A photothermal Janus nanofiber composite membrane, its preparation method and application

By preparing a photothermal Janus nanofiber composite membrane, utilizing the near-infrared photothermal effect of MXene nanosheets and the chemical antibacterial effect of baicalin, combined with a layer-by-layer electrospinning process, the problems of single antibacterial effect and poor exudate management of existing dressings in treating drug-resistant bacterial infected wounds are solved, achieving efficient antibacterial effect and rapid wound healing.

CN122856451BActive Publication Date: 2026-11-17ANHUI POLYTECHNIC UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611363433.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-09-04
Publication Date
2026-11-17
Estimated Expiration
2046-09-04

AI Technical Summary

Technical Problem

Existing dressings, when used to treat drug-resistant bacterial infections, suffer from limited antibacterial efficacy, poor exudate management, and poor interfacial bonding and mechanical properties in most composite dressings, failing to meet the clinical treatment needs of complex drug-resistant bacterial infections.

Method used

A photothermal Janus nanofiber composite membrane was prepared using a layer-by-layer electrospinning process. The membrane consists of a TM hydrophobic layer and a PCB hydrophilic layer. The TM layer contains MXene nanosheets and thermoplastic polyurethane, while the PCB layer contains polyvinyl alcohol, carboxymethyl chitosan, and baicalin, forming an asymmetric bilayer structure. This structure enables unidirectional liquid guidance and zoned protection. By combining near-infrared photothermal effects and chemical antibacterial effects, highly efficient antibacterial activity is achieved through the dual coupling of physical photothermal killing and chemical drug inhibition.

Benefits of technology

It achieves highly effective antibacterial activity against multidrug-resistant bacteria, high wound healing rate, excellent mechanical properties, good biocompatibility, and can significantly promote collagen deposition and angiogenesis in wounds, with a wound healing rate of nearly 100% in 14 days.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122856451B_ABST
    Figure CN122856451B_ABST
Patent Text Reader

Abstract

This invention relates to the field of biomedical textile materials technology, and discloses a photothermal Janus nanofiber composite membrane, its preparation method, and its applications. A photothermal Janus nanofiber composite membrane with a hydrophobic / hydrophilic asymmetric structure was prepared using a layer-by-layer electrospinning process. The outer layer of the composite membrane is a thermoplastic polyurethane hydrophobic layer containing MXene nanosheets, which achieves sterilization and effective barrier properties simultaneously through photothermal effects. The inner layer is a polyvinyl alcohol hydrophilic layer containing carboxymethyl chitosan and baicalin, exhibiting excellent wettability, swelling properties, and pH response characteristics. The components of the hydrophilic layer are reversibly cross-linked through dynamic hydrogen bonds, enabling pH-responsive sustained release of drugs. Simultaneously, hydrogen bonds enhance the wet strength and compatibility of the material, and baicalin acts as a cross-linking point to strengthen the fiber structure. The photothermal Janus nanofiber composite membrane prepared by this invention can be used to prepare dressings suitable for the treatment of infected wounds.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of biomedical textile materials technology, specifically to a photothermal Janus nanofiber composite membrane, its preparation method, and its application. Background Technology

[0002] The clinical treatment of infected wounds has long faced two core technical challenges: the difficulty in eradicating multidrug-resistant bacteria and the difficulty in managing wound exudate. With the widespread overuse of antibiotics, the clinical detection rate of "superbugs" such as methicillin-resistant Staphylococcus aureus (MRSA) and multidrug-resistant Escherichia coli (MRC) has been rising year by year. Drug-resistant bacteria can acquire antibiotic resistance through gene mutations and easily secrete extracellular polymers on the wound surface to form a dense biofilm, physically blocking antibiotic penetration and escaping the body's immune clearance, causing persistent wound infection, recurrent inflammation, and ultimately leading to chronic, difficult-to-heal wounds. Simultaneously, wound infection stimulates the wound surface to secrete large amounts of exudate rich in proteins and inflammatory factors. If this exudate cannot be drained in a timely and targeted manner, the excessively moist microenvironment of the wound surface will soak the surrounding healthy skin, providing a breeding ground for bacteria, forming a vicious cycle of "infection-inflammation aggravation-infection deterioration," significantly prolonging the wound healing period.

[0003] Currently, commonly used clinical dressings such as gauze and cotton pads have limited functions, only providing passive coverage and limited fluid absorption. They cannot precisely control wound exudate and lack specific antibacterial or anti-drug-resistant bacterial effects. Furthermore, dressings are prone to adhesion to the wound during dressing changes, causing secondary damage and failing to meet the clinical treatment needs of complex drug-resistant bacterial infections. Photothermal antibacterial therapy, as a non-antibiotic-dependent physical antibacterial technology, has advantages such as rapid response, broad antibacterial spectrum, and low likelihood of inducing bacterial resistance, making it an effective means of addressing drug-resistant bacterial infections. MXene, as a novel two-dimensional transition metal carbon / nitride, possesses high photothermal conversion efficiency, abundant surface functional groups, and excellent mechanical properties. It can be stably composited with polymer substrates, making it an ideal medical photothermal antibacterial material. Simultaneously, Janus asymmetric structure materials possess unidirectional fluid-guiding properties, enabling differentiated functions such as a waterproof and stain-resistant outer layer and a hydrophilic and absorbent inner layer, creating a dry and stable healing microenvironment for the wound.

[0004] In existing technologies, single photothermal dressings have limited antibacterial modes and poor exudate management capabilities, while single traditional Chinese medicine antibacterial dressings have low bactericidal efficiency and cannot eliminate drug-resistant bacteria. Furthermore, most composite dressings suffer from defects such as poor interfacial bonding, insufficient mechanical properties, and low biocompatibility. There is currently no multifunctional integrated medical dressing that simultaneously possesses precise exudate management, synergistic antibacterial properties of photothermal / traditional Chinese medicine, high biocompatibility, and efficient wound healing promotion. Therefore, developing an intelligent multifunctional nanofiber dressing suitable for the treatment of clinically infected wounds is of significant practical importance. Summary of the Invention

[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a photothermal Janus nanofiber composite membrane, its preparation method, and its application.

[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A photothermal Janus nanofiber composite membrane includes a TM hydrophobic layer and a PCB hydrophilic layer. The TM hydrophobic layer and the PCB hydrophilic layer are deposited in situ through layer-by-layer electrospinning to form an asymmetric bilayer nanofiber structure with continuous interfacial bonding. The TM hydrophobic layer comprises thermoplastic polyurethane and MXene nanosheets, wherein the MXene nanosheets are uniformly dispersed in the thermoplastic polyurethane matrix, thereby endowing the composite film with near-infrared photothermal conversion function. The hydrophilic layer of the PCB includes polyvinyl alcohol, carboxymethyl chitosan and baicalin. The polyvinyl alcohol, carboxymethyl chitosan and baicalin form a cross-linked network, which stably fixes baicalin in the three-dimensional fiber network. The mass ratio of MXene nanosheets to thermoplastic polyurethane in the TM hydrophobic layer is 1:(50~200); the mass ratio of polyvinyl alcohol, carboxymethyl chitosan and baicalin in the PCB hydrophilic layer is (16~48):(2.67~8):1.

[0007] The aforementioned photothermal Janus nanofiber composite membrane possesses an asymmetric bilayer structure of a TM hydrophobic layer and a PCB hydrophilic layer. The outer layer provides hydrophobic barrier properties, while the inner layer absorbs liquid, achieving unidirectional liquid guidance and zoned protection. The near-infrared photothermal effect of MXene nanosheets in the TM hydrophobic layer and the chemical antibacterial effect of baicalin in the PCB hydrophilic layer form a synergistic mechanism: under near-infrared light excitation, MXene nanosheets generate localized high temperatures, achieving thermal inactivation of drug-resistant bacteria. Simultaneously, the photothermal heating triggers the accelerated release of baicalin. Through the dual coupling of physical photothermal killing and chemical drug inhibition, highly efficient antibacterial activity against multidrug-resistant bacteria is achieved. Furthermore, baicalin can scavenge excess ROS free radicals generated by photothermal activity, reducing photothermal side effects, and prevents secondary recurrence of biofilms by blocking the QS quorum sensing pathway.

[0008] In this PCB hydrophilic layer, polyvinyl alcohol, carboxymethyl chitosan, and baicalin form a cross-linked network through reversible dynamic intermolecular hydrogen bonds, stably fixing baicalin within the three-dimensional fiber network to achieve pH-responsive sustained release. The hydrogen bonds remain stable in the dry state, but upon contact with a water environment, some hydrogen bonds reversibly dissociate, allowing baicalin to diffuse slowly and continuously. This ensures both effective local antibacterial concentration and avoids irritating the wound with a single high concentration. The dynamic hydrogen bonds also enhance the wet strength and blend compatibility of the fibers, solving the problem of pure polyvinyl alcohol fiber membranes collapsing upon contact with water.

[0009] Preferably, the thickness ratio of the TM hydrophobic layer to the PCB hydrophilic layer is (1~5):(1~5).

[0010] Furthermore, the thickness ratio of the TM hydrophobic layer to the PCB hydrophilic layer is (1~3):(1~3).

[0011] Furthermore, the thickness ratio of the TM hydrophobic layer to the PCB hydrophilic layer is (1~2):(1~2).

[0012] Preferably, the mass ratio of MXene nanosheets to thermoplastic polyurethane in the TM hydrophobic layer is 1:100.

[0013] Preferably, the mass ratio of polyvinyl alcohol, carboxymethyl chitosan and baicalin in the hydrophilic layer of the PCB is (16~36):(2.67~6):1.

[0014] Furthermore, the mass ratio of polyvinyl alcohol, carboxymethyl chitosan, and baicalin in the hydrophilic layer of the PCB is 24:4:1.

[0015] A method for preparing a photothermal Janus nanofiber composite membrane includes the following steps: MXene nanosheets were introduced into a thermoplastic polyurethane spinning solution to uniformly disperse the MXene nanosheets, thus obtaining a TM composite spinning solution. Carboxymethyl chitosan and baicalin were added sequentially to a polyvinyl alcohol aqueous solution and mixed evenly to obtain a PCB composite spinning solution. A layer-by-layer electrospinning process was adopted. First, the TM composite spinning solution was electrospinned on the same collection substrate to form a TM hydrophobic layer in situ. Maintaining continuous contact between the TM hydrophobic layer and the collection substrate, the TM composite spinning solution was replaced with a PCB composite spinning solution, and electrospinning was performed directly on the surface of the TM hydrophobic layer. This allowed the PCB hydrophilic layer to be deposited in situ on the surface of the TM hydrophobic layer, forming an asymmetric bilayer nanofiber structure with continuous interfacial bonding. After drying, a photothermal Janus nanofiber composite membrane was obtained.

[0016] In the above steps, the layer-by-layer electrospinning process constructs a hydrophobic / hydrophilic asymmetric Janus structure, with an outer hydrophobic barrier and an inner hydrophilic liquid absorbent layer, overcoming the single-function defect of homogeneous membranes and realizing adaptive regulation of the wound microenvironment.

[0017] Preferably, the thermoplastic polyurethane spinning solution is prepared by dissolving thermoplastic polyurethane particles in a DMF / THF mixed solvent.

[0018] Furthermore, the volume ratio of DMF to THF in the DMF / THF mixed solvent is 1:1.

[0019] Furthermore, the mass-volume concentration of the thermoplastic polyurethane particles in the DMF / THF mixed solvent is 8%~12%.

[0020] Furthermore, the thermoplastic polyurethane particles have a mass-volume concentration of 10% in the DMF / THF mixed solvent.

[0021] Preferably, the specific process of introducing MXene nanosheets into the TPU spinning solution includes: premixing an aqueous dispersion of MXene nanosheets with DMF, and then ultrasonically dispersing the mixture to obtain an MXene / DMF pre-dispersion; under continuous stirring, adding the MXene / DMF pre-dispersion dropwise to the TPU spinning solution at a rate of 40-60 drops / minute; after the addition is completed, magnetically stirring at 30-40°C and 300-500 rpm for 10-14 h, followed by ultrasonic dispersion at 0°C in an ice bath for 20-40 min.

[0022] Furthermore, the mass-volume concentration of the MXene nanosheet aqueous dispersion is 0.5%~2%.

[0023] Furthermore, the dropping rate of the MXene / DMF predispersant is 50 drops / min; the stirring conditions are stirring at 35°C and 400 rpm for 12 h; and the ice bath ultrasonication time is 30 min.

[0024] Preferably, the mass-volume concentration of the polyvinyl alcohol aqueous solution is 3% to 5%.

[0025] Furthermore, the volume concentration of the polyvinyl alcohol aqueous solution is 4%.

[0026] Preferably, the mass ratio of polyvinyl alcohol to carboxymethyl chitosan in the PCB composite spinning solution is (5~7):1.

[0027] Furthermore, the mass ratio of polyvinyl alcohol to carboxymethyl chitosan in the PCB composite spinning solution is 6:1.

[0028] Preferably, in step (2), the baicalin mass-volume concentration in the PCB composite spinning solution is 0.08% to 0.25% based on the volume of the aqueous phase of the PCB spinning solution, and preferably 0.17%.

[0029] Preferably, the specific process of sequentially adding carboxymethyl chitosan and baicalin to a polyvinyl alcohol aqueous solution and mixing them evenly includes: stirring polyvinyl alcohol in water at a constant temperature of 85-95°C for 1.5-2.5 h until it is completely dissolved to form a polyvinyl alcohol aqueous solution; cooling the temperature to 55-65°C and adding carboxymethyl chitosan and stirring for 0.5-1.5 h; then adding baicalin and stirring continuously for 5-7 h; and finally ultrasonically dispersing under 0°C ice bath conditions for 20-40 min.

[0030] Furthermore, the polyvinyl alcohol is dissolved at 90°C and stirred for 2 hours; after the polyvinyl alcohol aqueous solution is cooled to 60°C, carboxymethyl chitosan is added and stirred for 1 hour, then baicalin is added and stirred for 6 hours, and the ice bath ultrasonic time is 30 minutes.

[0031] Preferably, the electrospinning process of the TM hydrophobic layer includes: an ambient temperature of 23-27°C, a relative humidity of 45%-55%RH, a spinning voltage of 16-18 kV, a spinning rate of 0.6-0.8 mL / h, the use of a 21G stainless steel flat-mouth needle, a receiving distance of 14-16 cm, a receiving roller speed of 90-110 rpm, and a spinning time of 1-3 h.

[0032] Furthermore, the ambient temperature is 25℃, the relative humidity is 50%RH, the spinning voltage is 18 kV, the spinning rate is 0.8 mL / h, the receiving distance is 15 cm, the receiving drum speed is 100 rpm, and the spinning time is 2 h.

[0033] Preferably, the electrospinning process of the PCB hydrophilic layer includes: an ambient temperature of 23-27°C, a relative humidity of 45%-55% RH, a spinning voltage of 17-19 kV, a spinning rate of 0.6-0.8 mL / h, the use of a 22G stainless steel flat-mouth needle, a receiving distance of 14-16 cm, a receiving roller speed of 90-110 rpm, and a spinning time of 1-3 h.

[0034] Furthermore, the ambient temperature is 25℃, the relative humidity is 50% RH, the spinning voltage is 17 kV, the spinning rate is 0.6 mL / h, a 22G stainless steel flat-mouth needle is used, the receiving distance is 15 cm, the receiving roller speed is 100 rpm, and the spinning time is 2 h.

[0035] Preferably, the drying conditions include: vacuum drying at 35–45°C for 20–28 hours.

[0036] Furthermore, the drying conditions are vacuum drying at 40°C for 24 hours.

[0037] Preferably, the application of a photothermal Janus nanofiber composite membrane as described above in the preparation of wound dressings.

[0038] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. This invention constructs an asymmetric bilayer structure of a TM hydrophobic layer / PCB hydrophilic layer, with an outer hydrophobic barrier and an inner hydrophilic absorbent layer, achieving unidirectional liquid guidance and zoned protection. The near-infrared photothermal effect of MXene nanosheets in the TM hydrophobic layer and the chemical antibacterial effect of baicalin in the PCB hydrophilic layer form a synergistic mechanism: under near-infrared light excitation, MXene nanosheets generate local high temperatures, raising the surface temperature of the composite film to 58.4℃, achieving thermal inactivation of drug-resistant bacteria. Simultaneously, the photothermal heating triggers accelerated release of baicalin (cumulative release rate of approximately 35% at 20℃ and close to 75% at 60℃). Through the dual coupling of physical photothermal killing and chemical drug inhibition, the antibacterial rate against multidrug-resistant Escherichia coli and Staphylococcus aureus can reach over 99.8%. Furthermore, baicalin can scavenge excess ROS free radicals generated by photothermal activity, reducing photothermal side effects, and prevent secondary recurrence of biofilms by blocking the QS quorum sensing pathway.

[0039] In this PCB hydrophilic layer, PVA, CMCS, and baicalin form a cross-linked network through reversible dynamic intermolecular hydrogen bonds, stably immobilizing baicalin within the three-dimensional fiber network to achieve pH-responsive sustained release. The hydrogen bonds remain stable in the dry state, but some dissociate reversibly upon contact with water, allowing baicalin to diffuse slowly and continuously. This ensures both effective local antibacterial concentration and avoids irritating the wound with a single high concentration. The dynamic hydrogen bonds also enhance the wet strength and compatibility of the fibers, resolving the issue of pure PVA fiber membranes collapsing upon contact with water.

[0040] 2. The photothermal Janus nanofiber composite membrane of this invention exhibits excellent mechanical properties, with a tensile strength of 3.0 MPa, an elongation at break of 330%, and exhibits no delamination or breakage under tensile, torsional, or bending conditions; its water vapor permeability is 2278 g·m³. -2 ·day -1 The hemolysis rate was only 2.3% after 24 hours, and the cell survival rate reached 89%, demonstrating excellent biocompatibility. In vivo experiments showed that the composite membrane can significantly promote collagen deposition and angiogenesis in wounds, with a wound healing rate of nearly 100% after 14 days, and can effectively repair chronic wounds infected by drug-resistant bacteria.

[0041] 3. The outer layer of the photothermal Janus nanofiber composite membrane of the present invention is a TM hydrophobic layer, with thermoplastic polyurethane (TPU) as the three-dimensional fiber network skeleton and MXene nanosheets as photothermal functional fillers. As a hydrophobic layer matrix material, TPU has excellent mechanical strength, flexibility and biostability, and can construct a continuous and dense fiber network skeleton, providing stable mechanical support for the overall fiber membrane and preventing damage and deformation of the dressing during use.

[0042] The TPU concentration in the DMF / THF mixed solvent is 8%~12% by mass, preferably 10%. This concentration range ensures that the viscosity of the spinning solution is moderate and the fiber forming is uniform and continuous. If the concentration is too low, the viscosity of the spinning solution is insufficient, and defects such as beading and fiber breakage are prone to occur during the fiber forming process. The mechanical strength of the fiber membrane will decrease significantly, and it will not be able to provide effective mechanical support and hydrophobic barrier. If the concentration is too high, the viscosity of the spinning solution will be too high, the fiber diameter will be coarsened, the porosity will be reduced, the flexibility of the fiber membrane will be poor, and it will be difficult to adapt to the dynamic deformation requirements of the wound.

[0043] The mass ratio of MXene nanosheets to TPU is 1:(50~200), preferably 1:100. When the addition ratio is less than 1:200, the content of photothermal functional phase is insufficient, the photothermal conversion efficiency of the composite film is low, and the temperature rise under near-infrared light cannot reach the effective sterilization temperature threshold (>50℃), resulting in a significant decrease in antibacterial performance. When the addition ratio is greater than 1:50, excessive MXene is prone to layer stacking and agglomeration, directly blocking the porous channels of the fibers, reducing the material's air permeability and water vapor transmission rate, and at the same time destroying the continuity of the TPU fiber network, leading to a significant decrease in the mechanical stability and flexibility of the fiber membrane.

[0044] 4. The inner layer of the photothermal Janus nanofiber composite membrane of the present invention is a PCB hydrophilic layer, with polyvinyl alcohol (PVA) as the hydrophilic fiber network framework, carboxymethyl chitosan (CMCS) as the bioactive modifying component, and baicalin (BAI) as the natural antibacterial active drug. PVA, as the main film-forming matrix of the hydrophilic layer, has good water solubility, excellent flexibility, and good biocompatibility. It can construct a loose and porous hydrophilic fiber network, which facilitates rapid absorption of wound exudate and enables stable and sustained release of baicalin active drug, while improving the fit between the dressing and the wound.

[0045] The PVA aqueous solution has a mass-volume concentration of 3% to 5%, preferably 4%. This concentration range ensures that the hydrophilic fiber network is of moderate density, combining rapid liquid absorption with structural stability. If the concentration is too low, the fiber network is sparse, the mechanical strength of the hydrophilic layer is insufficient, and it is easy to dissolve and collapse after absorbing water, failing to maintain structural integrity. If the concentration is too high, the fiber network becomes dense, the porosity is greatly reduced, the water absorption rate and swelling rate decrease significantly, and it is unable to quickly absorb wound exudate.

[0046] CMCS is a modified natural biopolymer with excellent hemostatic, anti-inflammatory, antibacterial, and cell proliferation-promoting abilities. It can compensate for the insufficient bioactivity of PVA matrix alone, effectively inhibiting wound inflammation infiltration and accelerating wound tissue regeneration and repair. The mass ratio of PVA to CMCS is (5~7):1, preferably 6:1. This ratio range allows CMCS to be uniformly embedded in the PVA network, constructing a stable polymer interpenetrating structure, while ensuring that the bioactive function of CMCS is fully exerted. If the proportion of CMCS is too low, the enhancement effect of bioactivity is not significant and cannot effectively inhibit the wound inflammatory response; if the proportion of CMCS is too high, CMCS is prone to agglomeration in the PVA matrix, resulting in poor fiber network uniformity and decreased mechanical properties.

[0047] Baicalin (BAI) is a natural flavonoid active ingredient with extremely low biotoxicity and a broad antibacterial spectrum. It can effectively inhibit the activity of multidrug-resistant Escherichia coli and Staphylococcus aureus, while also possessing excellent anti-inflammatory and antioxidant effects. It can effectively alleviate oxidative stress damage to wounds and optimize the wound healing microenvironment. The mass ratio of PVA, CMCS, and BAI is (16~48):(2.67~8):1, preferably 24:4:1. This ratio range ensures that baicalin is evenly dispersed in the fibrous network, achieving stable sustained release and long-lasting antibacterial effect. If the proportion of baicalin is too low, the local drug concentration will be insufficient, and the antibacterial effect will be greatly reduced, failing to effectively eliminate multidrug-resistant bacteria. If the proportion of baicalin is too high, baicalin is prone to crystallization in the fibrous network, blocking porous channels. At the same time, the rapid release of excessive baicalin may irritate the wound and reduce biocompatibility.

[0048] 5. In the photothermal Janus nanofiber composite membrane of the present invention, the thickness ratio of the TM hydrophobic layer to the PCB hydrophilic layer is (1~5):(1~5), preferably (1~3):(1~3), and more preferably (1~2):(1~2). This thickness ratio range ensures a balanced and coordinated function of the two layers: if the TM layer is too thick, the overall hydrophobicity of the composite membrane is too strong, the hydrophilic liquid absorption function of the inner layer is weakened, and the exudate management ability decreases; if the PCB layer is too thick, the overall hydrophilicity of the composite membrane is too strong, the hydrophobic barrier function of the outer layer is weakened, and the risk of external pollutants and bacteria intrusion increases. The TM hydrophobic layer and the PCB hydrophilic layer are formed by a continuous deposition process, which helps to improve the interfacial bonding stability between the two layers and avoids the interfacial delamination problem caused by mechanical bonding after preparing two separate membranes. Attached Figure Description

[0049] Figure 1These are scanning electron microscope (SEM) images of the two nanofiber layers and their diameter distribution in the photothermal Janus nanofiber composite membrane prepared in Example 1 of this invention. In the images, (a1) is a scanning electron microscope image of the TM hydrophobic layer magnified 11,000 times, (a2) is a scanning electron microscope image of the TM hydrophobic layer magnified 20,000 times, and (a3) ​​is a fiber diameter distribution diagram of the TM hydrophobic layer; (b1) is a scanning electron microscope image of the PCB hydrophilic layer magnified 1,100 times and its fiber diameter distribution diagram, (b2) is a scanning electron microscope image of the PCB hydrophilic layer magnified 2,000 times, and (b3) is a fiber diameter distribution diagram of the PCB hydrophilic layer. Figure 2 These are photographs of the photothermal Janus nanofiber composite membrane prepared in Example 1 of this invention in its natural state, stretched state, torsional state, and bent state. In the figure, (a) is a photograph of the composite membrane in its natural state, (b) is a photograph of the composite membrane in its stretched state, (c) is a photograph of the composite membrane in its torsional state, and (d) is a photograph of the composite membrane in its bent state. Figure 3 The figures show the Fourier transform infrared (FTIR) spectra of each layer of the photothermal Janus nanofiber composite membrane prepared in Example 1 of this invention; in the figures, (a) is the FTIR spectrum of the TM hydrophobic layer; and (b) is the FTIR spectrum of the PCB hydrophilic layer. Figure 4 The above is the X-ray photoelectron spectroscopy (XPS) spectrum of the photothermal Janus nanofiber composite membrane prepared in Example 1 of this invention; in the figure, (a) is the full spectrum XPS analysis, (b) is the C1s spectrum analysis, (c) is the O1s spectrum analysis, (d) is the N1s spectrum analysis, (e) is the S2p spectrum analysis, and (f) is the Ti2p spectrum analysis. Figure 5 This is a comparison chart of the mechanical property test results of the photothermal Janus nanofiber composite membrane prepared in Example 1 of the present invention with those of Comparative Examples 1 and 2. Figure 6 This is a comparison chart of the water vapor transmission rate test results of the TM nanofiber membrane prepared in Comparative Example 1, the PCB nanofiber membrane prepared in Comparative Example 2, and the TM / PCB Janus nanofiber membrane prepared in Example 1 of the present invention. Figure 7 This is a comparison chart of the swelling performance test results of the TM nanofiber membrane prepared in Comparative Example 1, the PCB nanofiber membrane prepared in Comparative Example 2, and the TM / PCB Janus nanofiber membrane prepared in Example 1. In the figure, (a) is a comparison of the swelling rates of the nanofiber membranes prepared in Comparative Example 1, Comparative Example 2, and Example 1; (b) is the change in the swelling rate of the TM / PCB Janus nanofiber membrane prepared in Example 1 under different pH environmental conditions. Figure 8The results are as follows: (a1) is a real-shot image showing the change of water contact angle of the TM / PCB Janus nanofiber membrane with the TM hydrophobic layer over time; (a2) is a curve showing the trend of water contact angle change of the TM / PCB Janus nanofiber membrane with the TM hydrophobic layer over time; (b1) and (b2) are real-shot images showing the change of water contact angle of the TM / PCB Janus nanofiber membrane with the PCB hydrophilic layer over time; (b2) is a curve showing the trend of water contact angle change of the TM / PCB Janus nanofiber membrane with the PCB hydrophilic layer over time. Figure 9 This is a graph showing the in vitro drug release curves of the TM / PCB Janus nanofiber membrane prepared in Example 1 of this invention under different temperature conditions; Figure 10 The figures show the photothermal performance test results of the TM / PCB Janus nanofiber membrane prepared in Example 1, the TM nanofiber membrane prepared in Comparative Example 1, and the PCB nanofiber membrane prepared in Comparative Example 2. In the figures, (a) is the infrared thermal imaging of the TM, PCB, and TM / PCB nanofiber membranes after being irradiated with near-infrared laser for different durations; (b) is the temperature rise curve of the TM, PCB, and TM / PCB nanofiber membranes under irradiation with 0.7W near-infrared laser; (c) is the temperature rise curve of the TM, PCB, and TM / PCB nanofiber membranes under irradiation with near-infrared laser at different power densities; and (d) is the photothermal stability curve of the TM / PCB nanofiber membrane under repeated on-off cycles of near-infrared laser irradiation. Figure 11 The figures show the in vitro antibacterial performance test results of the TM / PCB Janus nanofiber membrane prepared in Example 1, the TM nanofiber membrane prepared in Comparative Example 1, and the PCB nanofiber membrane prepared in Comparative Example 2. In the figure, (a) is a photograph of the in vitro antibacterial experiment of TM, PCB and TM / PCB Janus nanofiber membranes; (b) is the statistical result of the in vitro antibacterial rate of different nanofiber membrane treatment groups. Figure 12 The results of the hemolysis test on the blood compatibility of the TM / PCB Janus nanofiber membrane prepared in Example 1, the TM nanofiber membrane prepared in Comparative Example 1, and the PCB nanofiber membrane prepared in Comparative Example 2 are shown in the figure. In the figure, (a) is a real photograph of the hemolysis test of TM, PCB and TM / PCB nanofiber membranes; (b) is the statistical result of the hemolysis rate of TM, PCB and TM / PCB nanofiber membranes after 24 h of treatment. Figure 13This is a comparison chart of the cytotoxicity test results of the TM / PCB Janus nanofiber membrane prepared in Example 1 of the present invention, the TM nanofiber membrane prepared in Comparative Example 1, and the PCB nanofiber membrane prepared in Comparative Example 2. Figure 14 This figure shows the healing results of wound treatment experiments on mice using the TM / PCB Janus nanofiber membrane prepared in Example 1, the TM nanofiber membrane prepared in Comparative Example 1, and the PCB nanofiber membrane prepared in Comparative Example 2. In the figure, (a) is a photograph of the wound healing process of mice in the TM nanofiber membrane group, PCB nanofiber membrane group, TM / PCB nanofiber membrane group, and blank dressing control group within 14 days; (b) is the statistical result of the wound healing rate of the TM nanofiber membrane group, PCB nanofiber membrane group, TM / PCB nanofiber membrane group, and blank dressing control group; (c) is the curve of weight change of mice in the TM nanofiber membrane group, PCB nanofiber membrane group, TM / PCB nanofiber membrane group, and blank dressing control group within 14 days; (d) is the healing time of the TM / PCB nanofiber membrane group promoting wound healing in mice. Figure 15 The hematoxylin content of the wound skin tissue of mice in the TM nanofiber membrane group, PCB nanofiber membrane group, TM / PCB nanofiber membrane group, and blank dressing control group on day 14 of treatment in this invention is... Representative pathological slide images stained with eosin (H&E) and Masson trichrome; Figure 16 These are H&E stained pathological sections of the heart, liver, spleen, lungs, and kidneys of mice in the TM nanofiber membrane group, PCB nanofiber membrane group, TM / PCB nanofiber membrane group, and blank dressing control group on day 14 of treatment. Detailed Implementation

[0050] The present invention will be further illustrated below through specific embodiments. The following embodiments are specific implementations of the present invention, but the implementation of the present invention is not limited to the following embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and are included within the protection scope of the present invention.

[0051] Example 1 This embodiment discloses a method for preparing a photothermal Janus nanofiber composite membrane, including the following steps: Step (1): Preparation of TM layer spinning solution 1000 mg of thermoplastic polyurethane (TPU) particles were weighed and dissolved in 10 mL of a DMF / THF mixed solvent with a DMF to THF volume ratio of 1:1, so that the mass concentration of TPU in the mixed solvent was 10% (w / v). The resulting mixture was placed at a constant temperature of 50 °C and magnetically stirred for 2 h until the TPU was completely dissolved, resulting in a uniform and transparent TPU spinning solution. Take 1 mL of 1% (w / v) MXene nanosheet aqueous dispersion (MXene nanosheet mass is 10 mg), premix the MXene nanosheet aqueous dispersion with 5 mL of DMF, and disperse under ultrasonic conditions for 10 min to obtain MXene / DMF predispersant.

[0052] Subsequently, under continuous magnetic stirring, the MXene / DMF pre-dispersion was slowly added dropwise to the TPU spinning solution at a rate of 50 drops / min. After the addition was complete, the mixture was placed at a constant temperature of 35°C and continuously magnetically stirred at 400 rpm for 12 h to ensure thorough dispersion of the MXene nanosheets in the TPU spinning solution. The resulting mixture was then ultrasonically dispersed in an ice bath at 0°C for 30 min to further improve the dispersion uniformity of the MXene nanosheets in the polymer spinning solution, yielding the TM composite spinning solution.

[0053] In the TM composite spinning process, the mass ratio of MXene nanosheets to TPU is 1:100.

[0054] Step (2): Preparation of PCB hydrophilic layer spinning solution Weigh 1.2 g of solid polyvinyl alcohol (PVA) and add it to 30 mL of deionized water to achieve a PVA concentration of 4% (w / v). Stir magnetically at 90°C for 2 h until the PVA is completely dissolved, obtaining a PVA aqueous solution. Cool the PVA aqueous solution to 60°C and add 0.2 g of carboxymethyl chitosan (CMCS). Stir for 1 h, then continue magnetic stirring for another 1 h to ensure the CMCS is fully dispersed and forms a homogeneous polymer system with the PVA. Subsequently, add 0.05 g of baicalin (BAI) and continue stirring for 6 h to ensure the baicalin is fully dispersed in the PVA / CMCS system. Finally, place the resulting mixture in a 0°C ice bath and ultrasonically disperse for 30 min to improve the dispersion uniformity of each component, obtaining a homogeneous PCB composite spinning solution.

[0055] The mass ratio of PVA to CMCS is 6:1, and the mass ratio of PVA, CMCS and BAI is 24:4:1.

[0056] Step (3) Double-layer film spinning and forming Janus bilayer nanofiber composite membranes were prepared using a layer-by-layer electrospinning process. This involved electrospinning different components of spinning solutions sequentially on the same collecting substrate, allowing the subsequently spun nanofibers to be directly deposited on the surface of the previous nanofiber layer, thus forming a Janus bilayer composite nanofiber structure with a continuous interface.

[0057] Specifically, in an electrospinning environment with a temperature of 25℃ and a relative humidity of 50%RH, the TM composite spinning solution obtained in step (1) was loaded into a syringe, and electrospinning was performed using a spinning voltage of 18 kV and a spinning rate of 0.8 mL / h. A 21G stainless steel flat-mouth needle (nozzle inner diameter 0.51 mm) was used as the spinneret. The receiving device was a grounded stainless steel roller collector with a diameter of 10 cm. The roller surface was covered with conductive aluminum foil, the roller speed was set to 100 rpm, and the receiving distance between the needle and the collector was set to 15 cm. Continuous spinning was performed for 2 h to form a TM nanofiber layer on the surface of the conductive aluminum foil. After the TM nanofiber layer is spun, there is no need to peel the nanofiber membrane off the roller or conductive aluminum foil surface, nor to transfer or refix it, thus maintaining continuous contact between the TM nanofiber layer and the original substrate. Then, the spinning solution in the syringe is replaced with the PCB composite spinning solution obtained in step (2), and the second stage of electrospinning is performed directly on the same collection substrate.

[0058] Specifically, in an electrospinning environment with a temperature of 25℃ and a relative humidity of 50%RH, the PCB composite spinning solution obtained in step (2) was loaded into a syringe, and electrospinning was performed using a spinning voltage of 17 kV and a spinning rate of 0.6 mL / h. A 22G stainless steel flat-mouth needle (nozzle inner diameter of 0.41 mm) was used as the spinneret. The receiving distance between the needle and the collector was 15 cm, and the roller speed was set to 100 rpm. Continuous spinning was performed on the surface of the TM hydrophobic layer for 2 h, so that the PCB nanofibers were directly deposited on the surface of the TM nanofiber layer to form a continuously bonded PCB hydrophilic layer, thereby obtaining the crude product of the TM / PCB Janus double-layer nanofiber composite membrane. Step (4) Vacuum drying The crude product of the TM / PCB Janus bilayer nanofiber composite membrane obtained in step (3) was removed from the collection substrate and placed in a vacuum drying oven at 40°C for 24 h to remove the residual organic solvent and moisture in the nanofiber membrane, thus obtaining the photothermal Janus nanofiber composite membrane, denoted as TM / PCB Janus nanofiber membrane.

[0059] In the above embodiments, the Janus bilayer nanofiber composite membrane is formed by a layer-by-layer continuous deposition method, which is beneficial to improving the interfacial bonding stability between the TM hydrophobic layer and the PCB hydrophilic layer, and avoids the interfacial delamination problem caused by mechanically bonding two separate membranes. The prepared TM / PCB Janus nanofiber membrane has a Janus structure with different compositions and wetting properties on the upper and lower sides, that is, an asymmetric bilayer structure of TM hydrophobic layer / PCB hydrophilic layer, with the outer layer being hydrophobic and the inner layer being hydrophilic and absorbent, achieving unidirectional liquid guidance and zoned protection.

[0060] The composite membrane is composed of a TM layer (hydrophobic photothermal layer) and a PCB layer (hydrophilic layer). MXene nanosheets in the TM layer impart photothermal conversion functionality to the composite membrane, while PVA and CMCS in the PCB layer construct a hydrophilic nanofiber network. Baicalin imparts corresponding bioactive functions to the composite membrane. Simultaneously, the near-infrared photothermal effect of the MXene nanosheets in the hydrophobic TM layer and the chemical antibacterial effect of baicalin in the hydrophilic PCB layer form a synergistic mechanism: MXene nanosheets generate localized high temperatures (58.4℃) under near-infrared light excitation, achieving thermal inactivation of drug-resistant bacteria. Simultaneously, the photothermal heating triggers accelerated release of baicalin (cumulative release rate of approximately 35% at 20℃ and close to 75% at 60℃). Through the dual coupling of physical photothermal killing and chemical antibacterial action, the inhibition rate against multidrug-resistant Escherichia coli and Staphylococcus aureus exceeds 99.8%. Furthermore, baicalin can scavenge excess ROS free radicals generated by photothermal activity, reducing photothermal side effects, and prevent secondary recurrence of biofilms by blocking the QS quorum sensing pathway.

[0061] Furthermore, PVA, CMCS, and baicalin in the PCB hydrophilic layer form a cross-linked network through reversible dynamic intermolecular hydrogen bonds, stably fixing baicalin within the three-dimensional fiber network and achieving pH-responsive sustained release. The hydrogen bonds remain stable in the dry state, but some dissociate reversibly upon contact with water, allowing baicalin to diffuse slowly and continuously. This ensures both effective local antibacterial concentration and avoids irritating the wound with a single high concentration. The dynamic hydrogen bonds also enhance the wet strength and compatibility of the fibers, solving the problem of pure PVA fiber membranes collapsing upon contact with water.

[0062] Example 2 This embodiment discloses a method for preparing a photothermal Janus nanofiber composite membrane. The difference from Example 1 is that the amount of MXene nanosheets added in the TM hydrophobic layer spinning solution is reduced, while the amount of other raw materials and process conditions are the same as in Example 1.

[0063] Specifically, in preparing the TM hydrophobic spinning solution: First, the TPU spinning solution was prepared according to the method described in step (1) of Example 1; 1 mL of MXene nanosheet aqueous dispersion with a concentration of 0.5% (w / v) (MXene nanosheet mass of 5 mg) was taken and premixed with 5 mL of DMF, and ultrasonically dispersed for 10 min. Subsequently, under continuous magnetic stirring, the MXene / DMF pre-dispersion was added dropwise to the TPU spinning solution at a rate of 50 drops / min. After the addition was completed, magnetic stirring was continued at 35℃ and 400 rpm for 12 h, and then ultrasonically dispersed for 30 min under 0℃ ice bath conditions to obtain the TM composite spinning solution. The mass ratio of MXene nanosheets to TPU was 1:200.

[0064] Example 3 This embodiment discloses a method for preparing a photothermal Janus nanofiber composite membrane. The difference from Example 1 is that the amount of MXene nanosheets added in the TM hydrophobic layer spinning solution is increased, while the amount of other raw materials and process conditions are the same as in Example 1.

[0065] Specifically, in preparing the TM hydrophobic spinning solution: First, the TPU spinning solution was prepared according to the method described in step (1) of Example 1; 1 mL of MXene nanosheet aqueous dispersion with a concentration of 2% (w / v) (MXene nanosheet mass of 20 mg) was taken and premixed with 5 mL of DMF, and ultrasonically dispersed for 10 min. Subsequently, it was added dropwise at a rate of 50 drops / min to the TPU spinning solution composed of 1000 mg TPU and 10 mL of DMF / THF mixed solvent, wherein the volume ratio of DMF to THF was 1:1. After the addition was completed, the solution was magnetically stirred at 35℃ and 400 rpm for 12 h, and ultrasonically dispersed at 0℃ in an ice bath for 30 min to obtain the TM composite spinning solution. The mass ratio of MXene nanosheets to TPU was 1:50.

[0066] Example 4 This embodiment discloses a method for preparing a photothermal Janus nanofiber composite membrane. The difference from Example 1 is that the amount of baicalin (BAI) added in step (2) is changed from 0.05 g to 0.025 g, while the amount of other raw materials and process conditions are the same as in Example 1.

[0067] Specifically, in preparing the PCB composite spinning solution: 1.2 g of PVA solid was weighed and added to 30 mL of deionized water. The solution was magnetically stirred at a constant temperature of 90℃ for 2 h until completely dissolved. After cooling to 60℃, 0.2 g of CMCS was added and stirring was continued for 1 h. Then, 0.025 g of baicalin (BAI) was added and magnetically stirred for 6 h. Finally, the solution was ultrasonically dispersed at 0℃ in an ice bath for 30 min to obtain a uniform PCB composite spinning solution.

[0068] In the TM / PCB Janus nanofiber composite film obtained in this embodiment, the mass ratio of PVA, CMCS and BAI is 48:8:1, that is, the mass ratio of PVA to BAI is 48:1.

[0069] Example 5 This embodiment discloses a method for preparing a photothermal Janus nanofiber composite membrane. The difference from Example 1 is that the amount of baicalin (BAI) added in step (2) is changed from 0.05 g to 0.075 g, while the amount of other raw materials and process conditions are the same as in Example 1.

[0070] Specifically, in preparing the PCB composite spinning solution: 1.2 g of PVA solid was weighed and added to 30 mL of deionized water. The solution was magnetically stirred at a constant temperature of 90℃ for 2 h until completely dissolved. After cooling to 60℃, 0.2 g of CMCS was added and stirring was continued for 1 h. Then, 0.075 g of baicalin (BAI) was added and magnetically stirred for 6 h. Finally, the solution was ultrasonically dispersed at 0℃ in an ice bath for 30 min to obtain a uniform PCB composite spinning solution.

[0071] In the TM / PCB Janus nanofiber composite film obtained in this embodiment, the mass ratio of PVA, CMCS and BAI is 16:2.67:1, that is, the mass ratio of PVA to BAI is 16:1.

[0072] Example 6 This embodiment discloses a method for preparing photothermal Janus nanofiber composite membranes with different bilayer thickness ratios. The difference from Example 1 is that the thickness ratio of the two nanofiber membranes is controlled by adjusting the electrospinning time of the TM hydrophobic layer and the PCB hydrophilic layer. The amounts of other raw materials and process conditions are the same as in Example 1.

[0073] Specifically, during the bilayer film spinning process: in an electrospinning environment with a temperature of 25℃ and a relative humidity of 50%RH, the TM composite spinning solution was loaded into a syringe, and electrospinning was performed using an 18 kV spinning voltage and a spinning rate of 0.8 mL / h. A 21G stainless steel flat-mouth needle (nozzle inner diameter 0.51 mm) was used as the spinneret. The receiving device was a 10 cm diameter grounded stainless steel roller collector, with the roller surface covered with conductive aluminum foil. The roller speed was set to 100 rpm, and the receiving distance between the needle and the collector was set to 15 cm. Continuous spinning was performed for 2 h to form a TM nanofiber layer on the surface of the conductive aluminum foil. After the TM nanofiber layer is spun, there is no need to peel the nanofiber membrane off the roller or conductive aluminum foil surface, nor to transfer or refix it, maintaining continuous contact between the TM nanofiber layer and the original substrate. Then, the spinning solution in the syringe is replaced with the PCB composite spinning solution obtained in step (2), and the second-stage electrospinning is performed directly on the same collection substrate. The specific process includes: In an electrospinning environment with a temperature of 25℃ and a relative humidity of 50%RH, the PCB composite spinning solution obtained in step (2) was loaded into a syringe, and electrospinning was performed using a spinning voltage of 17 kV and a spinning rate of 0.6 mL / h. A 22G stainless steel flat-mouth needle (nozzle inner diameter of 0.41 mm) was used as the spinneret. The receiving distance between the needle and the collector was 15 cm, and the roller speed was set to 100 rpm. Continuous spinning was performed on the surface of the TM hydrophobic layer for 1 h, so that the PCB nanofibers were directly deposited on the surface of the TM nanofiber layer to form a continuously bonded PCB hydrophilic layer, thereby obtaining the crude product of the TM / PCB Janus double-layer nanofiber composite membrane.

[0074] In the TM / PCB Janus nanofiber composite membrane obtained in this embodiment, the thickness ratio of the TM hydrophobic layer to the PCB hydrophilic layer can be adjusted by regulating the electrospinning time of the TM hydrophobic layer and the PCB hydrophilic layer respectively. This allows for the control of the composite membrane's photothermal conversion, surface wettability, moisture transport, interfacial heat transfer, and antibacterial properties.

[0075] Example 7 This embodiment discloses a method for preparing a photothermal Janus nanofiber composite membrane. The difference from Example 1 is that the electrospinning voltage of the TM hydrophobic layer in step (3) is adjusted from 18 kV to 16 kV. The amounts of other raw materials and process conditions are the same as in Example 1.

[0076] Example 8 This embodiment discloses a method for preparing a photothermal Janus nanofiber composite membrane. The difference from Example 1 is that the spinning rate of the TM hydrophobic layer in step (3) is adjusted from 0.8 mL / h to 0.6 mL / h. The amounts of other raw materials and process conditions are the same as in Example 1.

[0077] Example 9 This embodiment discloses a method for preparing a photothermal Janus nanofiber composite membrane. The difference from Embodiment 1 is that the electrospinning voltage of the PCB hydrophilic layer in step (3) is adjusted from 17 kV to 19 kV. The amounts of other raw materials and process conditions are the same as in Embodiment 1.

[0078] Example 10 This embodiment discloses a method for preparing a photothermal Janus nanofiber composite membrane. The difference from Example 1 is that the spinning rate of the PCB hydrophilic layer in step (3) is adjusted from 0.6 mL / h to 0.8 mL / h. The amounts of other raw materials and process conditions are the same as in Example 1.

[0079] Comparative Example 1 This comparative example discloses a method for preparing a TM monolayer hydrophobic fiber membrane, including the following steps: Step (1): Preparation of TM hydrophobic layer spinning solution Weigh 1000 mg of TPU particles and dissolve them in 10 mL of DMF / THF mixed solvent with a DMF to THF volume ratio of 1:1. Stir the solution magnetically at 50 °C for 2 h to obtain a uniform and transparent TPU spinning solution. Take the prepared 1% w / v MXene nanosheet aqueous dispersion and 5 mL DMF premix, ultrasonically disperse for 10 min, and slowly add it dropwise to TPU spinning solution at a rate of 50 d / min. Continuously stir magnetically for 12 h at 35℃ and 400 rpm, and finally ultrasonically disperse in an ice bath at 0℃ for 30 min to obtain TM composite spinning solution. Step (2), TM hydrophobic layer spinning and forming In a spinning environment of 25℃ and 50%RH, the TM hydrophobic layer spinning solution was electrospun using an 18kV spinning voltage and a spinning rate of 0.8mL / h, equipped with a 21G stainless steel flat-mouth needle (nozzle inner diameter 0.51mm). The receiving device was a 10cm diameter grounded stainless steel roller collector with conductive aluminum foil on the roller surface. The roller speed was set to 100rpm, the spinning time was 4h, and the receiving distance was 15cm. After spinning, it was vacuum dried at 40℃ for 24h to obtain a TM single-layer hydrophobic fiber membrane.

[0080] Comparative Example 2 This comparative example discloses a method for preparing a single-layer hydrophilic fiber membrane for PCBs, including the following steps: Step (1): Preparation of PCB hydrophilic layer spinning solution Weigh 1.2g of PVA solid, dissolve it in 30mL of deionized water, and stir at 90℃ for 2h until completely dissolved; cool to 60℃, add 0.2g of CMCS and stir for 1h, then add 0.05g of baicalin (BAI), continue stirring for 6h, and then ultrasonically disperse in an ice bath at 0℃ for 30min to obtain a uniform PCB composite spinning solution. Step (2): Spinning the hydrophilic layer of the PCB Electrospinning of PCB hydrophilic spinning solution was carried out in a spinning environment of 25℃ and 50%RH using a spinning voltage of 17kV and a spinning rate of 0.6mL / h, equipped with a 22G stainless steel flat-mouth needle (nozzle inner diameter 0.41mm). The receiving device was a 10cm diameter grounded stainless steel roller collector with conductive aluminum foil on the roller surface. The roller speed was set to 100rpm, the spinning time was 4h, and the receiving distance was 15cm. After spinning, the solution was vacuum dried at 40℃ for 24h to obtain a single-layer hydrophilic fiber membrane for PCB.

[0081] Comparative Example 3 This comparative example discloses a method for preparing a TPU fiber membrane, including the following steps: Weigh 1000 mg of TPU powder and dissolve it in 10 mL of DMF / THF mixed solvent with a volume ratio of DMF to THF of 1:1. Stir the solution magnetically at 50 °C for 2 h to obtain a uniform and transparent TPU spinning solution. In a spinning environment of 25℃ and 50%RH, the TPU spinning solution was electrospun using an 18kV spinning voltage and a spinning rate of 0.8mL / h, equipped with a 21G stainless steel flat-mouth needle (nozzle inner diameter 0.51mm). The receiving device was a 10cm diameter grounded stainless steel roller collector with conductive aluminum foil on the surface. The roller speed was set to 100rpm, the spinning time was 4h, and the receiving distance was 15cm. After spinning, the TPU fiber film was obtained by vacuum drying at 40℃ for 24h.

[0082] In the above examples and comparative examples, MXene nanosheets were prepared from Ti3AlC2MAX phase powder (from Xinxi Technology Co., Ltd.) using a mild lithium fluoride / hydrochloric acid etching reaction (Minimally Intensive Layer Delamination method). The MXene nanosheets prepared after etching had a size of 2~20 micrometers, an electrical conductivity of 1000±500 S / cm, good water dispersibility, and contained -OH, -F, =O, and -Cl groups on the surface. The specific preparation process of MXene nanosheets using the lithium fluoride / hydrochloric acid etching reaction method includes the following steps: S1. Measure 15.5 mL of concentrated hydrochloric acid (HCl, analytical grade) with a mass fraction of 37%, and add deionized water to make up to 20 mL to prepare a 9 mol / L HCl solution. Accurately weigh 1.6 g of lithium fluoride (LiF, analytical grade, purity ≥99%), add it to the above 20 mL of 9 mol / L HCl solution, place it in a polytetrafluoroethylene (PTFE) reaction flask, and stir at 300 r / min for 10 min on a magnetic stirrer until the LiF is completely dissolved to obtain a clear etching agent.

[0083] S2. Place the reaction flask containing the etching agent in a 35°C constant temperature water bath or oil bath. Under continuous magnetic stirring (300~500 r / min), add 1.0 g of Ti3AlC2MAX phase powder (from Xinxi Technology Co., Ltd.) in 3~5 portions. The addition process should be completed within 10 min to avoid violent exothermic reactions in some areas. After the addition is complete, maintain a constant temperature of 35°C and a sealed environment (with an exhaust vent) for continuous stirring and reaction for 24 h to selectively etch away the Al atomic layer. Hydrogen gas (H2) is generated during the reaction, so it must be carried out in a fume hood.

[0084] S3. After the etching reaction is complete, add 30 mL of deionized water to the reaction flask to dilute the suspension, transfer it to a 50 mL centrifuge tube, and centrifuge at 3500 r / min for 5 min. Discard the supernatant acidic clear liquid. Subsequently, add 30 mL of deionized water each time to redisperse the precipitate, centrifuge at 3500 r / min for 5 min, and repeat the washing and centrifugation operation 6-8 times until the pH value of the supernatant is ≥6, so as to completely remove residual Li. + Cl - F - And byproducts such as AlF3. After the final centrifugation, retain the dark precipitate at the bottom of the tube.

[0085] S4. Add 20 mL of deionized water to the above precipitate, purge with inert gas (argon or nitrogen) for 10 min to remove oxygen, seal, and manually shake vigorously for 5 min (or sonicate in an ice bath at 150 W for 10 min) to allow Li to precipitate. + The intercalated multilayer MXene was further exfoliated into few-layer / monolayer nanosheets. The nanosheets were then centrifuged at 3500 r / min for 60 min, and the upper dark green, clear dispersion was carefully aspirated; this was the aqueous dispersion of few-layer / monolayer MXene nanosheets. The resulting dispersion was sealed and protected from light, and stored at 4°C for later use.

[0086] In the above embodiments and comparative examples, the TPU particles were BASF polyurethane TPU, model Elastollan. 1180A10 was purchased from Shanghai Aichun Biotechnology Co., Ltd.; Carboxymethyl chitosan (CMCS) was purchased from Shanghai Maclean Biochemical Technology Co., Ltd., CAS: 83512-85-0, item number: C804727; Baicalin was purchased from Shanghai Maclean Biochemical Technology Co., Ltd., CAS: 21967-41-9, item number: B802696.

[0087] Experimental data characterization and performance testing Figure 1 The images show the scanning electron microscope (SEM) morphology and fiber diameter distribution of the two nanofiber layers in the photothermal Janus nanofiber composite membrane prepared in Example 1. (a1), (a2), and (a3) ​​are SEM images and fiber diameter distributions of the TM hydrophobic layer magnified at 11,000x and 20,000x, respectively. (b1), (b2), and (b3) are SEM images and fiber diameter distributions of the PCB hydrophilic layer magnified at 1,100x and 2,000x, respectively.

[0088] The microstructure characterization results in (a1) and (a2) show that the fibrous membrane of the TM hydrophobic layer has uniform and continuous fibers with a smooth surface, no beading or broken fiber defects, and an average fiber diameter of 219±21 nm. The MXene nanosheets are uniformly dispersed in the TPU matrix without obvious agglomeration. This is because the MXene nanosheets used in this invention have a lateral size of 2~20 μm, a sheet thickness of 1~5 nm, and an electrical conductivity of 1000±500 S / cm. The few-layer MXene nanosheets of this size can be uniformly interspersed in the gaps between TPU fibers, building a continuous photothermal network without blocking the porous channels. This effectively avoids the problems of large-size sheet agglomeration and stacking and insufficient photothermal efficiency of small-size sheets. At the same time, it can refine the micropore size of the fibers and further improve the structural stability of the fiber membrane.

[0089] The microstructure characterization results in (b1) and (b2) show that the PCB hydrophilic fiber membrane is densely interwoven with interconnected pores, and the average fiber diameter is 692±43 nm, which can be used to construct a three-dimensional porous biomimetic scaffold structure. This double-layer fiber membrane has excellent flexibility, and its structure remains intact without delamination or breakage under tension, torsion, and bending, which can adapt to the dynamic deformation of wound surfaces and the need for curvature adhesion.

[0090] from Figure 1 It can be seen that the composite membrane exhibits an asymmetric bilayer structure. The TM hydrophobic layer and the PCB hydrophilic layer are deposited in situ through electrospinning to form an asymmetric bilayer nanofiber structure with continuous interfacial bonding.

[0091] Figure 2These are photographs of the photothermal Janus nanofiber composite membrane prepared in Example 1 in its natural, stretched, torsional, and bent states. Figure 2 It is evident that the dressing, under natural conditions, is flat and flexible, stretches uniformly without breakage when stretched, maintains its structural integrity without delamination when twisted, and closely conforms to curved surfaces when bent, demonstrating its excellent mechanical flexibility and structural stability. This structural design ensures the mechanical stability of the fibrous membrane, enabling it to adapt to the dynamic deformation requirements of the wound, while also achieving rapid absorption and barrier of exudate, facilitating gas exchange and the release of functional components, and providing an excellent biomimetic scaffold for cell adhesion and proliferation.

[0092] Figure 3 The Fourier transform infrared (FTIR) spectra of each layer of the photothermal Janus nanofiber composite membrane prepared in Example 1 are shown; where (a) is the FTIR spectrum of the TM hydrophobic layer and (b) is the FTIR spectrum of the PCB hydrophilic layer.

[0093] like Figure 3 As shown in (a), a single TPU fiber membrane (Comparative Example 3) at 2860 cm⁻¹ -1 The peak of CH stretching vibration is observed at 1720 cm⁻¹. -1 The peak at 1230 cm⁻¹ is the C=O stretching vibration peak. -1 The peak at 3400 cm⁻¹ represents the COC stretching vibration, a characteristic absorption of TPU. In the TPU / MXene composite film, all of the above characteristic peaks are present, but their positions are slightly shifted, and the peak position at 3400 cm⁻¹ is also different. -1 The enhanced intensity of the OH stretching vibration peak at 570 cm⁻¹ indicates that the -OH groups on the surface of the MXene nanosheets have formed hydrogen bonds with the C=O groups in the TPU molecular chain; simultaneously, the peak intensity at 570 cm⁻¹... -1 The appearance of Ti-O-Ti lattice vibration peaks confirms that MXene nanosheets have been successfully loaded into the hydrophobic layer.

[0094] like Figure 3 As shown in (b), the pure PVA membrane mainly exhibits characteristic absorption peaks such as hydroxyl (–OH), C–H, and C–O, with the peak located at approximately 3300 cm⁻¹. -1 The broad peaks nearby are attributed to the stretching vibrations of hydroxyl groups in the PVA molecular chain. After the introduction of CMCS, due to its abundant hydroxyl, carboxyl, and amino active groups, it can undergo intermolecular hydrogen bonding with the hydroxyl groups in the PVA molecular chain, resulting in a more stable physical cross-linked structure between PVA segments. In the hydrophilic layer of the PCB, the FTIR spectrum shows that the characteristic peaks of PVA, CMCS, and BAI are all retained, but the hydroxyl region and C–O and C=O related absorption peaks show significant changes, indicating that the three components are not simply mixed. Specifically, PVA and CMCS interact through (PVA… OH…O CMCS; PVA OH…OH CMCS forms numerous hydrogen bonds, allowing the CMCS molecular chains to embed into the PVA network and construct a stable polymer interpenetrating structure. Simultaneously, the baicalin molecule contains multiple phenolic hydroxyl groups (–OH) and carbonyl groups (C=O) in the flavonoid backbone; these active groups can further participate in network construction. The carbonyl group in BAI can act as a hydrogen bond acceptor, forming (BAI) bonds with the hydroxyl or amino groups in PVA / CMCS. C=O…H O PVA; BAI C=O…H N The phenolic hydroxyl group in BAI can act as a hydrogen bond donor, interacting with the carboxyl and hydroxyl groups in CMCS (BAI). OH…O The PVA / CMCS structure allows BAI molecules to be stably embedded within the PVA / CMCS three-dimensional network, achieving network-based fixation of active molecules. Therefore, in the hydrophilic layer of the PCB, PVA, CMCS, and baicalin form a cross-linked network through reversible dynamic intermolecular hydrogen bonds, stably fixing baicalin within the fiber three-dimensional network and achieving pH-responsive sustained release. Specifically, after the electrospun membrane dries, the hydrogen bonds between the three components remain stable, stabilizing baicalin within the fiber three-dimensional network, preventing detachment and rapid release. When the electrospun membrane comes into contact with wound exudate (aqueous environment), some hydrogen bonds reversibly dissociate, the fibers absorb water and swell, and baicalin slowly and continuously diffuses, achieving pH-responsive sustained release. This ensures both effective local antibacterial concentration and avoids a single high-concentration stimulation of the wound. Dynamic intermolecular hydrogen bonds can also improve the mechanical and structural stability of fibers. CMCS and PVA rely on mutual hydrogen bonds to improve the compatibility of blending, solving the problems of low wet strength and excessive dissolution and collapse of pure PVA fiber membranes when exposed to water. Baicalin, as a small molecule hydrogen bond crosslinking point, slightly physically reinforces the nanofiber network, allowing the hydrophilic layer to maintain its integrity after absorbing water, without becoming soggy, flake, or sticking to the wound.

[0095] Figure 4 The X-ray photoelectron spectroscopy (XPS) spectrum of the photothermal Janus nanofiber composite membrane prepared in Example 1 is shown. Among them, (a) is the full-spectrum XPS analysis; (b) is the C1s spectrum analysis; (c) is the O1s spectrum analysis; (d) is the N1s spectrum analysis; (e) is the S2p spectrum analysis; and (f) is the Ti2p spectrum analysis.

[0096] Figure 4In (a), XPS further demonstrates the interfacial bonding relationship between PVA / CMCS / BAI. Full-spectrum XPS analysis shows that the PCB hydrophilic layer mainly contains elements such as C, O, and N. The C1s, O1s, and N1s signals are contributed by PVA, CMCS, and BAI, respectively. In addition, the presence of N element proves that the amino structure of CMCS was successfully introduced into the hydrophilic layer and participated in the formation of the composite network.

[0097] in, Figure 4 (b) is the C1s spectrum, which can be decomposed into: C–C / C–H (approximately 284.6 eV), C–O (approximately 285.8 eV), CN (approximately 286.2 eV), and C=O (approximately 288.5 eV). The C–O peak mainly originates from the hydroxyl groups in PVA, the sugar chain structure of CMCS, and the phenolic hydroxyl groups in BAI; the C=O peak corresponds to the carboxyl groups in CMCS and the carbonyl groups in the flavonoid structure of BAI. Compared to the single component, the chemical environment of C–O and C=O in PBC changes, indicating that these oxygen-containing functional groups participate in intermolecular interactions. In particular, the formation of hydrogen bonds between the carbonyl groups of BAI and the hydroxyl and amino groups in PVA / CMCS leads to a redistribution of electron cloud density, causing a shift in the C=O binding energy, proving that BAI is not simply adsorbed but participates in the construction of a hydrophilic network. The C–N peak mainly originates from the amino structure in the carboxymethyl chitosan molecular chain. Since neither PVA nor baicalin molecules contain nitrogen, the appearance of the C–N signal proves that carboxymethyl chitosan has been successfully introduced into the PVA / BAI composite network.

[0098] Figure 4 Image (c) shows the O1s high-resolution spectrum, mainly consisting of CO / Ti-O (approximately 531-532 eV) and C=O (approximately 533 eV). The CO component constitutes the majority, originating from hydroxyl groups in PVA, hydroxyl groups and ether bonds in CMCS, and phenolic hydroxyl groups in BAI. The high proportion of oxygen-containing structures indicates that the PBC layer possesses abundant polar interaction sites, providing a basis for hydrogen bonding crosslinking. Simultaneously, the presence of the C=O peak further confirms the retention of carbonyl structures in BAI and CMCS, participating in interactions between polymer chains.

[0099] Figure 4 (d) is the N1s spectrum, in which: NC=O, -NH2, -NH3 appear. + Characteristic peaks originate from the amino structure in CMCS. Specifically: NC=O corresponds to the residual acetamino group in CMCS; -NH2 / -NH3 + This indicates that the CMCS amino group possesses strong activity. The CMCS amino group not only enhances its own interchain interactions but also forms hydrogen bonds with the BAI carbonyl group (-NH2…O=C-BAI), thereby further improving the binding stability of BAI in the network.

[0100] Figure 4 (e) is the high-resolution spectrum of S2p: After peak fitting, the S2p orbital shows a distinct characteristic peak at 168 eV, which is attributed to the sulfonate terminal functional group; this confirms that the surface of MXene nanosheets is modified with sulfur terminal groups, and the sulfur-containing functional groups can connect MXene nanosheets, carboxymethyl chitosan and baicalin through hydrogen bonds and electrostatic interactions, thus stabilizing the interface structure of the composite membrane.

[0101] Figure 4 (f) shows the high-resolution Ti2p spectrum: multiple characteristic sub-peaks were obtained after fitting the Ti2p signal; the spins at 458.4 eV and 464.1 eV are shown. The orbital bimodal attributed to Ti O chemical bonds were established, demonstrating that MXene nanosheets can form Ti with oxygen-containing groups in carboxymethyl chitosan, PVA, and baicalin. O C-interface coordination bonds; low binding energy region sub-peaks correspond to MXene framework Ti C-bonds and low-valence titanium defects and sites can endow the composite membrane with reactive oxygen species scavenging properties, and synergistically achieve anti-inflammatory and antioxidant effects on wounds with baicalin.

[0102] In conclusion, Figure 3 and Figure 4 Chemical structural characterization results confirmed that stable hydrogen bonds were formed between MXene nanosheets and the TPU matrix, and between baicalin (BAI) and the PVA / CMCS matrix. The components were successfully compounded and the structure was stable, without any chemical reaction or deterioration. At the same time, the characteristic signals of MXene nanosheets and baicalin were completely preserved, providing a reliable chemical structural basis for the multifunctional synergistic effect.

[0103] Figure 5 The graph shows a comparison of the mechanical property test results of the photothermal Janus nanofiber composite membrane prepared in Example 1 with those of Comparative Examples 1 and 2. The mechanical property tests were conducted according to GB / T 3923.1 standard. Figure 5 As can be seen, the tensile strength of the TM hydrophobic layer prepared in Comparative Example 1 can reach 3.9 MPa, and the elongation at break is 380%, demonstrating excellent mechanical support and resistance to deformation. The tensile strength of the PCB hydrophilic layer prepared in Comparative Example 2 is 3.5 MPa, and the elongation at break is 360%. The TM / PCB Janus nanofiber membrane, which combines the TM hydrophobic layer and the PCB hydrophilic layer, has a tensile strength of 3.0 MPa and an elongation at break of 330%. There is no interfacial delamination during the stretching process, and the two layers are firmly bonded. The mechanical properties fully meet the standards for medical dressings and can withstand the deformation caused by wound contraction and limb movement, effectively avoiding the problem of secondary infection of the wound caused by dressing rupture.

[0104] The reason why the elongation at break of the TM / PCB Janus nanofiber membrane decreased compared with Comparative Examples 1 and 2 is that there are interfacial stress concentration points after the double-layer composite, and the two sets of hydrogen bond network structures of the TM hydrophobic layer and the PCB hydrophilic layer are superimposed, resulting in deformation mismatch and premature cracking during stretching. However, even though the elongation at break of the TM / PCB Janus nanofiber membrane decreased to 330%, the membrane still has high ductility, which is sufficient to adapt to the dynamic deformation of skin wounds and meet the requirements for use as medical dressings.

[0105] Figure 6 The results of water vapor transmission rate tests on the TM nanofiber membrane, PCB nanofiber membrane, and the TM / PCB Janus nanofiber membrane prepared in Example 1, along with air permeability and swelling performance tests, show that the water vapor transmission rate of the TM / PCB Janus nanofiber membrane can reach 2278 g·m³. -2 / day, with good breathability and gas exchange capacity, can prevent the wound from becoming damp and inflamed; Figure 7 The swelling performance test results of different nanofiber membranes are shown below; (a) is a comparison of the swelling rates of the nanofiber membranes prepared in Comparative Example 1, Comparative Example 2, and Example 1; (b) is the change in the swelling rate of the TM / PCB Janus nanofiber membrane prepared in Example 1 under different pH conditions. The swelling rate of the hydrophilic layer reached 288% after 24 h, while the swelling rate of the hydrophobic layer was less than 50%, and the swelling rate of the composite membrane was 164%, achieving synergistic moisture management of the two layers. Therefore, the TM / PCB Janus nanofiber membrane has significant pH response characteristics, and its swelling rate can be increased by 30% under alkaline infected wound conditions. It can adapt to the increased exudate in infected wounds and precisely regulate the moist microenvironment of the wound.

[0106] Figure 8 The water contact angle test results for the TM / PCB Janus nanofiber membrane prepared in Example 1 are shown below. (a1) and (a2) are actual photographs and trend curves of the water contact angle of the TM / PCB Janus nanofiber membrane with the hydrophobic TM layer changing over time, respectively. (b1) and (b2) are actual photographs and trend curves of the water contact angle of the TM / PCB Janus nanofiber membrane with the hydrophilic PCB layer changing over time, respectively. The wettability test was performed according to GB / T 30693 standard.

[0107] from Figure 8As can be seen, the initial contact angle of the TM hydrophobic layer in the TM / PCB Janus nanofiber membrane is 126.2°, and it remains above 125° after 150 s, demonstrating long-lasting hydrophobic and antifouling properties and the ability to block external pollution. The contact angle of the PCB hydrophilic layer in the TM / PCB Janus nanofiber membrane rapidly decreases from 53.4° to 0° within 7 s, which can quickly adsorb wound exudate and successfully realize the core functions of the Janus structure: one-way fluid guidance and zoned protection.

[0108] Figure 9 The in vitro drug release curves of the TM / PCB Janus nanofiber membrane prepared in Example 1 under different temperature conditions.

[0109] Figure 10 The photothermal performance test results of the TM / PCB Janus nanofiber membrane prepared in Example 1, and the nanofiber membranes prepared in Comparative Examples 1 and 2 are as follows: (a) Infrared thermal images of TM, PCB and TM / PCB nanofiber membranes after near-infrared laser irradiation for different durations; (b) Temperature rise curves of TM, PCB and TM / PCB nanofiber membranes under 0.7W near-infrared laser irradiation; (c) Temperature rise curves of TM, PCB and TM / PCB nanofiber membranes under near-infrared laser irradiation at different power densities; (d) Photothermal stability curve of TM / PCB nanofiber membrane under repeated on-off cycles of near-infrared laser irradiation.

[0110] from Figure 9 and Figure 10 It can be seen that the TM / PCB Janus nanofiber membrane possesses excellent controllable photothermal properties and temperature-responsive drug release characteristics. Figure 9 The curves show the cumulative release rate of baicalin from TM / PCB fiber membranes at 20℃, 40℃, and 60℃ as a function of release time. All three curves show that the cumulative release rate of the drug increases continuously with time, and the release rate and the final cumulative release amount increase synchronously with the increase of temperature. At room temperature of 20℃, the drug release is slow, with a cumulative release rate of only about 35%. At physiological temperature of 40℃, the release rate is significantly increased, with a cumulative release rate of 50%. At 60℃, which corresponds to a near-infrared photothermal heating environment, the polymer matrix chain segments are heated and the diffusion resistance is reduced, with a cumulative release rate close to 75%. This result confirms that near-infrared photothermal heating can accelerate the release of baicalin from the hydrophilic layer to increase the local drug concentration in the wound, forming a synergistic antibacterial effect with the photothermal destruction of bacterial cell membrane permeability. At the same time, the room temperature slow-release characteristic can achieve long-term antibacterial effect in the wound under no-light conditions.

[0111] In dressing systems, TM / PCB Janus nanofiber membranes exhibit excellent photothermal therapy (PTT) performance, such as... Figure 10The thermal images (a) and (b) and the heating curves are shown. Both TM / PCB Janus dressings exhibited significant heating effects under 0.7 W near-infrared laser irradiation. The surface temperature gradients of both the TM and TM / PCB dressings changed significantly, with peak values ​​reaching 62.8℃ and 58.4℃ respectively, verifying the excellent performance and controllability of photothermal heating. Figure 10 As shown in (c), with the increase of laser power density, the heating efficiency of the dressing increases synchronously, indicating that its photothermal performance can be flexibly controlled through power density; while Figure 10 In (d), the TM / PCB Janus dressing exhibited stable temperature cycling fluctuations in the laser “on-off” cycle experiment, demonstrating excellent photothermal stability; ultimately, the high efficiency of the TM / PCB Janus nanofiber membrane in photothermal therapy was fully demonstrated.

[0112] The reason lies in the fact that the Janus system can achieve a highly efficient synergistic effect of photothermal antibacterial and chemical antibacterial properties. MXene nanosheets in the hydrophobic layer serve as the core photothermal functional filler, with a resistivity of 0.5~2.0 Ω·cm. They possess low resistance, high conductivity, ultra-high near-infrared photothermal conversion efficiency, and good biocompatibility. Uniformly dispersed in the TPU matrix, they endow the material with controllable and stable photothermal response bactericidal properties. Under near-infrared light irradiation, they efficiently convert light energy into heat energy through localized surface plasmon resonance. The generated local high temperature can not only directly thermally ablate bacteria but also accelerate the release of baicalin in the hydrophilic layer through thermal activation, achieving photothermal-triggered drug release. The two work synergistically to achieve a dual killing effect of "thermal damage + drug damage". Based on the above photothermal performance test results, the TM / PCB Janus nanofiber membrane, as a dressing, exhibits excellent concentration- and power-dependent photothermal performance, good photothermal stability, and can further accelerate the release of baicalin through photothermal activation, successfully achieving a synergistic effect of photothermal antibacterial and chemical antibacterial effects, demonstrating outstanding potential for treating infected wounds.

[0113] Figure 11 The results of in vitro antibacterial performance tests of nanofiber membranes in Example 1 and Comparative Examples 1 and 2 are shown; (a) is a photograph of the in vitro antibacterial experiment of TM, PCB and TM / PCB Janus nanofiber membranes; (b) is the statistical results of the in vitro antibacterial rate of different nanofiber membrane treatment groups.

[0114] In vitro antibacterial experiments were conducted using colony counting to detect multidrug-resistant Escherichia coli (MDR). E. coli Multidrug-resistant Staphylococcus aureus (MDR) S.aureus The activity was evaluated. The in vitro antibacterial performance test was performed according to GB / T 20944.3-2008 "Evaluation of antibacterial properties of textiles - Part 3: Shaking method".

[0115] The specific testing included the following steps: Staphylococcus aureus (Gram-positive) and Escherichia coli (Gram-negative) were selected as test strains. The strains were inoculated into LB liquid medium and cultured at 37°C with shaking at 180 r / min until the logarithmic growth phase. The bacterial suspension concentration was adjusted to 1×10⁻⁶ using sterile PBS buffer. 6 (CFU / mL).

[0116] The fiber membrane samples prepared in Example 1, Comparative Example 1, and Comparative Example 2 with a size of 1 cm × 1 cm were cut, sterilized by ultraviolet light, and placed in sterile centrifuge tubes. 5 mL of the above bacterial suspension was added, and the samples were set as TM-NIR group, TM+NIR group, PCB, TM / PCB-NIR group, and TM / PCB+NIR group, respectively. A blank control group (i.e., blank group) was also set up.

[0117] The TM+NIR group and the TM / PCB+NIR group were irradiated with an 808nm near-infrared laser with a power density of 1.0W / cm² and an irradiation time of 5min. The TM-NIR and TM / PCB-NIR group samples were placed under the same environmental conditions without the near-infrared light source being turned on. After the light exposure, each group of samples was incubated in a 37℃ incubator for 24 hours. After incubation, sterile PBS buffer was added and the bacteria attached to the surface of the dressing were thoroughly vortexed to remove them. The bacterial solution was diluted using a 10-fold serial dilution method, and 0.1 mL of the diluted bacterial solution was evenly spread on an agar plate. The plates were incubated upside down at 37℃ for 24 hours. The number of colonies on the plates was counted, and the inhibition rate was calculated.

[0118] Under conditions without near-infrared light irradiation, the TM hydrophobic layer of Comparative Example 1 showed no significant antibacterial effect, with an antibacterial rate of less than 10%. The PCB hydrophilic layer of Comparative Example 2 relied on the bio-antibacterial effects of baicalin and carboxymethyl chitosan, achieving antibacterial rates of 53.2% and 41.8% against the two strains, respectively. The TM / PCB Janus nanofiber membrane of Example 1 showed a slightly improved antibacterial rate, but the antibacterial effect was limited.

[0119] After 5 minutes of irradiation with a 0.7 W / cm near-infrared laser, the photothermal synergistic mechanism was fully activated. The TM layer achieved efficient sterilization through photothermal high temperature, with antibacterial rates of 88.7% and 92.2%, respectively. Meanwhile, the TM / PCB Janus nanofiber membrane exhibited the best synergistic antibacterial effect, with antibacterial rates of 99.8% and 99.9% against two multidrug-resistant bacteria, respectively. It can almost completely eliminate drug-resistant bacteria from wounds, thus thoroughly solving the technical shortcomings of single antibacterial modes, such as incomplete sterilization and easy residue of drug-resistant bacteria.

[0120] The aforementioned data from in vitro drug release tests, photothermal performance tests, and in vitro antibacterial performance tests collectively demonstrate that the near-infrared photothermal effect of MXene nanosheets in the TM hydrophobic layer and the chemical antibacterial effect of baicalin in the PCB hydrophilic layer form a cross-layer synergistic mechanism. Specifically, the near-infrared high temperature of MXene nanosheets can instantly physically ablate the biofilm of drug-resistant bacteria, but after the loss of light stimulation, residual live bacteria will rebuild the biofilm through the QS quorum sensing system; baicalin has a specific antibacterial quorum sensing pathway, blocking the secretion of EPS mechanism at the gene level, preventing secondary recurrence of biofilm, and forming a progressive synergistic bactericidal effect of photothermal barrier disruption + drug blocking. At the same time, baicalin can scavenge excess ROS free radicals generated in photothermal therapy, counteracting the oxidative stress damage to granulation tissue caused by local high temperature and reducing photothermal side effects. In addition, the photothermal heating of MXene nanosheets can trigger the accelerated release of baicalin, achieving photothermally triggered concentration- and power-dependent drug release. The temperature-responsive drug release characteristic allows the composite membrane to significantly increase the local drug concentration on the wound under near-infrared light irradiation, forming a synergistic antibacterial effect with the photothermal disruption of bacterial cell membrane permeability. At the same time, the room temperature slow-release characteristic enables long-term antibacterial action on the wound under no-light conditions.

[0121] Figure 12 The results of hemolysis tests on the nanofiber membranes prepared in Example 1, Comparative Examples 1 and 2 are shown below: (a) Real photos of hemolysis tests on TM, PCB and TM / PCB nanofiber membranes; (b) Statistical results of hemolysis rates after 24 hours of treatment with different nanofiber membranes. Biocompatibility testing was conducted according to the general national standards for medical materials (GB / T 16886.4-2022, YY / T1651.1-2019). The hemolysis test results showed that the hemolysis rate of the TM / PCB Janus nanofiber membrane after 24 hours was only 2.3% ± 0.25%, far below the 5% medical safety threshold, indicating excellent blood compatibility and no risk of red blood cell rupture or aggravated wound inflammation.

[0122] Figure 13 The results of cytotoxicity assays for TM, PCB, and TM / PCB Janus nanofiber membranes were determined using the CCK-8 assay. The control group consisted of normal cells as a blank control group.

[0123] The nanofiber membranes prepared in Example 1, Comparative Example 1, and Comparative Example 2 were sterilized and then extracted with Dulbecco's Modified Eagle-Medium (DMEM) medium at 37°C for 24 h; L929 cells were inoculated at 1×10⁻⁶... 4Cells were seeded per well in 96-well plates for adherent culture, followed by incubation with material extract for 24 hours. CCK-8 chromogenic reagent was then added for further incubation, and cell viability was calculated by reading the absorbance at 450 nm using a microplate reader. Six parallel samples were set up for each group. The above in vitro cytotoxicity test was conducted according to the national standard GB / T16886.5-2022 "Biological Evaluation of Medical Devices Part 5: In Vitro Cytotoxicity Tests". The CCK-8 cytotoxicity test results showed that the cell viability of each experimental group after co-incubation with L929 fibroblasts was higher than 80%, with the TM / PCB Janus nanofiber membrane achieving a cell viability of 89% ± 3.2%, proving that the composite material did not have significant in vitro cytotoxicity. Simultaneously, the porous structure and active components of the fiber membrane can promote cell adhesion, proliferation, and migration, providing an excellent biological microenvironment for the growth of granulation tissue and re-epithelialization in wounds.

[0124] Figure 14 The following are the healing results of in vivo wound treatment experiments using TM / PCB Janus nanofiber membranes prepared in Example 1, TM nanofiber membranes prepared in Comparative Example 1, and PCB nanofiber membranes prepared in Comparative Example 2 on mice: (a) Photographs of the wound healing process in mice within 14 days after treatment with TM, PCB, and TM / PCB Janus nanofiber membranes, where the control group is the blank dressing control group (i.e., no dressing was used to treat the mouse wounds); (b) Statistical results of wound healing rate in different nanofiber membrane treatment groups; (c) Curves of body weight change in mice in each treatment group within 14 days; (d) Healing time graph of wound healing in mice promoted by TM / PCB Janus nanofiber membrane.

[0125] Further investigation was conducted using an ICR mouse model of full-thickness skin infection with drug-resistant bacteria to explore the in vivo wound repair efficacy of the Janus nanofiber membrane prepared in Example 1. All animal experiments were approved by the Experimental Animal Ethics Committee of Soochow University (Approval No.: 2025009A155).

[0126] The animal modeling process includes the following steps: ICR mice that have been acclimatized for one week (5 weeks) are anesthetized, and a circular full-thickness skin wound with a diameter of 15 mm is prepared on the back. The wound is then inoculated with a drug-resistant bacterial solution (drug-resistant Staphylococcus aureus, concentration 1×10⁻⁶). 7 Infected wounds were constructed using CFU / mL nanofiber membranes. Subsequently, each group of nanofiber membranes was cut into 20mm diameter discs to completely cover the wound surface. The dressings were changed once a day to construct the TM nanofiber membrane group, PCB nanofiber membrane group, and TM / PCB nanofiber membrane group, which were compared with the blank dressing control group.

[0127] In vivo experimental results showed that the TM / PCB Janus nanofiber membrane used in the TM / PCB nanofiber membrane group could rapidly inhibit wound redness and suppuration, reduce exudation, and regulate the wound repair microenvironment. The wound healing rate was close to 100% 14 days after surgery, and the healing effect was significantly better than the blank control group, the TM nanofiber membrane group alone, and the PCB nanofiber membrane group alone. Throughout the observation period, the mice's weight increased steadily and their survival status was good. The dressing did not have obvious in vivo toxic side effects.

[0128] Figure 15 Hematoxylin and oxychloride were extracted from the wound skin tissues of mice in the TM nanofiber membrane group, PCB nanofiber membrane group, TM / PCB nanofiber membrane group, and blank dressing control group on day 14 of treatment. Representative pathological slide images stained with eosin (H&E) and Masson's trichrome. Figure 16 The images show H&E-stained pathological sections of the heart, liver, spleen, lung, and kidney of mice in the TM nanofiber membrane group, PCB nanofiber membrane group, TM / PCB nanofiber membrane group, and blank dressing control group on day 14 of treatment. Figure 15 Histopathological staining results confirmed that the TM / PCB group had complete epithelialization of the wound, high collagen fiber deposition, and regular and orderly arrangement, which can effectively promote collagen remodeling and angiogenesis, and accelerate wound repair. Figure 16 No abnormal lesions such as inflammatory infiltration and cell necrosis were observed in the pathological staining of major organs of mice and hamsters, confirming that the TM / PCB Janus nanofiber membrane has excellent in vivo biocompatibility, no potential toxic side effects, and can be safely used for long-term treatment of infected wounds.

[0129] It should be noted that the embodiments described above are only for explaining the present invention and do not constitute any limitation on the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory terms, not limiting terms. Modifications can be made to the present invention within the scope of the claims, and revisions can be made to the present invention without departing from the scope and spirit of the present invention. Although the present invention described herein relates to specific methods, materials, and embodiments, it does not mean that the present invention is limited to the specific examples disclosed herein; on the contrary, the present invention can be extended to all other methods and applications with the same function.

Claims

1. A photothermal Janus nanofiber composite membrane, characterized in that, It includes a TM hydrophobic layer and a PCB hydrophilic layer, wherein the TM hydrophobic layer and the PCB hydrophilic layer are deposited in situ through layer-by-layer electrospinning to form an asymmetric bilayer nanofiber structure with continuous interfacial bonding. The TM hydrophobic layer comprises thermoplastic polyurethane and MXene nanosheets, wherein the MXene nanosheets are dispersed in the thermoplastic polyurethane matrix, thereby endowing the composite film with near-infrared photothermal conversion function; The PCB hydrophilic layer includes polyvinyl alcohol, carboxymethyl chitosan and baicalin. The polyvinyl alcohol, carboxymethyl chitosan and baicalin form a cross-linked network, fixing baicalin in the three-dimensional fiber network of the PCB hydrophilic layer. The mass ratio of MXene nanosheets to thermoplastic polyurethane in the TM hydrophobic layer is 1:(50~200); the mass ratio of polyvinyl alcohol, carboxymethyl chitosan and baicalin in the PCB hydrophilic layer is (16~48):(2.67~8):

1.

2. The photothermal Janus nanofiber composite membrane according to claim 1, characterized in that, The thickness ratio of the TM hydrophobic layer to the PCB hydrophilic layer is (1~5):(1~5).

3. A method for preparing a photothermal Janus nanofiber composite membrane as described in any one of claims 1-2, characterized in that, Includes the following steps: MXene nanosheets were introduced into a thermoplastic polyurethane spinning solution to disperse the MXene nanosheets, thus obtaining a TM composite spinning solution. Carboxymethyl chitosan and baicalin were added sequentially to a polyvinyl alcohol aqueous solution and mixed to obtain a PCB composite spinning solution. A layer-by-layer electrospinning process is adopted, in which the TM composite spinning solution is first electrospinned on the same collection substrate, and the TM hydrophobic layer is deposited in situ. Maintaining continuous contact between the TM hydrophobic layer and the collecting substrate, the TM composite spinning solution was replaced with the PCB composite spinning solution, and electrospinning was performed directly on the surface of the TM hydrophobic layer. This allowed the PCB hydrophilic layer to be deposited in situ on the surface of the TM hydrophobic layer, forming an asymmetric bilayer nanofiber structure with continuous interfacial bonding. After drying, a photothermal Janus nanofiber composite membrane was obtained.

4. The method for preparing the photothermal Janus nanofiber composite membrane according to claim 3, characterized in that, The specific process for introducing MXene nanosheets into thermoplastic polyurethane spinning solution includes: premixing an aqueous dispersion of MXene nanosheets with DMF, and then ultrasonically dispersing the mixture to obtain an MXene / DMF pre-dispersion; under continuous stirring, adding the MXene / DMF pre-dispersion dropwise to the thermoplastic polyurethane spinning solution at a rate of 40-60 drops / minute; after the addition is completed, magnetically stirring at 30-40℃ and 300-500 rpm for 10-14 h, followed by ultrasonic dispersion at 0℃ in an ice bath for 20-40 min.

5. The method for preparing the photothermal Janus nanofiber composite membrane according to claim 3, characterized in that, The specific process of adding carboxymethyl chitosan and baicalin sequentially to a polyvinyl alcohol aqueous solution includes: completely dissolving polyvinyl alcohol in water to form a polyvinyl alcohol aqueous solution; cooling and adding carboxymethyl chitosan while stirring, then adding baicalin while stirring continuously, and finally ultrasonically dispersing.

6. The method for preparing the photothermal Janus nanofiber composite membrane according to claim 5, characterized in that, The specific process of sequentially adding carboxymethyl chitosan and baicalin to a polyvinyl alcohol aqueous solution includes: stirring polyvinyl alcohol in water at a constant temperature of 85-95°C for 1.5-2.5 h until completely dissolved to form a polyvinyl alcohol aqueous solution; cooling to 55-65°C and adding carboxymethyl chitosan and stirring for 0.5-1.5 h; then adding baicalin and stirring continuously for 5-7 h; and finally ultrasonically dispersing under 0°C ice bath conditions for 20-40 min.

7. The method for preparing the photothermal Janus nanofiber composite membrane according to claim 3, characterized in that, The electrospinning process of the TM hydrophobic layer includes: spinning voltage of 16~18 kV, spinning rate of 0.6~0.8 mL / h, receiving distance of 14~16 cm, receiving roller speed of 90~110 rpm, and spinning time of 1~3 h.

8. The method for preparing the photothermal Janus nanofiber composite membrane according to claim 3, characterized in that, The electrospinning process of the PCB hydrophilic layer includes: spinning voltage of 17~19 kV, spinning rate of 0.6~0.8 mL / h, receiving distance of 14~16 cm, receiving roller speed of 90~110 rpm, and spinning time of 1~3 h.

9. The method for preparing the photothermal Janus nanofiber composite membrane according to claim 3, characterized in that, The electrospinning environment temperature for the TM hydrophobic layer and the PCB hydrophilic layer is 23~27℃, and the electrospinning relative humidity is 45%~55%RH.

10. The application of the photothermal Janus nanofiber composite membrane as described in claim 1 in the preparation of wound dressings.

Citation Information

Patent Citations

  • Dynamic hydrogel cooperating with photo-thermal therapy as well as preparation method and application of dynamic hydrogel

    CN117653776A

  • Chitosan for food packaging, preparation method of chitosan and preparation method of food packaging film

    CN122011234A