A method for preparing thick titanium alloy plates by cross-phase region direct rolling based on EB casting
By using EB rectangular billets as raw materials and combining homogenized heating, β-zone billet opening, multi-pass reversible rolling, and finished product annealing in a two-stage direct rolling process, the problems of as-cast structure defects and temperature non-uniformity in the EB billet forging-free direct rolling process were solved, realizing the efficient preparation of wide and medium-thick titanium alloy plates, reducing production costs and improving the quality of finished products.
Patent Information
- Application Number
- CN202611206058.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-10
- Publication Date
- 2026-11-10
AI Technical Summary
The existing EB casting billet forging-free direct rolling process has problems such as as-cast microstructure defects, temperature inhomogeneity, deformation inhomogeneity and insufficient mill capacity when preparing wide and medium-thick titanium alloy plates. This results in surface cracks, uneven microstructure and properties and unstable plate shape in the finished plates, and also leads to high production costs.
Using EB rectangular billets as raw materials, a two-stage direct rolling process is employed, consisting of homogenized heating, β-zone billet opening, multi-pass reversible rolling, α+β-zone finishing rolling, and finished product annealing. Combined with stepped heating, temperature compensation, and deformation path optimization, the defects in the as-cast structure are gradually resolved, resulting in a refined bi-state structure.
While reducing production costs, it has produced wide and medium-thick titanium alloy plates with uniform structure, straight shape, and consistent performance, solving the problems of long process, high cost, and limited specifications in existing technologies.
Smart Images

Figure CN123059934A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of rolling technology, and in particular to a method for preparing thick titanium alloy plates by direct rolling in the cross-phase region based on EB casting. Background Technology
[0002] Titanium alloys, due to their low density, high specific strength, and excellent corrosion resistance, are widely used in aerospace, weaponry, marine engineering, and automotive lightweighting. Wide, medium-thick plates are an indispensable basic material for large structural components. The traditional manufacturing route for titanium alloy medium-thick plates is: vacuum arc remelting (VAR) to produce round ingots—multi-stage forging—multi-stage rolling. In recent years, electron beam cold hearth furnace (EB) melting technology has developed rapidly. Compared to the VAR process, the EB furnace can directly cast large-sized ingots with rectangular cross-sections in a water-cooled copper crystallizer, and it has excellent refining and impurity removal capabilities for recycled materials. Since the geometry of the EB rectangular ingot is close to that of a slab prototype, forging can be omitted, and it can directly enter the rolling process, i.e., "forging-free direct rolling."
[0003] However, the existing EB billet forging-free direct rolling process is still immature and presents many problems when applied to the production of wide and medium-thick plates. First, the as-cast microstructure of EB billets contains inherent defects such as coarse columnar crystals, micro-segregation, and a surface chilling layer. Improper heating and deformation control can easily lead to surface cracks, folds, and uneven microstructure and properties in the finished plate. Second, titanium alloys have low thermal conductivity and a narrow temperature window. The temperature drop rate at the edge and core of wide and thick billets differs significantly after exiting the furnace, often resulting in uneven deformation in the width direction and wavy or warped plate shapes. Third, the rolling deformation resistance is high under wide and medium-thick specifications, placing extremely high demands on mill capacity and plate shape control. Simply increasing the single-pass reduction is insufficient to simultaneously achieve core deformation penetration and surface plate shape stability. Fourth, existing solutions generally lack systematic process design for heating regime, deformation path, pass sequence, edge temperature compensation, and finished product cooling, making it difficult to consistently obtain wide and medium-thick plates with uniform microstructure, straight plate shape, and consistent properties. Summary of the Invention
[0004] The summary section of this invention provides a brief overview of the concepts, which will be described in detail in the detailed description section that follows. This summary section is not intended to identify key or essential features of the claimed invention, nor is it intended to limit the scope of the claimed invention.
[0005] Some embodiments of the present invention provide a method for preparing thick titanium alloy plates by cross-phase region direct rolling based on EB casting, in order to solve the technical problems mentioned in the background section above.
[0006] This invention provides a method for preparing thick titanium alloy plates by direct rolling in the transphase region based on EB casting, comprising the following steps: S1. Rectangular billet preparation: The rectangular billet is prepared by electron beam cold hearth furnace melting using sponge titanium and intermediate alloy and / or titanium alloy return material as raw materials; S2. Homogenization heating: Heat the rectangular billet to 50~100℃ above the β phase transformation point and hold for 180~360min; S3. Initial rolling: After the rectangular billet exits the furnace, it undergoes multiple reversible rolling passes to prepare an intermediate slab; the thickness of the intermediate slab is 120~250mm. S4. Intermediate annealing: Heat the intermediate slab to 100~200°C below the β phase transformation point, hold for 60~180 min, and then air cool or furnace cool. S5. Finished product rolling: The intermediate slab is heated to 50~150℃ below the β phase transformation point, held for 30~60min, and then subjected to multiple passes of finishing rolling to prepare the finished slab. S6. Finished product processing: The finished billet is processed sequentially to obtain a titanium alloy plate with a thickness of 20~60mm and a width of 1500~2000mm.
[0007] Optionally, a stepped heating regime is adopted in step S2: first, the temperature is raised from room temperature to 50°C below the β phase transition point at a rate not exceeding 100°C / h, and held for 60~120 min; then, the temperature is raised to 50~100°C above the β phase transition point at a rate not exceeding 150°C / h, and held for 60~300 min.
[0008] Optionally, in step S3, the multi-pass reversible rolling adopts alternating transverse and longitudinal reversing rolling, specifically including: first, rolling along the length direction of the rectangular billet, and reversing when the cumulative deformation reaches 20%~30%; then, rolling along the width direction of the rectangular billet, and reversing again when the cumulative deformation reaches 15%~25%; and subsequently cyclically reversing until the thickness of the intermediate slab is 120~250mm.
[0009] Optionally, in step S5, the time from when the intermediate slab exits the furnace to when it is first pressed down does not exceed 90 seconds; the interval between two adjacent passes does not exceed 30 seconds.
[0010] Optionally, in step S5, temperature compensation is performed on the edges of the intermediate slab so that when the slab exits the furnace, the temperature distribution along the width direction of the intermediate slab satisfies the condition that the edge temperature is 10~30℃ higher than the center temperature.
[0011] Optionally, in step S5, alternating transverse and longitudinal rolling is used for the first two-thirds of the passes, and unidirectional rolling along the length of the finished plate is used for the last one-third of the passes.
[0012] Optionally, in step S6, the annealing temperature for the finished product treatment is 800~880℃, the holding time is 60~120min, and the cooling rate after annealing is 0.5~5℃ / s.
[0013] Optionally, the straightening process can be carried out using residual heat straightening, with a straightening temperature of 450~600℃.
[0014] Optionally, in step S6, after annealing, mechanical properties of the titanium alloy sheet are sampled and tested along the thickness, width, and length directions; when the room temperature tensile strength deviation of the titanium alloy sheet at different sampling locations is greater than 5%, and / or the elongation after fracture deviation is greater than 2%, the titanium alloy sheet is subjected to secondary annealing treatment.
[0015] Optionally, the titanium alloy plate is an α+β type titanium alloy or a near-α type titanium alloy; the rectangular casting has a thickness of 300~500mm and a width of 1000~1800mm.
[0016] The above embodiments of the present invention have the following beneficial effects: This solution uses EB rectangular billets as raw materials and employs a two-pass direct rolling process: homogenization heating—β-zone billet preparation—intermediate annealing—α+β-zone finishing rolling—finished product annealing and finishing. This eliminates the forging billet preparation step in traditional processes. Homogenization heating allows for sufficient diffusion in the β-zone, reducing as-cast segregation. Multi-pass reversible rolling breaks down columnar crystals through large deformation in the β-zone. Finish rolling at 50-150℃ below the β-phase transformation point yields a refined bimodal microstructure. By addressing as-cast microstructure defects at each step, this solution significantly reduces production costs while obtaining wide, medium-thick plates that meet application requirements, resolving the issues of long processes, high costs, and limited width and thickness specifications in existing technologies. Attached Figure Description
[0017] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0018] Figure 1 This is a process flow diagram of the titanium alloy plate preparation method provided in the embodiments of the present invention; Figure 2 This is a schematic diagram of edge temperature compensation for the billet / slab during the heating stage provided in an embodiment of the present invention; Figure 3 This is a schematic diagram of the temperature distribution of a slab when it exits the furnace, provided as an embodiment of the present invention.
[0019] 1. Heating furnace; 2. Heating element; 3. Slab. Detailed Implementation
[0020] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0021] In the description of this invention, it should be understood that the terms "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," and "counterclockwise," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limiting this invention.
[0022] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the stated features. In the description of this invention, "a plurality of" means two or more, unless otherwise explicitly specified. Furthermore, the terms "installed," "connected," and "linked" should be interpreted broadly; for example, they may refer to a fixed connection, a detachable connection, or an integral connection; they may refer to a mechanical connection or an electrical connection; they may refer to a direct connection or an indirect connection through an intermediate medium; and they may refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.
[0023] This disclosure will now be described in detail with reference to the accompanying drawings and embodiments.
[0024] Figure 1 This is a process flow diagram of the titanium alloy sheet preparation method provided in the embodiments of the present invention, as shown below. Figure 1 As shown, the present invention provides a method for preparing thick titanium alloy plates by direct rolling in the transphase region based on EB casting, comprising the following steps: S1. Rectangular billet preparation: Rectangular billets are prepared by melting sponge titanium and intermediate alloys and / or titanium alloy return materials in an electron beam cold hearth furnace; the rectangular billets are then subjected to head and tail trimming and surface machining to obtain clean and dimensionally regular rectangular billets ready for rolling. S2. Homogenization heating: Heat the rectangular billet to 50~100℃ above the β phase transformation point and hold for 180~360min; S3. Initial rolling: After the rectangular billet exits the furnace, it undergoes multi-pass reversible rolling to prepare intermediate slabs; the thickness of the intermediate slabs is 120~250mm; the single-pass reduction is controlled at 5%~15%, the total deformation is 50%~70%, and the final rolling temperature is not lower than 750℃. S4. Intermediate annealing: Heat the intermediate slab to 100~200℃ below the β phase transformation point, hold for 60~180min, and then air cool or furnace cool. S5. Finished product rolling: Heat the intermediate slab to 50~150℃ below the β phase transformation point, hold for 30~60min and then perform multi-pass finishing rolling to prepare the finished slab; control the single-pass reduction to be 3%~12%, the total deformation to be 40%~60%, and the final rolling temperature to be not lower than (β phase transformation point -200℃). S6. Finished product processing: The finished slab is subjected to annealing, straightening, edge trimming, length setting and surface grinding or polishing in sequence to obtain titanium alloy sheet. The titanium alloy sheet has a thickness of 20~60mm and a width of 1500~2000mm.
[0025] This solution uses EB rectangular billets as raw materials and employs a two-pass direct rolling process: homogenization heating—β-zone billet preparation—intermediate annealing—α+β-zone finishing rolling—finished product annealing and finishing. This eliminates the forging billet preparation step in traditional processes. Homogenization heating allows for sufficient diffusion in the β-zone, reducing as-cast segregation. Multi-pass reversible rolling breaks down columnar crystals through large deformation in the β-zone. Finish rolling at 50-150℃ below the β-phase transformation point yields a refined bimodal microstructure. By addressing as-cast microstructure defects at each step, this solution significantly reduces production costs while obtaining wide, medium-thick plates that meet application requirements, resolving the issues of long processes, high costs, and limited width and thickness specifications in existing technologies.
[0026] In some embodiments, a stepped heating regime is adopted in step S2: first, the temperature is raised from room temperature to 50°C below the β phase transformation point at a rate not exceeding 100°C / h, and held for 60-120 min; then, the temperature is raised to 50-100°C above the β phase transformation point at a rate not exceeding 150°C / h, and held for 60-300 min. The oxygen content in the furnace atmosphere is controlled below 5% to reduce oxidation on the billet surface and the depth of the oxygen-rich layer.
[0027] To address the issue of core-surface temperature differences and thermal stress cracking caused by rapid, one-time heating of thick billets (300-500mm), a stepped heating regime is adopted. The first stage raises the temperature to 50°C below the β phase transformation point and holds for 60-120 minutes to achieve pre-homogenization. The second stage then raises the temperature to the target temperature, ensuring that the core and surface temperatures of the billet enter the rolling window simultaneously, reducing the risk of thermal stress cracking. Simultaneously, the first stage of holding also pre-homogenizes some micro-segregations in the α+β region, creating a synergistic "two-stage diffusion" effect with the homogenization in the β region. The oxygen content in the furnace atmosphere is controlled below 5%, reducing the oxide layer thickness on the billet surface from 0.5-1.0mm in conventional heating to below 0.2mm, and the oxygen-rich layer depth from over 1.5mm to within 0.5mm. This provides a clean surface condition for subsequent rolling, significantly reducing the incidence of surface cracks and oxygen-rich layer indentation defects.
[0028] In some embodiments, in step S3, the multi-pass reversible rolling adopts alternating transverse and longitudinal reversing rolling, specifically including: first, rolling along the length direction of the rectangular slab, and reversing direction when the cumulative deformation reaches 20%~30%; then, rolling along the width direction of the rectangular slab, and reversing direction again when the cumulative deformation reaches 15%~25%; subsequent cycles of reversing direction until the intermediate slab thickness is 120~250mm. The total deformation of transverse rolling accounts for 25%~45% of the total rolling deformation.
[0029] To address the longitudinal-transverse property differences caused by the strong anisotropy of columnar crystals in EB billets, a rolling scheme driven by cumulative deformation and alternating longitudinal and transverse directions is adopted. In the first stage, longitudinal rolling reverses direction when the cumulative deformation reaches 20-30%, ensuring timely switching of deformation direction before the as-cast microstructure begins to break down but before a stable fibrous texture is formed. Subsequent rolling cycles repeat with cumulative deformation periods of 20-30% and 15-25%, keeping the transverse deformation within a reasonable range of 25-45% of the total deformation. This approach effectively utilizes transverse deformation to break down the anisotropy of columnar crystals while avoiding excessive transverse deformation that could lead to uncontrolled widening and deterioration of the billet shape.
[0030] In some embodiments, in step S5, the time from the intermediate slab exiting the furnace to the first pass reduction does not exceed 90 seconds; the interval between two adjacent passes does not exceed 30 seconds. When the interval between passes exceeds 60 seconds due to equipment adjustments or other reasons, the workpiece is covered with an insulation cover or subjected to induction heating to ensure that the surface temperature of the workpiece is not lower than the final rolling temperature limit for that cycle. Considering the characteristics of titanium alloys—low thermal conductivity, rapid temperature drop after exiting the furnace, and narrow temperature window—the time from exiting the furnace to the first pass reduction does not exceed 90 seconds, the interval between adjacent passes does not exceed 30 seconds, and insulation covers or induction heating are provided as a fallback for abnormal situations exceeding 60 seconds. This ensures that the workpiece temperature remains within the designed window throughout the entire cycle, avoiding process accidents such as forced decompression, remelting, or cracking due to temperature drops outside the window.
[0031] Figure 2 This is a schematic diagram of edge temperature compensation for the billet / slab during the heating stage, provided in an embodiment of the present invention. Figure 3 This is a schematic diagram of the temperature distribution of the slab when it exits the furnace, provided in an embodiment of the present invention. Figure 2 and 3 As shown, in some embodiments, in step S5, temperature compensation is performed on the edges of the intermediate slab so that the temperature distribution along the width of the intermediate slab when it exits the furnace satisfies that the edge temperature is 10~30℃ higher than the center temperature, ΔT=10~30℃. In the edge regions on both sides of the cast billet / slab within the heating furnace, the burner density is increased or auxiliary heating elements are added to ensure that the temperature distribution along the width of the cast billet / slab when it exits the furnace satisfies that the edge temperature is 10~30℃ higher than the center temperature, thus compensating for the additional temperature drop relative to the center at the edges during the process from exiting the furnace to the first pressing.
[0032] To address the issue of high edge deformation resistance, poor plasticity, and susceptibility to edge cracks and waviness caused by a 30-50°C temperature drop at the edges compared to the center after wide-width slabs exit the furnace, a pre-heating compensation of 10-30°C is applied to the edges of the cast billet / slab during the heating stage. This results in a temperature distribution with varying temperatures at the edges, center, and height upon exiting the furnace. After the time window from exiting the furnace to the first pressing, the temperature across the entire width of the slab becomes more uniform. This ensures consistent deformation resistance across the width of the slab during the first pressing, significantly reduces the incidence of edge cracks, and greatly improves the flatness of the slab.
[0033] In some embodiments, in step S5, alternating transverse and longitudinal rolling is used for the first two-thirds of the passes, and unidirectional rolling along the length of the finished plate is used for the last one-third of the passes.
[0034] To address the issue of difficulty in ensuring plate shape stability during the finished product rolling stage, a two-stage deformation path is adopted, consisting of alternating transverse and longitudinal rolling in the first two-thirds of the passes and unidirectional rolling in the last one-third of the passes. The first stage fully homogenizes the width extension through reversal, while the second stage locks the plate shape and eliminates the lateral unevenness accumulated in the first stage through unidirectional rolling, thus avoiding problems such as central waviness and excessive thickness in the middle.
[0035] In some embodiments, in step S6, the annealing temperature for the finished product is 800~880℃, the holding time is 60~120min, and the cooling rate after annealing is 0.5~5℃ / s. Straightening employs a residual heat straightening process with a straightening temperature of 450~600℃. The cooling rate is controlled within a specific range of 0.5~5℃ / s. This range avoids both new residual stress caused by excessively rapid cooling and excessive coarsening of the α phase caused by excessively slow cooling. The residual heat straightening process, with a temperature window of 450~600℃, represents the optimal range where the titanium alloy has sufficient plasticity for straightening but is low enough to avoid over-straightening, thus avoiding the risks of cracking during cold straightening and springback during high-temperature straightening. Ultimately, this ensures stable and controllable finished plate quality, enabling mass production and delivery.
[0036] In some embodiments, in step S6, mechanical property samples are taken from the titanium alloy sheet along the thickness, width, and length directions after annealing. When the room temperature tensile strength deviation at different sampling locations of the titanium alloy sheet is greater than 5%, and / or the elongation after fracture deviation is greater than 2%, the titanium alloy sheet undergoes a second annealing treatment. To address the potential differences in mechanical properties at different locations within wide-width medium-thick plates, a uniformity index is clearly defined, requiring a tensile strength deviation of ≤5% and an elongation deviation of ≤2 percentage points at different sampling locations within the same plate. A corrective mechanism of "secondary annealing for non-compliance" is also established. Quality control shifts from "post-process rejection" to "process correction," allowing plates that do not meet uniformity requirements to be salvaged through secondary annealing. This avoids scrapping the entire plate due to localized performance deficiencies, further improving yield and economy.
[0037] In some embodiments, the titanium alloy sheet is an α+β type titanium alloy or a near-α type titanium alloy; the thickness of the rectangular billet is 300~500mm, and the width is 1000~1800mm. Specifically, it can be TC4, TA15, TA17, TA18, TC11, etc.
[0038] The following describes three specific embodiments applied to the method of this application.
[0039] Example 1: TC4 titanium alloy wide medium-thick plate was prepared according to the method of the present invention. The target specifications were 60mm thickness × 1800mm width × ≥4000mm length. The specific steps are as follows.
[0040] S1. Rectangular billet preparation: Using electrode blocks pressed from sponge titanium and aluminum-vanadium master alloys, and 30wt% of TC4 grade return material as raw materials, TC4 rectangular billets were prepared by electron beam cold hearth furnace melting. The billet specifications were 380mm thick × 1700mm wide × 6500mm long. The billet was cut off at the head and tail, and 5mm of surface chilling layer and oxide scale were removed by single-sided machining. The machined billet was subjected to fluorescence penetrant testing to confirm that there were no surface defects extending to the substrate, resulting in a rectangular billet to be rolled with dimensions of 370mm × 1690mm × 6200mm.
[0041] S2. Homogenization Heating: A stepped heating regime is adopted. First, the temperature is increased from room temperature to 945℃ at a rate of 80℃ / h and held for 90 minutes; then, it is increased to 1060℃ (65℃ above the β phase transformation point) at a rate of 120℃ / h and held for 240 minutes. The oxygen content in the heating furnace is controlled below 4%; at the same time, the burner density is increased in the edge areas of the billet in the heating furnace so that the temperature distribution of the billet along the width direction when it exits the furnace meets the requirement that the edge temperature is about 20℃ higher than the center temperature.
[0042] S3. Initial Rolling: The first reduction is completed within 70 seconds of the billet exiting the furnace, using an alternating longitudinal and transverse rolling process. The first stage rolls along the length of the billet, with a cumulative deformation of 25% over 5 passes; the second stage rolls along the width of the billet, with a cumulative deformation of 20% over 3 passes; subsequent stages cycle longitudinal-transverse-longitudinal-transverse until an intermediate slab thickness of 130mm is achieved. Throughout the entire initial rolling process, the reduction per pass is controlled between 6% and 13%, the interval between adjacent passes does not exceed 25 seconds, the final rolling temperature is 825℃, and the total deformation is 65%, with transverse rolling accounting for 35% of the total deformation. The resulting intermediate slab has a thickness of 130mm and a width of 1850mm.
[0043] S4. Intermediate Annealing: Heat the intermediate slab to 850℃ (i.e., 145℃ below the β phase transformation point), hold for 120 minutes, and then air-cool to room temperature.
[0044] S5. Finished Product Rolling: The intermediate annealed slab is heated to 920℃ (75℃ below the β phase transformation point) and held for 45 minutes. Temperature compensation is applied to the edges during the heating process. The first reduction begins within 60 seconds of exiting the furnace. The first six passes use alternating transverse and longitudinal rolling, while the last three passes use unidirectional rolling along the length of the finished slab. The reduction per pass is controlled at 4%~10% throughout the entire finished product rolling process, with an interval of no more than 25 seconds between adjacent passes. The final rolling temperature is 805℃, and the total deformation is 54%. A finished slab with a thickness of 60mm and a width of 1850mm is obtained after rolling.
[0045] S6. Finished product processing: Hold the product in an annealing furnace at 850℃ for 90 minutes, then air cool it at a rate of about 2℃ / s. When the material cools to 530℃, straighten it while it is still warm. After straightening, trim the edges, cut to length, and grind the surface.
[0046] The final product was a wide, medium-thick TC4 titanium alloy plate with dimensions of 60mm × 1800mm × 4500mm. Mechanical properties were tested by sampling at multiple points along the thickness, width, and length directions: room temperature tensile strength 935~975MPa, yield strength 850~895MPa, elongation after fracture 13.5%~14.8%; the straightness deviation per meter along the length direction was ≤2.5mm, and the convexity was ≤0.25%.
[0047] Example 2: TA15 titanium alloy (near-α type, β phase transformation point about 990℃) wide medium-thick plate was prepared according to the method of the present invention, with a target specification of 60mm thickness × 2000mm width × ≥4000mm length.
[0048] S1. Rectangular billet preparation: Using electrode blocks pressed from sponge titanium and aluminum-vanadium master alloy as raw materials, TA15 rectangular billets were prepared by electron beam cold hearth furnace melting. The billet specifications were 480mm thick × 1800mm wide × 5500mm long. After cutting off the head and tail, 8mm was removed by single-sided machining. Ultrasonic testing showed no internal defects with a flat bottom hole reflection greater than Φ2.0mm, resulting in a rectangular billet to be rolled with dimensions of 464mm × 1784mm × 5300mm.
[0049] S2. Homogenization Heating: A stepped heating regime is adopted. First, the temperature is increased from room temperature to 940℃ at a rate of 60℃ / h and held for 120 min; then, it is increased to 1075℃ (i.e., 85℃ above the β phase transition point) at a rate of 100℃ / h and held for 320 min. The oxygen content of the furnace is controlled below 4.5%, and the temperature at the edge is about 25℃ higher than that in the center.
[0050] S3. Initial Rolling: Within 80 seconds of the billet exiting the furnace, the first rolling pass is performed using alternating longitudinal and transverse rolling. The first stage involves 4 passes along the length direction, with a cumulative deformation of 28%. The second stage involves 3 passes along the width direction, with a cumulative deformation of 22%. Subsequent rolling follows a longitudinal-transverse-longitudinal-transverse cycle. The total reduction per pass during the entire initial rolling process is 7%~14%, with a pass interval not exceeding 28 seconds. The final rolling temperature is 815℃, the total deformation is 68%, and the transverse deformation accounts for 38%. After rolling, an intermediate slab with a thickness of 150mm and a width of 2080mm is obtained.
[0051] S4. Intermediate annealing: Heat the intermediate slab to 820℃ (170℃ below the β phase transformation point), hold for 150 minutes, furnace cool to 600℃, and then air cool.
[0052] S5. Finished Product Rolling: The intermediate slab is heated to 880℃ (110℃ below the β phase transformation point), held for 50 minutes, and the edges are compensated for a temperature of 25℃. Within 75 seconds of exiting the furnace, the first pass is rolled down, followed by four passes of alternating transverse and longitudinal rolling, and the last two passes of unidirectional rolling along the length. The reduction per pass is 4%~11%, the pass interval does not exceed 28 seconds, the final rolling temperature is 790℃, and the total deformation is 60%. The resulting slab has a thickness of 60mm and a width of 2050mm.
[0053] S6. Finished product processing: Hold the product in an annealing furnace at 820℃ for 120 minutes, then air cool it at a rate of approximately 1.5℃ / s. When the sheet material cools to 560℃, straighten it using residual heat. After straightening, trim the edges, cut to length, and polish it.
[0054] The final product was a wide, medium-thick TA15 titanium alloy plate with dimensions of 60mm × 2000mm × 4000mm. Multi-point sampling mechanical properties: room temperature tensile strength 935~980MPa, yield strength 870~915MPa, elongation after fracture 11.2%~12.8%; straightness deviation per meter along the length of the plate ≤2.8mm, plate convexity ≤0.28%.
[0055] Example 3: TA17 titanium alloy (near-α type Ti-4Al-2V, β phase transformation point about 940℃) wide medium-thick plate was prepared according to the method of the present invention. The target specifications are 50mm thickness × 1500mm width × ≥3000mm length, mainly for marine engineering structural components.
[0056] S1. Rectangular billet preparation: Using electrode blocks pressed from sponge titanium and aluminum-vanadium master alloys, and 60wt% TA17 recycled material (including turning chips and scrap) as raw materials, a two-stage melting process in an electron beam cold hearth furnace is adopted. The first melting is used to fully remove impurities and volatilize volatile elements, and the second melting is used to homogenize the composition to prepare a TA17 rectangular billet with a thickness of 320mm × width of 1450mm × length of 8500mm. After cutting off the head and tail, 4mm is removed by single-sided machining. Fluorescent penetrant + ultrasonic flaw detection confirms that there are no extended defects on the surface and inside, resulting in a rectangular billet of 312mm × 1442mm × 8200mm to be rolled.
[0057] S2. Homogenization Heating: A stepped heating regime is adopted. First, the temperature is increased from room temperature to 890℃ at a rate of 90℃ / h and held for 60 minutes; then, it is increased to 1010℃ (70℃ above the β phase transition point) at a rate of 130℃ / h and held for 200 minutes. The oxygen content of the heating furnace is controlled below 5%, and the temperature at the edge is about 15℃ higher than that in the center.
[0058] S3. Initial Rolling: Within 65 seconds of the billet exiting the furnace, the first pass is rolled down, alternating between horizontal and vertical directions. The first stage involves 4 passes along the length direction, accumulating a deformation of 26%; the second stage involves 3 passes along the width direction, accumulating a deformation of 18%; subsequent stages involve cyclical reversal. The reduction per pass is 5%~12%, with pass intervals not exceeding 22 seconds. If a 50-second interval occurs due to mill adjustments, an insulation cover is immediately applied. The final rolling temperature is 760℃, with a total deformation of 60%, of which 30% is transverse deformation. The resulting intermediate slab has a thickness of 125mm and a width of 1500mm.
[0059] S4. Intermediate annealing: Heat the intermediate slab to 780℃ (160℃ below the β phase transformation point), hold for 90 minutes, and then air cool after removal from the furnace.
[0060] S5. Finished Product Rolling: The intermediate slab is heated to 855℃ (85℃ below the β phase transformation point), held at that temperature for 35 minutes, and the edge temperature is compensated by 15℃. Within 55 seconds of exiting the furnace, the first pass is rolled down, followed by alternating transverse and longitudinal passes for the first 7 passes, and then unidirectional rolling along the length for the last 3 passes. The reduction per pass is 3%~9%, the pass interval does not exceed 22 seconds, the final rolling temperature is 765℃, and the total deformation is 60%. The resulting slab has a thickness of 50mm and a width of 1530mm.
[0061] S6. Finished Product Processing: The sheet is held in an annealing furnace at 800℃ for 60 minutes, then air-cooled at a rate of approximately 4℃ / s. After cooling to 480℃, it undergoes residual heat straightening. In the first batch of sampling tests, tensile strength deviations of up to 5.6% were found in some locations, exceeding the 5% upper limit specified in claim 9. This batch of sheet underwent a second annealing treatment (790℃ × 60 minutes air cooling). After the second annealing, sampling was conducted again, and the strength deviation decreased to 3.8%, and the elongation deviation was 1.2 percentage points, meeting the uniformity requirements. Finally, the edges are trimmed, the sheet is cut to length, and the surface is ground.
[0062] The final product was a wide, medium-thick TA17 titanium alloy plate with dimensions of 50mm × 1500mm × 3000mm. Multi-point sampling mechanical properties: room temperature tensile strength 705~735MPa, yield strength 615~650MPa, elongation after fracture 18.5%~19.7%; straightness deviation per meter along the length of the plate ≤3.0mm, plate convexity ≤0.30%.
[0063] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing thick titanium alloy plates by direct rolling in the transphase region based on EB casting, characterized in that, Includes the following steps: S1. Rectangular billet preparation: The rectangular billet is prepared by electron beam cold hearth furnace melting using sponge titanium and intermediate alloy, and / or titanium alloy return material as raw materials; S2. Homogenization heating: Heat the rectangular billet to 50~100℃ above the β phase transformation point and hold for 180~360min; S3. Initial rolling: After the rectangular billet exits the furnace, it undergoes multiple reversible rolling passes to prepare an intermediate slab; the thickness of the intermediate slab is 120~250mm. S4. Intermediate annealing: Heat the intermediate slab to 100~200°C below the β phase transformation point, hold for 60~180 min, and then air cool or furnace cool. S5. Finished product rolling: The intermediate slab is heated to 50~150°C below the β phase transformation point, held for 30~60 minutes, and then subjected to multiple passes of finishing rolling to prepare the finished slab. S6. Finished product processing: The finished billet is processed sequentially to obtain a titanium alloy sheet, the titanium alloy sheet having a thickness of 20~60mm and a width of 1500~2000mm.
2. The method for preparing thick titanium alloy plates by direct rolling in the transphase region based on EB casting according to claim 1, characterized in that, In step S2, a stepped heating regime is adopted: first, the temperature is raised from room temperature to 50°C below the β phase transition point at a rate not exceeding 100°C / h, and held for 60~120 min; then, the temperature is raised to 50~100°C above the β phase transition point at a rate not exceeding 150°C / h, and held for 60~300 min.
3. The method for preparing thick titanium alloy plates by direct rolling in the transphase region based on EB casting according to claim 2, characterized in that, In step S3, the multi-pass reversible rolling adopts alternating transverse and longitudinal reversing rolling, specifically including: first, rolling along the length direction of the rectangular billet, and reversing when the cumulative deformation reaches 20%~30%; then, rolling along the width direction of the rectangular billet, and reversing again when the cumulative deformation reaches 15%~25%; and then cyclically reversing until the thickness of the intermediate slab is 120~250mm.
4. The method for preparing thick titanium alloy plates by direct rolling in the transphase region based on EB casting according to claim 1, characterized in that, In step S5, the time from when the intermediate slab exits the furnace to when it is first pressed down does not exceed 90 seconds; the interval between two adjacent passes does not exceed 30 seconds.
5. The method for preparing thick titanium alloy plates by direct rolling in the transphase region based on EB casting according to claim 4, characterized in that, In step S5, temperature compensation is performed on the edges of the intermediate slab so that when the slab exits the furnace, the temperature distribution along the width direction of the intermediate slab satisfies the condition that the edge temperature is 10~30℃ higher than the center temperature.
6. The method for preparing thick titanium alloy plates by direct rolling in the transphase region based on EB casting according to claim 5, characterized in that, In step S5, alternating transverse and longitudinal rolling is used for the first two-thirds of the passes, and unidirectional rolling along the length of the finished plate is used for the last one-third of the passes.
7. The method for preparing thick titanium alloy plates by direct rolling in the transphase region based on EB casting according to claim 1, characterized in that, In step S6, the annealing temperature for the finished product treatment is 800~880℃, the holding time is 60~120min, and the cooling rate after annealing is 0.5~5℃ / s.
8. The method for preparing thick titanium alloy plates by direct rolling in the transphase region based on EB casting according to claim 1, characterized in that, In step S6, the straightening process employs residual heat straightening, with a straightening temperature of 450~600℃.
9. The method for preparing thick titanium alloy plates by direct rolling in the transphase region based on EB casting according to claim 8, characterized in that, In step S6, after annealing, mechanical properties of the titanium alloy sheet are sampled and tested along the thickness, width, and length directions. When the room temperature tensile strength deviation of the titanium alloy sheet at different sampling locations is greater than 5%, and / or the elongation after fracture deviation is greater than 2%, the titanium alloy sheet is subjected to secondary annealing treatment.
10. A method for preparing thick titanium alloy plates by direct rolling in the transphase region based on EB casting according to any one of claims 1 to 9, characterized in that, The titanium alloy plate is an α+β type titanium alloy or a near-α type titanium alloy; the rectangular billet has a thickness of 300~500mm and a width of 1000~1800mm.