A high-bonding-strength thermal insulation coating material, its preparation method, and its application.
By using (Y1/3Cr1/3Co1/3)2Si2O7 hollow ceramic powder and inorganic silica resin film-forming agent to form a high bonding strength thermal insulation coating, the problems of insufficient bonding strength and cooling gradient of existing coating materials under high temperature service environment are solved, and excellent thermal insulation performance and high toughness at 500℃ are achieved.
Patent Information
- Application Number
- CN202611327648.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2046-08-31
AI Technical Summary
Existing thermal protection coating materials suffer from low bonding strength and insufficient cooling gradient in high-temperature service environments, making it difficult to meet the stringent service requirements of aerospace equipment.
(Y1/3Cr1/3Co1/3)2Si2O7 hollow ceramic powder is used as the heat insulation aggregate, combined with inorganic silica resin film-forming agent and filler, and a high-bonding heat insulation coating is formed by air spraying technology. The hollow structure and chemical bonding interface form a three-dimensional continuous network, which improves the heat insulation performance and bonding strength of the coating.
It achieves a coating bonding strength of ≥5MPa and a thermal conductivity of ≤0.3W·m-1·K-1 at a high temperature of 500℃, with a cooling gradient of up to 130℃. It is suitable for complex structural surfaces and has excellent thermal insulation performance and high toughness.
Smart Images

Figure CN122832613B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of high-temperature thermal protection coating technology, specifically relating to a high-bonding-strength thermal insulation coating material, its preparation method, and its application. Background Technology
[0002] Inorganic thermal / environmental barrier coating materials have attracted much attention due to their excellent high-temperature stability, mainly including rare earth tantalates (RETaO4, RE3TaO7, and RETa3O9) and rare earth hexaaluminates (REMA1). 11 O 19 Rare earth cerates (RE₂Ce₂O₇), rare earth silicates (RE₂SiO₅ and RE₂Si₂O₇), rare earth phosphates (REPO₄), rare earth stannates (RE₂Sn₂O₇), perovskite (ABO₃), yttrium aluminum garnet (YAG), and rare earth aluminates (RE₄Al₂O₉) are among the most common. Among these, the rare earth tantalate RETaO₄ system has become a research hotspot in the field of thermal / environmental barrier coatings in recent years due to its intrinsically low thermal conductivity, excellent high-temperature phase stability, and tunable coefficient of thermal expansion. Studies have shown that by using rare earth element doping and high-entropy design strategies, its thermophysical properties can be further optimized, achieving effective reduction of thermal conductivity and directional control of the coefficient of thermal expansion. However, the aforementioned inorganic coating materials are mainly prepared by atmospheric plasma spraying (APS) or electron beam physical vapor deposition (EB-PVD) technology. Due to the limitations of the preparation process, the coating thickness is usually no more than 0.5 mm, which is difficult to meet the technical requirements of large temperature gradient (>230℃); and when the thickness exceeds 1 mm, the coating bonding strength decreases sharply.
[0003] Organic polymer coating materials (such as polyurethane and epoxy resin) have the advantages of intrinsically low thermal conductivity and low coefficient of thermal expansion, and their preparation process is simple and low-cost. However, their inherent drawback lies in insufficient temperature resistance: when the operating temperature exceeds 200℃, organic polymer materials are prone to thermo-oxidative aging, molecular chain breakage, and ablation failure, making it difficult to meet the requirements for long-term high-temperature service. Even with modification using organic-inorganic hybrid technology, it is still difficult to solve the problems of poor ablation resistance and low service temperature.
[0004] Aerogel coatings possess extremely low thermal conductivity and density, and their temperature resistance and thermal insulation properties vary significantly with different inorganic solid content. However, aerogel coatings generally suffer from fatal defects such as extremely low bonding strength and poor erosion resistance, and are currently mainly used in the field of civil insulation materials.
[0005] In summary, current research on thermal protective coatings still has the following shortcomings: (1) Although inorganic thermal / environmental barrier coating materials have excellent high-temperature stability, they are limited by preparation processes such as atmospheric plasma spraying, resulting in thin coating thickness and insufficient cooling gradient; (2) Although organic polymer coating materials can be prepared into thick coatings, they have poor thermal stability and low service temperature, making it difficult to meet the long-term service requirements of medium-temperature operating conditions; (3) Aerogel coatings have extremely low bonding strength and poor erosion resistance, making them difficult to apply to harsh aerospace service environments. Therefore, it is necessary to develop thermal protective coating materials with high bonding strength and cooling gradient for low-temperature service environments (≤500℃). Summary of the Invention
[0006] The purpose of this invention is to overcome the shortcomings of the prior art and provide a high bonding strength heat insulation coating material, its preparation method and application. It is a high bonding strength and high heat insulation coating material with a temperature resistance of 200~500℃, which solves the problems of low temperature resistance of organic coatings, low cooling gradient of thermal barrier coatings and low bonding strength of aerogel coatings.
[0007] The objective of this invention is achieved through the following technical solution: The first aspect of this invention is to provide a high-bonding-strength thermal insulation coating material, the raw materials comprising: thermal insulation aggregate, film-forming aid, and filler in a mass ratio of (20~40):(40~50):(13~35), wherein the thermal insulation aggregate is (Y 1 / 3Cr 1 / 3 Co 1 / 3 The hollow ceramic powder of 2Si2O7 comprises Y2O3, Cr2O3, Co2O3, and SiO2 as raw materials; the film-forming aid is an inorganic silica resin film-forming agent, comprising polysilazane [H2Si-NH] in a mass ratio of (300~350):(5~7):(100~120):(1~3). n Coupling agent C 10 H 20 O5Si, nano-silica, and acrylic terpolymer.
[0008] This invention addresses the problems of poor thermal stability and low bonding strength with the substrate in existing heat-insulating coatings by designing a coating composition comprising (Y 1 / 3 Cr 1 / 3 Co 1 / 3 )2Si2O7 hollow ceramic powder is used as the heat insulation skeleton, inorganic silica resin film-forming agent is used as the binder matrix of the coating material, and filler is used as an auxiliary additive to adjust other properties of the coating. First, this application synthesizes (Y 1 / 3 Cr 1 / 3 Co 1 / 32Si₂O₇ is a rare-earth pyrosilicon with low intrinsic thermal conductivity. The Cr / Co solid solution in the crystal introduces lattice distortion, enhancing phonon scattering. Further employing a hollow structure utilizes the gas-solid interface to significantly increase phonon scattering, reducing the heat transfer rate and thus increasing the cooling gradient to form the main thermal barrier. The hollow structure also blocks heat conduction paths, disperses thermal stress, and maintains high thermal insulation performance over time. Regarding element selection, Cr / Co synergistic doping enhances the material's infrared radiation absorption capacity at high temperatures, improving heat dissipation efficiency and facilitating heat release to the surface. Multi-element solid solution suppresses high-temperature phase transitions, ensuring coating structural stability. The mass fraction of the thermal insulation aggregate is set between 20 and 40 parts. A fraction below 20 parts leads to increased thermal conductivity and a significant increase in back surface temperature, while a fraction above 40 parts easily causes increased internal stress in the coating and decreased bonding strength.
[0009] Specifically, this application selects Y2O3, Cr2O3, Co2O3, and SiO2 according to (Y 1 / 3 Cr 1 / 3 Co 1 / 3 The stoichiometric ratio of elements in 2Si2O7 is combined and sintered to obtain the product, in which (Y) 1 / 3 Cr 1 / 3 Co 1 / 3 In RE2Si2O7, Y, Cr, and Co occupy rare earth sites in an equimolar ratio of 1:1:1, and the stoichiometric ratio of total rare earth elements to silicon is RE:Si = 1:1, which is typical of RE2Si2O7 pyrosilicon structure. The equimolar ratio (each occupying 1 / 3) can increase the mixing entropy and lattice distortion, thereby maximizing the in-situ generation of lattice defects, increasing phonon scattering, and reducing the heat transfer rate.
[0010] Secondly, this application uses an inorganic silica resin film-forming agent, which possesses excellent film-forming properties. Combined with an ultrasonic dispersion process, this results in a dense coating structure and allows for the preparation of a uniform coating using air spraying technology. This ensures uniform coating on complex surfaces such as fastener protrusions / recesses, without issues of accumulation or missed coating. As a bonding matrix for the coating, it forms a continuous and dense ceramic resin network, not only imparting good film-forming properties and adhesion to the substrate but also uniformly dispersing hollow aggregates and fillers. More importantly, the inorganic silica resin film-forming agent prepared in this application exhibits high-temperature resistance (500~800℃) and extremely high bonding strength, overcoming the technical bottlenecks of commonly used organic polymer coating materials' low temperature tolerance and extremely low bonding strength of aerogel coatings. The addition of the film-forming aid is set at 40~50 parts by mass. Adding less than 40 parts leads to a significant decrease in coating bonding strength and uneven coating, while excessively high content results in insufficient thermal insulation filler and a decrease in thermal insulation performance.
[0011] Specifically, the film-forming aid used in this application is polysilazane [H2Si-NH]. nCoupling agent C 10 H 20 The mixture is prepared by dispersing O5Si, nano-silica, and an acrylic terpolymer and stirring until homogeneous. The selected coupling agent C... 10 H 20 O5Si corresponds to γ-(methacryloyloxy)propyltrimethoxysilane, also known as the common silane coupling agent KH-570. This coupling agent is an organosilicon monomer with bidirectional reactive groups. The trimethoxysilane group at one end can chemically bond with the hydroxyl groups on the surface of nano-silica and hollow ceramic powder, improving the dispersibility of the filler. The methacryloyloxy group at the other end participates in the cross-linking and curing reaction of polysilazane, enhancing the interfacial bonding force between the filler and the film-forming agent, and promoting the formation of organic-inorganic hybrid networks.
[0012] Finally, regarding the surfaces of metal and other substrates, the interfacial bonding between rare earth insulating aggregates and the substrate suffers from weak adhesion. Relying solely on insulating aggregates or film-forming base materials cannot simultaneously achieve both insulating performance and bonding strength, and it is difficult to balance these two properties. Furthermore, the poor dispersion and compatibility of components within the coating system are problematic. Firstly, the large polarity difference between inorganic rare earth aggregates and organic film-forming base materials leads to weak interfacial bonding, easily forming interfacial defects and weakening both coating adhesion and insulating performance. Secondly, aggregate powders are prone to agglomeration, resulting in uneven dispersion within the base material and inconsistent coating performance. Thirdly, the proportions are difficult to balance; a high aggregate content can cause film embrittlement, while a high base material content results in insufficient insulating effect, ultimately leading to uneven coating structure and performance. This application discovers a synergistic effect between the insulating aggregates and film-forming agents used and amplifies this synergistic effect through formulation ratio control.
[0013] Specifically, the hollow aggregate and film-forming agent of this application form a composite structure of "chemical bonding interface - three-dimensional continuous network," achieving a synergistic unity of high bonding strength and high thermal insulation: the hollow structure of the hollow aggregate forms a static air layer to block heat conduction, but the aggregate surface is smooth and the bonding force is poor; after the inorganic silica resin film-forming agent is cured, it reacts with the hydroxyl groups on the surface of the hollow aggregate through Si-O-RE and Si-O-Si chemical bonds to form a strong chemical bonding interface, which significantly improves the bonding strength between coating components. At the same time, the nano-silica dispersion system in the film-forming agent can penetrate and fill the gaps in the aggregate, uniformly wrapping the aggregate and forming a three-dimensional continuous silica network, which is transformed into silica ceramic at high temperature, enhancing thermal stability and inhibiting the sintering collapse of the hollow aggregate, significantly improving the bonding strength between the coating and the substrate.
[0014] Preferably, the (Y) 1 / 3 Cr 1 / 3 Co 1 / 3 The particle size of the 2Si2O7 hollow ceramic powder is 20~80μm, and the purity is ≥99.9%. It is understandable that even strictly following (Y...) 1 / 3 Cr1 / 3 Co 1 / 3 The raw materials are prepared by weighing them according to the stoichiometric ratio of 2Si2O7. Impurities may still be introduced into the raw materials themselves or during the preparation process. Using the above-mentioned high-purity inorganic raw materials can avoid the introduction of impurities that affect the heat insulation and high-temperature stability of the coating. The inorganic silica resin film-forming agent with appropriate solid content can ensure the film-forming properties and the dispersibility of each component of the coating, thus ensuring the forming quality of the coating.
[0015] Preferably, the acrylic terpolymer is copolymerized from acrylic acid, butyl acrylate and acrylamide in a ratio of 1:1:2. The inorganic silica resin film-forming agent has a solid content of 30-50%, which is used to disperse nano-silica and facilitate the formation of a cross-linked resin network.
[0016] Preferably, the filler is basalt fiber powder and glass powder, with a mass ratio of basalt fiber powder : glass powder = (3~10) : (10~25). Basalt fiber powder is preferred as a toughening component, as it can form a fiber skeleton network in the coating. Its high elastic modulus and large aspect ratio effectively absorb crack propagation energy, improving the coating's resistance to mechanical impact and thermal shock. When its mass fraction is less than 3 parts, the toughening effect is not significant; when it is more than 10 parts, it leads to fiber agglomeration and an increase in internal defects in the coating. Glass powder is preferred as a self-healing filler, as it can melt into a glass phase during high-temperature service (approximately 500~800℃), filling pores and microcracks in the coating, achieving coating densification and self-repair of defects, improving high-temperature stability and corrosion resistance. Without glass powder, the coating is prone to microcracks at high temperatures, resulting in increased back temperature and significantly reduced bonding strength. Excessive glass powder content leads to excessive softening of the coating at high temperatures, affecting its mechanical properties.
[0017] More preferably, the basalt fiber powder has a length of 50-150 μm, a diameter of 5-10 μm, and an aspect ratio of (15-30):1; the glass powder has a particle size of 15-25 μm. Using raw materials with the above-mentioned particle size and morphology allows for the close packing of the solid components, reducing internal porosity in the coating. Simultaneously, the basalt fiber powder can be uniformly dispersed to form a tough support, further improving the coating's density and mechanical properties.
[0018] Specifically, the viscosity of the heat insulation coating material is 0.95~0.98 Pa·s, which can ensure good atomization and uniform distribution of filler while achieving effective film formation in a single pass, avoiding common process defects such as sagging, gun clogging and filler protrusion.
[0019] In a preferred embodiment of the present invention, the mass ratio of each raw material is hollow (Y). 1 / 3 Cr 1 / 3 Co 1 / 3The ratio of 2Si₂O₇: inorganic silica resin film-forming agent: basalt fiber powder: glass powder is 30:45:5:20. Using this optimal mass ratio of raw materials, the performance of each functional component can be maximized through synergy. The resulting composite thermal insulation coating material achieves an optimal balance of thermal insulation, toughness, bonding strength, and high-temperature stability, meeting the core thermal protection requirements of alternating high-temperature conditions up to 500℃.
[0020] A second aspect of the present invention is to provide a method for preparing the above-mentioned high bonding strength heat-insulating coating material, comprising the following steps: Preparation of insulating aggregate: according to (Y 1 / 3 Cr 1 / 3 Co 1 / 3 The stoichiometric ratio of Y₂O₃, Cr₂O₃, Co₂O₃, and SiO₂ was weighed and ball-milled in a planetary ball mill for 10-15 hours at a speed of 300-350 r / min. The mixture was then calcined in a high-temperature box furnace at 1400℃ for 5 hours, furnace-cooled, and sieved through a 180-mesh sieve to obtain coarse powder. This coarse powder was then granulated using a centrifugal spray granulator with water as the solvent and a spray nozzle frequency of 31-33 Hz to obtain the (Y₂O₃)₂Si₂O₇. 1 / 3 Cr 1 / 3 Co 1 / 3 )2Si2O7 hollow ceramic powder.
[0021] This application describes the preparation of hollow insulating aggregate (Y) using a combination of solid-state method and centrifugal spray granulation. 1 / 3 Cr 1 / 3 Co 1 / 3 The present invention, using 2Si2O7, reveals that the proportion of hollow spheres can be effectively controlled by adjusting the nozzle frequency and solvent type. When the solvent is water and the nozzle frequency is higher than 31Hz, the proportion of hollow spheres in the aggregate is relatively large; when the solvent is changed to industrial alcohol and the nozzle frequency is 26~30Hz, the proportion of solid spheres in the aggregate is relatively large.
[0022] Preparation of film-forming aid: Weigh the polysilazane [H2Si-NH] according to the specified mass ratio. n The coupling agent C 10 H 20 The inorganic silica resin film-forming agent is obtained by mixing O5Si, the nano-silica, and the acrylic terpolymer, followed by ultrasonic dispersion and uniform stirring.
[0023] Preparation of heat-insulating coating material: Weigh the following (Y) according to the mass ratio 1 / 3 Cr 1 / 3 Co 1 / 3 The heat-insulating coating material is obtained by mixing 2Si2O7 hollow ceramic powder, the inorganic silica resin film-forming agent, and the filler in a mixer.
[0024] Preferably, when preparing the film-forming aid, the polysilazane [H2Si-NH] is used. n The coupling agent C 10 H 20 The inorganic silica resin film-forming agent is obtained by mixing O5Si, the nano-silica, and the acrylic terpolymer and then ultrasonically dispersing the mixture at 180W for 15 minutes under water bath protection at 5-10℃.
[0025] A third aspect of the present invention is to provide an application of the above-mentioned high bonding strength heat insulation coating material, wherein the heat insulation coating material is coated onto the surface of a metal substrate using air spraying technology, and after curing, a heat insulation coating is formed. The bonding strength of the heat insulation coating is 5~8MPa, and the back temperature is below 70℃ within a test temperature of 400~500℃ and a test time of 600s.
[0026] Specifically, when spraying the heat-insulating coating material, the spray gun distance is 200~250mm, and the spray thickness is 2~3mm; it is cured at room temperature for 20 hours or heated and cured at 80℃ for 3 hours. The spray thickness meets the basic requirements of the heat-insulating coating without sagging or uneven coating, and the bonding strength between the coating materials is good.
[0027] The beneficial effects of this invention are: (1) This invention designs hollow ceramic powder (Y) 1 / 3 Cr 1 / 3 Co 1 / 3 The main components of the hollow (Y) core are 2Si2O7, inorganic silica resin film-forming agent, basalt fiber powder, and glass powder. 1 / 3 Cr 1 / 3 Co 1 / 3 2Si2O7 provides excellent thermal insulation performance, inorganic silica resin film-forming agent ensures film density, basalt fiber powder significantly enhances toughness, and glass powder melts at high temperature to achieve coating self-healing, filling pores and cracks. By precisely controlling the mass ratio, the functions of each raw material are complementary and the performance is enhanced. Compared with the prior art, the coating prepared by this invention has advantages such as excellent thermal insulation performance, high toughness, strong adhesion, excellent formability and coating properties, high temperature stability and simple preparation process.
[0028] (2) The coating of this application, after optimization of the raw material formula, can achieve an internal air temperature of ≤70℃ and a thermal conductivity of ≤0.3W·m under a high temperature environment of 500℃. -1 ·K -1 It has a bonding strength of ≥5MPa, a temperature gradient of up to 130℃, and can maintain uniform thickness on the surface of raised / depressed structures without accumulation or peeling.
[0029] (3) The coating of this application is easy to spray and the preparation process is simple and controllable. It can form an effective coating with high bonding strength by using only air spraying process. It is easy to implement in engineering and is suitable for coating the surface of connection and separation devices of different sizes and structures. Attached Figure Description
[0030] Figure 1 For the present invention (Y) 1 / 3 Cr 1 / 3 Co 1 / 3 SEM image of 2Si2O7 hollow ceramic powder.
[0031] Figure 2 The back temperature curves of the thermal insulation coatings in Examples 1 and 1-7 are shown.
[0032] Figure 3 The graph shows a comparison of the thermal conductivity of the heat-insulating coatings of Examples 1 and 1-4 at different temperatures. Detailed Implementation
[0033] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0034] See Figure 1-3 The present invention provides a technical solution: A high-bonding-strength thermal insulation coating material, comprising: thermal insulation aggregate, film-forming aid, and filler in a mass ratio of (20~40):(40~50):(13~35), wherein the thermal insulation aggregate is (Y 1 / 3 Cr 1 / 3 Co 1 / 3 The hollow ceramic powder of 2Si2O7 comprises Y2O3, Cr2O3, Co2O3, and SiO2 as raw materials; the film-forming aid is an inorganic silica resin film-forming agent, comprising polysilazane [H2Si-NH] in a mass ratio of (300~350):(5~7):(100~120):(1~3). n Coupling agent C 10 H 20 O5Si, nano-silica, and acrylic terpolymer.
[0035] Preferably, the (Y) 1 / 3 Cr 1 / 3 Co 1 / 3 The particle size of the 2Si2O7 hollow ceramic powder is 20~80μm and the purity is ≥99.9%.
[0036] Preferably, the acrylic terpolymer is copolymerized from acrylic acid, butyl acrylate and acrylamide in a ratio of 1:1:2; the inorganic silica resin film-forming agent has a solid content of 30-50%.
[0037] Preferably, the filler is basalt fiber powder and glass powder, and the mass ratio of the two is basalt fiber powder: glass powder = (3~10): (10~25).
[0038] More preferably, the basalt fiber powder has a length of 50~150μm, a diameter of 5~10μm, and an aspect ratio of (15~30):1; the glass powder has a particle size of 15~25μm.
[0039] Specifically, the viscosity of the heat-insulating coating material is 0.95~0.98 Pa·s.
[0040] A method for preparing the above-mentioned high bonding strength heat-insulating coating material includes the following steps: Preparation of insulating aggregate: according to (Y 1 / 3 Cr 1 / 3 Co 1 / 3 The stoichiometric ratio of Y₂O₃, Cr₂O₃, Co₂O₃, and SiO₂ was weighed and ball-milled in a planetary ball mill for 10-15 hours at a speed of 300-350 r / min. The mixture was then calcined in a high-temperature box furnace at 1400℃ for 5 hours, furnace-cooled, and sieved through a 180-mesh sieve to obtain coarse powder. This coarse powder was then granulated using a centrifugal spray granulator with water as the solvent and a spray nozzle frequency of 31-33 Hz to obtain the (Y₂O₃)₂Si₂O₇. 1 / 3 Cr 1 / 3 Co 1 / 3 )2Si2O7 hollow ceramic powder.
[0041] Preparation of film-forming aid: Weigh the polysilazane [H2Si-NH] according to the specified mass ratio. n The coupling agent C 10 H 20 The inorganic silica resin film-forming agent is obtained by mixing O5Si, the nano-silica, and the acrylic terpolymer, followed by ultrasonic dispersion and uniform stirring.
[0042] Preparation of heat-insulating coating material: Weigh the following (Y) according to the mass ratio 1 / 3 Cr 1 / 3 Co 1 / 3 The heat-insulating coating material is obtained by mixing 2Si2O7 hollow ceramic powder, the inorganic silica resin film-forming agent, and the filler in a mixer.
[0043] Preferably, when preparing the film-forming aid, the polysilazane [H2Si-NH] is used.n The coupling agent C 10 H 20 The inorganic silica resin film-forming agent is obtained by mixing O5Si, the nano-silica, and the acrylic terpolymer and then ultrasonically dispersing the mixture at 180W for 15 minutes under water bath protection at 5-10℃.
[0044] One application of the above-mentioned high bonding strength heat insulation coating material is to coat the heat insulation coating material onto the surface of a metal substrate using air spraying technology, and form a heat insulation coating after curing. The bonding strength of the heat insulation coating is 5~8MPa, and the back temperature is below 70℃ within a test temperature of 400~500℃ and a test time of 600s.
[0045] Specifically, when spraying the heat-insulating coating material, the spray gun distance is 200~250mm, and the spray thickness is 2~3mm; it is cured at room temperature for 20h or heated and cured at 80℃ for 3h.
[0046] Example 1
[0047] The preparation process and spraying method of the high bonding strength heat insulation coating material in this embodiment 1 are basically the same as those in the specific implementation method, and the specific implementation is as follows: Insulating aggregate (Y) 1 / 3 Cr 1 / 3 Co 1 / 3 Preparation of 2Si2O7 hollow ceramic powder: Y2O3 (22.581g), Cr2O3 (15.2g), Co2O3 (16.586g), and SiO2 (36.051g) were weighed and ball-milled in a planetary ball mill for 10 hours at a speed of 350 r / min. The powder was then calcined in a high-temperature box furnace at 1400℃ for 5 hours. After furnace cooling, the powder was sieved through a 180-mesh sieve to obtain coarse powder. This coarse powder was granulated using a centrifugal spray granulator with water as the solvent and a spray nozzle frequency of 33 Hz to obtain hollow ceramic powder. Electron microscopy (EM) analysis of the hollow ceramic powder was performed; the EM images are shown below. Figure 1 As shown, by Figure 1 It can be seen that ceramic powder with a distinct hollow structure can be obtained by using the raw material formulation and preparation method of this application.
[0048] Preparation of inorganic silica resin film-forming agent: Weigh polysilazane [H2Si-NH] at a mass ratio of 300:5:100:1. n Coupling agent C 10 H 20 O5Si, nano-silica, and acrylic terpolymer were ultrasonically dispersed for 15 minutes at 180W under a water bath protection at 5-10℃, and then stirred until homogeneous. The acrylic terpolymer was composed of acrylic acid, butyl acrylate, and acrylamide monomers in a 1:1:2 ratio.
[0049] Coating preparation: according to mass ratio (Y) 1 / 3 Cr 1 / 3 Co 1 / 3 The following raw materials were prepared: 2Si₂O₇ hollow ceramic powder : inorganic silica resin film-forming agent : basalt fiber powder : glass powder = 20 : 40 : 3 : 10. The mixture was stirred evenly in a mixer, and the viscosity of the coating was adjusted to 0.95 Pa·s to obtain the heat-insulating coating.
[0050] Coating preparation: The obtained heat insulation coating was sprayed onto a titanium alloy with a diameter of 25.4 mm and a thickness of 3 mm using air spraying technology. The spray gun distance was 225 mm, and the coating thickness was controlled to be 2 mm. The coating was cured at room temperature for 20 hours.
[0051] Example 2
[0052] The preparation process and spraying method of the high bonding strength heat insulation coating material in Example 2 are consistent with those in Example 1, the only difference being that the mass ratio of each raw material is (Y). 1 / 3 Cr 1 / 3 Co 1 / 3 2Si2O7 hollow ceramic powder: inorganic silica resin film-forming agent: basalt fiber powder: glass powder = 30:45:5:20.
[0053] Example 3
[0054] The preparation process and spraying method of the high bonding strength heat insulation coating material in Example 3 are consistent with those in Example 1, the only difference being that the mass ratio of each raw material is (Y). 1 / 3 Cr 1 / 3 Co 1 / 3 2Si2O7 hollow ceramic powder: inorganic silica resin film-forming agent: basalt fiber powder: glass powder = 40:50:10:25.
[0055] Example 4
[0056] The raw material ratio and preparation process of the high bonding strength heat insulation coating material in Example 4 are the same as those in Example 1. The only difference is that the coating thickness is 3mm during spraying.
[0057] Comparative Example 1
[0058] The preparation process and spraying method of the heat insulation coating material in Comparative Example 1 are consistent with those in Example 1, the only difference being that the mass ratio of each raw material is (Y). 1 / 3 Cr 1 / 3 Co 1 / 3 )2Si2O7 hollow ceramic powder : inorganic silica resin film-forming agent : basalt fiber powder : glass powder = 10 : 40 : 3 : 10, i.e., thermal insulation aggregate (Y 1 / 3 Cr1 / 3 Co 1 / 3 The mass ratio of 2Si2O7 hollow ceramic powder is less than 20%.
[0059] Comparative Example 2
[0060] The preparation process and spraying method of the heat insulation coating material in Comparative Example 2 are consistent with those in Example 1, the only difference being that the mass ratio of each raw material is (Y). 1 / 3 Cr 1 / 3 Co 1 / 3 The ratio of 2Si2O7 hollow ceramic powder: inorganic silica resin film-forming agent: basalt fiber powder: glass powder is 20:30:3:10, which means reducing the content of inorganic silica resin film-forming agent.
[0061] Comparative Example 3
[0062] The preparation process and spraying method of the heat-insulating coating material in Comparative Example 3 are consistent with those in Example 1, the only difference being that the mass ratio of each raw material is (Y). 1 / 3 Cr 1 / 3 Co 1 / 3 The ratio of 2Si2O7 hollow ceramic powder: inorganic silica resin film-forming agent: basalt fiber powder: glass powder is 20:40:3:0, i.e., no glass powder is added.
[0063] Comparative Example 4
[0064] The preparation process and spraying method of the heat-insulating coating material in Comparative Example 4 are consistent with those in Example 1, the only difference being: the material used (Y 1 / 3 Cr 1 / 3 Co 1 / 3 )2Si2O7 is a solid ceramic powder.
[0065] It is understandable that the hollow ceramic powder (Y) in Example 1 1 / 3 Cr 1 / 3 Co 1 / 3 The preparation method of 2Si2O7 is as follows: according to (Y 1 / 3 Cr 1 / 3 Co 1 / 3 The stoichiometric ratio of Y₂O₃, Cr₂O₃, Co₂O₃, and SiO₂ was weighed and ball-milled in a planetary ball mill for 10 hours at 350 r / min. The mixture was then calcined in a high-temperature box furnace at 1400℃ for 5 hours. After furnace cooling, the powder was sieved through a 180-mesh sieve to obtain coarse powder. This coarse powder was then granulated using a centrifugal spray granulator with water as the solvent and a spray nozzle frequency of 33 Hz to obtain (Y₂O₃, Cr₂O₃, Co₂O₃, and SiO₂) 1 / 3 Cr 1 / 3 Co 1 / 3 2Si2O7 hollow ceramic powder In Comparative Example 4, the solid ceramic powder (Y) 1 / 3Cr 1 / 3 Co 1 / 3 The preparation method of 2Si2O7 is basically the same as the above method, with the only difference being that the solvent is alcohol and the nozzle frequency is 26Hz.
[0066] Comparative Example 5
[0067] The mass ratios of each raw material and the spraying method in Comparative Example 5 are consistent with those in Example 1, except that the raw material of the heat insulation coating material (Y) 1 / 3 Cr 1 / 3 Co 1 / 3 )2Si2O7 hollow ceramic powder replaced with (Y 0.5 Cr 0.3 Co 0.2 )2Si2O7 hollow ceramic powder.
[0068] Comparative Example 6
[0069] The raw materials and preparation process of the heat insulation coating material in Comparative Example 6 are the same as those in Example 1, except that the coating thickness is 1 mm during spraying.
[0070] Comparative Example 7
[0071] The raw materials and preparation process of the heat insulation coating material in Comparative Example 7 are basically the same as those in Example 1, except that the coating thickness is 4 mm during spraying.
[0072] Test case
[0073] Core performance tests were conducted on the coatings of Examples 1-4 and Comparative Examples 1-7. The tests included: the back surface temperature (°C) of the coatings in Examples 1-4 and Comparative Examples 1-6 at 500°C, thermal conductivity, coating-substrate bonding strength, and coating uniformity on raised surfaces. The test methods were as follows: (1) Back temperature (substrate temperature) test: Fix the gun distance and sample position, place the coating sample, test the surface temperature and back temperature of the coating sample by thermocouple, turn on the hot air gun, the heating rate is 100℃ / min, start timing when the coating surface temperature is 500℃, and keep warm for 10min.
[0074] (2) Thermal conductivity test: The thermal diffusivity of the thermal insulation coating material was determined using a laser thermal conductivity analyzer (LFA, Laser Flash Analyzer, NETZSCH LFA427, Germany). α Archimedes' drainage method for testing coating thermal conductivity ( ρ ), Popular science law for calculating coating heat capacity ( C p According to the formula κ=ρ C pα is used to calculate the thermal conductivity (κ) of the coating and analyze its thermal insulation performance.
[0075] (3) Adhesion test: The thermal insulation coating material was sprayed onto a titanium alloy substrate with a diameter of 25.4 mm and a thickness of 3 mm, and the adhesion strength was tested using a universal testing machine. ASTM C633–2008 (Standard Test Method for Adhesion or Bond Strength of Thermally Sprayed Coatings) was adopted.
[0076] (4) Coating condition: Visually inspect the coating sample to see if it shows any damage such as cracking, bubbling, or peeling after the test.
[0077] The test results are shown in Table 1-3. Figure 2 , 3 As shown in Table 1, the back temperature (substrate temperature) changes and bonding strength of Examples 1-4 and Comparative Examples 1-7 at a test temperature of 500°C are illustrated. Table 2 and... Figure 2 The table shows the changes in back temperature (substrate temperature) of Examples 1 and Comparative Examples 1-7 at test temperatures of 300-500℃. Figure 3 The thermal conductivity comparison graphs of the heat insulation coatings of Examples 1-4 and Comparative Examples 1-5 at different temperatures are shown.
[0078] Table 1. Backside temperature and adhesion strength of coatings under different conditions at a test temperature of 500℃.
[0079] Table 2. Back temperature of coatings in Examples 1 and Comparative Examples 1-7 at test temperatures of 300~500℃
[0080] Table 3. Thermal conductivity of the insulating coatings of Examples 1-4 and Comparative Examples 1-5 at different temperatures.
[0081] From Tables 1, 2, and 3, Figure 2 , 3 It can be seen that: 1. Comparative Example 1 and Comparative Example 1, the heat-insulating aggregate (Y 1 / 3 Cr 1 / 3 Co 1 / 3 When the mass ratio of 2Si2O7 is less than 20, its relative content decreases, thermal conductivity increases, and the thermal insulation performance of the coating decreases. When the test temperature is 500℃, the back temperature is much higher than 70℃.
[0082] 2. Comparative Example 1 and Comparative Example 2 show that when the mass ratio of inorganic silica resin film-forming agent is less than 40, its relative content decreases, the bonding strength between the coating and the substrate decreases significantly, and the uniformity of the raised surface deteriorates.
[0083] 3. Compared with Example 1 and Comparative Example 3, without the addition of glass powder, the coating is prone to microcracks at high temperatures, resulting in a decrease in long-term heat insulation performance and a significant reduction in bonding strength.
[0084] 4. Compared with Example 1 and Comparative Example 4, replacing hollow ceramic powder with solid ceramic powder results in a significant increase in the thermal conductivity of the coating and a sharp deterioration in the heat insulation effect.
[0085] 5. Comparing Example 1 and Comparative Example 5, using (Y) 0.5 Cr 0.3 Co 0.2 )2Si2O7 hollow ceramic powder replacement (Y 0.5 Cr 0.3 Co 0.2 )2Si2O7 is a solid ceramic powder. When a solid structure is used, the matching between its surface chemical activity and the film-forming agent and coupling agent decreases, the Si-O-RE bond density decreases, the synergistic chemical bonding interface cannot be effectively established, the thermal conductivity of the coating increases significantly, and the heat insulation effect deteriorates sharply.
[0086] 6. Compared with Example 1 and Comparative Example 6, when the coating thickness is reduced to 1 mm, the cross-linking effect between molecules is weaker, the thermal insulation temperature difference is greatly reduced, and the internal temperature of 500°C is significantly increased.
[0087] 7. Compared with Example 1 and Comparative Example 7, although increasing the coating thickness to 4mm can enhance heat insulation, it will lead to increased internal stress, decreased bonding strength, and exacerbate the problem of uneven thickness in the raised parts.
[0088] The above description is merely a preferred embodiment of the present invention. It should be understood that the present invention is not limited to the forms disclosed herein and should not be construed as excluding other embodiments. It can be used in various other combinations, modifications, and environments, and can be altered within the scope of the concept described herein through the above teachings or related technologies or knowledge. Modifications and variations made by those skilled in the art that do not depart from the spirit and scope of the present invention should be within the protection scope of the appended claims.
Claims
1. A high-bonding-strength thermal insulation coating material, characterized in that: Raw materials include: The heat-insulating aggregate, film-forming aid, and filler are present in a mass ratio of (20~40):(40~50):(13~35), wherein the heat-insulating aggregate is (Y 1 / 3 Cr 1 / 3 Co 1 / 3 )2Si2O7 hollow ceramic powder, the raw materials include: Y2O3, Cr2O3, Co2O3 and SiO2; The film-forming aid is an inorganic silica resin film-forming agent, and the raw materials include polysilazane [H2Si-NH] in a mass ratio of (300~350):(5~7):(100~120):(1~3). n Coupling agent C 10 H 20 O5Si, nano-silica, and acrylic terpolymer.
2. The high bonding strength thermal insulation coating material according to claim 1, characterized in that: The (Y) 1 / 3 Cr 1 / 3Co 1 / 3 The particle size of the 2Si2O7 hollow ceramic powder is 20~80μm and the purity is ≥99.9%.
3. The high bonding strength thermal insulation coating material according to claim 1, characterized in that: The acrylic terpolymer is copolymerized from acrylic acid, butyl acrylate and acrylamide in a ratio of 1:1:2; the inorganic silica resin film-forming agent has a solid content of 30-50%.
4. The high bonding strength heat-insulating coating material according to claim 1, characterized in that: The filler is basalt fiber powder and glass powder, and the mass ratio of the two is basalt fiber powder: glass powder = (3~10): (10~25).
5. The high bonding strength heat-insulating coating material according to claim 4, characterized in that: The basalt fiber powder has a length of 50~150μm, a diameter of 5~10μm, and an aspect ratio of (15~30):1; the glass powder has a particle size of 15~25μm.
6. The high bonding strength thermal insulation coating material according to claim 1, characterized in that: The viscosity of the heat-insulating coating material is 0.95~0.98 Pa·s.
7. A method for preparing a high-bonding-strength thermal insulation coating material as described in any one of claims 1-6, characterized in that: Includes the following steps: Preparation of insulating aggregate: according to (Y 1 / 3 Cr 1 / 3 Co 1 / 3 The stoichiometric ratio of Y₂O₃, Cr₂O₃, Co₂O₃, and SiO₂ was weighed and ball-milled in a planetary ball mill for 10-15 hours at a speed of 300-350 r / min. The mixture was then calcined in a high-temperature box furnace at 1400℃ for 5 hours, furnace-cooled, and sieved through a 180-mesh sieve to obtain coarse powder. This coarse powder was then granulated using a centrifugal spray granulator with water as the solvent and a spray nozzle frequency of 31-33 Hz to obtain the (Y₂O₃)₂Si₂O₇. 1 / 3 Cr 1 / 3 Co 1 / 3 )2Si2O7 hollow ceramic powder; Preparation of film-forming aid: Weigh the polysilazane [H2Si-NH] according to the specified mass ratio. n The coupling agent C 10 H 20 O5Si, the nano-silica and the acrylic terpolymer are mixed and then ultrasonically dispersed and stirred evenly to obtain the inorganic silica resin film-forming agent. Preparation of heat-insulating coating material: Weigh the following (Y) according to the mass ratio 1 / 3 Cr 1 / 3 Co 1 / 3 The heat-insulating coating material is obtained by mixing 2Si2O7 hollow ceramic powder, the inorganic silica resin film-forming agent, and the filler in a mixer.
8. The method for preparing the high bonding strength thermal insulation coating material according to claim 7, characterized in that: In preparing the film-forming aid, the polysilazane [H2Si-NH] is used. n The coupling agent C 10 H 20 The inorganic silica resin film-forming agent is obtained by mixing O5Si, the nano-silica, and the acrylic terpolymer and then ultrasonically dispersing the mixture at 180W for 15 minutes under water bath protection at 5-10℃.
9. An application of a high-bonding-strength thermal insulation coating material as described in any one of claims 1-6, characterized in that: The heat insulation coating material is applied to the surface of a metal substrate using air spraying technology. After curing, a heat insulation coating is formed. The bonding strength of the heat insulation coating is 5~8MPa, and the back temperature is below 70℃ within a test temperature of 400~500℃ and a test time of 600s.
10. The application of the high bonding strength thermal insulation coating material according to claim 9, characterized in that: When spraying the heat-insulating coating material, the spray gun distance is 200~250mm, and the spray thickness is 2~3mm; cure at room temperature for 20h or heat to cure at 80℃ for 3h.
Citation Information
Patent Citations
Method for producing oligosilane and device for producing oligosilane
CN109923067A
Inorganic high-temperature-resistant heat-insulating coating as well as preparation method and application thereof
CN121450133A