A composite photocatalyst, its preparation method and application

By loading imidazole ionic liquids onto the surface of V2O5/g-C3N4 heterojunctions, the problems of fast photogenerated carrier recombination rate and limited visible light absorption range of g-C3N4 photocatalysts were solved, achieving high CO2 reduction performance and stable catalytic performance.

CN122828757BActive Publication Date: 2026-11-17XIAN UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611309469.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-17
Estimated Expiration
2046-08-27

AI Technical Summary

Technical Problem

Existing graphitic carbon nitride (g-C3N4) photocatalysts suffer from problems such as fast photogenerated carrier recombination rate, low quantum efficiency, small specific surface area, few active sites, weak adsorption and activation ability for CO2 molecules, and limited visible light absorption range. Furthermore, ionic liquid modification is unstable, affecting the catalyst's recyclability.

Method used

By loading imidazole ionic liquids onto the surface of V2O5/g-C3N4 heterojunctions and using a methanol solvent-mediated ultrasonic-assisted impregnation method, the ionic liquids are bonded to the catalyst surface through hydrogen bonding to form CO2 adsorption sites, thereby optimizing the band structure of the catalyst, broadening the visible light response range, and suppressing electron-hole recombination.

Benefits of technology

It significantly improves the specific surface area and CO2 adsorption capacity of the catalyst, broadens the visible light response range, delays electron-hole recombination efficiency, and enhances the CO yield and selectivity of photocatalytic CO2 reduction. It also exhibits good stability and recyclability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122828757B_ABST
    Figure CN122828757B_ABST
Patent Text Reader

Abstract

This invention discloses a composite photocatalyst, its preparation method, and its application, belonging to the field of photocatalytic materials technology. This invention utilizes a methanol solvent-mediated ultrasonic-assisted impregnation method to stably bond the imidazole ring cations of an ionic liquid with the amino groups on the surface of VOCN through hydrogen bonding. The composite photocatalyst, its preparation method, and its application, as described above, increase the specific surface area and CO2 adsorption capacity of the catalyst, broaden the visible light response range, delay electron-hole recombination efficiency, and significantly improve photocatalytic performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of photocatalytic materials technology, and in particular to a composite photocatalyst, its preparation method, and its application. Background Technology

[0002] Photocatalytic CO2 reduction technology has become an important way to achieve carbon neutrality because it can use solar energy to convert the greenhouse gas CO2 into high-value-added chemicals.

[0003] Graphitic carbon nitride (g-C3N4), as a non-metallic semiconductor photocatalyst, has advantages such as simple preparation, suitable band structure, and high chemical stability, and is widely used in the field of photocatalytic CO2 reduction. However, pure g-C3N4 has the following technical problems: fast photogenerated carrier recombination rate and low quantum efficiency; small specific surface area and few active sites; weak adsorption and activation ability for CO2 molecules and high reaction overpotential; and limited visible light absorption range.

[0004] Constructing heterojunctions can promote effective charge separation and reduce carrier recombination rate, but the interfacial charge transport efficiency is still limited, and the surface CO2 reaction kinetics are sluggish, resulting in unsatisfactory photocatalytic efficiency.

[0005] Ionic liquids, as green functional materials, possess excellent CO2 dissolving capabilities and designable molecular structures, showing broad application prospects in the field of photocatalysis. Existing technologies for modifying photocatalysts with ionic liquids often employ complex synthetic routes, and the bond between ionic liquids and catalysts is unstable, easily detaching during the reaction process, severely impacting the catalyst's recyclability.

[0006] Therefore, developing an ionic liquid-modified V2O5 / g-C3N4 heterojunction photocatalyst that is simple to prepare, has excellent performance, and good stability has important theoretical and application value. Summary of the Invention

[0007] The purpose of this invention is to address the shortcomings of existing technologies by providing a composite photocatalyst, its preparation method, and its application. By loading an imidazole ionic liquid onto the surface of a V2O5 / g-C3N4 heterojunction, a composite photocatalyst is obtained, which increases the specific surface area and CO2 adsorption capacity of the catalyst, broadens the visible light response range, delays electron-hole recombination efficiency, and significantly improves photocatalytic performance.

[0008] To achieve the above objectives, the present invention provides a method for preparing a composite photocatalyst, comprising the following steps: S1. Melamine is heated to undergo thermal polymerization, then cooled and ground to obtain g-C3N4 powder; S2. Mix g-C3N4 powder with ammonium metavanadate, grind, calcine, cool, wash, vacuum dry, and grind to obtain V2O5 / g-C3N4 heterojunction, denoted as VOCN; S3. Imidazole-based ionic liquid is dispersed in methanol solvent, and subjected to first stirring and first sonication. V2O5 / g-C3N4 heterojunction is added and subjected to second stirring and second sonication. After centrifugation, vacuum drying and grinding, a composite photocatalyst modified with ionic liquid V2O5 / g-C3N4 heterojunction is obtained.

[0009] Preferably, in S1, the heating rate of thermal polymerization is 4-6℃ / min, the temperature of thermal polymerization is 540-560℃, and the time of thermal polymerization is 2-4h.

[0010] Preferably, in S2, the mass ratio of g-C3N4 powder to ammonium metavanadate is 5-20:1, the calcination heating rate is 4-6℃ / min, the calcination temperature is 490-510℃, the calcination time is 2-4h, the vacuum drying temperature is 60℃, and the vacuum drying time is 12h.

[0011] Furthermore, the mass ratio of g-C3N4 powder to ammonium metavanadate is 10:1.

[0012] Preferably, in S3, the imidazole ionic liquid includes one or more of 1-butyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium tetrafluoroborate, and 1-octyl-3-methylimidazolium tetrafluoroborate.

[0013] Furthermore, imidazole ionic liquids include 1-butyl-3-methylimidazolium tetrafluoroborate.

[0014] Preferably, in S3, the mass-to-volume ratio of imidazole ionic liquid, V2O5 / g-C3N4 heterojunction, and methanol is 5-15 mg: 0.1 g: 15-25 mL.

[0015] Preferably, in S3, the first stirring time is 30 min, the first ultrasonic time is 30 min, the second stirring time is 2-4 h, the second ultrasonic time is 0.5-1.5 h, the vacuum drying temperature is 60℃, and the vacuum drying time is 12 h.

[0016] The present invention also provides a composite photocatalyst prepared by the above-described preparation method. The catalyst comprises a V₂O₅ / g-C₃N₄ heterojunction support and an imidazole-based ionic liquid supported on its surface. The imidazole-based ionic liquid is bonded to the amino groups on the surface of the V₂O₅ / g-C₃N₄ heterojunction via hydrogen bonding.

[0017] The present invention also provides an application of the composite photocatalyst, which is used in the photocatalytic reduction of CO2.

[0018] Therefore, the present invention, employing the above-mentioned composite photocatalyst, its preparation method, and its application, has the following beneficial effects: (1) This invention utilizes a methanol solvent-mediated ultrasonic-assisted impregnation method to stably bond the imidazole ring cations of the ionic liquid with the amino groups on the surface of VOCN through hydrogen bonding, while simultaneously BF4 - Anions create a microenvironment rich in CO2 adsorption sites on the catalyst surface. Compared to other solvents such as water, ethanol, isopropanol, and acetone, methanol can maximize the formation of hydrogen bonds and the uniform dispersion of ionic liquids.

[0019] (2) The composite photocatalyst prepared in this invention has a large specific surface area and high CO2 adsorption capacity, a wide visible light response range, and low electron-hole recombination efficiency. Under visible light driving, the photocatalytic reduction of CO2 to produce CO yield reaches 375.2 μmol / g (4 hours), with a CO selectivity as high as 94%, which is 22 times higher than that of pure g-C3N4 and 2.66 times higher than that of unmodified VOCN heterojunction with ionic liquid. At the same time, the catalyst has good stability and recyclability, and its activity remains basically unchanged after 4 cycles.

[0020] (3) The composite photocatalyst prepared in this invention incorporates imidazole ionic liquids, which are then processed by BF4. - Anions enrich CO2 adsorption sites, increasing the catalyst's CO2 adsorption capacity; imidazole cations form an active intermediate with CO2, reducing the overpotential of the CO2 reduction reaction; the anion-cation structure of the ionic liquid promotes charge separation at the V2O5 / g-C3N4 heterojunction interface, effectively suppressing electron-hole recombination; and the optimized band structure of the catalyst broadens the visible light response range to 540 nm.

[0021] (4) The composite photocatalyst prepared by the present invention is prepared by a simple two-step method of high-temperature calcination + ultrasonic-assisted impregnation. It does not require complex equipment and harsh conditions, and is simple, convenient and easy to scale up.

[0022] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description

[0023] Figure 1 This is a schematic diagram of the preparation method of Embodiment 1 of the present invention; Figure 2 These are the X-ray diffraction patterns of Embodiments 1-3 and Comparative Examples 1-2 of the present invention; Figure 3 These are the Fourier transform infrared spectra of Embodiments 1-3 and Comparative Examples 1-2 of the present invention; Figure 4This is a transmission electron microscope-EDS elemental distribution diagram of Embodiment 2 of the present invention; in, Figure 4 Image (a) is a transmission electron microscope (TEM) image. Figure 4 (b) in the diagram is the distribution of element C. Figure 4 (c) in the diagram is the distribution of element N. Figure 4 (d) in the diagram is the distribution of element O. Figure 4 (e) in the diagram is the distribution map of element V. Figure 4 (f) in the diagram is the distribution map of element B. Figure 4 (g) in the diagram represents the distribution of element F. Figure 4 (h) in the figure represents the elemental distribution map; Figure 5 These are N2 adsorption-desorption and CO2 adsorption performance graphs for Example 2 and Comparative Example 2 of the present invention; in, Figure 5 (a) in the diagram is the N2 adsorption-desorption isotherm. Figure 5 (b) in the figure is the aperture distribution curve. Figure 5 (c) in the diagram is the CO2 adsorption performance graph; Figure 6 These are the ultraviolet-visible spectra and Tauc band gap diagrams of Examples 1-3 and Comparative Examples 1-2 of the present invention; in, Figure 6 (a) in the image is the ultraviolet-visible spectrophotometer. Figure 6 (b) in the diagram is the Tauc bandgap plot; Figure 7 These are the photoluminescence spectra, photocurrent responses, and electrochemical impedance spectroscopy of Examples 1-3 and Comparative Examples 1-2 of the present invention. in, Figure 7 (a) in the image is the photoluminescence spectrum. Figure 7 (b) in the diagram is the photocurrent response spectrum. Figure 7 (c) in the diagram is an electrochemical impedance spectroscopy (EIS). Figure 8 These are the photocatalytic CO2 reduction reaction performance diagrams of Examples 1-3 and Comparative Examples 1-6 of the present invention; in, Figure 8 (a) in the figure is a CO production graph for Examples 1-3 and Comparative Examples 1-2. Figure 8 (b) in the figure is a CH4 yield graph for Examples 1-3 and Comparative Examples 1-2. Figure 8 (c) in the figure is a graph showing the product yield and selectivity of Examples 1-3 and Comparative Examples 1-2. Figure 8 (d) in the figure is the product yield graph of Example 2 and Comparative Examples 3-6; Figure 9 This is a test graph of the photocatalytic cycle stability of Example 2 of the present invention; in, Figure 9 (a) in the figure is a graph showing the product yield and selectivity after four cycles of the reaction in Example 2. Figure 9 (b) in the figure is the X-ray diffraction pattern before and after the cycle in Example 2. Figure 9 (c) in the figure is the Fourier transform infrared spectrum before and after the cycle in Example 2. Detailed Implementation

[0024] The technical solution of the present invention will be further described below with reference to the accompanying drawings and embodiments.

[0025] Unless otherwise defined, the technical or scientific terms used in this invention shall have the ordinary meaning as understood by one of ordinary skill in the art to which this invention pertains.

[0026] In this invention, unless otherwise specified, the test materials and instruments are all conventional test materials in the field and can be purchased through commercial channels.

[0027] Example 1 A composite photocatalyst comprises a V2O5 / g-C3N4 heterojunction support and a 1-butyl-3-methylimidazolium tetrafluoroborate (imidazolium-based ionic liquid) supported on its surface, wherein the imidazolium-based ionic liquid is bonded to the amino groups on the surface of the V2O5 / g-C3N4 heterojunction via hydrogen bonding.

[0028] The preparation method of the above photocatalyst, such as Figure 1 As shown, it includes the following steps: S1. Place 5g of melamine powder in a covered alumina crucible and heat it to 550℃ in a tube furnace under air atmosphere at a heating rate of 5℃ / min. Maintain the temperature at the target temperature for 3h. After the program is completed, allow it to cool naturally to room temperature and grind it to obtain g-C3N4 powder. S2. Weigh 1g of g-C3N4 powder and 0.1g of ammonium metavanadate (NH4VO3) and place them in an agate mortar. Grind thoroughly until the mixture is homogeneous and free of obvious particles. Place the ground powder in a covered alumina crucible and heat it to 500℃ in a tube furnace under air atmosphere at a heating rate of 5℃ / min. Maintain the temperature at the target temperature for 3h. After the program is completed, allow it to cool naturally to room temperature. Then wash the sample several times with alternating ethanol and deionized water. Dry the washed sample under vacuum at 60℃ for 12h. Grind the powder to obtain V2O5 / g-C3N4 heterojunction powder, denoted as VOCN. S3. Dissolve 5 mg of 1-butyl-3-methylimidazolium tetrafluoroborate (imidazolium ionic liquid) in 20 mL of methanol, stir magnetically for 30 min, and sonicate for 30 min; add 0.1 g of V2O5 / g-C3N4 heterojunction powder to the solution, stir magnetically for 3 h, and sonicate for 1 h; centrifuge the mixture, collect the precipitate, vacuum dry at 60 °C for 12 h, and grind to obtain the composite photocatalyst, denoted as VOCN-IL5.

[0029] Example 2 This embodiment operates the same as in Example 1, except that in S3, the amount of 1-butyl-3-methylimidazolium tetrafluoroborate added is 10 mg, and the resulting composite photocatalyst is denoted as VOCN-IL10.

[0030] Example 3 This embodiment operates the same as in Example 1, except that in S3, the amount of 1-butyl-3-methylimidazolium tetrafluoroborate added is 15 mg, and the resulting composite photocatalyst is denoted as VOCN-IL15.

[0031] Comparative Example 1 The operation of this comparative example is the same as that of Example 1, except that only S1 is performed to obtain g-C3N4 powder.

[0032] Comparative Example 2 This comparative example operates in the same way as Example 1, except that only S1 and S2 are performed to obtain V2O5 / g-C3N4 heterojunction powder, denoted as VOCN.

[0033] Comparative Example 3 This comparative example operates the same as Example 2, except that in S3, methanol is replaced with deionized water.

[0034] Comparative Example 4 This comparative example operates the same as Example 2, except that in S3, methanol is replaced with anhydrous ethanol.

[0035] Comparative Example 5 This comparative example operates the same as Example 2, except that in S3, methanol is replaced with isopropanol.

[0036] Comparative Example 6 This comparative example operates the same as Example 2, except that in S3, methanol is replaced with propanol.

[0037] The molecular structures of Examples 1-3 and Comparative Examples 1-2 were characterized by X-ray diffraction (XRD), with the XRD pattern of the standard sample V₂O₅ (denoted as VO) used as a control. The results are as follows: Figure 2 As shown. From Figure 2As can be seen from the data, the diffraction peak at 13.2° in Comparative Example 1 corresponds to the (100) crystal plane, and the diffraction peak at 27.4° corresponds to the (002) crystal plane, which is attributed to the interlayer superposition of typical conjugated aromatic sheets. Comparative Example 2 contains the (100) and (002) characteristic peaks of Comparative Example 1, indicating that it was successfully prepared. As the ionic liquid loading increases in Examples 1-3, the (002) peak shifts to a higher angle compared to Comparative Example 1, indicating that the introduction of the ionic liquid reduces the interlayer spacing of Comparative Example 1, proving the successful loading of the ionic liquid. No new diffraction peaks appeared in Examples 1-3, indicating that the prepared samples have high purity and do not contain other impurities.

[0038] The molecular structures of Examples 1-3 and Comparative Examples 1-2 were characterized using Fourier transform infrared spectroscopy (FT-IR), with the FT-IR spectrum of the standard sample V2O5 (denoted as VO) used as a control. The results are as follows: Figure 3 As shown. From Figure 3 As can be seen from this, Comparative Example 1 is at 810cm -1 The absorption peak corresponds to the out-of-plane bending vibration of the heptaazine ring unit, 1200-1650 cm⁻¹. -1 The absorption peaks in the range correspond to the stretching vibrations of the CN heterocycle in the heptaazine ring framework, 3100-3300 cm⁻¹. -1 The broad peak in the range is due to the stretching vibration of the NH component or OH, accompanied by the absorption of uncondensed amino groups and H2O molecules; Comparative Example 2 shows a peak at 1014 cm⁻¹. -1 A weak absorption peak appeared nearby, attributed to the stretching vibration of the V=O bond; the characteristic peaks in Examples 1-3 were clearly visible, similar to Comparative Example 2, indicating that the loading of the ionic liquid did not disrupt the functional group structure of VOCN; Examples 1-3 showed absorption peaks at 3100-3300 cm⁻¹. -1 The vibrational peaks in the region broadened slightly with increasing ionic liquid loading, which is attributed to the hydrogen bonding interaction between the cations of the ionic liquid and the NH or OH groups of g-C3N4, which weakened the absorption of its characteristic peaks.

[0039] The composite catalyst of Example 2 was characterized by transmission electron microscopy (TEM) and elemental mapping scanning, and the results are as follows: Figure 4 As shown. From Figure 4 As can be seen, C, N, O, V, B and F elements are uniformly dispersed on the surface of the composite catalyst of Example 2 without elemental segregation, indicating that the ionic liquid is uniformly loaded on the VOCN surface, which further proves the successful preparation of Example 2.

[0040] The pore structure and gas adsorption performance of Example 2 and Comparative Example 2 were characterized using N2 adsorption-desorption and CO2 adsorption tests. The results are as follows: Figure 5 As shown. N2 adsorption-desorption tests were performed on Example 2 and Comparative Example 2. The specific surface area and pore volume of both were calculated using the BET method. The specific surface area of ​​Example 2 was 51.07 m².2 ·g -1 The pore volume is 0.31 cm. 3 ·g -1 The specific surface area of ​​Comparative Example 2 is 29.44 m². 2 ·g -1 The pore volume is 0.22cm. 3 ·g -1 The specific surface area and pore volume of Example 2 are higher than those of Comparative Example 2. Figure 5 As can be seen from (a) in the figure, both Example 2 and Comparative Example 2 exhibit typical type IV adsorption isotherms accompanied by type H3 hysteresis loops, indicating that they both have mesoporous structures. Figure 5 As can be seen from (b) in the figure, the pore sizes of Example 2 and Comparative Example 2 are mainly distributed between 30-100 nm. The average pore size of Example 2 is 20.74 nm, which is slightly smaller than that of Comparative Example 2 (23.07 nm). This indicates that the pore structure of the material after being loaded with ionic liquid is more uniform, which is more conducive to the diffusion and adsorption of gas molecules. Figure 5 As can be seen from (c), the CO2 adsorption capacity of Example 2 is significantly higher than that of Comparative Example 2, indicating that the loading of ionic liquid effectively improves its CO2 adsorption performance.

[0041] The light absorption properties of Examples 1-3 and Comparative Examples 1-2 were characterized using ultraviolet-visible spectrophotometry (UV-Vis), and the results are as follows: Figure 6 As shown. From Figure 6 As shown in (a), the absorption edge of Comparative Example 1 is located at approximately 450 nm, corresponding to an optical band gap of 2.78 eV. The absorption edges of Examples 1-3 exhibit a redshift compared to Comparative Examples 1 and 2, indicating that ionic liquid loading effectively enhances the catalyst's absorption capacity for visible light. With increasing ionic liquid content, the maximum absorption wavelength first increases and then decreases, with Example 2 showing the best visible light absorption performance at an absorption edge of 540 nm. Figure 6 (b) is the Tauc bandgap diagram calculated according to the Kubelka-Munk method. The calculated bandgap values ​​for Comparative Examples 1-2 and Examples 1-3 are 2.78, 2.79, 2.77, 2.75 and 2.81 eV, respectively.

[0042] The photogenerated carrier dynamics of Examples 1-3 and Comparative Examples 1-2 were characterized using photoluminescence spectroscopy (PL), photocurrent response, and electrochemical impedance spectroscopy. The results are as follows: Figure 7 As shown. From Figure 7As shown in (a), at an excitation wavelength of 400 nm, the peak intensity of Comparative Example 1 is significantly higher than that of other samples, indicating a high photogenerated electron-hole recombination rate. The peak intensity of Comparative Example 2 is lower than that of Comparative Example 1. The peak intensities of Examples 1-3 decrease with increasing ionic liquid loading, with Example 2 exhibiting the lowest fluorescence peak intensity, indicating that the ionic liquid-modified material can effectively suppress electron-hole recombination and improve the separation efficiency of photogenerated carriers. Figure 7 As can be seen from (b) in the figure, Comparative Example 1 has the lowest photocurrent response, Comparative Example 2 shows an improved photocurrent response, but the response intensity is limited; Example 2 has the highest photocurrent response, indicating that ionic liquid modification effectively promotes electron transfer. Figure 7 As shown in (c), the arc radius corresponds to the influence of interfacial charge transfer resistance. The impedance arc in Comparative Example 1 is relatively the largest, indicating that its interfacial charge transfer is difficult. The arc radius in Example 2 is the smallest, indicating that its interfacial resistance is smaller and its charge transfer rate is faster. All the above results prove that the method of modifying photocatalytic materials with ionic liquids can significantly improve their electron transfer ability.

[0043] The photocatalytic CO2 reduction performance of Examples 1-3 and Comparative Examples 1-6 was tested under visible light: The CO2 photocatalytic reduction performance was evaluated using a gas-solid interface reaction mode in a 50 mL quartz glass reaction vessel, with H2O as the reducing agent, and a 300W xenon lamp at an incident light intensity of 1000 mW / cm². 2 The light source was set at a wavelength range of 350-780 nm (CEL HXF300-T3). Specifically, 10 mL of deionized water was added to a quartz glass reactor, and a triangular support was placed inside. 1 mg of catalyst powder from Examples 1-3 and Comparative Examples 1-6 was uniformly coated onto the surface of the quartz plate supported by the triangular support. The reactor was sealed, and CO2 gas was bubbled into the device for 30 min to expel the air inside the reactor. Subsequently, the reaction system was continuously irradiated with a xenon lamp for 4 h. During this period, 1 mL of gaseous product was extracted from the reactor every 1 h, and the amount of CO and CH4 generated was detected by a gas chromatograph (GC 7820) equipped with a flame ionization detector (FID).

[0044] The results are as follows Figure 8 As shown. From Figure 8 As can be seen from (a)-(c) in the figures, Examples 1-3 and Comparative Examples 1 and 2 all exhibit catalytic activity, with Example 2 showing the best performance. After reacting for 4 hours under visible light irradiation, the CO and CH4 production amounts reached 375.2 and 23.4 μmol·g, respectively. -1 The CO selectivity reached 94%; the CO yield of Comparative Example 1 after 4 hours of reaction was 17 μmol·g. -1 The CO yield of Comparative Example 2 after 4 hours of reaction was 140.8 μmol·g.-1 The CO yield in Example 2 was increased by 22 and 2.66 times compared to Comparative Examples 1 and 2, respectively, indicating that the ionic liquid-modified material has superior photocatalytic CO2 reduction activity. Figure 8 As can be seen from (d) in the figure, the composite photocatalysts prepared in different solvents can all catalyze the CO2 photoreduction reaction. The sample prepared in Example 2 under methanol solvent conditions has the best catalytic activity.

[0045] The cyclic stability of Example 2 in the visible light catalytic CO2 reduction reaction was tested, and the results are as follows: Figure 9 As shown. From Figure 9 As can be seen from (a) in the figure, after four cycles, the CO yield and selectivity of Example 2 remained essentially unchanged. Figure 9 As can be seen from (b) and (c) in Example 2, the molecular structure did not change in the XRD and FT-IR spectra before and after cycling, further proving that Example 2 has excellent cycling stability.

[0046] In summary, the composite photocatalyst with ionic liquid modified V2O5 / g-C3N4 heterojunction provided by this invention exhibits excellent activity, selectivity and stability in the photocatalytic reduction of CO2 to CO reaction, and has important application prospects.

[0047] Therefore, the present invention employs the above-mentioned photocatalyst and its preparation method and application, using a methanol solvent-mediated ultrasonic-assisted impregnation method to stably combine the imidazole ring cations of the ionic liquid with the amino groups on the surface of VOCN through hydrogen bonding, thereby increasing the specific surface area and CO2 adsorption capacity of the catalyst, broadening the visible light response range, delaying electron-hole recombination efficiency, and significantly improving photocatalytic performance.

[0048] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit them. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the technical solutions of the present invention, and these modifications or equivalent substitutions cannot cause the modified technical solutions to deviate from the spirit and scope of the technical solutions of the present invention.

Claims

1. A method for preparing a composite photocatalyst, characterized in that: Includes the following steps: S1. Melamine is heated to undergo thermal polymerization, then cooled and ground to obtain g-C3N4 powder; S2. Mix g-C3N4 powder with ammonium metavanadate, grind, calcine, cool, wash, vacuum dry, and grind to obtain V2O5 / g-C3N4 heterojunction; S3. Imidazole-based ionic liquids are dispersed in methanol solvent, and subjected to first stirring and first sonication. V2O5 / g-C3N4 heterojunctions are added and subjected to second stirring and second sonication. The mixture is then centrifuged, vacuum dried, and ground to obtain a composite photocatalyst modified with ionic liquids on V2O5 / g-C3N4 heterojunctions. In S3, the imidazole ionic liquid includes one or more of 1-butyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium tetrafluoroborate, and 1-octyl-3-methylimidazolium tetrafluoroborate.

2. The method for preparing a composite photocatalyst according to claim 1, characterized in that: In S1, the heating rate of thermal polymerization is 4-6℃ / min, the temperature of thermal polymerization is 540-560℃, and the time of thermal polymerization is 2-4h.

3. The method for preparing a composite photocatalyst according to claim 1, characterized in that: In S2, the mass ratio of g-C3N4 powder to ammonium metavanadate is 5-20:1, the calcination heating rate is 4-6℃ / min, the calcination temperature is 490-510℃, the calcination time is 2-4h, the vacuum drying temperature is 60℃, and the vacuum drying time is 12h.

4. The method for preparing a composite photocatalyst according to claim 1, characterized in that: In S3, the mass-to-volume ratio of imidazole ionic liquid, V2O5 / g-C3N4 heterojunction, and methanol is 5-15 mg: 0.1 g: 15-25 mL.

5. The method for preparing a composite photocatalyst according to claim 1, characterized in that: In S3, the first stirring time is 30 min, the first ultrasonic time is 30 min, the second stirring time is 2-4 h, the second ultrasonic time is 0.5-1.5 h, the vacuum drying temperature is 60℃, and the vacuum drying time is 12 h.

6. A composite photocatalyst, characterized in that: It was prepared using the method described in any one of claims 1-5 for the preparation of a composite photocatalyst.

7. The application of the composite photocatalyst as described in claim 6 in photocatalytic CO2 reduction.

Citation Information

Patent Citations

  • Ionic liquid catalyst as well as preparation method and application thereof

    CN117069763A

  • Photocatalytic composite material, preparation method thereof and application of photocatalytic composite material in reduction of carbon dioxide

    CN117548143A