A particle self-assembled bulk single crystal and its rapid preparation method
By employing a variable-temperature sintering method involving a mixture of nano- and micro-sized single-crystal particles, the problems of high energy consumption and high cost in the preparation of large-size bulk single crystals have been solved, achieving efficient and low-cost solid-state single-crystal production, which is suitable for the industrial production of various metal materials.
Patent Information
- Application Number
- CN202611249199.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-18
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2046-08-18
AI Technical Summary
Existing methods for preparing large-size bulk single crystals are energy-intensive, costly, and sensitive to process parameters, making it difficult to achieve efficient and low-cost solid-state single crystal formation. In particular, the self-assembly process of micron-sized grains suffers from low efficiency and poor reproducibility.
By using a mixture of nano- and micron-sized single-crystal powders and subjecting them to variable-temperature sintering under high pressure, and through multiple cycles of heating, holding, and cooling, the particles self-assemble to prepare large-size bulk single crystals, thus avoiding the melting process and the use of seed crystals or templates.
It enables the efficient preparation of large-size bulk single crystals at temperatures far below the material's melting point, reducing energy consumption and equipment costs, simplifying the process, improving growth efficiency, and is applicable to the single crystallization of various metal materials, making it suitable for industrial production.
Smart Images

Figure CN122773465B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of bulk single crystal technology, and in particular to a particle self-assembled bulk single crystal and its rapid preparation method. Background Technology
[0002] Single-crystal materials, due to their boundary-free microstructure, exhibit significantly superior mechanical, electrical, magnetic, and optical properties compared to polycrystalline materials, and are widely used in electronic functional devices, high-temperature alloy seed crystals, optical windows, and fundamental scientific research. For example, single-crystal nickel-based superalloys, with their excellent high-temperature creep and fatigue resistance, have become core materials for advanced aero-engine turbine blades; single-crystal copper, possessing both extremely high conductivity and ductility, has significant application value in high-frequency signal transmission and superconducting technology.
[0003] Currently, the industrial-scale preparation of large-size bulk single crystals mainly relies on melt growth techniques such as the Czochralski method, the Bridgman method, and the zone melting method. These methods share the common characteristic of requiring the raw materials to be heated above their melting point and completely melted before directional solidification to achieve single crystal growth. These methods are not only energy-intensive and require large equipment investments, but are also extremely sensitive to process parameters such as temperature gradient, pulling speed control, and crucible material, resulting in high preparation costs and making it difficult to meet the needs of large-scale applications.
[0004] In recent years, solid-state single-crystalization strategies based on the Abnormal Grain Growth (AGG) phenomenon have attracted widespread attention. AGG refers to the phenomenon during annealing where a small number of grains with specific orientations or energy advantages grow abnormally by engulfing surrounding smaller grains, eventually forming a single crystal or coarse-grained structure. Compared to the melting method, the solid-state AGG process does not require a liquid-solid phase transition and can theoretically achieve single-crystal conversion at temperatures far below the melting point, possessing significant energy-saving potential. However, existing AGG technologies mainly rely on a grain boundary diffusion-controlled atomic / ion migration mechanism (i.e., the classic Ostwald ripening mechanism). The grain growth rate is limited by the long-range diffusion of atoms at the grain boundaries, resulting in low growth efficiency, and the final grain size is often constrained by the initial microstructure and annealing time. Furthermore, this process is highly sensitive to the distribution of second-phase particles, texture type, and heat treatment window, leading to poor process reproducibility and limiting practical industrial applications.
[0005] On the other hand, in a liquid environment, nanocrystals can achieve directional self-assembly growth through the oriented attachment (OA) mechanism, where adjacent particles fuse directly after rotational orientation and lattice matching, exhibiting extremely high crystal growth efficiency. However, under solid-state conditions, the free rotation and ordered arrangement of micron-sized grains are greatly suppressed due to the presence of lattice rigidity and grain boundary pinning effects.
[0006] In summary, there is still a lack of a solid-state method for achieving orientational self-assembly of micron-sized grains without the aid of a liquid medium, which has become a key bottleneck in the development of solid-state single crystal preparation technology.
[0007] There is an urgent need to develop a particle self-assembled bulk single crystal and its rapid preparation method. The above-mentioned solid single crystal preparation method has the characteristics of high efficiency, low cost and simple process. Summary of the Invention
[0008] The purpose of this invention is to solve the technical problems existing in the prior art, and to propose a particle self-assembled bulk single crystal and its rapid preparation method.
[0009] This method has the following characteristics: By using nanoparticles to mediate the directional alignment and assembly of micron-sized grains, large-size bulk single crystals can be efficiently prepared under solid-state conditions without heating to above the material's melting point or using seed crystals or templates. The process is simple and inexpensive.
[0010] To achieve the above objectives, the present invention adopts the following technical solution: A rapid preparation method for particle self-assembled bulk single crystals includes the following preparation steps: (1) Mix powder materials of different particle sizes in a certain proportion to obtain mixed powder; The powder material consists of micron-sized single-crystal particles and nano-sized single-crystal particles; (2) Press the mixed powder obtained in step (1) into a preform under a protective atmosphere to obtain a preform; (3) The preform obtained in step (2) is subjected to variable temperature sintering under high pressure. Each variable temperature sintering process includes a heating section, a heat preservation section and a cooling section. (4) Repeat the variable temperature sintering cycle described in step (3) 5 to 20 times to obtain bulk single crystal material; In step (1), the molar ratio of the micron-sized single crystal particles to the nano-sized single crystal particles is 1:2 to 1:20; In step (3), the preform is subjected to variable temperature sintering under a pressure of 2~10 GPa. As a further improvement to this plan, In step (1), the average particle size of the micron-sized single crystal particles is 0.5~10 μm, and the average particle size of the nano-sized single crystal particles is 10~100 nm.
[0011] As a further improvement to this plan, In step (3), during the variable-temperature sintering process, The heating section heats the material from room temperature to 0.4~0.6Tm (Tm is the melting point of a metallic material at room temperature and pressure) at a rate of 5~50℃ / min. The insulation section is kept at 0.4-0.6Tm for 5-30 minutes; The cooling method of the cooling section is rapid water cooling quenching, and the interval between two adjacent temperature-changing sintering times (the time from the end of the previous heating to the start of the next heating) is controlled at 10-20 minutes.
[0012] As a further improvement to this plan, The single crystal material is selected from any one of nickel, copper, aluminum, gold, silver and their alloys.
[0013] A particle-self-assembled bulk single crystal is prepared by a rapid preparation method for particle-self-assembled bulk single crystals.
[0014] This invention provides a particle self-assembled bulk single crystal and its rapid preparation method, which has the following beneficial effects: (1) No melting required: The present invention can complete the preparation of single crystals at a temperature far below the melting point of the material (0.4-0.6Tm, where Tm is the melting point of the material), which greatly reduces energy consumption and equipment costs.
[0015] (2) No seed crystal or template required: This invention does not rely on pre-placed seed crystals or complex templates, which simplifies the process and reduces the difficulty of operation.
[0016] (3) High growth efficiency: The present invention drives grain self-assembly through variable temperature sintering cycle, and the single crystal growth rate is much higher than the abnormal grain growth under the traditional Ostwald ripening mechanism.
[0017] (4) Wide applicability: This invention can be further extended to the single crystal preparation of face-centered cubic metals and their alloys such as copper, aluminum, gold, and silver, and has good universality.
[0018] (5) Suitable for mass production: The process of this invention is simple, the cycle is short and the cost is controllable, making it suitable for large-scale industrial production. Attached Figure Description
[0019] Figure 1 This is a schematic diagram illustrating a method for achieving rapid growth of bulk single crystals using particle self-assembly.
[0020] Figure 2 The images show the SEM morphology of the micron-sized and nano-sized single-crystal particles in Example 1 of this invention. (a) Size distribution of nano-nickel (20 nm) particles; (b) Scanning electron morphology (SEM) of nano-nickel (20 nm) particles; (c) Transmission electron morphology (TEM) of nano-nickel (20 nm) particles; (d) Scanning electron morphology (SEM) of micron (1µm) nickel (particle) powder.
[0021] Figure 3 This is a schematic diagram comparing the variable temperature sintering and constant temperature sintering processes in Embodiment 1 of the present invention.
[0022] Figure 4 This is a crystal orientation distribution diagram of the bulk single crystal nickel prepared by the variable temperature sintering method in Example 1 of the present invention.
[0023] Figure 5 This is a SEM image of the micron-sized grain self-assembly process in Example 1 of the present invention.
[0024] Figure 6 This is a crystal orientation distribution diagram of the bulk single crystal nickel prepared by the variable temperature sintering method in Example 2 of the present invention.
[0025] Figure 7 This is a crystal orientation distribution diagram of the bulk single crystal nickel prepared by the isothermal sintering method in Comparative Example 1 of the present invention.
[0026] Figure 8 This is a crystal orientation distribution diagram of the sample prepared by temperature-controlled sintering of single-size micron-sized particles in Comparative Example 2 of this invention.
[0027] Figure 9 This is a crystal orientation distribution diagram of the sample prepared by temperature-variable sintering of single-size nanoparticles in Comparative Example 3 of the present invention. Detailed Implementation
[0028] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Example
[0029] (1) Take 60g of nickel microcrystalline particles with an average particle size of 1μm and 300g of nickel nanocrystalline particles with an average particle size of 20 nm, and mix them in a mixer for 8 hours at a molar ratio of 1:5 to obtain mixed powder.
[0030] (2) The mixed powder is pressed into a circular preform under the protective atmosphere of a glove box.
[0031] (3) The preform is encapsulated in a molybdenum crucible, placed in the high-pressure chamber of a large press, and then a pressure of 4 GPa is applied at a pressurization rate of 100 MPa / min. (4) After the target pressure of 4 GPa stabilizes, turn on the heating and perform variable temperature sintering: The temperature was increased from room temperature to 800℃ at a rate of 30℃ / min (800℃≈0.55Tm, where Tm is the melting point of nickel at room temperature and pressure), which is much lower than the melting point of nickel at 1453℃. The temperature was held for 10 minutes, then heating was stopped, and the temperature was then rapidly cooled to room temperature by water cooling to complete one cycle.
[0032] (5) Repeat the above variable temperature sintering cycle 5 times. The time interval between two adjacent variable temperature sintering cycles (the time from the end of the previous heating to the start of the next heating) should be controlled within 15 minutes.
[0033] (6) After the temperature-controlled sintering is completed, cut off the power supply and stop heating.
[0034] After the sample cools to room temperature, it is depressurized to atmospheric pressure at a rate of 100 MPa / min to obtain the nickel sample.
[0035] (7) Polish the surface of the sample after temperature sintering.
[0036] Characterized by white light Laue diffraction analysis, the obtained bulk single crystal nickel has a size of over 100 μm and a single grain orientation.
[0037] Figure 2 The images show the SEM morphology of the micron-sized and nano-sized single-crystal particles in Example 1 of this invention. It can be seen that the particle size distribution is relatively uniform, and the sphericity is good.
[0038] Figure 3 This is a schematic diagram comparing the variable temperature sintering and constant temperature sintering processes in Embodiment 1 of the present invention.
[0039] Figure 4 This is a crystal orientation distribution diagram of bulk single-crystal nickel prepared by the variable-temperature sintering method in Example 1 of the present invention. As can be seen from the figure, the size of the nickel single crystal can reach over 100 μm.
[0040] Figure 5 This is a SEM image of the micron-sized grain self-assembly process in Example 1 of the present invention. As can be seen from the image, the micron-sized particles are orderly embedded in the parent single crystal, confirming that the nanoparticles drive the self-assembly of the micron-sized particles into a larger single crystal during the variable-temperature sintering process. Example
[0041] Take 60g of nickel microcrystalline particles with an average particle size of 1 μm and 300g of nickel nanocrystalline particles with an average particle size of 20 nm, and mix them in a mixer for 8 hours at a molar ratio of 1:5 to obtain a mixed powder.
[0042] [Note: Because they are single crystals of the same metallic element:] Molar ratio = n(A) : n(B) = (60 / MA) : (300 / MB); That is, mass ratio = molar ratio. (2) The mixed powder is pressed into a circular preform under the protective atmosphere of a glove box.
[0043] (3) The preform is encapsulated in a molybdenum crucible, placed in the high-pressure chamber of a large press, and then a pressure of 4 GPa is applied at a pressurization rate of 100 MPa / min. (4) After the target pressure of 4 GPa stabilizes, turn on the heating and perform variable temperature sintering: The temperature is increased from room temperature to 800℃ (800℃≈0.55Tm, where Tm is the melting point of nickel material at room temperature and pressure) at a heating rate of 30℃ / min, held at that temperature for 10 minutes, then heating is stopped, and then the temperature is rapidly cooled to room temperature by water cooling to complete one cycle.
[0044] (5) Repeat the above variable temperature sintering cycle 10 times. The time interval between two adjacent variable temperature sintering cycles (the time from the end of the previous heating to the start of the next heating) should be controlled within 15 minutes.
[0045] (Compared to Example 1, Example 2 increased the number of cycles, indicating that the final single crystal size increases with the number of cycles.)
[0046] (6) After the temperature-controlled sintering is completed, the power supply is cut off and heating is stopped. After the sample cools to room temperature, the pressure is released to atmospheric pressure at a rate of 100 MPa / min to obtain the nickel sample.
[0047] (7) The surface of the sample after temperature sintering is polished. Characterized by white light Laue diffraction analysis, the obtained bulk single crystal nickel has a size of more than 300 μm and a single grain orientation.
[0048] Figure 6 This is a crystal orientation distribution diagram of bulk single-crystal nickel prepared by the variable-temperature sintering method in Example 2 of the present invention. As shown in the diagram, increasing the number of variable-temperature sintering cycles allows for further growth of the crystal size. This indicates that the grain size can be controlled by increasing the number of sintering cycles.
[0049] Comparative Example 1: (1) Take 60g of nickel microcrystalline particles with an average particle size of 1 μm and 300g of nickel nanocrystalline particles with an average particle size of 20 nm, mix them in a mixer at a molar ratio of 1:5 for 8 hours to obtain mixed powder.
[0050] (2) The mixed powder is pressed into a circular preform under the protective atmosphere of a glove box.
[0051] (3) The preform is encapsulated in a molybdenum crucible, placed in the high-pressure chamber of a large press, and then a pressure of 4 GPa is applied at a pressurization rate of 100 MPa / min.
[0052] (4) After the target pressure of 4 GPa stabilizes, turn on the heating and perform isothermal sintering: The temperature was increased from room temperature to 800℃ (800℃≈0.55Tm, where Tm is the melting point of nickel material at room temperature and pressure) at a heating rate of 30℃ / min, and then held at that temperature for 100 minutes and 200 minutes respectively. After heating was stopped, the temperature was rapidly cooled to room temperature by water cooling. [Comparative Example 1 did not have a cyclic temperature change and only included one heating → holding → cooling process, while Example 1 or 2 included the above multiple heating and cooling processes].
[0053] (5) After the isothermal sintering is completed, the power supply is cut off and heating is stopped. After the sample cools to room temperature, the pressure is released to atmospheric pressure at a rate of 100 MPa / min to obtain the nickel sample.
[0054] (6) Polish the surface of the sample after constant temperature sintering and perform microstructure characterization analysis.
[0055] Figure 7 This is a crystal orientation distribution diagram of the bulk single-crystal nickel prepared by the isothermal sintering method in Comparative Example 1 of this invention. Compared with Example 1, it can be found that isothermal sintering of the same composition does not effectively induce grain growth; the grain size is less than 10 μm, much smaller than that of the sample sintered at variable temperatures. Even extending the heat treatment time cannot yield larger single-crystal materials.
[0056] Comparative Example 2: (1) Take 300g of nickel micron-sized particles with an average particle size of 1μm and press them into a circular preform under the protective atmosphere of a glove box.
[0057] (2) The preform is encapsulated in a molybdenum crucible, placed in the high-pressure chamber of a large press, and then a pressure of 4 GPa is applied at a pressurization rate of 100 MPa / min.
[0058] (3) After the target pressure of 4 GPa stabilizes, start heating and perform variable temperature sintering: The temperature is increased from room temperature to 800℃ (800℃≈0.55Tm, where Tm is the melting point of nickel material at room temperature and pressure) at a heating rate of 30℃ / min, held at that temperature for 10 minutes, then heating is stopped and the material is rapidly cooled to room temperature by water cooling to complete one cycle.
[0059] (4) Repeat the above variable temperature sintering cycle 10 times. The time interval between two consecutive variable temperature sintering cycles should be controlled at 15 minutes.
[0060] (5) After the temperature-controlled sintering is completed, the power supply is cut off and heating is stopped. After the sample cools to room temperature, the pressure is released to atmospheric pressure at a rate of 100 MPa / min to obtain the nickel sample.
[0061] (6) Polish the surface of the sample after temperature sintering and perform microstructure characterization and analysis.
[0062] Figure 8 This is a crystal orientation distribution diagram of the sample prepared by temperature-controlled sintering of single-sized micron-sized particles in Comparative Example 2 of this invention. As can be seen from the diagram, only the micron-sized particles did not exhibit large-sized single crystals after sintering. This indicates that without nano-sized grains as a medium, micron-sized particles cannot easily self-assemble into single crystals through self-adjustment of orientation or ordered arrangement.
[0063] Comparative Example 3: Similarly, 300g of nickel nanocrystal particles with an average particle size of 20 nm were pressed into a circular preform under the protective atmosphere of a glove box.
[0064] The preform is encapsulated in a molybdenum crucible, placed in the high-pressure chamber of a large press, and then a pressure of 4 GPa is applied at a pressurization rate of 100 MPa / min.
[0065] After the target pressure of 4 GPa stabilizes, heating is started for variable temperature sintering: the temperature is increased from room temperature to 800℃ at a rate of 30℃ / min (800℃≈0.55Tm, where Tm is the melting point of nickel material at room temperature and pressure), held for 10 minutes, then heating is stopped and the material is rapidly cooled to room temperature by water cooling to complete one cycle.
[0066] Repeat the above variable-temperature sintering cycle 10 times. The time interval between two consecutive variable-temperature sintering cycles should be controlled at 15 minutes.
[0067] After the variable-temperature sintering is completed, the power supply is cut off and heating is stopped. After the sample cools to room temperature, the pressure is released to atmospheric pressure at a rate of 100 MPa / min to obtain the nickel sample.
[0068] The surface of the sample after variable-temperature sintering was polished and its microstructure was characterized and analyzed.
[0069] Figure 9 This is a crystal orientation distribution diagram of the sample prepared by temperature-controlled sintering of single-size nanoparticles in Comparative Example 3 of this invention. As can be seen from the figure, only the nanoparticles show localized grain growth after sintering, but the size is still relatively small compared to the mixed size. This is related to the large surface energy of the nanoparticles and the rapid grain boundary diffusion.
[0070] In Comparative Examples 2 and 3, only single-sized grains were used as the initial powder, and no larger single crystals were observed. This indicates that both micron-sized and nano-sized particles are indispensable in the self-assembly process for preparing single crystals.
[0071] During variable-temperature sintering, nanoscale single-crystal particles, due to their high surface energy and low melting point, undergo surface softening and partial melting during the heating stage, forming a viscous dielectric layer encapsulating the micron-sized grains. During the cooling stage, the partially molten nanoparticles epitaxially crystallize on the surface of the micron-sized grains, forming an ordered atomic arrangement and inducing rotational orientation of the micron-sized grains.
[0072] Due to the lattice-matching relationship between nanoparticles and micron-sized grains, driven by the thermal stress and interfacial energy generated by temperature cycling, the micron-sized grains embedded in the nanoparticle medium gradually rotate to the same orientation as the surrounding nanocrystals. As the number of temperature cycles increases, more and more micron-sized grains align and eventually come into contact with each other and merge to form large-sized single crystals.
[0073] Compared with traditional isothermal sintering, variable temperature sintering introduces internal stress through thermal cycling, providing a continuous driving force for the rotation and orientation of micron-sized grains. At the same time, the "gluing" effect of nanoparticles ensures orientation consistency, thereby realizing grain self-assembly growth.
[0074] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for rapid preparation of a self-assembled bulk single crystal of particles, comprising: The preparation steps include the following: (1) Mix powder materials of different particle sizes in a certain proportion to obtain mixed powder; The powder material consists of micron-sized single-crystal particles and nano-sized single-crystal particles; (2) Press the mixed powder obtained in step (1) into a preform under a protective atmosphere to obtain a preform; (3) The preform obtained in step (2) is subjected to variable temperature sintering under high pressure. Each variable temperature sintering process includes a heating section, a heat preservation section and a cooling section. (4) Repeat the variable temperature sintering cycle described in step (3) 5 to 20 times to obtain bulk single crystal material; In step (1), the molar ratio of the micron-sized single crystal particles to the nano-sized single crystal particles is 1:2 to 1:20; In step (3), the preform is subjected to variable-temperature sintering under a pressure of 2~10 GPa; In step (1), the average particle size of the micron-sized single crystal particles is 0.5~10 μm, and the average particle size of the nano-sized single crystal particles is 10~100 nm. In step (3), during the variable-temperature sintering process, The heating section heats the material from room temperature to 0.4~0.6Tm, where Tm is the melting point of the metal material at room temperature and pressure, and the heating rate is 5~50℃ / min. The insulation section is kept at 0.4~0.6Tm for 5~30 minutes; The cooling method of the cooling section is rapid water cooling quenching, and the time interval between two adjacent temperature-changing sintering is controlled at 10 to 20 minutes. The single crystal material is selected from any one of nickel, copper, aluminum, gold, silver and their alloys.
Citation Information
Patent Citations
Preparation method of NiTi single crystal cyclic heat treatment in solid state
CN109136806A
Method for preparing single-crystal positive electrode material, single-crystal positive electrode material and lithium ion battery
CN118529785A
Method for synthesizing Se crystal at high temperature and high pressure
CN120485948A