A modified coal gangue biochar composite adsorbent material, its preparation method and application

By performing multi-scale functionalization of coal gangue and biomass and constructing an organic-inorganic hybrid network, the problems of weak interfacial bonding, limited pore structure and insufficient active sites in existing coal gangue-biochar composite materials have been solved, achieving efficient and deep purification of various pollutants in complex water bodies.

CN123059615APending Publication Date: 2026-11-10ORDOS INST OF APPLIED TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611532482.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing coal gangue-biochar composite adsorbent materials suffer from weak interfacial bonding, limited pore structure, insufficient density of surface active sites, and inadequate synergistic removal capacity of pollutants, resulting in poor performance in treating complex water bodies.

Method used

By activating coal gangue through alkali melting and acid hydrolysis, combined with multi-scale functionalization of biomass, including graded screening, deashing, hydrogen peroxide oxidation, hydrothermal carbonization, phosphorus modification, acid washing and alkali passivation, and silane pre-anchoring, a hierarchical porous structure is constructed. Furthermore, an organic-inorganic hybrid network is formed through in-situ polycondensation and crosslinking with tannic acid, introducing multiple active sites, loading iron centers, forming iron oxide/hydroxide, and constructing a multifunctional adsorption interface.

Benefits of technology

It significantly enhances the interfacial bonding force of the material, enriches the pore structure and active sites, and achieves a broad-spectrum adsorption and removal capacity for heavy metal ions, anionic pollutants and organic micro-pollutants. The material maintains a high adsorption capacity after multiple cycles of use, reducing the cost of use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention discloses a modified coal gangue biochar composite adsorbent material, its preparation method, and its application, belonging to the field of environmental functional materials technology. The material uses coal gangue and biomass as raw materials. The coal gangue is prepared by alkaline melting and acid hydrolysis to obtain a silica-alumina precursor solution. The biomass undergoes graded deashing, hydrogen peroxide oxidation, low-temperature pre-activation, hydrothermal carbonization, phosphorus modification, acid washing and alkali passivation, and silane pre-anchoring to obtain functionalized hydrothermal carbon microparticles. The two are then subjected to in-situ polycondensation under tannic acid crosslinking, followed by sodium periodate oxidation aldehyde stylation, diethylenetriamine Schiff base chelation functionalization, and near-neutral FeCl3 hydrolysis to support iron centers, resulting in the composite adsorbent material. This material exhibits broad-spectrum adsorption and removal capabilities, suitable for the deep purification of complex water bodies such as wastewater from mines, electroplating plants, metallurgy, coal-fired power plants, coal gangue leachate, and domestic sewage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of environmental functional materials technology, and in particular to a modified coal gangue biochar composite adsorbent material, its preparation method, and its application. Background Technology

[0002] Heavy metal ions (such as Pb) are often present in polluted water bodies, including mine wastewater, electroplating wastewater, metallurgical wastewater, coal-fired power plant wastewater, coal gangue leachate, and domestic sewage. 2+ Cu 2+ Cd 2+ Cr 6+ Water quality is complex, with a wide range of pollutants, including heavy metal cations, inorganic anions (such as phosphate, nitrate, and arsenate), and organic micropollutants (such as phenols, antibiotics, and dyes). Treatment is challenging due to the diverse composition of these pollutants. Traditional single-type adsorbents typically only show good adsorption effects on a specific type of pollutant, making it difficult to achieve synergistic and deep purification of multiple types of pollutants in complex water bodies. Therefore, developing efficient and low-cost adsorbents with broad-spectrum adsorption capabilities for heavy metal cations, inorganic anions, and organic micropollutants has become an important research direction in the field of water treatment.

[0003] In existing technologies, biochar is widely used for the adsorption and removal of pollutants in water bodies due to its wide availability of raw materials, rich pore structure, numerous oxygen-containing functional groups on the surface, and low cost. However, the specific surface area and surface active site density of raw biochar are limited, and its adsorption capacity and selectivity for pollutants still need to be improved. Furthermore, its poor mechanical strength and difficulty in solid-liquid separation limit its large-scale application. To overcome these shortcomings, researchers have attempted to functionalize biochar through methods such as acid washing and activation, metal salt impregnation, heteroatom doping, and silane coupling agent grafting to increase the types and number of surface active sites and improve adsorption performance.

[0004] Coal gangue is a large-scale solid waste generated during coal mining and washing. Its massive stockpiles not only occupy land but also cause serious soil and groundwater pollution due to weathering and leaching. The main components of coal gangue are SiO2 and Al2O3, representing a potential silicon-aluminum resource. Through processes such as alkali fusion activation and acid hydrolysis, coal gangue can be transformed into silicon-aluminum materials with adsorption activity, achieving high-value resource utilization and becoming a research hotspot in the field of solid waste resource utilization. Combining coal gangue with biomass carbon materials to construct composite adsorption materials that combine the activity of inorganic silicon-aluminum with the porous structure of organic carbonaceous matter holds promise for improving the synergistic removal capacity of materials for various types of pollutants in complex water bodies while simultaneously realizing solid waste resource utilization.

[0005] However, existing coal gangue-biochar composite adsorption materials still have the following shortcomings: First, the interaction between coal gangue and biochar is mostly a simple physical mixing or loading through precipitation or impregnation, resulting in weak interfacial bonding, poor compatibility between the organic and inorganic phases, insufficient material structural stability, and significant degradation of adsorption performance after recycling. Second, the pretreatment methods for biochar are relatively simple, mostly involving conventional operations such as crushing, washing, and drying, failing to systematically classify, deash, pore-forming, and heteroatom doping of biomass, leading to limited specific surface area, pore structure, and surface active site density. Third, the functionalization modification of the material surface mostly uses single silane coupling agents such as mercapto and amino groups, resulting in a single type of chelation site and insufficient synergistic removal capacity and selectivity for multiple pollutants. Fourth, the ash ions remaining in the coal gangue activation stage and the acid and base species remaining in the biomass pretreatment stage are prone to mutual interference in the subsequent composite process, affecting the formation and stability of the hybrid network structure.

[0006] Therefore, there is an urgent need to develop a modified coal gangue biochar composite adsorbent material that can be widely used in the deep purification treatment of complex water bodies such as mine wastewater, electroplating wastewater, metallurgical wastewater, coal-fired power plant wastewater, coal gangue leaching liquid and domestic sewage. Summary of the Invention

[0007] The purpose of this invention is to address the shortcomings of existing technologies by proposing a modified coal gangue biochar composite adsorbent material, its preparation method, and its application.

[0008] To achieve the above objectives, the present invention adopts the following technical solution:

[0009] This invention provides a method for preparing a modified coal gangue biochar composite adsorbent material, comprising the following steps:

[0010] S1. Alkali fusion-acid hydrolysis activation of coal gangue: Coal gangue is crushed to a particle size ≤0.15mm, mixed evenly with anhydrous Na2CO3, placed in a muffle furnace, heated to 800-850℃ at a heating rate of 8-12℃ / min, and calcined for 3-4h to obtain alkali fused clinker. After grinding the alkali fused clinker, it is mixed with 1-1.5mol / L HCl solution at a liquid-solid ratio of 20-30mL / g, and acid hydrolyzed at 60-80℃ and 200-400rpm for 2-4h. After filtration, the pH of the filtrate is adjusted to 2-4 with 0.1-1mol / L NaOH solution to obtain a silicon-aluminum precursor solution.

[0011] During the co-roasting of coal gangue and anhydrous Na2CO3 at 800-850℃, Na... +It enters the coal gangue skeleton and destroys the silicon-aluminum polymer structure of kaolinite, quartz and other materials, forming an activated phase that is easily acid-hydrolyzed, thereby improving the release capacity of silicon and aluminum components in subsequent acid treatment. Then, it is acid-hydrolyzed with HCl at 60-80℃, and silicon and aluminum elements enter the liquid phase in the form of silicic acid and aluminum ions. After filtration, the pH of the filtrate is adjusted to 2-4 with NaOH. This weakly acidic range helps to keep the silicon-aluminum precursor solution stable, providing an inorganic phase source for subsequent in-situ polycondensation and composite with functionalized biochar.

[0012] S2. Multi-scale functionalization of biomass feedstocks:

[0013] S2.1. Raw material grading and screening and targeted deashing: The biomass raw material is dried to constant weight at 60-80℃, pulverized and then passed through 0.5mm, 0.15mm and 0.075mm sieves to obtain coarse powder, medium powder and fine powder. The three powders are mixed with deionized water at a liquid-solid ratio of 8-15mL / g, and 3-5wt% acetic acid aqueous solution is added. The mixture is soaked at 60-80℃ and 200-400rpm for 1-3h, filtered, washed 3-5 times with deionized water at 60-70℃, and then washed with deionized water at room temperature until the filtrate is neutral. The mixture is then vacuum dried at 60-80℃ for 6-12h to obtain deashed biomass.

[0014] S2.2. Chemical pretreatment and low-temperature preactivation: The deashed biomass obtained in S2.1 is mixed with 4-6 wt% H2O2 aqueous solution at a liquid-solid ratio of 10-15 mL / g, oxidized in a water bath at 50-70℃ and 200-400 rpm for 1-3 h. After the reaction is completed, the mixture is cooled to room temperature, filtered, washed with deionized water until the filtrate is neutral, and vacuum dried at 60-80℃ for 6-12 h to obtain oxidized pretreated biomass. The oxidized pretreated biomass is ground and mixed with 1-2 wt% KOH aqueous solution at a liquid-solid ratio of 10-20 mL / g, impregnated at room temperature and 100-200 rpm for 3-4 h, filtered, vacuum dried at 80-100℃ for 4-8 h, and then vacuum dried at 100-110℃ for 6-12 h to obtain the preactivated precursor.

[0015] S2.3. Hydrothermal carbonization and pore shaping: The pre-activated precursor obtained in S2.2 was pulverized to ≤0.3 mm, mixed with deionized water at a liquid-to-solid ratio of 10-15 mL / g, oxalic acid was added, and the mixture was transferred to a hydrothermal reactor. The reaction was carried out at 200-220℃ for 8-10 h. After the reaction was completed, the mixture was cooled to room temperature, and the pH was neutralized to 6-7 with 0.1-0.5 mol / L NaOH solution. The mixture was filtered, and then washed with deionized water until the filtrate was neutral. The filtrate was then vacuum dried at 60-80℃ for 6-12 h to obtain hydrothermal carbon microspheres.

[0016] S2.4. Surface in-situ phosphorus modification: The hydrothermal carbon microspheres obtained in S2.3 were mixed with deionized water at a liquid-solid ratio of 8-15 mL / g, and ammonium dihydrogen phosphate was added. The mixture was immersed at 70-80℃ and 200-400 rpm for 2-3 hours, filtered, washed 2-3 times with deionized water at 60-70℃, and then washed with deionized water at room temperature until the filtrate was neutral. The mixture was then vacuum dried at 60-80℃ for 6-12 hours to obtain phosphorus-modified hydrothermal carbon microspheres.

[0017] S2.5 Acid washing-alkali passivation treatment: The phosphorus-modified hydrothermal carbon microspheres obtained in S2.4 are washed with hot water 2-3 times, acid washed with 0.2-0.3 mol / L dilute HCl 3-5 times, and washed with deionized water until the filtrate is neutral to obtain acid-washed hydrothermal carbon microparticles. The acid-washed hydrothermal carbon microparticles are mixed with 0.1-0.15 mol / L Na2CO3 aqueous solution at a liquid-solid ratio of 10-20 mL / g and treated at 50-60℃ and 200-300 rpm for 0.5-1.5 h. After filtration, the microspheres are washed with deionized water until the filtrate is neutral and vacuum dried at 60-80℃ for 6-12 h to obtain alkali passivated hydrothermal carbon microparticles.

[0018] S2.6. Silane pre-anchoring: The alkaline passivated hydrothermal carbon microparticles obtained in S2.5 were mixed with 75wt% ethanol aqueous solution at a liquid-solid ratio of 10-20 mL / g, γ-glycidoxypropyltrimethoxysilane was added, and 0.1-1 mol / L acetic acid was added dropwise to adjust the pH to 4-5. The mixture was refluxed at 40-60℃ and 200-300 rpm for 2-4 h, filtered, washed 2-3 times with anhydrous ethanol, and then washed with deionized water until the filtrate was neutral. The mixture was then vacuum dried at 60-80℃ for 6-12 h to obtain functionalized hydrothermal carbon microparticles.

[0019] By grading and screening biomass raw materials and deashing them with acetic acid, combined with pre-treatment with hydrogen peroxide oxidation, ash removal, biomass component deconstruction, and the introduction of abundant oxygen-containing functional groups on their surface are facilitated, thereby enhancing the reactivity and subsequent modifiability of the biomass. The pre-loading of potassium ions in KOH can play an activating and pore-forming role in the subsequent hydrothermal carbonization process. Under high-temperature hydrothermal conditions, it reacts with the carbon precursor, achieving initial pore development through the erosion of the carbon skeleton and the release of gases. Simultaneously, potassium species are embedded in the carbon matrix, leaving abundant mesoporous and microporous structures after subsequent acid washing, which helps to construct a hierarchical porous carbon skeleton. Furthermore, alkaline pretreatment can promote the partial hydrolysis and dissolution of hemicellulose and lignin in the biomass, further improving the microstructural uniformity of the carbonization precursor. The resulting hydrothermal carbon microspheres are then surface-modified with phosphorus by impregnation with ammonium dihydrogen phosphate, followed by sequential acid treatment with dilute acids. The process involves washing and sodium carbonate alkaline treatment. Acid washing helps remove residual salt and ash from the surface, exposes active sites of oxygen-containing functional groups, and washes away residual potassium ions after potassium activation. The dissolution of potassium ions leaves a large number of pores, further enriching the pore structure. Alkaline treatment, to a certain extent, passivates overactive sites and loads sodium species, thereby regulating surface chemical properties. Finally, under weakly acidic conditions, γ-glycidoxypropyltrimethoxysilane is introduced. The silanol groups generated by the hydrolysis of the silane coupling agent can undergo dehydration condensation with the hydroxyl groups on the surface of biochar to form stable covalent silicon-oxygen bonds. This grafts the epoxy-containing organic segments onto the surface of hydrothermal carbon particles, thus completing a multi-scale functionalization process of hierarchical porous structure construction, surface functionalization, and organic / inorganic interface anchoring. This provides a carbonaceous matrix with abundant active sites and organic bridging capabilities for subsequent in-situ polycondensation and composite with coal gangue silica-alumina precursors.

[0020] S3. In-situ polycondensation: The silicon-aluminum precursor solution obtained in S1 is mixed with the functionalized hydrothermal carbon microparticles obtained in step S2. A crosslinking agent and a composite polycondensation catalyst are added, and the mixture is transferred to a hydrothermal reactor. The reaction is carried out at 140-150℃ for 8-10 hours. After the reaction is completed, the mixture is cooled, filtered, and washed with deionized water until the filtrate is neutral. The mixture is then vacuum dried at 60-80℃ for 6-12 hours to obtain the hybrid network precursor.

[0021] Under a composite polycondensation catalyst and a hydrothermal environment of 140-150℃, silicic acid and aluminum species in the silicon-aluminum precursor solution undergo controlled polycondensation, gradually forming a silicon-aluminum inorganic network framework. Simultaneously, tannic acid, acting as a crosslinking agent, interacts with the silicon-aluminum precursor polycondensation product and the surface of functionalized hydrothermal carbon particles through multiple points due to its abundant phenolic hydroxyl groups in its molecular structure. These interactions may include covalent bonding, coordination complexation, and hydrogen bonding. Under the above reaction conditions, the silicon-aluminum inorganic polycondensation and the polyphenolic crosslinking of tannic acid synergistically... Simultaneously, tannic acid not only participates in network construction itself, but also acts as a bridge to tightly connect functionalized hydrothermal carbon microparticles with the silicon-aluminum inorganic phase, ultimately constructing an organic-inorganic interpenetrating hybrid network structure on the surface and in the pores of the functionalized hydrothermal carbon microparticles. The resulting hybrid network precursor retains the rigid framework and adsorption activity of the silicon-aluminum components of coal gangue, and introduces abundant chelating sites such as phenolic hydroxyl groups and catechols through tannic acid, providing a continuous organic functional interface for subsequent sodium periodate oxidation aldehyde hydration and Schiff base chelation of metal center loading.

[0022] S4. Surface aldehyde-based oxidation: The hybrid network precursor obtained in S3 was mixed with 90wt% ethanol aqueous solution at a liquid-solid ratio of 15-30 mL / g, sodium periodate was added, and the mixture was oxidized at room temperature, in the dark, at 200-300 rpm for 8-10 h. After the reaction was completed, ethylene glycol was added, and the mixture was stirred in the dark for 0.5-1 h. The mixture was filtered, washed 2-3 times with anhydrous ethanol, and then washed with deionized water until the filtrate was neutral. The mixture was then vacuum dried at 40-50℃ for 6-12 h to obtain the aldehyde-based hybrid network precursor.

[0023] Under room temperature and light-protected conditions, sodium periodate acts as a selective oxidant, reacting with tannic acid molecules in the hybrid network precursor and the vicinal diol structure on the surface of biochar. The two hydroxyl groups of the vicinal diol coordinate with the periodate ion to form a five-membered cyclic periodate intermediate. Subsequently, the C-C bonds are collaboratively broken to generate the corresponding aldehyde group, and the periodate ion itself is reduced to iodate. This reaction exhibits high selectivity for the vicinal diol structure under mild conditions, allowing for the controllable introduction of aldehyde active sites on the surface of the hybrid network. This provides reaction sites for the Schiff base condensation of the aldehyde group with the primary amino group of diethylenetriamine in subsequent steps. It should be noted that the oxidation of polyphenols such as tannic acid with sodium periodate may be accompanied by side reactions such as the oxidation of phenolic hydroxyl groups to quinones and polymerization. Therefore, by controlling the amount of sodium periodate and adding ethylene glycol to quench unreacted sodium periodate after the reaction, sufficient aldehyde groups can be introduced while reducing the risk of hybrid network breakage due to deep oxidation, ultimately achieving the controllable construction of the aldehyde-based hybrid network precursor.

[0024] S5. Schiff base chelation functionalization and metal center loading: The aldehyde-modified hybrid network precursor obtained in S4 was mixed with anhydrous ethanol at a liquid-to-solid ratio of 15-30 mL / g, and diethylenetriamine was added. The mixture was refluxed at 60-70℃ and 200-300 rpm for 4-8 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, and washed 2-3 times with anhydrous ethanol to obtain the imino-modified hybrid network precursor. The imino-modified hybrid network precursor was mixed with deionized water at a liquid-to-solid ratio of 10-20 mL / g, and 0.1 mol / L... FeCl3 solution was used to adjust the pH to 6.5-7.5 with 0.1-1 mol / L ammonia water. The complexation reaction was carried out at 50-60℃ and 200-300 rpm for 3-4 hours. After the complexation reaction was completed, the solution was cooled to room temperature, filtered, washed 2-3 times with anhydrous ethanol, and then washed with deionized water until the filtrate was neutral. The solution was then vacuum dried at 50-70℃ for 6-12 hours and ground through a 100-200 mesh sieve to obtain the modified coal gangue biochar composite adsorbent material.

[0025] Under reflux conditions at 60-70℃, the primary amino group of diethylenetriamine undergoes a nucleophilic addition-dehydration condensation reaction with the aldehyde group on the surface of the aldehyde-modified hybrid network precursor to generate an imino-Schiff base structure, thereby introducing abundant amino chelation sites on the surface of the hybrid network, yielding the imino-modified hybrid network precursor. This precursor is then mixed with FeCl3 solution, and the pH is adjusted to near-neutral conditions of 6.5-7.5 with ammonia. At this point, Fe... 3+ Hydrolysis can occur, tending to generate amorphous iron hydroxides / hydroxides. In the form of amorphous iron hydroxides / hydroxides, they are loaded into a hybrid network matrix through surface complexation to form iron-centered modified coal gangue biochar composite adsorbents. The imino-Schiff base structure, phenolic hydroxyl groups and other chelating sites can form coordination interactions with iron species to jointly construct an iron-centered composite system with chelation and redox activities.

[0026] Preferably, the SiO2 content in the coal gangue in S1 is 45-60wt%, and the Al2O3 content is 18-30wt%.

[0027] Preferably, the mass ratio of coal gangue to anhydrous Na2CO3 in S1 is 1:0.8-1.2.

[0028] Preferably, the biomass raw material in S2.1 is one or more of straw, bamboo powder, reed powder, rice husk, and sawdust.

[0029] Preferably, in S2.1, the coarse powder has a particle size of 0.15-0.5mm, the medium powder has a particle size of 0.075-0.15mm, and the fine powder has a particle size of ≤0.075mm, with a mass ratio of 1:0.5-2:0.5-1.5.

[0030] Preferably, the amount of acetic acid used in the acetic acid aqueous solution in step S2.1 is 1-2% of the total mass of the three powders: coarse powder, medium powder, and fine powder.

[0031] Preferably, the amount of oxalic acid in step S2.3 is 3-5% of the mass of the pre-activated precursor.

[0032] Preferably, the amount of ammonium dihydrogen phosphate added in S2.4 is 1-2% of the mass of the hydrothermal carbon microspheres.

[0033] Preferably, the amount of γ-glycidyl etheroxypropyltrimethoxysilane in step S2.6 is 3-5% of the mass of the alkali passivated hydrothermal carbon particles.

[0034] Preferably, the mass ratio of the silicon-aluminum precursor solution to the functionalized hydrothermal carbon microparticles in S3 is 1-3:1.

[0035] Preferably, the crosslinking agent in S3 is tannic acid, and the amount used is 5-15% of the mass of the functionalized hydrothermal carbon particles.

[0036] Preferably, the composite polycondensation catalyst in S3 is a mixture of NaOH and trisodium citrate in a mass ratio of 1:1, and the amount of composite polycondensation catalyst is 0.2-0.5% of the mass of functionalized hydrothermal carbon particles.

[0037] Preferably, the amount of sodium periodate in S4 is 30-40% of the mass of the hybrid network precursor.

[0038] Preferably, the amount of ethylene glycol in S4 is 15-25% of the mass of the hybrid network precursor.

[0039] Preferably, the amount of diethylenetriamine in S5 is 5-15% of the mass of the aldehyde-modified hybrid network precursor.

[0040] Preferably, the amount of 0.1 mol / L FeCl3 solution used in S5 is 10-20% of the mass of the imino hybrid network precursor.

[0041] The present invention also provides a modified coal gangue biochar composite adsorbent material prepared by the method described above.

[0042] Preferably, the mechanism of action of the modified coal gangue biochar composite adsorbent material in this invention is explained as follows:

[0043] The iron oxides / hydroxides, imino groups, amino groups, phenolic hydroxyl groups, and coal gangue-derived silica-alumina components distributed on the material surface and within the pores collectively constitute a multifunctional adsorption interface. The removal of water pollutants is synergistically contributed by multiple mechanisms. On one hand, the hierarchical porous structure provides pore filling and physical retention sites. Iron species and oxygen-containing functional groups on the surface can bind to pollutants through surface complexation, coordination chelation, and ion exchange. The Fe-O and Fe-OH functional groups introduced by the iron oxides / hydroxides can also undergo ligand exchange with anionic pollutants. On the other hand, under near-neutral pH conditions, the material surface can exhibit certain electrical characteristics, allowing electrostatic attraction or repulsion to participate in regulating the interfacial migration of pollutants. Furthermore, for certain variable-valence pollutants (such as Cr...),... 6+ The redox activity of iron species may further participate in reduction reactions, and some pollutants can also be fixed through coprecipitation. The synergistic contribution of multiple mechanisms such as pore filling, electrostatic interaction, surface complexation, coordination chelation, ion exchange, reduction and coprecipitation enables this composite adsorbent material to exhibit a broad-spectrum adsorption and removal capacity for heavy metal ions, anionic pollutants and organic micro-pollutants.

[0044] The present invention also provides a modified coal gangue biochar composite adsorbent material that can be used to treat heavy metal ions, anionic pollutants and organic micro-pollutants in polluted water bodies, and is especially suitable for the deep purification of complex water bodies such as wastewater from mines, electroplating, metallurgy, coal-fired power plants, coal gangue leaching liquid, and domestic sewage.

[0045] Compared with the prior art, the beneficial effects of the present invention are:

[0046] 1. This invention utilizes in-situ polycondensation of an active silica-alumina precursor solution with functionalized hydrothermal carbon microparticles under a composite polycondensation catalyst and at 140-150°C to construct an organic-inorganic interpenetrating hybrid network using tannic acid as a crosslinking agent. This significantly enhances the interfacial bonding force and fundamentally overcomes the shortcomings of existing technologies where coal gangue and biochar are mostly simple physical mixtures or precipitates and impregnated, resulting in weak interfacial bonding and significant degradation of adsorption performance after recycling.

[0047] 2. This invention employs a multi-scale functionalization process for biomass raw materials, including graded screening, deashing, hydrogen peroxide oxidation, low-temperature pre-activation, hydrothermal carbonization for pore formation, phosphorus modification, acid washing and alkali passivation, and silane pre-anchoring. Through low-temperature pre-loading with KOH and synergistic hydrothermal pore formation, the resulting hydrothermal carbon microspheres possess a graded porous structure. Subsequently, aldehyde groups are introduced through selective oxidation with sodium periodate, imino chelating sites are constructed via diethylenetriamine Schiff base reaction, and amorphous iron oxides / hydroxides are loaded via near-neutral hydrolysis with FeCl3. This results in the distribution of multiple types of active sites on the material surface, including imino, amino, phenolic hydroxyl, iron species, and silicon-aluminum components. This overcomes the shortcomings of existing technologies where single silane coupling agent modification leads to a limited range of chelating site types and insufficient synergistic removal capacity.

[0048] 3. This invention utilizes a five-level composite structure consisting of a coal gangue silica-alumina skeleton, hierarchical porous biochar, tannic acid crosslinking bridges, imino chelating sites, and iron centers. This structure enables multiple mechanisms, including pore filling, electrostatic interaction, surface complexation, coordination chelation, ion exchange, reduction, and coprecipitation, to work synergistically. As a result, it exhibits a broad-spectrum adsorption and removal capacity for heavy metal cations, anions, and organic micropollutants.

[0049] 4. The organic-inorganic hybrid network structure makes the active sites less likely to fall off during repeated adsorption-desorption processes. The iron centers are stably loaded in the hybrid matrix in the form of amorphous iron oxide / hydroxide. The material after adsorption saturation can be desorbed and regenerated by acid, alkali or EDTA solution. It can still maintain a high adsorption capacity after multiple cycles, which reduces the actual use cost. It has the ability to deeply purify a variety of pollutants in complex water bodies such as mine wastewater, electroplating wastewater, metallurgical wastewater, coal-fired power plant wastewater, coal gangue leachate and domestic sewage. Detailed Implementation

[0050] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with existing known technologies. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments.

[0051] Example 1: A method for preparing a modified coal gangue biochar composite adsorbent material, comprising the following steps:

[0052] S1. Alkali fusion-acid hydrolysis activation of coal gangue: 20g of coal gangue with SiO2 content of 45wt% and Al2O3 content of 18wt% was crushed to a particle size of ≤0.15mm, mixed evenly with 16g of anhydrous Na2CO3, placed in a muffle furnace, heated to 800℃ at a heating rate of 8℃ / min, and calcined for 4h to obtain alkali fused clinker. After grinding the alkali fused clinker, it was mixed with 1mol / L HCl solution at a liquid-solid ratio of 20mL / g, and acid hydrolyzed at 60℃ and 200rpm for 4h. After filtration, the pH of the filtrate was adjusted to 2 with 0.1mol / L NaOH solution to obtain a silicon-aluminum precursor solution.

[0053] S2. Multi-scale functionalization of biomass feedstocks:

[0054] S2.1. Raw material grading and screening and targeted deashing: 30g of straw was dried to constant weight at 60℃, crushed and then passed through 0.5mm, 0.15mm and 0.075mm sieves in sequence to obtain 15g of coarse powder with a particle size of 0.15-0.5mm, 7.5g of medium powder with a particle size of 0.075-0.15mm and 7.5g of fine powder with a particle size ≤0.075mm. The three powders were mixed with deionized water at a liquid-solid ratio of 8mL / g, and 10g of 3wt% acetic acid aqueous solution was added. The mixture was soaked at 60℃ and 200rpm for 3h, filtered, washed 5 times with 60℃ deionized water, and then washed with room temperature deionized water until the filtrate was neutral. The mixture was then vacuum dried at 60℃ for 12h to obtain deashed biomass.

[0055] S2.2. Chemical pretreatment and low-temperature preactivation: 24g of deashed biomass was mixed with 4wt% H2O2 aqueous solution at a liquid-solid ratio of 10mL / g and oxidized at 50℃ water bath and 200rpm for 3h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed with deionized water until the filtrate was neutral, and vacuum dried at 60℃ for 12h to obtain oxidized pretreated biomass. The oxidized pretreated biomass was ground and mixed with 1wt% KOH aqueous solution at a liquid-solid ratio of 10mL / g and impregnated at room temperature and 100rpm for 4h. After filtration, the mixture was first vacuum dried at 80℃ for 8h and then vacuum dried at 100℃ for 12h to obtain the preactivated precursor.

[0056] S2.3. Hydrothermal carbonization and pore shaping: 20g of the pre-activated precursor obtained in S2.2 was crushed to ≤0.3mm, mixed with deionized water at a liquid-to-solid ratio of 10mL / g, 0.6g of oxalic acid was added, and the mixture was transferred to a hydrothermal reactor. The reaction was carried out at 200℃ for 10h. After the reaction was completed, the mixture was cooled to room temperature, and the pH was first neutralized to 6 with 0.1mol / L NaOH solution. The mixture was then filtered, washed with deionized water until the filtrate was neutral, and vacuum dried at 60℃ for 12h to obtain hydrothermal carbon microspheres.

[0057] S2.4. Surface in-situ phosphorus modification: 12g of hydrothermal carbon microspheres obtained in S2.3 were mixed with deionized water at a liquid-solid ratio of 8mL / g, and 0.12g of ammonium dihydrogen phosphate was added. The mixture was soaked at 70℃ and 200rpm for 3h, filtered, washed twice with deionized water at 60℃, and then washed with deionized water at room temperature until the filtrate was neutral. The mixture was then vacuum dried at 60℃ for 12h to obtain phosphorus-modified hydrothermal carbon microspheres.

[0058] S2.5 Acid washing-alkali passivation treatment: 10g of phosphorus-modified hydrothermal carbon microspheres obtained from S2.4 were washed twice with hot water, five times with 0.2mol / L dilute HCl, and washed with deionized water until the filtrate was neutral to obtain acid-washed hydrothermal carbon microparticles. The acid-washed hydrothermal carbon microparticles were mixed with 0.1mol / L Na2CO3 aqueous solution at a liquid-solid ratio of 10mL / g and treated at 50℃ and 200rpm for 1.5h. After filtration, the microspheres were washed with deionized water until the filtrate was neutral and dried under vacuum at 60℃ for 12h to obtain alkali passivated hydrothermal carbon microparticles.

[0059] S2.6. Silane pre-anchoring: 8g of alkali passivated hydrothermal carbon microparticles obtained in S2.5 were mixed with 75wt% ethanol aqueous solution at a liquid-to-solid ratio of 10mL / g, 0.24g of γ-glycidyl etheroxypropyltrimethoxysilane was added, and 0.1mol / L acetic acid was added dropwise to adjust the pH to 5. The mixture was refluxed at 40℃ and 200rpm for 4h, filtered, washed twice with anhydrous ethanol, and then washed with deionized water until the filtrate was neutral. The mixture was then vacuum dried at 60℃ for 12h to obtain functionalized hydrothermal carbon microparticles.

[0060] S3. In-situ polycondensation: 8g of the silicon-aluminum precursor solution obtained in S1 was mixed with 8g of the functionalized hydrothermal carbon microparticles obtained in step S2. 0.4g of tannic acid and 0.016g of the composite polycondensation catalyst (NaOH and trisodium citrate mass ratio 1:1) were added and transferred to a hydrothermal reactor. The mixture was reacted at 140℃ for 10h. After the reaction was completed, the mixture was cooled, filtered, and washed with deionized water until the filtrate was neutral. The filtrate was then vacuum dried at 60℃ for 12h to obtain the hybrid network precursor.

[0061] S4. Surface aldehyde-based oxidation: 10 g of the hybrid network precursor obtained in S3 was mixed with 90 wt% ethanol aqueous solution at a liquid-solid ratio of 15 mL / g, 3 g of sodium periodate was added, and the mixture was oxidized at 200 rpm for 10 h at room temperature in the dark. After the reaction was completed, 1.5 g of ethylene glycol was added, and the mixture was stirred in the dark for another 1 h. The mixture was filtered, washed twice with anhydrous ethanol, and then washed with deionized water until the filtrate was neutral. The mixture was then vacuum dried at 40 °C for 12 h to obtain the aldehyde-based hybrid network precursor.

[0062] S5. Schiff base chelation functionalization and metal center loading: 8g of the aldehyde-modified hybrid network precursor obtained in S4 was mixed with anhydrous ethanol at a liquid-to-solid ratio of 15mL / g, and 0.4g of diethylenetriamine was added. The mixture was refluxed at 60℃ and 200rpm for 8h. After the reaction was completed, the mixture was cooled to room temperature, filtered, and washed twice with anhydrous ethanol to obtain the imino-modified hybrid network precursor. 7g of the imino-modified hybrid network precursor was mixed with deionized water at a liquid-to-solid ratio of 10mL / g, and 0.7g of 0.1mol / L FeCl3 solution was added. The pH was adjusted to 6.5 with 0.1mol / L ammonia water, and the mixture was complexed at 50℃ and 200rpm for 4h. After the complexation reaction was completed, the mixture was cooled to room temperature, filtered, washed twice with anhydrous ethanol, and then washed with deionized water until the filtrate was neutral. The filtrate was vacuum dried at 50℃ for 12h and ground through a 100-mesh sieve to obtain the modified coal gangue biochar composite adsorbent material.

[0063] Example 2: A method for preparing a modified coal gangue biochar composite adsorbent material, comprising the following steps:

[0064] S1. Alkali fusion-acid hydrolysis activation of coal gangue: 20g of coal gangue with SiO2 content of 52wt% and Al2O3 content of 24wt% was crushed to a particle size of ≤0.15mm, mixed evenly with 24g of anhydrous Na2CO3, placed in a muffle furnace, heated to 825℃ at a heating rate of 10℃ / min, and calcined for 3.5h to obtain alkali fused clinker. After grinding the alkali fused clinker, it was mixed with 1.2mol / L HCl solution at a liquid-solid ratio of 25mL / g, and acid hydrolyzed at 70℃ and 300rpm for 3h. After filtration, the pH of the filtrate was adjusted to 3 with 0.5mol / L NaOH solution to obtain a silicon-aluminum precursor solution.

[0065] S2. Multi-scale functionalization of biomass feedstocks:

[0066] S2.1. Raw material grading and screening and targeted deashing: 30g of bamboo powder was dried to constant weight at 70℃, pulverized and then passed through 0.5mm, 0.15mm and 0.075mm sieves in sequence to obtain 9.23g of coarse powder with a particle size of 0.15-0.5mm, 11.54g of medium powder with a particle size of 0.075-0.15mm and 9.23g of fine powder with a particle size ≤0.075mm. The three powders were mixed with deionized water at a liquid-solid ratio of 12mL / g, and 11.25g of 4wt% acetic acid aqueous solution was added. The mixture was soaked at 70℃ and 300rpm for 2h, filtered, washed 4 times with 65℃ deionized water, and then washed with room temperature deionized water until the filtrate was neutral. The mixture was then vacuum dried at 70℃ for 9h to obtain deashed biomass.

[0067] S2.2. Chemical pretreatment and low-temperature preactivation: 24g of deashed biomass was mixed with 5wt% H2O2 aqueous solution at a liquid-solid ratio of 12mL / g and oxidized at 60℃ water bath and 300rpm for 2h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed with deionized water until the filtrate was neutral, and vacuum dried at 70℃ for 9h to obtain oxidized pretreated biomass. The oxidized pretreated biomass was ground and mixed with 1.5wt% KOH aqueous solution at a liquid-solid ratio of 15mL / g and impregnated at room temperature and 150rpm for 3.5h. After filtration, the mixture was first vacuum dried at 90℃ for 6h and then vacuum dried at 105℃ for 9h to obtain the preactivated precursor.

[0068] S2.3. Hydrothermal carbonization and pore shaping: 20g of the pre-activated precursor obtained in S2.2 was crushed to ≤0.3mm, mixed with deionized water at a liquid-to-solid ratio of 12mL / g, 0.8g of oxalic acid was added, and the mixture was transferred to a hydrothermal reactor. The reaction was carried out at 210℃ for 9h. After the reaction was completed, the mixture was cooled to room temperature, and the pH was first neutralized to 6.5 with 0.3mol / L NaOH solution. The mixture was then filtered, washed with deionized water until the filtrate was neutral, and vacuum dried at 70℃ for 9h to obtain hydrothermal carbon microspheres.

[0069] S2.4. Surface in-situ phosphorus modification: 12g of hydrothermal carbon microspheres obtained in S2.3 were mixed with deionized water at a liquid-solid ratio of 12mL / g, 0.18g of ammonium dihydrogen phosphate was added, and the mixture was immersed at 75℃ and 300rpm for 2.5h. After filtration, the microspheres were washed three times with deionized water at 65℃, and then washed with deionized water at room temperature until the filtrate was neutral. The microspheres were then vacuum dried at 70℃ for 9h to obtain phosphorus-modified hydrothermal carbon microspheres.

[0070] S2.5 Acid washing-alkali passivation treatment: 10g of phosphorus-modified hydrothermal carbon microspheres obtained from S2.4 were washed three times with hot water, four times with 0.25mol / L dilute HCl, and washed with deionized water until the filtrate was neutral to obtain acid-washed hydrothermal carbon microparticles. The acid-washed hydrothermal carbon microparticles were mixed with 0.12mol / L Na2CO3 aqueous solution at a liquid-solid ratio of 15mL / g and treated at 55℃ and 250rpm for 1h. After filtration, the microspheres were washed with deionized water until the filtrate was neutral and dried under vacuum at 70℃ for 9h to obtain alkali passivated hydrothermal carbon microparticles.

[0071] S2.6. Silane pre-anchoring: 8g of alkali passivated hydrothermal carbon microparticles obtained in S2.5 were mixed with 75wt% ethanol aqueous solution at a liquid-solid ratio of 15mL / g, 0.32g of γ-glycidyl etheroxypropyltrimethoxysilane was added, and 0.5mol / L acetic acid was added dropwise to adjust the pH to 4.5. The mixture was refluxed at 50℃ and 250rpm for 3h, filtered, washed 3 times with anhydrous ethanol, and then washed with deionized water until the filtrate was neutral. The mixture was then vacuum dried at 70℃ for 9h to obtain functionalized hydrothermal carbon microparticles.

[0072] S3. In-situ polycondensation: 16g of the silicon-aluminum precursor solution obtained in S1 was mixed with 8g of the functionalized hydrothermal carbon microparticles obtained in step S2. 0.8g of tannic acid and 0.028g of the composite polycondensation catalyst (NaOH and trisodium citrate mass ratio 1:1) were added and transferred to a hydrothermal reactor. The mixture was reacted at 145℃ for 9h. After the reaction was completed, the mixture was cooled, filtered, and washed with deionized water until the filtrate was neutral. The filtrate was then vacuum dried at 70℃ for 9h to obtain the hybrid network precursor.

[0073] S4. Surface aldehyde-based oxidation: 10 g of the hybrid network precursor obtained in S3 was mixed with 90 wt% ethanol aqueous solution at a liquid-solid ratio of 22 mL / g, 3.5 g of sodium periodate was added, and the mixture was oxidized at room temperature, in the dark, at 250 rpm for 9 h. After the reaction was completed, 2 g of ethylene glycol was added, and the mixture was stirred in the dark for another 0.8 h. The mixture was filtered, washed three times with anhydrous ethanol, and then washed with deionized water until the filtrate was neutral. The mixture was then vacuum dried at 45 °C for 9 h to obtain the aldehyde-based hybrid network precursor.

[0074] S5. Schiff base chelation functionalization and metal center loading: 8g of the aldehyde-modified hybrid network precursor obtained in S4 was mixed with anhydrous ethanol at a liquid-to-solid ratio of 22mL / g, and 0.8g of diethylenetriamine was added. The mixture was refluxed at 65℃ and 250rpm for 6h. After the reaction was completed, the mixture was cooled to room temperature, filtered, and washed three times with anhydrous ethanol to obtain the imino-modified hybrid network precursor. 7g of the imino-modified hybrid network precursor was mixed with deionized water at a liquid-to-solid ratio of 15mL / g, and 1g of 0.1mol / L FeCl3 solution was added. The pH was adjusted to 7 with 0.5mol / L ammonia water, and the mixture was complexed at 55℃ and 250rpm for 3.5h. After the complexation reaction was completed, the mixture was cooled to room temperature, filtered, washed three times with anhydrous ethanol, and then washed with deionized water until the filtrate was neutral. The filtrate was dried under vacuum at 60℃ for 9h and ground through a 150-mesh sieve to obtain the modified coal gangue biochar composite adsorbent material.

[0075] Example 3: A method for preparing a modified coal gangue biochar composite adsorbent material, comprising the following steps:

[0076] S1. Alkali fusion-acid hydrolysis activation of coal gangue: 20g of coal gangue with SiO2 content of 60wt% and Al2O3 content of 30wt% was crushed to a particle size of ≤0.15mm, mixed evenly with 24g of anhydrous Na2CO3, placed in a muffle furnace, heated to 850℃ at a heating rate of 12℃ / min, and calcined for 3h to obtain alkali fused clinker. After grinding the alkali fused clinker, it was mixed with 1.5mol / L HCl solution at a liquid-solid ratio of 30mL / g, and acid hydrolyzed at 80℃ and 400rpm for 2h. After filtration, the pH of the filtrate was adjusted to 4 with 1mol / L NaOH solution to obtain a silicon-aluminum precursor solution.

[0077] S2. Multi-scale functionalization of biomass feedstocks:

[0078] S2.1. Raw material grading and screening and targeted deashing: 30g of rice husks were dried to constant weight at 80℃, pulverized and then passed through 0.5mm, 0.15mm and 0.075mm sieves in sequence to obtain 6.67g of coarse powder with a particle size of 0.15-0.5mm, 13.33g of medium powder with a particle size of 0.075-0.15mm and 10g of fine powder with a particle size ≤0.075mm. The three powders were mixed with deionized water at a liquid-solid ratio of 15mL / g, and 12g of 5wt% acetic acid aqueous solution was added. The mixture was soaked at 80℃ and 400rpm for 1h, filtered, washed 3 times with 70℃ deionized water, and then washed with room temperature deionized water until the filtrate was neutral. The mixture was then vacuum dried at 80℃ for 6h to obtain deashed biomass.

[0079] S2.2. Chemical pretreatment and low-temperature preactivation: 24g of deashed biomass was mixed with 6wt% H2O2 aqueous solution at a liquid-solid ratio of 15mL / g and oxidized at 70℃ water bath and 400rpm for 1h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed with deionized water until the filtrate was neutral, and vacuum dried at 80℃ for 6h to obtain oxidized pretreated biomass. The oxidized pretreated biomass was ground and mixed with 2wt% KOH aqueous solution at a liquid-solid ratio of 20mL / g and impregnated at room temperature and 200rpm for 3h. After filtration, the mixture was first vacuum dried at 100℃ for 4h and then vacuum dried at 110℃ for 6h to obtain the preactivated precursor.

[0080] S2.3. Hydrothermal carbonization and pore shaping: 20g of the pre-activated precursor obtained in S2.2 was crushed to ≤0.3mm, mixed with deionized water at a liquid-to-solid ratio of 15mL / g, 1g of oxalic acid was added, and the mixture was transferred to a hydrothermal reactor. The reaction was carried out at 220℃ for 8h. After the reaction was completed, the mixture was cooled to room temperature, and the pH was first neutralized to 7 with 0.5mol / L NaOH solution. The mixture was then filtered, washed with deionized water until the filtrate was neutral, and vacuum dried at 80℃ for 6h to obtain hydrothermal carbon microspheres.

[0081] S2.4. Surface in-situ phosphorus modification: 12g of hydrothermal carbon microspheres obtained in S2.3 were mixed with deionized water at a liquid-solid ratio of 15mL / g, and 0.24g of ammonium dihydrogen phosphate was added. The mixture was soaked at 80℃ and 400rpm for 2h, filtered, washed 3 times with 70℃ deionized water, and then washed with room temperature deionized water until the filtrate was neutral. The mixture was then vacuum dried at 80℃ for 6h to obtain phosphorus-modified hydrothermal carbon microspheres.

[0082] S2.5 Acid washing-alkali passivation treatment: 10g of phosphorus-modified hydrothermal carbon microspheres obtained from S2.4 were washed three times with hot water, three times with 0.3mol / L dilute HCl, and washed with deionized water until the filtrate was neutral to obtain acid-washed hydrothermal carbon microparticles. The acid-washed hydrothermal carbon microparticles were mixed with 0.15mol / L Na2CO3 aqueous solution at a liquid-solid ratio of 20mL / g and treated at 60℃ and 300rpm for 0.5h. After filtration, the microspheres were washed with deionized water until the filtrate was neutral and dried under vacuum at 80℃ for 6h to obtain alkali passivated hydrothermal carbon microparticles.

[0083] S2.6. Silane pre-anchoring: 8g of alkali passivated hydrothermal carbon microparticles obtained in S2.5 were mixed with 75wt% ethanol aqueous solution at a liquid-solid ratio of 20mL / g, 0.4g of γ-glycidyl etheroxypropyltrimethoxysilane was added, and 1mol / L acetic acid was added dropwise to adjust the pH to 4. The mixture was refluxed at 60℃ and 300rpm for 2h, filtered, washed 3 times with anhydrous ethanol, and then washed with deionized water until the filtrate was neutral. The mixture was then vacuum dried at 80℃ for 6h to obtain functionalized hydrothermal carbon microparticles.

[0084] S3. In-situ polycondensation: 24g of the silicon-aluminum precursor solution obtained in S1 was mixed with 8g of the functionalized hydrothermal carbon microparticles obtained in step S2. 1.2g of tannic acid and 0.04g of the composite polycondensation catalyst (NaOH and trisodium citrate mass ratio 1:1) were added and transferred to a hydrothermal reactor. The mixture was reacted at 150℃ for 8h. After the reaction was completed, the mixture was cooled, filtered, and washed with deionized water until the filtrate was neutral. The filtrate was then vacuum dried at 80℃ for 6h to obtain the hybrid network precursor.

[0085] S4. Surface aldehyde-based oxidation: 10 g of the hybrid network precursor obtained in S3 was mixed with 90 wt% ethanol aqueous solution at a liquid-solid ratio of 30 mL / g, 4 g of sodium periodate was added, and the mixture was oxidized at 300 rpm for 8 h at room temperature in the dark. After the reaction was completed, 2.5 g of ethylene glycol was added, and the mixture was stirred in the dark for another 0.5 h. The mixture was filtered, washed three times with anhydrous ethanol, and then washed with deionized water until the filtrate was neutral. The mixture was then vacuum dried at 50 °C for 6 h to obtain the aldehyde-based hybrid network precursor.

[0086] S5. Schiff base chelation functionalization and metal center loading: 8g of the aldehyde-modified hybrid network precursor obtained in S4 was mixed with anhydrous ethanol at a liquid-to-solid ratio of 30mL / g, and 1.2g of diethylenetriamine was added. The mixture was refluxed at 70℃ and 300rpm for 4h. After the reaction was completed, the mixture was cooled to room temperature, filtered, and washed three times with anhydrous ethanol to obtain the imino-modified hybrid network precursor. 7g of the imino-modified hybrid network precursor was mixed with deionized water at a liquid-to-solid ratio of 20mL / g, and 1.4g of 0.1mol / L FeCl3 solution was added. The pH was adjusted to 7.5 with 1mol / L ammonia water, and the mixture was complexed at 60℃ and 300rpm for 3h. After the complexation reaction was completed, the mixture was cooled to room temperature, filtered, washed three times with anhydrous ethanol, and then washed with deionized water until the filtrate was neutral. The filtrate was vacuum dried at 70℃ for 6h and ground through a 200-mesh sieve to obtain the modified coal gangue biochar composite adsorbent material.

[0087] Comparative Example 1: Based on Example 2, the difference is that the alkaline fusion-acid hydrolysis activation of coal gangue is omitted, and direct physical mixing is used. The specific preparation method is as follows:

[0088] S1. Preparation of coal gangue slurry: 20g of coal gangue with SiO2 content of 52wt% and Al2O3 content of 24wt% was directly crushed to a particle size of ≤0.15mm, and mixed with deionized water at a liquid-solid ratio of 25mL / g (i.e., 500mL). The mixture was stirred at 70℃ and 300rpm for 3h, and then filtered to obtain coal gangue slurry.

[0089] S2. Same as Example 2;

[0090] S3. Physical mixing and compounding: The coal gangue slurry obtained in S1 (20g based on solid content) is mixed with 10g of functionalized hydrothermal carbon microparticles obtained in S2. The mixture is stirred at room temperature and 300rpm for 6h, filtered, and then washed with deionized water until the filtrate is neutral. The mixture is then vacuum dried at 70℃ for 9h to obtain the physical mixing precursor.

[0091] S4-S5. Same as Example 2.

[0092] Comparative Example 2: Based on Example 2, the difference is that the biomass grading and screening and targeted deashing steps are omitted. The specific preparation method is as follows:

[0093] S1. Same as Example 2;

[0094] S2. Pretreatment and multi-scale functionalization of biomass feedstocks:

[0095] S2.1. Biomass pretreatment: Take 30g of bamboo powder, dry it at 70℃ to constant weight, and directly pulverize it to a particle size ≤0.15mm;

[0096] S2.2-S2.6. Same as Example 2;

[0097] S3-S5. Same as Example 2.

[0098] Comparative Example 3: Based on Example 2, the difference is that the hydrothermal carbonization step is omitted, and direct pyrolysis carbonization is performed. The specific preparation method is as follows:

[0099] S1. Same as Example 2;

[0100] S2. Pretreatment and multi-scale functionalization of biomass feedstocks:

[0101] S2.1-S2.2. Same as Example 2;

[0102] S2.3. Direct pyrolysis carbonization: 20g of pre-activated precursor was placed in a tube furnace and heated to 600℃ at 5℃ / min under N2 protection. After pyrolysis for 2h, the precursor was cooled and ground to ≤0.3mm to obtain pyrolytic carbon particles.

[0103] S2.4-S2.6. Same as Example 2;

[0104] S3-S5. Same as Example 2.

[0105] Comparative Example 4: Based on Example 2, the difference is that the crosslinking agent tannic acid is omitted in the in-situ polycondensation composite step. The specific preparation method is as follows:

[0106] S1-S2. Same as Example 2;

[0107] S3. In-situ polycondensation: 16g of the silicon-aluminum precursor solution obtained in S1 was mixed with 8g of the functionalized hydrothermal carbon microparticles obtained in step S2. 0.028g of the composite polycondensation catalyst (NaOH and trisodium citrate mass ratio 1:1) was added and transferred to a hydrothermal reactor. The mixture was reacted at 145℃ for 9h. After the reaction was completed, the mixture was cooled, filtered, and washed with deionized water until the filtrate was neutral. The filtrate was then vacuum dried at 70℃ for 9h to obtain the hybrid network precursor.

[0108] S4-S5. Same as Example 2.

[0109] Comparative Example 5: Based on Example 2, the difference is that the surface aldehyde methylation step S4 is omitted, and the hybrid network precursor obtained in step S3 is directly reacted in step S5. The rest is the same as in Example 2.

[0110] Comparative Example 6: Based on Example 2, the difference is that the diethylenetriamine step in the Schiff base functionalization process is omitted. The specific preparation method is as follows:

[0111] S1-S4. Same as in Example 2;

[0112] S5. Metal-centered loading: 7g of the aldehyde-modified hybrid network precursor obtained in S4 was mixed with deionized water at a liquid-to-solid ratio of 15mL / g. 1g of 0.1mol / L FeCl3 solution was added, and the pH was adjusted to 7 with 0.5mol / L ammonia. The complexation reaction was carried out at 55℃ and 250rpm for 3.5h. After the complexation reaction was completed, the mixture was cooled to room temperature, filtered, washed three times with anhydrous ethanol, and then washed with deionized water until the filtrate was neutral. The mixture was then vacuum dried at 60℃ for 9h and ground through a 150-mesh sieve to obtain the modified coal gangue biochar composite adsorbent material.

[0113] Comparative Example 7: Based on Example 2, the difference is that the FeCl3 metal center loading is omitted, and the specific preparation method is as follows:

[0114] S1-S4. Same as in Example 2;

[0115] S5. Schiff base chelation functionalization: 8g of the aldehyde-modified hybrid network precursor obtained in S4 was mixed with anhydrous ethanol at a liquid-to-solid ratio of 22mL / g, and 0.8g of diethylenetriamine was added. The mixture was refluxed at 65℃ and 250rpm for 6h. After the reaction was completed, the mixture was cooled to room temperature, filtered, and washed three times with anhydrous ethanol to obtain the imino-modified hybrid network precursor. The precursor was directly vacuum dried at 60℃ for 9h and ground through a 150-mesh sieve to obtain the modified coal gangue biochar composite adsorbent material.

[0116] Performance testing:

[0117] 1. Single-component adsorption capacity test: Accurately weigh 0.05 g of each adsorbent material prepared in each example and comparative example, place them in 250 mL Erlenmeyer flasks, and add 100 mL of solution containing heavy metal ions (Pb). 2+ A single-component simulated wastewater solution consisting of inorganic anionic pollutants (phosphate solution) and organic micropollutants (p-nitrophenol solution); among which, Pb 2+ The solutions were prepared using lead nitrate with an initial concentration of 200 mg / L; the phosphate solution was prepared using potassium dihydrogen phosphate with an initial concentration of 50 mg / L (calculated as phosphorus); and the p-nitrophenol solution had an initial concentration of 100 mg / L. The initial pH of all solutions was adjusted to 6.0 ± 0.1. The conical flasks were placed in a constant-temperature shaker and shaken at 25℃ and 200 rpm for adsorption. Samples were taken at 5 min, 6 h, and 24 h. The supernatant was filtered through a 0.45 μm filter membrane, and the concentration of residual contaminants in the solution was determined using a UV-Vis spectrophotometer. Among these, Pb... 2+ The concentrations were determined using the dithizone spectrophotometric method at a wavelength of 510 nm, the phosphate concentrations were determined using the molybdenum-antimony spectrophotometric method at a wavelength of 700 nm, and the p-nitrophenol concentrations were directly determined at a wavelength of 400 nm; the adsorption capacity was calculated using the formula q. e (mg / g) = (C0 - C) e)×V / m, where C0 and C e The values ​​represent the pollutant concentrations in the solution before and after adsorption (mg / L), respectively; V represents the solution volume (L); and m represents the mass of the adsorbent material (g).

[0118] 2. Multi-component adsorption capacity test: Preparation of Pb-containing... 2+ A mixed simulated wastewater containing three pollutants—(100 mg / L), phosphate (25 mg / L as phosphorus), and p-nitrophenol (50 mg / L)—was subjected to adsorption by shaking at 25°C and 200 rpm for 24 h. The adsorption capacity retention rate of each material for each pollutant in the multi-pollutant coexistence system was then determined.

[0119] 3. Cyclic Regeneration Performance Test: After adsorption for 24 hours, the adsorbent materials of each example and comparative example were filtered and collected. A three-step desorption and regeneration method was used: elution with 0.1 mol / L HCl solution for 2 hours, elution with 0.1 mol / L NaOH solution for 2 hours, washing with deionized water until neutral, elution with 0.01 mol / L EDTA-2Na solution for 1 hour, washing with deionized water until neutral, and vacuum drying at 60℃ to constant weight to obtain the regenerated material. Single-component adsorption experiments were then performed again. This adsorption-desorption-regeneration cycle was repeated 5 and 10 times. The adsorption capacity after each cycle was measured, and the cyclic regeneration adsorption capacity retention rate of each material was calculated (with the first adsorption capacity as 100%).

[0120] Table 1. Results of single-component adsorption capacity test

[0121]

[0122] As shown in Table 1, all three examples exhibited excellent single-component adsorption capacity for the three pollutants. After 24 hours of adsorption, the adsorption capacity for Pb was [missing information]. 2+ The adsorption capacity is 187.3-203.5 mg / g, the adsorption capacity for phosphate is 42.6-46.8 mg / g, and the adsorption capacity for p-nitrophenol is 88.4-95.7 mg / g.

[0123] Comparative Example 1: Coal gangue, without alkali fusion-acid hydrolysis activation and directly physically mixed, showed the largest decrease in adsorption capacity for each pollutant, with Pb being the most significant. 2+ The adsorption capacity was only 82.5 mg / g, and the phosphate adsorption capacity was only 15.3 mg / g, indicating that alkali fusion-acid hydrolysis activation is the fundamental prerequisite for releasing the active silicon-aluminum components and constructing a chemically bonded hybrid network. Comparative Example 2 omitted fractional screening and acetic acid deashing, and Comparative Example 3 used pyrolysis carbonization instead of hydrothermal carbonization. Pb 2+The adsorption capacities were 112.4 and 124.6 mg / g, respectively, indicating that staged deashing and hydrothermal carbonization are crucial for pore development and active site density. In Comparative Example 4, omitting the tannic acid crosslinking agent, the phosphate adsorption capacity decreased to 22.4 mg / g. The lack of the crosslinking agent led to separation of the inorganic and organic phases, with particularly significant impairment in anion adsorption. In Comparative Example 5, omitting sodium periodate oxidation aldehyde oxidization, Pb... 2+ The adsorption capacity was 131.5 mg / g, and for p-nitrophenol it was 80.3 mg / g. The absence of aldehyde grouping severely impaired cation adsorption, but p-nitrophenol adsorption primarily relied on the π-π stacking of biochar itself and was less affected by aldehyde grouping. Comparative Example 6 omitted diethylenetriamine Schiff base grafting, Pb 2+ The adsorption capacity was only 98.6 mg / g. Comparative Example 7 omitted the FeCl3 metal center loading, and Pb... 2+ The adsorption capacity was only 76.3 mg / g, indicating that imino chelation sites and iron species play a key role in cation adsorption.

[0124] Table 2. Results of 24-hour adsorption capacity retention test for multi-components

[0125]

[0126] As shown in Table 2, the adsorption capacity retention rates of the three pollutants in the three examples were all maintained between 79.3% and 80.3%, which were highly consistent with each other. This indicates that the various types of active sites have clear division of labor, low competitive interference, and excellent synergistic removal ability.

[0127] Comparative Example 1: Coal gangue was directly physically mixed without alkali fusion-acid hydrolysis activation, Pb 2+ The lowest adsorption capacity retention rate was only 62.2%, indicating a lack of chemical bonding networks in the physically mixed materials, resulting in severely insufficient specific adsorption under competitive conditions. Comparative Example 2, omitting graded screening and acetic acid deashing, showed low adsorption capacity retention rates (64.8-69.9%) for all three pollutants, with ash impurities occupying pores and exacerbating site competition. Comparative Example 3, replacing hydrothermal carbonization with pyrolysis carbonization, maintained adsorption capacity retention rates of 67.1-73.4% for the three pollutants. While pyrolysis carbonization can form a certain pore structure, its surface functional group types and densities are inferior to hydrothermal carbonization, resulting in poor pore regularity and reduced selective adsorption capacity under competitive conditions. Comparative Example 4, omitting the tannic acid crosslinking agent, showed a phosphate adsorption capacity retention rate of only 60.3%. The lack of crosslinking agent led to the separation of the silica-alumina inorganic phase and the organic carbon phase, severely inhibiting inorganic active sites in a competitive environment, particularly impacting phosphate adsorption dependent on inorganic sites. Comparative Example 5, omitting sodium periodate oxidation aldehyde conversion, achieved a p-nitrophenol adsorption capacity retention rate of 78.1%, but Pb... 2+The adsorption capacity retention rate was only 71.0%, as the lack of imine chelating sites in the competing environment made cation adsorption more susceptible to interference. Comparative Example 6 omitted diethylenetriamine Schiff base grafting and Comparative Example 7 omitted FeCl3 metal center loading, and the adsorption capacity retention rates of the three pollutants were all low (64.7-72.9%). In the competing environment, the adsorption of the three types of pollutants were affected to varying degrees, and the overall anti-interference ability was comprehensively deteriorated.

[0128] Table 3. Results of single-component cyclic regeneration adsorption capacity retention test

[0129]

[0130] As shown in Table 3, all three embodiments exhibit excellent recycling performance. After 5 cycles, the adsorption capacity retention rate of the three pollutants is higher than 86%, and after 10 cycles, the adsorption capacity retention rate of the three pollutants is still higher than 80%. This is attributed to the organic-inorganic interpenetrating hybrid network structure constructed in this invention and the spatial confinement stabilization effect of the iron center.

[0131] Comparative Example 1: Coal gangue without alkali fusion-acid hydrolysis activation, directly physically mixed, after 10 cycles, Pb 2+ The adsorption capacity retention rate was only 35.6%, indicating the most severe degradation, due to the loss of inorganic particles and pore blockage caused by the lack of chemical bonding. Comparative Example 2, omitting graded screening and acetic acid deashing, saw its adsorption capacity retention rate for the three pollutants drop to 50.3-58.4% after 10 cycles. Residual ash slowly dissolved during the regeneration process, leading to gradual collapse of the pore structure and poor cycle stability. Comparative Example 3, replacing hydrothermal carbonization with pyrolysis carbonization, saw its adsorption capacity retention rate for the three pollutants reach 55.8-63.2% after 10 cycles, but with low surface functional group density and easy micropore collapse. Comparative Example 4, omitting tannic acid crosslinking agent, showed that after 10 cycles, Pb... 2+ The adsorption capacity retention dropped to 49.3%. In the absence of a cross-linking agent, phase separation led to a significant loss of inorganic active components. Comparative Example 5, which omitted sodium periodate oxidation for aldehyde alkylation, showed that after 10 cycles, Pb... 2+ The adsorption capacity retention rate was 62.4%, and the non-covalently grafted amine groups were easily eluted. Comparative Example 6, omitting the diethylenetriamine Schiff base grafting, showed an adsorption capacity retention rate of 52.6-56.8% for the three pollutants after 10 cycles, lacking imino sites and with easily deactivated phenolic hydroxyl groups. Comparative Example 7, omitting the FeCl3 metal center loading, showed that after 10 cycles, Pb... 2+ The adsorption capacity retention rate was only 41.5%, and the Pb adsorbed at the weak complexation sites... 2+ It is difficult to wash off, and the residue accumulates and blocks the active site.

[0132] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.

Claims

1. A method for preparing a modified coal gangue biochar composite adsorbent material, characterized in that, Includes the following steps: S1. Alkali fusion-acid hydrolysis activation of coal gangue: Coal gangue is crushed to a particle size ≤0.15mm, mixed evenly with anhydrous Na2CO3, placed in a muffle furnace, heated to 800-850℃ at a heating rate of 8-12℃ / min, and calcined for 3-4h to obtain alkali fused clinker. After grinding the alkali fused clinker, it is mixed with 1-1.5mol / L HCl solution at a liquid-solid ratio of 20-30mL / g, and acid hydrolyzed at 60-80℃ and 200-400rpm for 2-4h. After filtration, the pH of the filtrate is adjusted to 2-4 with 0.1-1mol / L NaOH solution to obtain a silicon-aluminum precursor solution. S2. Multi-scale functionalization of biomass feedstocks: S2.

1. Raw material grading and screening and targeted deashing: The biomass raw material is dried to constant weight at 60-80℃, pulverized and then passed through 0.5mm, 0.15mm and 0.075mm sieves to obtain coarse powder, medium powder and fine powder. The three powders are mixed with deionized water at a liquid-solid ratio of 8-15mL / g, and 3-5wt% acetic acid aqueous solution is added. The mixture is soaked at 60-80℃ and 200-400rpm for 1-3h, filtered, washed 3-5 times with deionized water at 60-70℃, and then washed with deionized water at room temperature until the filtrate is neutral. The mixture is then vacuum dried at 60-80℃ for 6-12h to obtain deashed biomass. S2.

2. Chemical pretreatment and low-temperature preactivation: Deashed biomass is mixed with 4-6wt% H2O2 aqueous solution at a liquid-solid ratio of 10-15 mL / g, oxidized in a water bath at 50-70℃ and 200-400 rpm for 1-3 h. After the reaction is completed, it is cooled to room temperature, filtered, washed with deionized water until the filtrate is neutral, and vacuum dried at 60-80℃ for 6-12 h to obtain oxidized pretreated biomass. The oxidized pretreated biomass is ground and mixed with 1-2wt% KOH aqueous solution at a liquid-solid ratio of 10-20 mL / g, impregnated at room temperature and 100-200 rpm for 3-4 h, filtered, vacuum dried at 80-100℃ for 4-8 h, and then vacuum dried at 100-110℃ for 6-12 h to obtain the preactivated precursor. S2.

3. Hydrothermal carbonization and pore shaping: The pre-activated precursor obtained in S2.2 was pulverized to ≤0.3 mm, mixed with deionized water at a liquid-to-solid ratio of 10-15 mL / g, oxalic acid was added, and the mixture was transferred to a hydrothermal reactor. The reaction was carried out at 200-220℃ for 8-10 h. After the reaction was completed, the mixture was cooled to room temperature, and the pH was neutralized to 6-7 with 0.1-0.5 mol / L NaOH solution. The mixture was filtered, and then washed with deionized water until the filtrate was neutral. The filtrate was then vacuum dried at 60-80℃ for 6-12 h to obtain hydrothermal carbon microspheres. S2.

4. Surface in-situ phosphorus modification: The hydrothermal carbon microspheres obtained in S2.3 were mixed with deionized water at a liquid-solid ratio of 8-15 mL / g, and ammonium dihydrogen phosphate was added. The mixture was immersed at 70-80℃ and 200-400 rpm for 2-3 hours, filtered, washed 2-3 times with deionized water at 60-70℃, and then washed with deionized water at room temperature until the filtrate was neutral. The mixture was then vacuum dried at 60-80℃ for 6-12 hours to obtain phosphorus-modified hydrothermal carbon microspheres. S2.5 Acid washing-alkali passivation treatment: The phosphorus-modified hydrothermal carbon microspheres obtained in S2.4 are washed with hot water 2-3 times, acid washed with 0.2-0.3 mol / L dilute HCl 3-5 times, and washed with deionized water until the filtrate is neutral to obtain acid-washed hydrothermal carbon microparticles. The acid-washed hydrothermal carbon microparticles are mixed with 0.1-0.15 mol / L Na2CO3 aqueous solution at a liquid-solid ratio of 10-20 mL / g and treated at 50-60℃ and 200-300 rpm for 0.5-1.5 h. After filtration, the microspheres are washed with deionized water until the filtrate is neutral and vacuum dried at 60-80℃ for 6-12 h to obtain alkali passivated hydrothermal carbon microparticles. S2.

6. Silane pre-anchoring: The alkaline passivated hydrothermal carbon microparticles obtained in S2.5 were mixed with 75wt% ethanol aqueous solution at a liquid-solid ratio of 10-20 mL / g, γ-glycidoxypropyltrimethoxysilane was added, and 0.1-1 mol / L acetic acid was added dropwise to adjust the pH to 4-5. The mixture was refluxed at 40-60℃ and 200-300 rpm for 2-4 h, filtered, washed 2-3 times with anhydrous ethanol, and then washed with deionized water until the filtrate was neutral. The mixture was then vacuum dried at 60-80℃ for 6-12 h to obtain functionalized hydrothermal carbon microparticles. S3. In-situ polycondensation: The silicon-aluminum precursor solution obtained in S1 is mixed with the functionalized hydrothermal carbon microparticles obtained in step S2. A crosslinking agent and a composite polycondensation catalyst are added, and the mixture is transferred to a hydrothermal reactor. The reaction is carried out at 140-150℃ for 8-10 hours. After the reaction is completed, the mixture is cooled, filtered, and washed with deionized water until the filtrate is neutral. The mixture is then vacuum dried at 60-80℃ for 6-12 hours to obtain the hybrid network precursor. S4. Surface aldehyde-based oxidation: The hybrid network precursor obtained in S3 was mixed with 90wt% ethanol aqueous solution at a liquid-solid ratio of 15-30 mL / g, sodium periodate was added, and the mixture was oxidized at room temperature, in the dark, at 200-300 rpm for 8-10 h. After the reaction was completed, ethylene glycol was added, and the mixture was stirred in the dark for 0.5-1 h. The mixture was filtered, washed 2-3 times with anhydrous ethanol, and then washed with deionized water until the filtrate was neutral. The mixture was then vacuum dried at 40-50℃ for 6-12 h to obtain the aldehyde-based hybrid network precursor. S5. Schiff base chelation functionalization and metal center loading: The aldehyde-modified hybrid network precursor obtained in S4 was mixed with anhydrous ethanol at a liquid-to-solid ratio of 15-30 mL / g, and diethylenetriamine was added. The mixture was refluxed at 60-70℃ and 200-300 rpm for 4-8 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, and washed 2-3 times with anhydrous ethanol to obtain the imino-modified hybrid network precursor. The imino-modified hybrid network precursor was mixed with deionized water at a liquid-to-solid ratio of 10-20 mL / g, and 0.1 mol / L... FeCl3 solution was used to adjust the pH to 6.5-7.5 with 0.1-1 mol / L ammonia water. The complexation reaction was carried out at 50-60℃ and 200-300 rpm for 3-4 hours. After the complexation reaction was completed, the solution was cooled to room temperature, filtered, washed 2-3 times with anhydrous ethanol, and then washed with deionized water until the filtrate was neutral. The solution was then vacuum dried at 50-70℃ for 6-12 hours and ground through a 100-200 mesh sieve to obtain the modified coal gangue biochar composite adsorbent material.

2. The preparation method of the modified coal gangue biochar composite adsorbent material according to claim 1, characterized in that, The coal gangue in S1 contains 45-60 wt% SiO2 and 18-30 wt% Al2O3; the mass ratio of the coal gangue to anhydrous Na2CO3 is 1:0.8-1.

2.

3. The preparation method of the modified coal gangue biochar composite adsorbent material according to claim 1, characterized in that, The biomass raw material mentioned in S2.1 is one or more of straw, bamboo powder, reed powder, rice husk, and sawdust; the coarse powder has a particle size of 0.15-0.5 mm, the medium powder has a particle size of 0.075-0.15 mm, and the fine powder has a particle size ≤0.075 mm, with a mass ratio of 1:0.5-2:0.5-1.5; the amount of acetic acid in the acetic acid aqueous solution is 1-2% of the total mass of the coarse, medium, and fine powders; the amount of oxalic acid mentioned in S2.3 is 3-5% of the mass of the pre-activated precursor; the amount of ammonium dihydrogen phosphate added in S2.4 is 1-2% of the mass of the hydrothermal carbon microspheres; and the amount of γ-glycidyl etheroxypropyltrimethoxysilane mentioned in S2.6 is 3-5% of the mass of the alkali-passivated hydrothermal carbon microparticles.

4. The preparation method of the modified coal gangue biochar composite adsorbent material according to claim 1, characterized in that, The mass ratio of the silicon-aluminum precursor solution to the functionalized hydrothermal carbon microparticles in S3 is 1-3:1; the crosslinking agent is tannic acid, and the amount used is 5-15% of the mass of the functionalized hydrothermal carbon microparticles; the composite polycondensation catalyst is a mixture of NaOH and trisodium citrate in a mass ratio of 1:1, and the amount of the composite polycondensation catalyst used is 0.2-0.5% of the mass of the functionalized hydrothermal carbon microparticles.

5. The preparation method of the modified coal gangue biochar composite adsorbent material according to claim 1, characterized in that, The amount of sodium periodate used in S4 is 30-40% of the mass of the hybrid network precursor; the amount of ethylene glycol used is 15-25% of the mass of the hybrid network precursor.

6. The method for preparing a modified coal gangue biochar composite adsorbent material according to claim 1, characterized in that, The amount of diethylenetriamine used in S5 is 5-15% of the mass of the aldehyde-modified hybrid network precursor; the amount of the 0.1 mol / L FeCl3 solution used is 10-20% of the mass of the imino-modified hybrid network precursor.

7. A modified coal gangue biochar composite adsorbent material, characterized in that, It is prepared by the preparation method described in any one of claims 1-6.

8. The application of the modified coal gangue biochar composite adsorbent material according to claim 7 in polluted water bodies, characterized in that, It can be used to treat heavy metal ions, anionic pollutants and organic micro-pollutants in polluted water bodies, and is especially suitable for the deep purification of complex water bodies such as wastewater from mines, electroplating, metallurgy, coal-fired power plants, coal gangue leachate, and domestic sewage.