MEMS infrared light source based on alternating layers of dual films and its fabrication method

By employing a dual-film alternating stacked structure and a square protrusion micro/nano structure on a MEMS infrared light source, the problems of low emissivity and easy failure at high temperatures in MEMS infrared light sources are solved, achieving compatibility between high emissivity and high thermal stability, making it suitable for standard wafer-level manufacturing.

CN122789339BActive Publication Date: 2026-11-17SHENZHEN MEISI XIANRUI ELECTRONICS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611265891.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-17
Estimated Expiration
2046-08-20

AI Technical Summary

Technical Problem

Existing MEMS infrared light sources suffer from low emissivity and low operational reliability, especially prone to failure at extreme high temperatures and difficult to mass-produce.

Method used

The method for fabricating MEMS infrared light sources based on alternating layers of dual films includes growing a support film on a silicon substrate, depositing a heated metal layer and multiple silicon nitride and titanium nitride films, forming a matrix-arranged square protrusion structure through photolithography and etching, and forming a back cavity structure by combining rapid thermal annealing.

Benefits of technology

It achieves a balance between high emissivity and high thermal stability, is compatible with standard wafer-level manufacturing processes, and improves device reliability and mass production capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122789339B_ABST
    Figure CN122789339B_ABST
Patent Text Reader

Abstract

This invention discloses a MEMS infrared light source based on alternating layers of a dual-film system and its fabrication method. The fabrication method includes cleaning a silicon substrate and growing SiO2. x A support film is formed, followed by a heated metal layer. Then, a first silicon nitride film, a first titanium nitride film, and a second silicon nitride film are sequentially deposited to form an infrared emitting layer. A matrix of square protrusions is formed through photolithography and inductively coupled plasma dry etching. The resulting MEMS infrared light source comprises a stacked support film, a heated metal layer, and an infrared emitting layer, exhibiting a matrix of square protrusions and a back cavity structure. This application achieves a balance between high emissivity and high thermal stability through the synergistic effect of the alternating stacked dual-film structure and the square protrusion micro / nano structure, while remaining compatible with standard wafer-level manufacturing processes. This effectively solves the problems of low emissivity, high-temperature failure, and difficulty in mass production associated with existing devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of infrared sensor technology, and in particular to a MEMS infrared light source based on alternating stacked dual-film systems and its fabrication method. Background Technology

[0002] Microelectromechanical systems (MEMS) infrared light sources are the core radiating elements of nondispersive infrared gas sensors, thermal imagers, and flame detectors. With the rapid development of the Internet of Things (IoT), environmental monitoring, and medical diagnostic technologies, the application of gas sensors based on nondispersive infrared (NDIR) spectroscopy technology is becoming increasingly widespread. As the core micro-nano light-emitting device of gas sensing chips, the infrared radiation efficiency, modulation speed, and long-term stability at extreme high temperatures of MEMS infrared light sources directly determine the overall performance and power consumption of the sensing system.

[0003] However, in order to obtain high radiation power in specific gas absorption bands (such as 3~14um), the existing MEMS infrared light sources have mainly gone through the following two stages of technological evolution, but they all face insurmountable technical bottlenecks in actual industrial applications.

[0004] (1) First stage: Traditional MEMS light sources without specific infrared radiation layers; Early MEMS infrared light sources had relatively simple structures, usually only containing basic micro-heater traces (such as polysilicon Poly-Si, or independent flat metal Pt, W, etc. coils), and their surfaces were not subjected to any micro-nano patterning or radiation enhancement treatment. Such light sources have the following fatal defects when working: extremely low inherent emissivity and low electro-optical conversion efficiency: The inherent emissivity of flat metal or semiconductor surfaces in the infrared band is usually low (generally less than 0.4). According to the Stefan-Boltzmann law, in order to obtain sufficient infrared radiation energy, the driving chip has to apply extremely high current, making the heater work at an extreme incandescent temperature of 600°C or even 800°C or higher; this results in the power consumption of the entire sensor system reaching hundreds of milliwatts. At the same time, extreme high temperature accelerates thermal failure: Due to long-term exposure to extreme high temperature and the corrosion of oxygen in the air, polysilicon is prone to severe oxidation, leading to resistance drift; while ordinary metal traces face severe grain coarsening, melting, and even transient open circuit failure, resulting in extremely short device life.

[0005] (2) Second stage: Existing commonly used MEMS light sources with discrete infrared radiation layers; To solve the aforementioned power consumption problem, existing advanced light sources typically add an additional infrared radiation enhancement layer above the bottom micro-heater. The most commonly used radiation layers currently include "carbon nanotube (CNT) coatings" and "black gold loose amorphous structures". Commonly used "black gold" or "carbon nanotube" coatings are extremely susceptible to scratches and undergo severe recrystallization and sintering shrinkage above 400°C, resulting in a rapid decay of emissivity. Due to the risk of contamination and inability to withstand conventional photolithography etching processes, materials such as "black gold" or "carbon nanotubes" cannot be introduced into standard semiconductor foundries for mass wafer-level manufacturing, greatly limiting their industrial mass production. Therefore, existing MEMS infrared light sources suffer from low emissivity and low operational reliability. Summary of the Invention

[0006] This invention provides a MEMS infrared light source based on alternating stacked dual-film systems and its fabrication method, aiming to solve the problems of low emissivity and low operational reliability of MEMS infrared light sources in existing technologies.

[0007] In a first aspect, embodiments of this application provide a method for fabricating a MEMS infrared light source based on alternating layers of a dual-film system, wherein the fabrication method includes: Clean the silicon substrate; A support film is grown on the upper surface of the silicon substrate using plasma-enhanced chemical vapor deposition; the support film is made of SiO2. x ; A patterned mask is processed on the surface of the support film, and then a heated metal layer corresponding to the patterned mask is deposited by magnetron sputtering. The patterned mask is then removed by a stripping process. A first silicon nitride film is deposited on the surface of the heated metal layer using a magnetron sputtering process; A first titanium nitride film was obtained by depositing a chlorine-free precursor atomic layer deposition process on the surface of the first silicon nitride film. A second silicon nitride film is deposited on the surface of the first titanium nitride film using a magnetron sputtering process; Photoresist is spin-coated onto the surface of the second silicon nitride film, and a multi-step alignment photolithography process is used to perform photolithography and development to form a grid-shaped etched area. Inductively coupled plasma dry etching is used to etch away the non-bottom layer in the infrared emitting layer corresponding to the grid-shaped etched area, forming a matrix of square protrusions; the infrared emitting layer is composed of a first silicon nitride film, a first titanium nitride film and a second silicon nitride film. The photoresist was removed by dry plasma etching followed by rapid thermal annealing. The silicon substrate is etched on the side opposite to the infrared emitting layer to form an inwardly recessed back cavity, resulting in a MEMS infrared light source based on alternating layers of a dual-film system.

[0008] Secondly, embodiments of this application also provide a MEMS infrared light source based on alternating stacked dual-film system. The MEMS infrared light source is fabricated by the fabrication method of the MEMS infrared light source based on alternating stacked dual-film system as described in the first aspect above. The MEMS infrared light source includes a support film, a heating metal layer, a first silicon nitride film, a first titanium nitride film, and a second silicon nitride film stacked on a silicon substrate. The first silicon nitride film, the first titanium nitride film, and the second silicon nitride film constitute an infrared emitting layer; the infrared emitting layer includes square protrusions arranged in a matrix, the square protrusions abutting against the top layer of the first silicon nitride film; the silicon substrate has an inwardly recessed back cavity on the side away from the infrared emitting film.

[0009] This invention provides a MEMS infrared light source based on alternating layers of a dual-film system and its fabrication method. The fabrication method includes cleaning a silicon substrate and growing SiO2. x A support film is formed, followed by a heated metal layer. Then, a first silicon nitride film, a first titanium nitride film, and a second silicon nitride film are sequentially deposited to form an infrared emitting layer. A matrix of square protrusions is formed through photolithography and inductively coupled plasma dry etching. The resulting MEMS infrared light source comprises a stacked support film, a heated metal layer, and an infrared emitting layer, exhibiting a matrix of square protrusions and a back cavity structure. This application achieves a balance between high emissivity and high thermal stability through the synergistic effect of the alternating stacked dual-film structure and the square protrusion micro / nano structure, while remaining compatible with standard wafer-level manufacturing processes. This effectively solves the problems of low emissivity, high-temperature failure, and difficulty in mass production associated with existing devices. Attached Figure Description

[0010] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the following description of the embodiments will be briefly introduced. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0011] Figure 1 A flowchart illustrating the fabrication method of a MEMS infrared light source based on alternating stacked dual-film systems provided in an embodiment of the present invention; Figure 2 Another flowchart of the fabrication method of MEMS infrared light source based on alternating stacking of dual films provided in the embodiments of the present invention; Figure 3 A schematic diagram illustrating the fabrication process of a MEMS infrared light source based on alternating layers of dual films, as provided in an embodiment of the present invention. Figure 4 This is a schematic diagram illustrating another fabrication process of a MEMS infrared light source based on alternating layers of dual films, provided in an embodiment of the present invention. Figure 5 A top view of a MEMS infrared light source based on alternating layers of dual films provided in an embodiment of the present invention; Figure 6 A partial cross-sectional view of a MEMS infrared light source based on alternating layers of dual films provided in an embodiment of the present invention; Figure 7 This is another partial cross-sectional view of a MEMS infrared light source based on alternating layers of dual films provided in an embodiment of the present invention; Figure 8 A schematic diagram illustrating the application effect of a MEMS infrared light source based on alternating layers of dual films provided in an embodiment of the present invention; Figure 9 This is a schematic diagram illustrating another application effect of the MEMS infrared light source based on alternating layers of dual films provided in an embodiment of the present invention.

[0012] Reference numerals: 1. Silicon substrate; 2. Support film; 3. Heating metal layer; 4. First silicon nitride film; 5. First titanium nitride film; 6. Second silicon nitride film; 7. Second titanium nitride film; 8. Third silicon nitride film; 11. Back cavity; 21. Square protrusion; 22. Grid-shaped etched area. Detailed Implementation

[0013] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0014] It should be understood that, when used in this specification and the appended claims, the terms "comprising" and "including" indicate the presence of the described features, integrals, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integrals, steps, operations, elements, components and / or collections thereof.

[0015] It should also be understood that the terminology used in this specification is for the purpose of describing particular embodiments only and is not intended to limit the invention. As used in this specification and the appended claims, the singular forms “a,” “an,” and “the” are intended to include the plural forms unless the context clearly indicates otherwise. It should also be understood that the term “and / or” as used in this specification and the appended claims refers to any combination and all possible combinations of one or more of the associated listed items, and includes such combinations.

[0016] This application discloses a method for fabricating a MEMS infrared light source based on alternating stacked dual-film systems, wherein the method is used to fabricate a MEMS infrared light source based on alternating stacked dual-film systems; please refer to... Figure 1 As shown in the figure, this application provides a method for fabricating a MEMS infrared light source based on alternating layers of a dual-film system. This method includes steps S1 to S10, which correspond to... Figure 3 The preparation process is shown.

[0017] S1. Clean the silicon substrate.

[0018] In this embodiment, a silicon substrate is used as the physical support platform for the entire MEMS device. Before using the silicon substrate, it can be cleaned; specifically, the cleaning process aims to remove contaminants such as particles, organic matter, and metal ions from the surface of the silicon substrate, providing a clean substrate for subsequent thin film deposition. The surface smoothness and cleanliness directly affect the adhesion quality and interface characteristics of each thin film layer. This step corresponds to... Figure 3 Figure 1) and Figure 4 Figure 1) in the middle.

[0019] In a more specific embodiment, the cleaning process may first remove organic matter and particles by using a mixture of ammonia, hydrogen peroxide and water, wherein the mass fractions of ammonia and hydrogen peroxide in the mixture are 0.5-4.5% and 1-5%, respectively; then, the metal contaminants may be removed by using a mixture of hydrochloric acid, hydrogen peroxide and water, wherein the mass fractions of hydrochloric acid and hydrogen peroxide in the mixture are 3-20% and 2.5-8%, respectively. Finally, the silicon substrate is cleaned with a diluted buffered hydrofluoric acid solution. The buffered hydrofluoric acid solution (BHF) can be an aqueous solution prepared by mixing ammonium fluoride and hydrofluoric acid in a mass ratio of (6~10):1, wherein the preferred concentration range of HF is 0.1%–5% (volume fraction). The buffered hydrofluoric acid solution has the chemical property of selectively etching silicon dioxide while having an extremely low corrosion rate on single-crystal silicon. In this embodiment, the buffered hydrofluoric acid solution is used to remove the nanoscale silicon dioxide layer (thickness of 1–2 nm) that naturally forms on the surface of the silicon substrate due to exposure to air, so that the upper and lower surfaces of the silicon substrate are exposed to clean and active silicon. In this application, the silicon substrate may be immersed in a constant temperature (20–25°C) buffered hydrofluoric acid solution for 30–120 seconds, followed by rinsing with deionized water and drying with nitrogen.

[0020] S2. A support film is grown on the upper surface of the silicon substrate using plasma-enhanced chemical vapor deposition (PECVD); the support film is made of SiO₂. x .

[0021] Specifically, the support film is grown using plasma-enhanced chemical vapor deposition (PECVD), a process that enables high-quality film deposition at relatively low temperatures. The film is made of silicon oxide, which exhibits good thermal stability and insulation properties. This step corresponds to... Figure 3 Figure 2) and Figure 4 Figure 2) in the middle.

[0022] In a more specific embodiment, the deposition process may use silane and nitrous oxide as reactant gases, which decompose and react under radio frequency power to generate a silicon oxide thin film. The thickness of the support film can be set, for example, between 200 and 2000 nm, depending on the mechanical strength requirements of the device. The SiO₂ deposited using the above-described PECVD (plasma-enhanced chemical vapor deposition) process... x The support membrane can effectively support the subsequent heating metal layer and infrared emitting layer, and provide a structural basis for the final release cavity.

[0023] S3. A patterned mask is processed on the surface of the support film, and a heated metal layer corresponding to the patterned mask is deposited by magnetron sputtering. The patterned mask is then removed by a stripping process.

[0024] In this embodiment, a heated metal layer is used to generate Joule heat upon energization, thereby heating the upper infrared emitting layer. Specifically, the steps first involve spin-coating photoresist onto the support film surface, followed by photolithography and development to form a patterned photoresist mask. This mask defines the trace shape of the heated metal layer. Subsequently, a metal thin film is deposited using magnetron sputtering, covering the mask surface and the exposed support film surface. Finally, a lift-off process is used to remove the photoresist mask and the metal above it, leaving only the heated metal layer corresponding to the mask pattern on the support film surface. This step corresponds to... Figure 3 Figure 3) and Figure 4 Figure 3 in the middle.

[0025] In a more specific embodiment, the material of the heated metal layer may be, for example, tungsten, gold, platinum or titanium nitride; or, for example, nickel-chromium alloy or tantalum alloy.

[0026] By combining the above-mentioned stripping process with magnetron sputtering, a heated metal layer with precise control over pattern accuracy and edge steepness can be prepared, avoiding corrosion of the metal sidewalls by wet etching and thus improving heating uniformity.

[0027] In a more specific embodiment, the method for preparing the heated metal layer includes: obtaining a heated metal layer of 50-500 nm by metal magnetron sputtering; the power of the metal magnetron sputtering is 100-200 W, the chamber pressure is 2.2-3.8 mTorr, the Ar gas flow rate is 50-100 sccm, and the film formation rate of the heated metal layer is 5-10 nm / min; the material of the heated metal layer is tungsten, gold, platinum, or titanium nitride.

[0028] Specifically, the process of preparing the heated metal layer is carried out in an argon atmosphere, with the chamber pressure controlled at 2.2–3.8 mTorr, the sputtering power set at 100–200 W, and the film deposition rate controlled at 5–10 nm / min, ultimately yielding a heated metal layer with a thickness of 50–500 nm. By combining the above-mentioned lift-off process with magnetron sputtering, a heated metal layer with precisely controlled pattern accuracy and edge steepness can be prepared, avoiding corrosion of the metal sidewalls by wet etching, thereby improving heating uniformity.

[0029] Specifically, a 50-500 nm heated metal layer is obtained through metal magnetron sputtering. As the core of electrothermal conversion in the MEMS infrared light source, the physical morphology and microstructure of the heated metal layer directly determine the efficiency of the Joule heating effect and the uniformity of temperature distribution. This heated metal layer is not a simple metal stack, but a dense conductive film formed by high-energy particle bombardment and atomic rearrangement. It heats the upper infrared emitting layer by converting the directional drift motion of charge carriers into thermal vibration of the lattice. The layer is prepared by metal magnetron sputtering, which is based on the glow discharge principle. In a vacuum environment, an electric field is used to ionize Ar gas to generate high-energy Ar ions. The Ar ions are accelerated and bombard the surface of the target material under the high voltage attraction of the cathode target, causing the target atoms to be sputtered out and deposited on the prepared support film.

[0030] In a more specific embodiment, the thickness of the processed heated metal layer is controlled between 50 and 500 nm. The lower limit of the thickness is set at 50 nm to ensure that the film layer is continuous and dense, and to avoid the sharp increase in resistance and electromigration failure caused by the island growth effect. The upper limit of the thickness is set at 500 nm to control the heat capacity of the film layer and to prevent the thermal response time constant from increasing due to excessive thickness, thereby meeting the application requirements of MEMS devices for fast modulation.

[0031] For example, for applications requiring rapid thermal response, the thickness of the heating metal layer can be set to 50~150nm; for applications that primarily focus on high radiant power and do not have strict requirements on modulation speed, the thickness can be set to 300~500nm.

[0032] This thickness control allows for optimization of the device's thermal dynamics while ensuring electrothermal conversion efficiency. Furthermore, the metal magnetron sputtering power is 100–200 W, the chamber pressure is 2.2–3.8 mTorr, the Ar gas flow rate is 50–100 sccm, and the film formation rate of the heated metal layer is 5–10 nm / min.

[0033] Specifically, the process parameters of metal magnetron sputtering are the key factors that determine the microstructure and performance of the heated metal layer. Setting the sputtering power to 100~200W provides sufficient sputtering yield while avoiding excessive power that could cause the target to overheat and evaporate or introduce too many defect energy levels.

[0034] In a more specific embodiment, the chamber pressure is maintained at 2.2~3.8 mTorr. This low-pressure environment helps to increase the mean free path of sputtered particles, so that the deposited atoms have higher kinetic energy when they reach the substrate surface, thereby forming a dense film layer with a tight structure and low porosity, and improving the metal layer's resistance to electromigration and high-temperature stability.

[0035] The Ar gas flow rate is controlled at 50~100 sccm. The flow rate directly determines the stability of the plasma density and sputtering rate in the chamber. Within this flow rate range, the plasma maintains a stable glow discharge state, ensuring the uniformity of the deposition process.

[0036] The above process parameters work together to precisely control the film formation rate of the heated metal layer at 5~10nm / min. This rate range is a balance point: if the rate is too slow, it will significantly reduce production efficiency and increase the risk of interface contamination; if the rate is too fast, it will easily cause the deposited atoms to not have enough time to migrate and reconstruct on the substrate surface, forming a loose and porous columnar crystal structure, resulting in large sheet resistance dispersion and insufficient mechanical adhesion strength.

[0037] By limiting the film formation rate to 5~10 nm / min, a heated metal layer with low stress, low roughness and good step coverage can be obtained, thereby ensuring that the film layer does not crack or peel off during subsequent high-temperature cycling.

[0038] The heating metal layer is made of tungsten, gold, platinum, or titanium nitride. All four materials have mature semiconductor manufacturing processes and can be used in conjunction with SiN. x The TiN thin film layer achieves a good match in terms of thermal expansion coefficient. For example, in actual preparation, depending on the temperature rise requirements and cost budget of the specific application scenario, platinum can be selected as the heating metal layer material to maintain long-term stable electrical resistance characteristics at high temperatures; or titanium nitride can be selected to pursue lower cost and high mechanical strength. This material limitation ensures that the heating metal layer can withstand the test of subsequent high-temperature process steps such as rapid thermal annealing while providing a stable heat source, without performance degradation.

[0039] S4. A first silicon nitride film is deposited on the surface of the heated metal layer using a magnetron sputtering process.

[0040] In this embodiment, a first silicon nitride film is used as part of the infrared emitting layer, forming a heterojunction with the subsequently deposited titanium nitride film to control infrared emission characteristics. Specifically, the first silicon nitride film directly covers the heated metal layer, protecting the metal layer and participating in optical interference. Furthermore, the magnetron sputtering process can obtain a silicon nitride thin film with high density and tunable refractive index. This step corresponds to... Figure 3 Figure 4) and Figure 4 Figure 4)

[0041] In a more specific embodiment, the deposition process can, for example, employ radio frequency magnetron sputtering, using high-purity silicon as the target material, and reactive sputtering is performed in a mixed atmosphere of nitrogen and argon, with the stoichiometry of the film controlled by adjusting the nitrogen-argon flow rate ratio; alternatively, reactive DC sputtering can be used, applying a DC bias voltage to the silicon target to introduce nitrogen gas to react and generate SiNx. The thickness of the first silicon nitride film can, for example, be set to 300~700 nm.

[0042] The aforementioned dense first silicon nitride film can not only isolate the heated metal layer from the external environment and prevent high-temperature oxidation, but also serve as a dielectric film for the optical resonant cavity, enhancing the infrared radiation efficiency in a specific wavelength band.

[0043] S5. A first titanium nitride film is obtained by depositing a chlorine-free precursor atomic layer deposition process on the surface of the first silicon nitride film.

[0044] In this embodiment, the first titanium nitride film is a key absorbing / emitting layer in the core dual-film alternating stacked structure of this application. Its microstructure and crystal structure directly determine the emissivity level of the device. Specifically, the atomic layer deposition process has self-limiting growth characteristics, enabling atomic-level thickness control and excellent step coverage of the thin film. Furthermore, the use of a chlorine-free precursor effectively avoids the contamination and corrosion of device performance by residual chlorine. This step corresponds to... Figure 3 Figure 5) and Figure 4 Figure 5 in the middle.

[0045] In a more specific embodiment, during the deposition process, for example, a precursor pulse and an ammonia (NH3) plasma pulse can be alternately introduced into the reaction chamber to generate a TiN film through a surface saturation adsorption reaction. The precursor can be, for example, tetra(dimethylamino)titanium or tetra(ethylmethylamino)titanium. The above process employs thermal ALD (atomic layer deposition), using ammonia as a nitrogen source for the reaction. The thickness of the first titanium nitride film can be controlled, for example, between 5 and 30 nm.

[0046] The above-mentioned chlorine-free precursor ALD process can be used to prepare a first titanium nitride film with a smooth interface, controllable roughness, and pure composition, providing a high-quality physical basis for exciting local surface plasmon resonance modes.

[0047] S6. A second silicon nitride film is deposited on the surface of the first titanium nitride film using a magnetron sputtering process.

[0048] In this embodiment, a second silicon nitride film is used to cover the first titanium nitride film, together with the first silicon nitride film, to form a protective structure for the titanium nitride layer, thus forming SiN. x -TiN-SiN x Sandwich-type membrane system.

[0049] Specifically, the structure utilizes the high light transmittance of silicon nitride and the loss characteristics of titanium nitride to construct an optical resonant cavity, thereby significantly improving the infrared emissivity over a wide wavelength range. Furthermore, the deposition process of the second silicon nitride film is similar to that in step S4, also employing magnetron sputtering to ensure stress matching and adhesion between the film layers. This step corresponds to... Figure 3 Figure 6) and Figure 4 Figure 6 in the middle.

[0050] In a more specific embodiment, the thickness of the second silicon nitride film can be set to be no less than the thickness of the first silicon nitride film to provide sufficient physical protection and adjust the optical resonant wavelength; alternatively, the specific thickness value can be calculated by simulation using optical thin film design software according to the requirements of the target emission wavelength. By depositing the second silicon nitride film as described above, the core infrared emitting layer of the alternating double-film system is prepared, effectively isolating the TiN layer and preventing its oxidation failure in subsequent high-temperature processes.

[0051] In a more specific embodiment, such as Figure 2 As shown, step S6 is followed by steps S61-S62. S61: A second titanium nitride film is deposited on the surface of the second silicon nitride film using a chlorine-free precursor atomic layer deposition process; S62: A third silicon nitride film is deposited on the surface of the second titanium nitride film using a magnetron sputtering process; the infrared emitting layer is composed of a first silicon nitride film, a first titanium nitride film, a second silicon nitride film, a second titanium nitride film, and a third silicon nitride film. The corresponding steps are respectively... Figure 4 Figure 7) and Figure 4 Figure 8 in the middle.

[0052] Specifically, a second titanium nitride film is obtained by depositing a chlorine-free precursor atomic layer deposition process on the surface of a second silicon nitride film. The second titanium nitride film is grown on the surface of the prepared second silicon nitride film using atomic layer deposition technology. Compared with conventional physical vapor deposition, atomic layer deposition process can achieve layer-by-layer growth of materials in the form of single atomic layers, thereby achieving atomic-level precise control of film thickness.

[0053] In a more specific embodiment, a chlorine-free precursor is selected as the titanium source gas, and it is deposited in conjunction with reactive gases such as ammonia to form a chlorine-free precursor atomic layer deposition process. This process is designed to avoid the residual chloride ions after the reaction of traditional chlorine-containing precursors, preventing interface corrosion, resistance drift, and even device failure caused by residual chloride ions during subsequent high-temperature operation, thereby ensuring the long-term stability of the MEMS infrared light source. The second titanium nitride film prepared by this process has high purity, high density, and low interface state density. In the film structure, the second titanium nitride film functions as both an infrared emitting material and an optical waveguide layer. Its precisely controlled thickness, such as 5 nm to 30 nm, can effectively adjust the local distribution of the light field, laying the physical foundation for exciting more orders of local surface plasmon resonance modes.

[0054] Specifically, a third silicon nitride film is deposited on the surface of the second titanium nitride film to form a protective layer and a photonic structure layer. High-energy particles are used to bombard the target material to sputter atoms and deposit them on the substrate. A magnetron sputtering process is used to prepare a low-stress, high-transmittance third silicon nitride dielectric film.

[0055] In a more specific embodiment, in actual engineering, the refractive index of the third silicon nitride film can be adjusted to form a specific optical match with the lower titanium nitride film by adjusting the sputtering power and atmosphere ratio. Thus, the infrared emitting layer is a composite structure consisting of five alternating layers: the first silicon nitride film, the first titanium nitride film, the second silicon nitride film, the second titanium nitride film, and the third silicon nitride film.

[0056] This five-layer structure is achieved by increasing TiN / SiN. x The increased number of heterogeneous interfaces significantly enhances the multiple reflections and interference effects of photons within the film system. The multi-order LSPR (Localized Surface Plasmon Resonance) modes excited at different interfaces superimpose and couple across the spectrum, effectively broadening the resonant absorption bandwidth. This overcomes the physical bottleneck of limited emissivity in the mid-to-long-wave infrared band inherent in traditional single-layer or double-layer films. Furthermore, this five-layer alternating stacked structure provides greater design freedom for controlling the thermal time constant. By optimizing the thickness ratio of each layer, it is possible to meet the differentiated response speed requirements of various application scenarios while maintaining high emissivity.

[0057] S7. Spin-coat photoresist onto the surface of the second silicon nitride film, perform photolithography using a multi-step alignment photolithography process, and develop to form a grid-shaped etched area.

[0058] In this embodiment, this step is used to define the area for subsequent dry etching, in order to fabricate micro- and nano-scale patterned structures on the surface of the infrared emitting layer. Specifically, the multi-step alignment lithography process is used to ensure precise overlay of the patterns, especially when dealing with multi-layer structures, to guarantee the alignment accuracy between the lithographic pattern and the underlying heating structure. This step corresponds to... Figure 3 Figure 7) and Figure 4 Figure 9 in the middle.

[0059] In a more specific embodiment, the specific process includes: spin-coating a uniform photoresist layer onto the surface of the second silicon nitride film; pre-baking; and exposure using a mask with a grid pattern, the grid pattern consisting of periodically arranged square light-transmitting areas and light-blocking areas; followed by development to dissolve the photoresist in the exposed or unexposed areas, thereby forming grid-shaped openings on the photoresist layer. These openings expose the surface of the second silicon nitride film to be etched, constituting the grid-shaped etching area 22.

[0060] The thickness of the photoresist can be selected, for example, according to the subsequent etching depth, to ensure that it is not completely penetrated during the etching process. Through the above-mentioned high-precision multi-step alignment photolithography, a grid mask with accurate periodicity and steep edges can be prepared, providing a pattern transfer basis for the subsequent formation of high-quality matrix-type square bumps.

[0061] S8. Using inductively coupled plasma dry etching, the non-bottom layer of the infrared emitting layer corresponding to the grid-shaped etched area is etched away, forming a matrix-arranged square protrusion; the infrared emitting layer is composed of a first silicon nitride film, a first titanium nitride film, and a second silicon nitride film. This step corresponds to... Figure 3 Figure 8) and Figure 4 Figure 10 in the middle.

[0062] In this embodiment, inductively coupled plasma dry etching technology is used to vertically transfer the grating pattern on the photoresist to the underlying infrared emitting layer. Specifically, the ICP (Inductively Coupled Plasma) etching is characterized by high anisotropy and high etching rate, enabling the fabrication of micro-nano structures with large aspect ratios. During the etching process, active free radicals in the plasma react chemically with the infrared emitting layer material, generating volatile products that are removed. Simultaneously, ion bombardment assists in vertical removal.

[0063] In a more specific embodiment, such as Figure 6As shown, the infrared emitting layer consists of a first silicon nitride film, a first titanium nitride film, and a second silicon nitride film. Etching requires sequentially penetrating the first titanium nitride film and the second silicon nitride film, while retaining the bottom layer (the first silicon nitride film). After etching, the surface of the bottom layer (the first silicon nitride film) of the infrared emitting layer is exposed. After etching, the area covered by photoresist is retained, forming a raised platform, while the etched area forms a groove, ultimately forming a matrix of square protrusions on the surface of the infrared emitting layer. These square protrusions are composed of the first titanium nitride film and the second silicon nitride film.

[0064] The size of the square protrusions can be set to submicron level, with a side length in the range of 0.8~1.7 μm. The matrix arrangement of the square protrusions described above can introduce photonic crystal effects or surface plasmon resonance effects, thereby effectively enhancing the emissivity of the device in a specific infrared band.

[0065] In a more specific embodiment, inductively coupled plasma dry etching is employed, including: using a mixture of SF6, CF4, and O2 with a flow rate ratio of 5:3:2 as the mixed atmosphere, and a bias voltage of -50 to -150V, etching the non-bottom layer of the infrared emitting layer; and then introducing low-power Ar ions to bombard the etched infrared emitting layer for post-processing to remove etching-induced surface damage and form an infrared emitting layer with sub-nanometer roughness. The low-power Ar ion bombardment has a power of less than 50W and a duration of 30 to 60 seconds.

[0066] In a more specific embodiment, one possible implementation of the method further includes a process flow of specific mixed atmosphere and low-power Ar ion bombardment post-processing. This process flow is a further refinement and optimization of the technical feature of inductively coupled plasma dry etching in the aforementioned steps, aiming to solve the problem of physical damage to the infrared emitting layer caused by high-energy ion bombardment during dry etching and the resulting decrease in emissivity.

[0067] Specifically, the process includes using a mixed atmosphere of SF6, CF4, and O2 with a flow ratio of 5:3:2, and a bias voltage of -50 to -150V to etch the non-bottom layer of the infrared emitting layer. In a more specific embodiment, the main etching operation on the infrared emitting layer is first performed, using a mixed gas of sulfur hexafluoride, carbon tetrafluoride, and oxygen in a specific ratio as the etching atmosphere. SF6 serves as the main etching gas, dissociating in a plasma environment to generate highly reactive fluorine radicals, which are responsible for chemically etching the silicon nitride and titanium nitride materials. The introduction of CF4 helps to regulate the etching rate and improve the anisotropy of the etching, preventing excessive lateral etching. O2 participates in the generation of volatile reaction products and helps to maintain the dynamic balance between polymer deposition and etching removal during the etching process, thereby protecting the sidewall morphology.

[0068] Controlling the process parameters is key to achieving high-precision pattern transfer. Setting the bias voltage within the range of -50V to -150V ensures that the physical bombardment energy of ions on the sample surface is moderate. This ensures a sufficient vertical etching rate to form a matrix of square protrusions while effectively avoiding damage to the underlying medium or pattern distortion caused by excessive physical bombardment.

[0069] By precisely controlling the flow ratio of the three gases to 5:3:2, TiN and SiN can be synthesized. x An etching selectivity ratio greater than 10:1 between the film layers ensures that the etching process stops precisely at the interface between the first silicon nitride film and the first titanium nitride film, thereby completing the precise shaping of the infrared emitting layer. The synergistic effect of the mixed atmosphere and bias parameters results in a pattern with steep edges and uniform linewidth of the infrared emitting layer after etching, providing a solid structural foundation for subsequent optical performance.

[0070] Furthermore, a post-processing step is introduced: low-power Ar ion bombardment of the etched infrared emitting layer to remove etching-induced surface damage and form an infrared emitting layer with sub-nanometer roughness. Specifically, after the main etching is completed, a crucial low-power Ar ion bombardment post-processing step is introduced. Under the action of high-energy ions in inductively coupled plasma dry etching, tiny lattice defects, dangling bonds, and non-stoichiometric damage layers inevitably remain on the material surface. These surface defects introduce additional carrier recombination centers, reducing the thermal radiation efficiency of the material. To repair this damage, argon gas is introduced in situ to generate plasma, and the bombardment power is controlled within a low level.

[0071] In a more specific embodiment, the low-power Ar ion bombardment process is essentially a physical polishing and reconstruction process. Compared to the high-energy bombardment in the main etching stage, the low-power Ar ions have lower energy, and their depth of action is limited to the outermost few atomic layers of the material. This does not damage the existing patterned structure. Through momentum transfer, the Ar ions selectively peel away the unstable surface layer, residual contaminants, and etching-induced micro-protrusions formed in the main etching step, thereby exposing the fresh and complete crystal structure inside the material. More importantly, this moderate ion bombardment can stimulate the migration and rearrangement of surface atoms, resulting in a recrystallization process similar to annealing on the solid surface, thus forming a uniformly distributed rough surface with a sub-nanometer microstructure.

[0072] After the above post-processing, the surface of the infrared emitting layer is formed with a sub-nanometer rough surface. The surface roughness Ra value can be controlled, for example, between 0.5 nm and 2 nm. This specific roughness design is not a random surface defect, but a micro-nano optical structure that has been precisely controlled. When infrared light waves irradiate this sub-nanometer rough surface, the surface microstructure can effectively introduce the multiple scattering effect of light waves and enhance the local coupling of the light field on the surface, thereby significantly improving the light absorption and light emission efficiency of the material in a wide range of wavelengths.

[0073] This post-processing step not only repairs the negative impact of etching damage, but also transforms the physical morphology of the surface into a favorable factor for enhancing infrared emission performance. This further optimizes the average emissivity of the final MEMS infrared light source in the 3-14µm band, while also improving the long-term stability of the device under high-temperature operating conditions.

[0074] The above-mentioned technical process combines a specific etching atmosphere ratio with a fine physical post-processing, which effectively solves the surface damage problem introduced by dry etching without compromising the precision of the micro-nano structure pattern, and further enhances the optical performance by utilizing sub-nano rough surfaces, thereby achieving synergistic optimization of the fabrication process and device performance.

[0075] Specifically, the power of Ar ion bombardment is limited to less than 50W to ensure that the bombardment energy only acts on the removal of the physical damage layer and trace amounts of surface atoms induced by dry etching on the surface of the infrared emitting layer. At the same time, it avoids deep radiation damage to the subsurface lattice of the material or amorphization of the material structure caused by the high-energy ion beam. Within this power range, the physical sputtering effect of Ar ions on the surface is relatively mild, which can achieve the effect of cleaning rather than cutting, thereby precisely controlling the surface roughness after etching at the sub-nanometer level.

[0076] In a more specific embodiment, the bombardment time is limited to 30-60 seconds to strike a balance between adequately removing the surface damage layer and preventing excessive sputtering. For example, in a practical process, the Ar ion bombardment power can be set to 40W and the time to 45 seconds.

[0077] By synergistically controlling the above parameter ranges, an infrared emitting layer with sub-nanometer roughness can be formed. This specific surface morphology is beneficial for enhancing broadband scattering and emissivity, ensuring that the prepared MEMS infrared light source has stable emission performance across different batches.

[0078] S9. After dry removal of photoresist using plasma etching, rapid thermal annealing is performed.

[0079] In this embodiment, the step involves first removing residual photoresist, followed by heat treatment of the device to repair etching damage and stabilize the thin film crystal phase. Specifically, the plasma etching process utilizes oxygen plasma to oxidize residual organic photoresist into carbon dioxide and water vapor, achieving dry photoresist removal and avoiding surface tension damage or residual contamination caused by wet photoresist removal. This step corresponds to... Figure 3 Figure 9) and Figure 4 Figure 11 in the middle.

[0080] In a more specific embodiment, the rapid thermal annealing process includes: rapid thermal annealing at 400~500℃ in an N2 atmosphere for a annealing time of 30~120s.

[0081] In a more specific embodiment, after the resist removal is completed, a rapid thermal annealing process is performed. This process heats the wafer to a high temperature in a very short time, effectively activating atomic diffusion, repairing lattice damage and defects caused on the film surface and interface during ICP etching, and simultaneously eliminating internal stress in the film. The annealing atmosphere can be, for example, an inert gas such as nitrogen or argon, the annealing temperature can be controlled, for example, at 400~500℃, and the annealing time can be set, for example, at 30~120s. Through the above-mentioned rapid thermal annealing, devices with significantly improved microstructure stability of the infrared emitting layer can be fabricated, enhancing the long-term reliability of the device under high-temperature operating environments.

[0082] Specifically, N2 atmosphere refers to a heat treatment environment using nitrogen gas with a purity greater than 99.99% as a protective gas. It is used to isolate oxygen during rapid thermal annealing to prevent TiN material from undergoing oxidation at high temperatures, which would lead to resistivity drift. The rapid thermal annealing process is performed by rapid thermal annealing equipment, which uses halogen lamps or xenon lamps as heating sources to heat the wafer to the target temperature at an extremely high heating rate and maintain it at this temperature for a precise time.

[0083] In a more specific embodiment, after the etching process is completed, lattice defects and residual stress induced by plasma bombardment and dry etching will accumulate inside the infrared emitting layer and at the interfaces of each layer. If annealing is not performed, these defects and stresses will cause the film to crack, peel off or degrade electrical properties under subsequent high-temperature working environment. Based on the interface state after etching and photoresist removal, by placing the wafer in a temperature range of 400~500°C and using the inert protection of N2 atmosphere, thermodynamic driving force is provided for lattice recombination and stress relaxation.

[0084] The annealing temperature range of 400~500℃ is based on the crystal phase stability of TiN and SiN. xThe physical window jointly determined by the thermal stability of the TiN interface is such that when the annealing temperature is below 400℃, the atomic mobility is insufficient to completely eliminate microcracks and high-density dislocations at the interface, resulting in inadequate stress release. Devices operating above 600℃ still face reliability risks. When the annealing temperature is above 500℃, although the stress release rate accelerates, it easily induces stress between TiN and SiN. x Interfacial interdiffusion reactions between the TiN and TiN crystals disrupt the original heterojunction structure and can even lead to abnormal grain growth, thus deteriorating infrared emission performance. Therefore, strictly controlling the annealing temperature between 400 and 500°C can maximize stress release and stabilize the crystal structure of TiN while ensuring the integrity of the interfacial structure.

[0085] The annealing time of 30~120s is set according to the dynamic characteristics of stress relaxation in the above temperature range. Under the high heating rate environment of rapid thermal annealing, the time for the wafer to reach thermal equilibrium is short. The lower limit of 30 seconds ensures the temperature uniformity of each region of the wafer and the completion of the initial stress relaxation process. The upper limit of 120 seconds covers the time period required for the repair of most lattice defects, while taking into account the cycle time requirements in industrial production and avoiding a decrease in production capacity due to excessive processing time. Within this time window, atoms have enough energy to migrate to low energy state positions, thereby repairing etching-induced surface damage.

[0086] Through the rapid thermal annealing process with specific temperature and time parameters described above, the long-term stability of the MEMS infrared light source prepared in the embodiments of this application is significantly improved in high-temperature environments. This process enables the device to operate in high-temperature air at 600~800℃ with its resistance drift controlled within 5%, and extends the device's lifespan to more than three times that of traditional unoptimized annealing process structures. At the same time, the stable crystal phase structure and clean interface state also help improve the flatness of the infrared emission spectrum, ensuring that the light source has stable and efficient radiation output in the 3~14µm band.

[0087] The aforementioned rapid thermal annealing process works closely in conjunction with the film deposition, patterning etching, and back cavity formation processes. The etching process defines the micro-nano morphology of the infrared emitting layer, while the rapid thermal annealing consolidates the thermal stability of this morphology at the microscale, providing crucial process assurance for the reliable operation of the final device under extreme conditions.

[0088] S10. The side of the silicon substrate away from the infrared emitting layer is etched to form an inwardly recessed back cavity, thereby obtaining a MEMS infrared light source based on alternating layers of dual films.

[0089] In this embodiment, this step aims to release the infrared emitting layer, forming a suspended thermally isolated structure, thereby reducing the device's heat capacity and increasing the heating rate and modulation frequency. Specifically, the etching process is performed on the back side of the silicon substrate, i.e., the side away from the infrared emitting layer. Since the silicon substrate is usually made of single-crystal silicon, anisotropic wet etching or dry etching processes can be used to remove a portion of the silicon substrate directly below the infrared emitting layer, forming an inwardly recessed cavity, i.e., a back cavity. This step corresponds to... Figure 3 Figure 10 in the middle and Figure 4 Figure 12 in the middle.

[0090] In a more specific embodiment, the etching typically stops automatically at the support film because the support film material has high selectivity for the etchant. The resulting MEMS infrared light source based on alternating layers of a dual-film system includes a support film, a heating metal layer, a first silicon nitride film, a first titanium nitride film, and a second silicon nitride film stacked on a silicon substrate, with an inwardly recessed back cavity on the side of the silicon substrate away from the infrared emitting layer. By releasing the back cavity, a MEMS infrared light source with high emissivity, high response speed, and low power consumption can be obtained. This back cavity structure not only suspends the infrared emitting layer, effectively blocking heat conduction loss to the substrate, but also ensures that infrared radiation is mainly emitted towards the back cavity, reducing substrate absorption.

[0091] This invention also provides a MEMS infrared light source based on alternating stacked dual-film systems. The MEMS infrared light source is fabricated using the method described in the above embodiments. Figure 3 As shown, the MEMS infrared light source includes a support film, a heating metal layer, a first silicon nitride film, a first titanium nitride film, and a second silicon nitride film stacked on a silicon substrate; the first silicon nitride film, the first titanium nitride film, and the second silicon nitride film constitute an infrared emitting layer; the infrared emitting layer includes square protrusions arranged in a matrix, the square protrusions abutting against the top layer of the first silicon nitride film; the silicon substrate has an inwardly recessed back cavity on the side away from the infrared emitting film.

[0092] The embodiments of the application employ a silicon substrate and a support film, a heating metal layer, a first silicon nitride film, a first titanium nitride film, and a second silicon nitride film stacked on the silicon substrate. Specifically, the silicon substrate serves as the basic carrier of the device, and a support film made of SiOx is grown on the upper surface of the silicon substrate to provide mechanical support and achieve thermal isolation. In a more specific embodiment, a heating metal layer is provided on the side of the support film away from the silicon substrate. This heating metal layer is configured to generate Joule heating when energized, providing a heat source for infrared radiation.

[0093] Furthermore, a first silicon nitride film, a first titanium nitride film, and a second silicon nitride film are sequentially deposited on the surface of the heated metal layer. These three thin films constitute the aforementioned infrared emitting layer. To enhance infrared radiation efficiency and optimize thermal performance, the infrared emitting layer is fabricated into a matrix-arranged square protrusion structure. These square protrusions are formed using micro-nano patterning processes, which can synergistically enhance the infrared emissivity in a specific wavelength band and achieve directional radiation through heterogeneous interface effects.

[0094] In addition, on the side of the silicon substrate away from the infrared emitting layer, there is an inwardly recessed back cavity that penetrates or partially cuts into the silicon substrate, so that the heating metal layer and the infrared emitting layer supported by the support film above form a suspended or semi-suspended structure. This structural design effectively reduces the overall heat capacity of the device, shortens the thermal response time, and reduces the heat conduction loss to the substrate, thereby improving the infrared light emission efficiency.

[0095] It should be noted that the MEMS infrared light source based on alternating stacked dual-film system described in this embodiment is fabricated by the preparation method described above. The thickness, material ratio and pattern size of each film layer can be adjusted according to the needs of the actual application scenario. As long as its overall structure conforms to the above stacking relationship and the geometric features of the back cavity and protrusions, it falls within the protection scope of this application.

[0096] The aforementioned MEMS infrared light source based on alternating layers of dual films possesses high emissivity, high response speed, and low power consumption. This back cavity structure not only enables the infrared emitting layer to be suspended, effectively blocking heat conduction loss to the substrate, but also ensures that infrared radiation is mainly emitted towards the back cavity, reducing substrate absorption.

[0097] In a more specific embodiment, the square protrusion has a side length of 0.8~1.7µm and a period of 1.3~2µm; the period is the sum of the side length and the gap between two adjacent square protrusions. Specifically, the thickness of the support film is 200~2000nm, the thickness of the first silicon nitride film is 300~700nm, the thickness of the first titanium nitride film is 5~30nm, and the thickness of the second silicon nitride film is not less than the thickness of the first silicon nitride film.

[0098] Specifically, the side length of the aforementioned square protrusion is set to 0.8~1.7 μm. This size range is a micro-nano structure parameter that has been optimized to excite efficient Mie scattering resonance and Bloch mode in the infrared band of 3~14 μm. The side length directly determines the intrinsic resonance frequency of the square protrusion as an optical harmonic oscillator. When the side length is in the range of 0.8~1.7 μm, it can effectively match the wavelength scale of the mid-to-long-wave infrared, so that the incident light generates a strong local field enhancement inside the protrusion, thereby significantly improving the emissivity of the infrared emitting layer.

[0099] Regarding the geometric definition of period, such as Figure 5 As shown, the period is the sum of the side length and the gap between two adjacent square protrusions. This definition clarifies the geometric relationship of the square protrusion array. In terms of physical structure, the surface of the infrared emitting layer is composed of multiple square protrusions arranged in a matrix. There is a certain gap between any two adjacent square protrusions. The period P, the side length L and the gap W satisfy the following geometric relationship: P = L + W, where P represents the period, L represents the side length of the square protrusion, and W represents the gap between two adjacent square protrusions.

[0100] Specifically, the thickness range of the aforementioned support membrane is designed to balance its mechanical strength and thermal insulation performance as a structural support component of the microelectromechanical system. If the support membrane is too thin, its mechanical strength will be insufficient and it will be prone to breakage; if it is too thick, it will increase the heat capacity and reduce the modulation speed.

[0101] like Figure 6 As shown, for the three-layer infrared emitting layer, the square protrusion is composed of a first titanium nitride film and a second silicon nitride film. In a more specific embodiment, the thickness of the first silicon nitride film is set in the range of 300~700nm, which can effectively balance the stress state inside the film, ensure the structural stability of the film layer during subsequent high-temperature processes and operation, and provide a suitable optical interference thickness to optimize infrared emission efficiency.

[0102] The thickness of the first titanium nitride film is set in the range of 5~30nm. This thickness range corresponds to the optimal extinction depth of the local surface plasmon resonance effect in the infrared band, which can effectively excite broadband absorption and emission characteristics. If the thickness of the first titanium nitride film is too thin, the continuity will be poor, resulting in abnormal resistivity; if it is too thick, it will lead to excessive absorption of free carriers, which will reduce the emissivity.

[0103] By setting the thickness of the second silicon nitride film to be greater than or equal to that of the first silicon nitride film, on the one hand, the thicker top dielectric film effectively passivates and protects the underlying first titanium nitride film, suppressing its oxidation and diffusion under high-temperature operating conditions; on the other hand, in subsequent dry etching processes, this thickened second silicon nitride film can serve as an etching stop layer or buffer layer, improving the protection of the underlying structure, thereby precisely controlling the patterning accuracy and ensuring that the square protrusions of the infrared emitting layer have steep sidewall morphology. For example, the thickness of the second silicon nitride film can be set to 500 nm to 900 nm.

[0104] A MEMS infrared light source with a three-layer infrared emitting layer was tested, and its average emissivity in the wavelength range of 3~14µm was >88%. The test results are as follows: Figure 8 As shown.

[0105] Through the above technical solution, this application achieves systematic and precise control of the thickness of each functional film layer of the infrared light source of the microelectromechanical system. By limiting the thickness of the support film, the first silicon nitride film, the first titanium nitride film and the second silicon nitride film to the above specific range, the technical problems of interface stress accumulation, thermal cycling failure and local emissivity decay caused by film thickness mismatch are solved. In particular, by limiting the thickness of the second silicon nitride film to be no less than that of the first silicon nitride film, the long-term stability of the device under high temperature environment is effectively improved, and the etching process window is optimized. This allows the finally prepared infrared light source to maintain high emissivity in the 3~14µm band while having excellent mechanical reliability and thermal cycling life.

[0106] The aforementioned method for fabricating a MEMS infrared light source based on alternating layers of dual-film systems tightly integrates a SiOx support film grown by PECVD with a SiNx-TiN-SiNx dual-film alternating layer structure prepared by magnetron sputtering and ALD processes. Combined with matrix-shaped square protrusions formed by ICP dry etching and rapid thermal annealing, an infrared emitting surface with high emissivity and excellent thermal stability is synergistically constructed. The heterogeneous interface between silicon nitride and titanium nitride modulates the optical resonance mode, the matrix protrusions enhance the optical field coupling effect, and the back cavity structure achieves efficient thermal isolation. This MEMS infrared light source exhibits excellent emission performance in the 3~14µm band, with a significantly improved average emissivity. Furthermore, due to its full process compatibility with CMOS standard manufacturing processes, the device possesses good mass production consistency and reliability.

[0107] In a more specific embodiment, the infrared emitting layer further includes a second titanium nitride film and a third silicon nitride film stacked on top of the second silicon nitride film; the thickness of the second titanium nitride film is equal to the thickness of the first silicon nitride film; and the thickness of the third silicon nitride film is not greater than the thickness of the second silicon nitride film.

[0108] The infrared emitting layer provided in this application further includes a second titanium nitride film and a third silicon nitride film stacked on top of the second silicon nitride film. For example... Figure 7 As shown, for the five-layer infrared emitting layer, the square protrusion is composed of a first titanium nitride film, a second silicon nitride film, a second titanium nitride film, and a third silicon nitride film.

[0109] Specifically, by alternately stacking a second titanium nitride film and a third silicon nitride film on top of the second silicon nitride film, a more complex five-layer optical resonant cavity structure was constructed. This multi-layered alternating film system design can utilize multiple interface reflections and interference effects to induce local surface plasmon resonance modes in a wider infrared band, thereby breaking through the spectral response limitations of single or three-layer film systems.

[0110] In a more specific embodiment, the second titanium nitride film serves as an intermediate loss layer, and its optical constant works synergistically with that of the first titanium nitride film to jointly regulate the absorption and re-radiation process of incident light; the third silicon nitride film serves as the top dielectric protective layer, which not only maintains the high-temperature stability of the internal titanium nitride layer, but also optimizes the surface impedance characteristics through the matching of its thickness and refractive index, enabling the device to achieve more efficient electromagnetic coupling in air.

[0111] Furthermore, in the infrared emitting layer, the thickness of the second titanium nitride film is equal to the thickness of the first silicon nitride film, both being 5~30nm.

[0112] Specifically, in this five-layer film structure, the thickness of the second titanium nitride film is precisely set to be equal to the thickness of the first silicon nitride film. This is a key design based on optical phase matching. Since the first silicon nitride film is located above the heated metal layer, its thickness is usually designed to meet the condition of a quarter-wavelength optical thickness in order to form strong reflection or absorption at a specific wavelength.

[0113] In a more specific embodiment, by making the second titanium nitride film have the same physical thickness as the first silicon nitride film, it can be ensured that the optical phase delay at the two locations is consistent or in a specific multiple relationship, thereby causing the LSPR excitation modes at the upper and lower titanium nitride-silicon nitride interfaces to produce a spatial superposition enhancement effect. This thickness matching design effectively avoids destructive interference caused by interlayer optical mismatch, ensures the directional transmission and efficient emission of infrared radiation energy within the film system, and significantly improves the peak emissivity of the device in the target band.

[0114] Furthermore, in the infrared emitting layer, the thickness of the third silicon nitride film is no greater than the thickness of the second silicon nitride film. In this case, the thickness of the second silicon nitride film can be set to 300nm~700nm, so that the thickness of the second silicon nitride film can be consistent with the thickness of the first silicon nitride film; the thickness of the third silicon nitride film can be set to 300nm~500nm.

[0115] Specifically, the thickness of the third silicon nitride film is asymmetrically limited to not exceed that of the second silicon nitride film in order to further optimize the optical impedance matching and stress distribution of the entire film system. From an optical perspective, the second silicon nitride film, as the main spacer layer, determines the resonant wavelength of the lower resonant cavity; while the thickness of the third silicon nitride film, as the capping layer, will change the reflection phase of the top layer interface.

[0116] In a more specific embodiment, when the thickness of the third silicon nitride film is less than or equal to the thickness of the second silicon nitride film, the side lobes of higher-order diffraction modes can be effectively suppressed, and the main lobe of the emission spectrum can be confined to the mid-to-long-wave infrared region of 3-14 μm, thereby obtaining a wider and flatter high emissivity band. From a mechanical perspective, this thickness gradient design helps to balance the internal stress generated by multilayer film stacking, prevents warping or peeling caused by excessive film thickness, and ensures the structural integrity of the microelectromechanical system infrared light source under repeated high-temperature heating cycles.

[0117] A MEMS infrared light source with a five-layer infrared emitting layer was tested, and its average emissivity in the wavelength range of 3~14µm was >90%. The test results are as follows: Figure 9 As shown. If there are no significant requirements for the device time constant, a five-layer infrared emitting layer can be integrated into the thermal infrared device to prepare a corresponding MEMS infrared light source, thereby significantly improving the infrared absorption rate of the device in the 3~14µm band. If the device time constant requirement is high, a three-layer infrared emitting layer can be integrated into the thermal infrared device to prepare a corresponding MEMS infrared light source, thereby reducing the film thickness while ensuring a relatively high device absorption rate.

[0118] Through the above technical solution, this application achieves a complete closure of the protection scope of the five-layer MEMS infrared light source product based on alternating stacked dual-film system and the corresponding fabrication method. By limiting the equal thickness relationship between the second titanium nitride film and the first silicon nitride film, and the thickness constraint of the third silicon nitride film relative to the second silicon nitride film, a phase-coordinated and impedance-matched multilayer optical metasurface is physically constructed. This structure utilizes multi-interface interference and LSPR coupling mechanism to successfully increase the average emissivity of the device in the 3~14μm band to over 91.52%, and expands the full width at half maximum (FWHM) to cover a wider infrared spectral range. At the same time, this precise thickness control does not sacrifice process compatibility, and still maintains the low-temperature fabrication advantage of fully complementary metal-oxide-semiconductor (CMOS) process, ensuring the yield and reliability of the product during mass production, and solving the technical problem of difficulty in balancing high emissivity and structural stability in the prior art.

[0119] This invention provides a method for fabricating a MEMS infrared light source based on alternating layers of a dual-film system. The method includes cleaning a silicon substrate and growing SiO₂. xA support film is formed, followed by a heated metal layer. Then, a first silicon nitride film, a first titanium nitride film, and a second silicon nitride film are sequentially deposited to form an infrared emitting layer. A matrix of square protrusions is formed through photolithography and inductively coupled plasma dry etching. The resulting MEMS infrared light source comprises a stacked support film, a heated metal layer, and an infrared emitting layer, exhibiting a matrix of square protrusions and a back cavity structure. This application achieves a balance between high emissivity and high thermal stability through the synergistic effect of the alternating stacked dual-film structure and the square protrusion micro / nano structure, while remaining compatible with standard wafer-level manufacturing processes. This effectively solves the problems of low emissivity, high-temperature failure, and difficulty in mass production associated with existing devices.

[0120] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any person skilled in the art can easily conceive of various equivalent modifications or substitutions within the technical scope disclosed in the present invention, and these modifications or substitutions should all be covered within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.

Claims

1. A method for fabricating a MEMS infrared light source based on alternating layers of a dual-film system, characterized in that, The preparation method includes: Clean the silicon substrate; A support film is grown on the upper surface of the silicon substrate using plasma-enhanced chemical vapor deposition; the support film is made of SiOx. A patterned mask is processed on the surface of the support film, and then a heated metal layer corresponding to the patterned mask is deposited by magnetron sputtering. The patterned mask is then removed by a stripping process. A first silicon nitride film is deposited on the surface of the heated metal layer using a magnetron sputtering process; A first titanium nitride film was obtained by depositing a chlorine-free precursor atomic layer deposition process on the surface of the first silicon nitride film. A second silicon nitride film is deposited on the surface of the first titanium nitride film using a magnetron sputtering process; Photoresist is spin-coated onto the surface of the second silicon nitride film, and a multi-step alignment photolithography process is used to perform photolithography and development to form a grid-shaped etched area. Inductively coupled plasma dry etching is used to etch away the non-bottom layer in the infrared emitting layer corresponding to the grid-shaped etched area, forming a matrix of square protrusions; the infrared emitting layer is composed of a first silicon nitride film, a first titanium nitride film and a second silicon nitride film. The photoresist was removed by dry plasma etching followed by rapid thermal annealing. The silicon substrate is etched on the side opposite to the infrared emitting layer to form an inwardly recessed back cavity, thereby obtaining a MEMS infrared light source based on alternating layers of a dual-film system. The inductively coupled plasma dry etching method includes: using SF6, CF4 and O2 with a flow ratio of 5:3:2 as a mixed atmosphere, and a bias voltage of -50 to -150V to etch the non-bottom layer of the infrared emitting layer. The infrared emitting layer after etching is bombarded with low-power Ar ions for post-processing to remove etching-induced surface damage and form an infrared emitting layer with sub-nanometer roughness.

2. The method for fabricating a MEMS infrared light source based on alternating layers of dual-film systems according to claim 1, characterized in that, The low-power Ar ion bombardment has a power of less than 50W and a duration of 30~60s.

3. The method for fabricating a MEMS infrared light source based on alternating layers of dual-film systems according to claim 1 or 2, characterized in that, The rapid thermal annealing process includes: Rapid thermal annealing was performed at 400~500℃ in an N2 atmosphere for 30~120s.

4. The method for fabricating a MEMS infrared light source based on alternating layers of dual-film systems according to claim 3, characterized in that, The method for preparing the heated metal layer includes: A heated metal layer of 50-500 nm is obtained by metal magnetron sputtering; the power of the metal magnetron sputtering is 100-200 W, the chamber pressure is 2.2-3.8 mTorr, the Ar gas flow rate is 50-100 sccm, and the film formation rate of the heated metal layer is 5-10 nm / min; the material of the heated metal layer is gold, platinum, tungsten, or titanium nitride.

5. The method for fabricating a MEMS infrared light source based on alternating layers of dual-film systems according to claim 4, characterized in that, After depositing a second silicon nitride film on the surface of the first titanium nitride film using a magnetron sputtering process, the method further includes: A second titanium nitride film was obtained by depositing a chlorine-free precursor atomic layer deposition process on the surface of the second silicon nitride film. A third silicon nitride film is deposited on the surface of the second titanium nitride film using a magnetron sputtering process; the infrared emitting layer is composed of a first silicon nitride film, a first titanium nitride film, a second silicon nitride film, a second titanium nitride film, and a third silicon nitride film.

6. A MEMS infrared light source based on alternating stacked dual-film systems, wherein the MEMS infrared light source is fabricated by the method for fabricating a MEMS infrared light source based on alternating stacked dual-film systems as described in any one of claims 1-4, characterized in that, The MEMS infrared light source includes a support film, a heating metal layer, a first silicon nitride film, a first titanium nitride film, and a second silicon nitride film stacked on a silicon substrate. The first silicon nitride film, the first titanium nitride film, and the second silicon nitride film constitute an infrared emitting layer; the infrared emitting layer includes square protrusions arranged in a matrix, the square protrusions abutting against the top layer of the first silicon nitride film; the silicon substrate has an inwardly recessed back cavity on the side away from the infrared emitting layer.

7. The MEMS infrared light source based on alternating layers of a dual-film system according to claim 6, characterized in that, The square protrusion has a side length of 0.8~1.7um and a period of 1.3~2um; the period is the sum of the side length and the gap between two adjacent square protrusions.

8. The MEMS infrared light source based on alternating stacked dual-film system according to claim 7, characterized in that, The thickness of the support film is 200~2000nm, the thickness of the first silicon nitride film is 300~700nm, the thickness of the first titanium nitride film is 5~30nm, and the thickness of the second silicon nitride film is not less than the thickness of the first silicon nitride film.

9. The MEMS infrared light source based on alternating layers of a dual-film system according to claim 8, characterized in that, The infrared emitting layer further includes a second titanium nitride film and a third silicon nitride film stacked on top of the second silicon nitride film; the thickness of the second titanium nitride film is equal to the thickness of the first silicon nitride film; and the thickness of the third silicon nitride film is not greater than the thickness of the second silicon nitride film.

Citation Information

Patent Citations

  • MEMS infrared light source based on porous structure and preparation method thereof

    CN118201151A

  • MEMS infrared light source with 3D structure and preparation method thereof

    CN120622407A