 1 converges from its initial value and remains stable at 95–105°C, consistently below the decomposition initiation temperature of aluminum hydroxide (approximately 180°C), while the outlet gas temperature of Comparative Example 5 rises to approximately 175°C and fluctuates to approximately 195°C, exceeding this initiation temperature. Figure 4 As can be seen in (b), a high endothermic enthalpy retention rate is preferred for Group A, approximately 98% for Example 1 and approximately 99% for Comparative Example 4, while the retention rate for Comparative Example 5 without temperature control drops to approximately 82%. A low coefficient of variation for elemental content is preferred, approximately 4.5% for Example 1 and approximately 6.0% for Comparative Example 5, while the coefficient of variation for mechanically blended Comparative Example 4 rises to approximately 14.0%. Combined with Table 4, Example 1 exhibits the longest time to heat the back surface to 300°C, the lowest residual thermal conductivity, and the lowest temperature at which the ceramic phase appears.

[0124] The closed-loop temperature control in step S4 of this invention ensures that the outlet gas temperature is lower than the decomposition initiation temperature of group A, preventing premature decomposition of group A during the drying process and preserving its heat absorption capacity. In contrast, Comparative Example 5 shows a significant decrease in retention rate due to the outlet temperature exceeding the decomposition initiation temperature, indicating that step S4 of this invention can guarantee the heat absorption performance of the finished product and achieve stable closed-loop control of the outlet temperature and fire resistance performance. The combination of in-situ deposition in step S2 and spray drying in step S4 of this invention ensures uniform distribution of each component within the particles. Comparative Example 4 shows a significant increase in the coefficient of variation of elemental content due to mechanical blending, and synergistic components cannot coexist closely within the particle micro-regions, demonstrating that the composite particle structure of this invention is a prerequisite for the effective synergistic effects of each level within the micro-regions.

[0125] Table 4. Data on thermal insulation barrier, retention rate of Group A, and microscopic uniformity:

[0126]

[0127] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing a mineral fireproofing powder based on endothermic decomposition synergy, characterized in that, The mineral fire-retardant powder, by weight of raw materials, consists of group A, group B, group C, and other components; wherein: Group A consists of 20-35 parts aluminum hydroxide, 10-20 parts boehmite, 10-20 parts hydromagnesia, and 8-15 parts calcium magnesium carbonate. Group B consists of 5-10 parts sepiolite, 4-8 parts fluorophlogopite, and 3-6 parts aluminum dihydrogen phosphate. Group C consists of 1.5–4 parts zinc hydroxystannate, 1–3 parts zinc molybdate, and 1.5–3 parts zinc borate; The other components consist of 3-8 parts expanded vermiculite, 0.5-2 parts 3-aminopropyltriethoxysilane, and 0.3-1 parts sodium hexametaphosphate; The zinc hydroxystannate of group C is partially deposited on the surface of the aluminum hydroxide, boehmite, hydromagnesia, and calcium magnesium carbonate particles of group A, forming a zinc hydroxystannate deposition coating layer; the particle surface also has a silanized layer formed by the hydrolysis and condensation of 3-aminopropyltriethoxysilane of the other components. The preparation method includes the following steps: S1, crush and classify each component of group A into multiple particle sizes, determine the blending ratio of each particle size according to the target particle size distribution curve of continuous gradation that makes the particles compact, blend them, stir and mix until uniform, and obtain heat-absorbing mineral gradation powder. S2, the heat-absorbing mineral grade powder is dispersed in water, sodium stannate and zinc sulfate are added to generate the zinc hydroxystannate deposition coating layer of group C on the particle surface in situ, and then 3-aminopropyltriethoxysilane of the other components is added to modify the particle surface, and the deposition-coated modified particles are obtained by filtration. S3, disperse the components of group B in water, then add zinc molybdate and zinc borate of group C, expanded vermiculite and sodium hexametaphosphate of the other components, and the deposited coated modified particles, mix at below 25°C to obtain a slurry, and carry out S4 within 30 minutes after the slurry is mixed; S4, the slurry is atomized and fed into a spray drying tower for drying and granulation. The temperature of the outlet gas of the spray drying tower is detected by a temperature sensor and fed back to the controller. The controller adjusts the slurry feed flow rate and hot air heating power according to the deviation between the outlet gas temperature and the set value, so that the outlet gas temperature is maintained within the set range that will not cause the decomposition of group A, and composite particles are obtained. S5, the composite particles are sieved to obtain the mineral fireproof powder; S4 includes: S41, the slurry is fed into the atomizer via a frequency conversion feed pump and atomized into droplets and then fed into the spray drying tower. Hot air heated by an electric heater is introduced into the spray drying tower to dry and granulate the droplets, and the temperature sensor is installed at the outlet of the spray drying tower. S42, the controller acquires the outlet gas temperature detected by the temperature sensor at a sampling period of 0.5 to 10 seconds, and obtains the deviation by subtracting the set value from the outlet gas temperature; S43, the controller calculates the increment of the speed setpoint of the variable frequency feed pump according to the deviation between the current sampling period and the two previous sampling periods using an incremental proportional-integral-derivative algorithm, and updates the speed setpoint accordingly, so that when the outlet gas temperature is higher than the set value, the speed setpoint is increased to increase the slurry feed flow rate and decrease the outlet gas temperature; S44, the controller limits the updated speed setpoint between a preset upper speed limit and a lower speed limit, and limits the integral action of the incremental proportional-integral-derivative algorithm; when the speed setpoint reaches the upper speed limit but the outlet gas temperature is still higher than the upper limit of the set range, the controller reduces the heating power of the electric heater; when the speed setpoint reaches the lower speed limit but the outlet gas temperature is still lower than the lower limit of the set range, the controller increases the heating power of the electric heater. S45, repeat S42 to S44 to maintain the outlet gas temperature within the set range; the set value is the target outlet gas temperature selected within the range of 85 to 115°C, the set range is the temperature range 2 to 10°C above and below the set value, and the upper limit of the set range is not higher than 115°C; the coefficient of variation of aluminum, magnesium, calcium and zinc content at different sampling points in the obtained composite particles is not greater than 10%, and the obtained composite particles do not show the characteristic peaks of oxides formed by the thermal decomposition of group A when detected by X-ray diffraction.

2. The method for preparing a mineral fireproofing powder based on endothermic decomposition synergy according to claim 1, characterized in that, Group A consists of 26-30 parts aluminum hydroxide, 13-17 parts boehmite, 12-16 parts hydromagnesia, and 9-13 parts calcium magnesium carbonate; Group B consists of 6-8 parts sepiolite, 5-7 parts fluorophlogopite, and 3-5 parts aluminum dihydrogen phosphate; Group C consists of 2-4 parts zinc hydroxystannate, 1.5-2.5 parts zinc molybdate, and 2-3 parts zinc borate; the other components consist of 4-6 parts expanded vermiculite, 0.8-1.5 parts 3-aminopropyltriethoxysilane, and 0.4-0.6 parts sodium hexametaphosphate.

3. The method for preparing a mineral fireproofing powder based on endothermic decomposition synergy according to claim 1, characterized in that, The mineral fire retardant powder is a composite particle with a median particle size of 20–40 μm.

4. The method for preparing a mineral fireproofing powder based on endothermic decomposition synergy according to claim 1, characterized in that, S1 includes: S11, aluminum hydroxide, boehmite, hydromagnesia and calcium magnesium carbonate of group A are respectively subjected to air jet milling and air jet classification to obtain powders of multiple particle sizes; S12, the volumetric particle size distribution of each particle size class was determined by laser diffraction particle size analysis to obtain the upper and lower limits of particle size for each particle size class; S13, calculate the volume fraction of each particle size according to the target particle size distribution curve, then convert the volume fraction to the mass fraction according to the density of each particle size powder, and weigh the powder of the corresponding particle size according to the mass fraction. S14, the weighed powders of each particle size are added to a mixer and stirred. The contents of aluminum hydroxide, boehmite, hydromagnesia and calcium magnesium carbonate in different sampling points of the mixer are determined by X-ray diffraction quantitative phase analysis. The coefficient of variation of the contents of the above four components at each sampling point is calculated. Mixing is stopped when the coefficient of variation is no greater than 5%, and the endothermic mineral graded powder is obtained.

5. The method of claim 4, wherein the mineral fireproofing powder is prepared by the endothermic decomposition synergy-based method, characterized in that, In S13, the target particle size distribution curve is determined by the following formula: ; wherein is the cumulative volume fraction of particles having a particle size less than is the cumulative volume fraction of particles having a particle size less than is the particle size of a particle; is the maximum particle size of a particle in the heat-absorbing mineral graded powder; is the minimum particle size of a particle in the heat-absorbing mineral graded powder; is the distribution modulus, taken as 0.21-0.30; the volume fraction of the first particle size is calculated according to the following formula: ; In the formula, For the first The volume fraction of each particle size in the heat-absorbing mineral powder; For the first Upper limit of particle size for each particle size class; For the first Lower limit of particle size for each particle size class; and The particle size calculated by the above formula is equal to and Cumulative volume fraction at time; The number represents the particle size, ranging from 1 to... , For the total number of particles, when When equal to 1 equal ,when equal hour equal ,and Greater than 0; convert the volume fraction to the first volume fraction using the following formula. Mass fraction per particle size: ; In the formula, For the first Mass fraction of each particle size; For the first Density of individual particle sizes; For the first Volume fraction of each particle size; for From 1 to The sum of the products of density and volume fraction of powder particles of each particle size; For the first Density of individual particle sizes; For the first Volume fraction of each particle size; The particle size index is used for summation; based on the mass fraction of each particle size. Weigh out the powder of the appropriate particle size.

6. The preparation method of mineral fire retardant powder based on endothermic decomposition synergy according to claim 1, characterized in that, S2 include: S21, the heat-absorbing mineral grade powder is dispersed in deionized water to obtain a suspension. Sodium stannate and zinc sulfate are added to the suspension at a molar ratio of tin to zinc of 1:

1. The mixture is reacted for 0.5 to 3 hours at a pH of 7.0 to 9.0 and a temperature of 25 to 60°C to allow zinc hydroxystannate to be deposited in situ on the particle surface. The amount of sodium stannate and zinc sulfate added is calculated as the mass fraction of zinc hydroxystannate in group C based on the theoretical production of zinc hydroxystannate. S22, add pre-hydrolyzed 3-aminopropyltriethoxysilane to the suspension after depositing zinc hydroxystannate, stir to graft a silanized layer onto the particle surface, then filter and wash until the filtrate is free of white turbidity when tested with barium chloride solution, and dry at a temperature not exceeding 120°C to obtain deposited and coated modified particles.

7. The method for preparing mineral fire retardant powder based on endothermic decomposition synergy according to claim 1, characterized in that, The incremental proportional-integral-differential algorithm described in S43 calculates the increment of the given speed value and updates the given speed value according to the following formula: ; In the formula, For the first The increment of the given rotational speed value in each sampling period; For the first The given rotational speed value for each sampling period; For the first The given rotational speed value for each sampling period; , , These are the non-negative discrete proportional gain, integral gain, and differential gain calculated based on the sampling period, respectively. , , The first , No. , No. Deviation per sampling period; The sampling period number is a positive integer; the deviation is calculated using the following formula: ; In the formula, For the first Deviation per sampling period; For the first The outlet gas temperature detected in each sampling cycle; The setpoint; the updated speed setpoint It is limited to between the lower speed limit and the upper speed limit.

8. A mineral fire-retardant powder based on endothermic decomposition synergy, characterized in that, It is prepared by the method of preparing mineral fire retardant powder based on endothermic decomposition synergy as described in any one of claims 1-7.

Citation Information

Patent Citations

  • Fireproofing flame retardation glass bead for reflective membrane and preparation method of fireproofing flame retardation glass bead

    CN104965249A

  • Fireproof and heat-insulating nano ceramic coating for lithium battery and preparation method of fireproof and heat-insulating nano ceramic coating

    CN121950144A

  • Preparation of vermiculite-based flame-retardant smoke-suppression filler and application of vermiculite-based flame-retardant smoke-suppression filler in silicone foam