A method for arranging single-layer diamond particles based on a narrow-slit pocket structure and a method for preparing a heat dissipation substrate for metal matrix composites.
By using a narrow-slit pocket structure and gravity filling method, a single-layer arrangement of diamond particles in a metal matrix composite heat dissipation substrate was achieved, solving the problems of high cost and non-uniformity in existing technologies, and improving thermal conductivity and production efficiency.
Patent Information
- Application Number
- CN202611203600.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-10
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies require precise machining of positioning features when preparing metal/diamond composite heat dissipation substrates, resulting in high costs and uneven particle arrangement, making it difficult to achieve a single-layer arrangement of diamond particles.
Employing a narrow-slit pocket structure, the diamond particles are naturally arranged in a single layer under gravity by controlling the gap height between two sheet metals. This eliminates the need for precision machining and positioning features, and utilizes hot pressing and sintering to form a closed narrow-slit pocket-shaped filling structure.
It significantly reduces manufacturing costs, improves the uniformity of single-layer diamond particle arrangement and thermal conductivity, reduces particle loss and arrangement disturbance risks, and simplifies the process flow.
Smart Images

Figure CN123060104A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the fields of powder metallurgy and electronic packaging heat dissipation materials. Specifically, it relates to a method for achieving a single-layer arrangement of diamond particles using a narrow-slit pocket structure and gravity filling, and a method for preparing a metal / diamond composite heat dissipation substrate based on this method. Background Technology
[0002] In the process of preparing a metal / diamond composite heat dissipation substrate, the formation of a single layer of diamond particles along the thickness direction (i.e., the particles do not basically overlap each other) is one of the key structural features that ensures the composite material has both high thermal conductivity and a reasonable coefficient of thermal expansion.
[0003] Existing single-layer positioning technologies (such as pre-grooved metal plates, stepped metal substrates, metal limiting frames, honeycomb thin-walled structures, microporous metal plates, convex arrays, template positioning, scraper leveling methods, and roll-pressed pitted metal foils) generally rely on processing positioning features (grooves, steps, holes, convex points, etc.) that match the particle size on the surface of the metal substrate / foil. This requires precision machining processes such as mechanical milling, electrical discharge machining, etching, or roll embossing, resulting in high processing costs. In addition, some methods (such as scraper leveling methods) require additional vibration or scraping equipment, and the uniformity of particle arrangement depends on the precision of process control.
[0004] In the existing publicly disclosed patent technology US8531026B2, the single-layer arrangement of diamond particles is generally achieved by "spreading on the surface of a metal layer," that is, the particles are directly spread on an open metal surface to form a single layer. The spreading process relies on manual or auxiliary equipment control, and the particle positioning features require additional structural support. Therefore, developing a method that is simple in structure, requires no precision machining of positioning features, and can naturally form a single-layer arrangement using the gravity of the particles themselves is of great practical significance. Summary of the Invention
[0005] This invention proposes a method for arranging single-layer diamond particles based on a narrow-slit pocket structure and a method for preparing a heat dissipation substrate of a metal matrix composite material. By controlling the gap height between two sheet metals, the diamond particles are naturally arranged in a single layer after being filled through the narrow slit under the action of gravity. There is no need to process positioning features on the surface of the sheet metal, which reduces the manufacturing cost of the single-layer positioning structure and simplifies the filling process.
[0006] To achieve the above objectives, the present invention provides the following technical solution: This invention proposes a method for arranging single-layer diamond particles based on a narrow-slit pocket structure, comprising the following steps: A pocket-shaped cavity with a predetermined gap height is formed between the first sheet metal and the second sheet metal, and the pocket-shaped cavity has at least one unclosed opening edge; Diamond particles are injected into the pocket-shaped cavity through the edge of the opening to form a single-layer particle layer; The opening edges are sealed, and then a closed, narrow-slit, pocket-shaped filling structure is formed by hot pressing and sintering.
[0007] Furthermore, the first sheet metal and the second sheet metal are each independently selected from one of pure copper, copper alloy, pure aluminum, or aluminum alloy; the preset gap height is 1.0 to 1.5 times the average particle size of the diamond particles.
[0008] Furthermore, the diamond particles are one of HPHT single-crystal diamond, CVD diamond, or natural diamond; the injection method into the pocket-shaped cavity is pure gravity injection.
[0009] The pocket-shaped cavity can be achieved through two structural methods: a double-sealed type or a grooved foil-covered type, and either method can be used.
[0010] Furthermore, the double-sealed pocket-shaped cavity is formed by sealing the first sheet metal and the second sheet metal together with spacers along three edges, and the fourth edge without the spacers constitutes the opening edge.
[0011] Furthermore, the spacer is a metal strip or wire with a circular, square, or rectangular cross-sectional shape; the spacer is temporarily fixed to the first sheet metal and the second sheet metal by spot welding, mechanical clamping, or thermally conductive adhesive.
[0012] Furthermore, in the grooved foil-covered pocket-shaped cavity, the surface of the first sheet metal is processed with a groove, at least one edge of the groove extends through the edge of the first sheet metal to form the opening edge; the second sheet metal covers the opening surface of the groove, and together with the first sheet metal, forms the pocket-shaped cavity, and the depth of the groove is the preset gap height.
[0013] Furthermore, the groove is formed on the surface of the first sheet metal by any one of mechanical milling, electrical discharge machining, or laser processing; the second sheet metal is a foil.
[0014] Furthermore, the hot pressing sintering is low-temperature high-pressure sintering, and the parameters of the low-temperature high-pressure sintering are: sintering temperature 550~650℃, pressure 250~350MPa, and holding time 10~30min.
[0015] A metal-based composite material heat dissipation substrate, the heat dissipation substrate comprising upper and lower surface metals formed by a first sheet metal and a second sheet metal, a single layer of diamond particles located between the upper and lower surface metals, and an edge metal frame region surrounding the single layer of diamond particles.
[0016] Furthermore, the edge metal frame region is substantially free of diamond particles, and the edge metal frame region originates from the location of the spacer member or from the edge region of the first sheet metal where no groove is formed.
[0017] Compared with the prior art, the beneficial effects of the present invention are as follows: This invention requires only two sheet metals and conventional metal strips / wires, eliminating the need to process positioning features such as grooves, steps, and holes on the metal surface. It also eliminates processes such as precision machining, electrical discharge machining, etching, or roll embossing, significantly reducing the manufacturing cost of a single-layer positioning structure.
[0018] This invention utilizes the natural formation of a single layer of diamond particles through a narrow slit by their own gravity, eliminating the need for vibration equipment, templates, or other auxiliary devices. The narrow slit cavity simultaneously serves as a filling channel and a single-layer limiting mechanism, integrating the filling process with the single-layer limiting mechanism into one, simplifying the process.
[0019] In this invention, the single-layer characteristics are directly determined by the ratio of the gap height to the particle size. Different diamond particles of different sizes can be adapted by adjusting the size of the spacer components, without the need to redesign / process the positioning structure.
[0020] In this invention, the loading and hot pressing are integrated. The pocket-shaped structure itself is a loading container. After sealing, it can be directly used for hot pressing and sintering, reducing intermediate steps such as particle transfer and pouring, avoiding particle displacement, loss, and stacking defects, and reducing the risk of diamond particle loss and arrangement disturbance.
[0021] This invention can utilize existing equipment and capacity for groove processing, requiring only adjustments to the groove depth and opening position, without the need for additional equipment investment, thus reducing high-cost processes and significantly lowering costs. Attached Figure Description
[0022] Various other advantages and benefits will become apparent to those skilled in the art upon reading the following detailed description of preferred embodiments. The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings: Figure 1 This is a top view of the double-sealed loading structure in an embodiment of the present invention.
[0023] Figure 2 This is a cross-sectional view of the double-sealed loading structure in an embodiment of the present invention.
[0024] Figure 3 This is a top view of the grooved foil-covered material loading structure in an embodiment of the present invention.
[0025] Figure 4 This is a cross-sectional view of the grooved foil-covered material loading structure in an embodiment of the present invention.
[0026] Figure 5 This is a schematic diagram of the sealed loading structure and the double-sealed loading structure of the finished product after hot pressing and sintering according to the present invention.
[0027] Figure 6 This is a schematic diagram of the sealed loading structure and the finished product groove foil-covered loading structure after hot pressing and sintering according to the present invention. Detailed Implementation
[0028] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention. It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the present invention.
[0029] Furthermore, regarding the numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Every smaller range between any stated value or intermediate value within a stated range, and any other stated value or intermediate value within said range, is also included within this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.
[0030] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.
[0031] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be apparent to those skilled in the art. This specification and embodiments are merely exemplary.
[0032] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.
[0033] This invention provides a method for arranging single-layer diamond particles based on a narrow-slit pocket structure, comprising the following steps: A pocket-shaped cavity with a predetermined gap height is formed between the first sheet metal and the second sheet metal, and the pocket-shaped cavity has at least one unclosed opening edge; Diamond particles are injected into the pocket-shaped cavity through the edge of the opening to form a single-layer particle layer; The opening edges are sealed, and then a closed, narrow-slit, pocket-shaped filling structure is formed by hot pressing and sintering.
[0034] In this invention, the first sheet metal and the second sheet metal are each independently selected from one of pure copper, copper alloy, pure aluminum or aluminum alloy; the preset gap height is 1.0 to 1.5 times the average particle size of the diamond particles.
[0035] The present invention does not impose any specific limitation on the type of sheet metal, and any type known to those skilled in the art can be used. In the embodiments of the present invention, T2 copper is used.
[0036] In this invention, the diamond particles are one of HPHT single-crystal diamond, CVD diamond, or natural diamond; the injection method into the pocket-shaped cavity is pure gravity injection.
[0037] The pocket-shaped cavity can be achieved through two structural methods: a double-sealed type or a grooved foil-covered type, and either method can be used.
[0038] In this invention, the double-sealed pocket-shaped cavity is formed by sealing the first sheet metal and the second sheet metal together with spacers along three edges, and the fourth edge without the spacers constitutes the opening edge.
[0039] In this invention, the spacer is a metal strip or wire with a circular, square, or rectangular cross-sectional shape; the spacer is temporarily fixed to the first sheet metal and the second sheet metal by spot welding, mechanical clamping, or thermally conductive adhesive.
[0040] In this invention, the surface of the first sheet metal in the grooved foil-covered pocket-shaped cavity is processed with a groove, and at least one edge of the groove extends through the edge of the first sheet metal to form the opening edge; the second sheet metal covers the opening surface of the groove and together with the first sheet metal forms the pocket-shaped cavity, and the depth of the groove is the preset gap height.
[0041] In this invention, the groove is formed on the surface of the first sheet metal by any one of mechanical milling, electrical discharge machining or laser processing; the second sheet metal is a foil.
[0042] In this invention, the hot pressing sintering is low-temperature high-pressure sintering. The preferred parameters of the low-temperature high-pressure sintering are: sintering temperature 550-650℃, pressure 250-350MPa, and holding time 10-30min. More preferably, the parameters are: sintering temperature 550-600℃, pressure 250-300MPa, and holding time 10-20min.
[0043] A metal-based composite material heat dissipation substrate, the heat dissipation substrate comprising upper and lower surface metals formed by a first sheet metal and a second sheet metal, a single layer of diamond particles located between the upper and lower surface metals, and an edge metal frame region surrounding the single layer of diamond particles.
[0044] In this invention, the edge metal frame region is substantially free of diamond particles, and the edge metal frame region originates from the position of the spacer member or from the edge region of the first sheet metal where no groove is formed.
[0045] In this invention, unless otherwise specified, all raw materials required for preparation are commercially available products well known to those skilled in the art.
[0046] The technical solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0047] Example 1 Take two pieces of T2 copper foil, each 0.1 mm thick, and clamp a copper wire with a diameter of 600 μm along three edges to fix the two copper foils into a pocket-shaped structure with a gap height of 600 μm, leaving the fourth edge open.
[0048] HPHT single-crystal diamond particles with an average particle size of 500μm were selected and poured into the cavity through the opening. The particles settled to the bottom of the cavity under the action of gravity and naturally formed a single layer arrangement without obvious stacking.
[0049] After the filling is completed, a 600μm copper wire of the same specification is clamped at the opening to seal it, thus obtaining a closed bag filling structure.
[0050] The enclosed material structure is subjected to a low-temperature high-pressure sintering process. Hot pressing sintering is carried out at 600℃ and 300MPa, followed by holding at the temperature for 20 minutes and hot pressing sintering again to obtain a metal / diamond composite heat dissipation substrate.
[0051] Example 2 Take a 2mm thick T2 copper plate and machine a channel-type groove with a depth of 600μm on its upper surface by mechanical milling. One end of the groove passes through the edge of the copper plate to form an opening, and the other three sides are closed by the groove wall of the copper plate itself.
[0052] HPHT single-crystal diamond particles with an average particle size of 500μm are poured into the groove through the opening. The particles settle continuously along the length of the groove under the action of gravity. Since the groove depth (600μm) is less than twice the particle size, the particles naturally form a single layer.
[0053] After the material is loaded, a copper strip of the same width as the groove is covered at the opening end of the groove and pressed and sealed. Then, a layer of 0.1mm thick copper foil is covered on the entire opening surface of the groove, forming a closed pocket-shaped material loading structure together with the copper plate.
[0054] The enclosed material structure was subjected to a low-temperature, high-pressure sintering process, which involved hot pressing and sintering at 600℃ and 300MPa, followed by holding at that temperature for 20 minutes to obtain a metal / diamond composite heat dissipation substrate.
[0055] Example 3 On the first sheet of T2 copper with a large area, multiple independent spacer wires are arranged horizontally and parallelly on the surface through multiple sets of spacer components or multiple parallel grooves to divide multiple parallel independent narrow slit pocket cavity units. Each cavity is reserved with an independent feeding opening, and diamond particles are filled through their respective openings to complete gravity filling and single-port sealing in sequence. Then, the entire upper copper foil is covered and the whole is clamped and fixed to form an integrated multi-cavity prefabricated part.
[0056] Temperature 800℃, pressure 50MPa, vacuum ≤10 -2 Under the condition of Pa, hot pressing and sintering were carried out once, followed by holding at the temperature for 15 minutes; After sintering and heat preservation, the furnace is cooled to 350°C at a cooling rate of 50°C / min and held for 2 hours for annealing to achieve batch preparation of multiple single-layer diamond arrangement units. After sintering, the units are cut and separated along the area where the spacer or groove wall is located to obtain multiple independent single-layer diamond heat dissipation substrates at one time.
[0057] Comparative Example 1 Configuration: T2 copper plate, 0.1mm thick copper foil, HPHT single crystal diamond particles with an average particle size of 500μm; groove depth set to 600μm; Preparation method: The surface of a 2mm thick T2 copper plate is machined with a completely enclosed square groove on all four sides. The groove has no side openings and each groove is an independent closed cavity. The groove size matches the diamond particles. After processing, diamond particles are manually placed from the top of the groove into each individual groove. A vibrating table is used to vibrate and level the surface, and a scraper removes excess diamonds from the top of the groove. Single-layer arrangement is achieved by relying on the physical limit of the grid wall. The entire surface of the grooves is covered with 0.1mm copper foil and sealed to obtain a sealed prefabricated part; The same low-temperature high-pressure sintering process was used: 600℃, 300MPa, heat preservation for 20 minutes, and heat dissipation substrate was obtained after cooling.
[0058] Comparative Example 2 T2 copper strips with a width of 3mm and a height of 2mm and a 3×3 grid (4 horizontal + 4 vertical strips, a total of 8 strips) are fixed to the bottom copper sheet of 120mm×2mm thick T2 copper by spot welding. The diameter of the weld spot is 0.5–3mm. Diamond (HPHT, 210–230 μm) was placed within a grid cell and subjected to a temperature of 800℃, a pressure of 50 MPa, and a vacuum of ≤10 °C. -2 SPS sintering was carried out under Pa conditions and held at that temperature for 15 min. After sintering and holding, the furnace is cooled to 350°C at a rate of 50°C / min and held for 2 hours to eliminate interfacial thermal stress. The horizontal and vertical strips of the copper grid can simultaneously serve as the outer copper frame of each cell. After one sintering, the copper strips are cut along the copper strips, approximately Φ32mm equivalent (square unit ~28×28mm), a total of 9, to obtain multiple substrates with machinable outer perimeters.
[0059] Performance testing: All samples had an average diamond particle size of 500 μm and a uniform diamond volume fraction of 60 vol%. The finished substrate size was 100 mm × 50 mm. Fifty wafers were prepared simultaneously for yield statistics for each group of samples, and 10 wafers were randomly selected for thermal and microscopic testing. (1) Thermal conductivity: The laser scintillation method was used, and the test was conducted in accordance with T / CIET 1209-2025 "Test Method for Thermal Conductivity of Diamond / Copper Composite Materials"; (2) Coefficient of thermal expansion (CTE): The average coefficient of thermal expansion in the range of 25 to 150℃ is used, and the test is based on GB / T4339; (3) Diamond single-layer integrity: The percentage of the effective heat dissipation area with no particle stacking and no missing material is counted by using SEM scanning of the longitudinal section of the substrate; (4) First-time production yield: The proportion of qualified substrates with no double-layer stacking, no large-area material shortage, and no interface delamination in the total output. (5) Relative processing cost and relative loading time: Dimensionless comparison was made with Example 1 as the baseline value of 1.00.
[0060] The test results of the substrates prepared in Examples 1-3 and Comparative Examples 1-2 are shown in Table 1 below. Table 1. Substrate performance test results in Examples 1-3 and Comparative Examples 1-2
[0061] Data analysis: In Comparative Examples 1-2, the thermal conductivity was only 594-601 W / (m·K), and the CTE was high at 6.84-6.91 ppm / ℃. In Examples 1-3 of this invention, the thermal conductivity range was 628-632 W / (m·K), and the CTE was stable at 6.52-6.58 ppm / ℃. This is because manual filling of independent grid cells easily leads to local double-layer stacking of particles and local blank areas with insufficient material. The double-layer diamond will form a thermal barrier, and the proportion of pure copper in the blank area will increase, resulting in a decrease in overall thermal conductivity and an increase in the coefficient of thermal expansion. The narrow-slit gravity continuous filling of this invention has a uniform single-layer distribution of particles, and the effective thermal conduction path of diamond is continuous and complete, resulting in better thermal performance and less batch fluctuation. Comparative Example 1 had an integrity of 86.3%, with about 10% of the area having double-layer diamond stacking and blank areas at the corners of the grid. The array batch scheme of Comparative Example 2 had an integrity of only 83.6%, with poor consistency of multi-grid independent filling, and larger areas of stacking and blank areas. The present invention achieves a single-layer integrity of ≥97.9%, with only a very small amount of minor material shortage at the edges, and no double-layer stacking areas. It relies on the gap height and particle size for self-limitation, eliminating particle displacement caused by manual leveling or vibration disturbance throughout the process. The single-cavity solution of the present invention has a yield of 92%–94%, and the array batch solution has a yield of 91.5%. In contrast, the yield of a single substrate in Comparative Example 1 is only 73%, and the yield of the batch array in Comparative Example 2 is as low as 68%. A large number of defective products are due to particle stacking, large-area material shortage, and local metal foil bulging and delamination. Furthermore, Comparative Examples 1 and 2 require milling a large number of independent square grid four-sided groove walls, which greatly increases the precision machining time and the processing cost is more than 30% higher than that of the present invention. The present invention's double-plate sealed design does not require milling grooves and relies only on spacer wires for positioning, resulting in the lowest processing cost. Manual filling, vibration, and scraper leveling of each grid takes about 3 times longer than the gravity filling solution of the present invention, while the present invention only requires continuous gravity feeding through end openings, without the need for auxiliary tooling. Batch array multi-channels can be filled simultaneously, further reducing the processing time.
[0062] In summary, compared to the closed, independent groove technology in Comparative Example 1, this invention eliminates the precision machining of the compartment walls corresponding to each particle, and uses end-through narrow slits to achieve continuous gravity filling, eliminating the need for vibration and scraper fixtures, resulting in significant advantages in processing costs and filling efficiency. Compared to the array-closed square batch technology in Comparative Example 2, although the method described in this invention retains the batch processing approach of integrated sintering and cutting, the cavity structure and filling process are different. Its array-type multi-channel narrow slit pockets do not require the machining of a large number of separating metal ribs, and multiple cavities can be simultaneously and continuously filled by gravity, resulting in batches... Mass production time and processing costs are significantly reduced, and batch products exhibit better uniformity. Furthermore, while the technical solutions in Comparative Examples 1-2 rely on solid groove walls to divide particles to achieve a single layer, this invention achieves self-single-layer arrangement by relying on the size constraints of narrow slit gaps and diamond particle size. This eliminates the need for processing precise positioning structures that correspond one-to-one with the particles, significantly reducing processing costs. Its gravity filling integration completes single-layer positioning and filling, making the process simple, adaptable to diamond particles of different sizes, and capable of multi-cavity arrays for batch preparation. The resulting metal matrix composite heat dissipation substrate has a uniform diamond single-layer distribution and excellent high thermal conductivity.
[0063] The above embodiments are merely preferred embodiments of the present invention and are not intended to limit the present invention. The scope of protection of the present invention is determined by the appended claims.
[0064] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the specific implementation of the present invention. Any modifications or equivalent substitutions that do not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. A method for arranging single-layer diamond particles based on a narrow-slit pocket structure, characterized in that, Includes the following steps: A pocket-shaped cavity with a predetermined gap height is formed between the first sheet metal and the second sheet metal, and the pocket-shaped cavity has at least one unclosed opening edge; Diamond particles are injected into the pocket-shaped cavity through the edge of the opening to form a single-layer particle layer; The opening edges are sealed, and then a closed, narrow-slit, pocket-shaped filling structure is formed by hot pressing and sintering.
2. The method for arranging single-layer diamond particles based on a narrow-slit pocket structure according to claim 1, characterized in that, The first sheet metal and the second sheet metal are each independently selected from one of pure copper, copper alloy, pure aluminum or aluminum alloy; the preset gap height is 1.0 to 1.5 times the average particle size of the diamond particles.
3. The method for arranging single-layer diamond particles based on a narrow-slit pocket structure according to claim 1, characterized in that, The diamond particles are one of HPHT single-crystal diamond, CVD diamond, or natural diamond; the injection method into the pocket-shaped cavity is pure gravity injection.
4. The method for arranging single-layer diamond particles based on a narrow-slit pocket structure according to claim 1, characterized in that, The pocket-shaped cavity is formed by sealing the first sheet metal and the second sheet metal together with spacers along three edges, and the fourth edge without the spacers constitutes the opening edge.
5. The method for arranging single-layer diamond particles based on a narrow-slit pocket structure according to claim 4, characterized in that, The spacer is a metal strip or wire with a circular, square, or rectangular cross-section. The spacer is temporarily fixed to the first sheet metal and the second sheet metal by spot welding, mechanical clamping, or thermally conductive adhesive.
6. The method for arranging single-layer diamond particles based on a narrow-slit pocket structure according to claim 1, characterized in that, The surface of the first sheet metal is processed with a groove, at least one edge of the groove extends through the edge of the first sheet metal to form the opening edge; the second sheet metal covers the opening surface of the groove and together with the first sheet metal forms the pocket-shaped cavity, and the depth of the groove is the preset gap height.
7. The method for arranging single-layer diamond particles based on a narrow-slit pocket structure according to claim 6, characterized in that, The groove is formed on the surface of the first sheet metal by any one of mechanical milling, electrical discharge machining or laser processing; the second sheet metal is a foil.
8. The method for arranging single-layer diamond particles based on a narrow-slit pocket structure according to claim 1, characterized in that, The hot pressing sintering is low-temperature high-pressure sintering, and the parameters of the low-temperature high-pressure sintering are: sintering temperature 550~650℃, pressure 250~350MPa, and holding time 10~30min.
9. A metal-based composite material heat dissipation substrate, characterized in that, The heat dissipation substrate is prepared by the method according to any one of claims 1-8, and comprises upper and lower surface metals formed by a first sheet metal and a second sheet metal, a single layer of diamond particles located between the upper and lower surface metals, and an edge metal frame region surrounding the single layer of diamond particles.
10. A metal matrix composite heat dissipation substrate according to claim 9, characterized in that, The edge metal frame region is essentially free of diamond particles, and the edge metal frame region originates from the location of the spacer member or from the edge region of the first sheet metal where no groove is formed.
Citation Information
Patent Citations
Diamond particle mololayer heat spreaders and associated methods
US8531026B2