Welding process and tooling for thin-plate austenitic stainless steel profiles with long weld seams

By employing efficient laser welding technology and specialized tooling, the problems of welding deformation and defects in large-size thin-plate austenitic stainless steel profiles with long welds have been solved, achieving high-precision and high-reliability welding results that meet the manufacturing requirements of nuclear fusion devices.

CN123060263APending Publication Date: 2026-11-10HEFEI INSTITUTE OF PHYSICAL SCIENCE CHINESE ACADEMY OF SCIENCES +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611534717.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing welding processes and tooling cannot effectively address defects such as large welding deformation, uneven weld formation, residual stress concentration, and welding porosity in large-size, thin-plate, long-weld austenitic stainless steel profiles, making it difficult to meet the high precision and high reliability requirements of nuclear fusion devices.

Method used

The process employs high-efficiency laser welding technology combined with specialized tooling, including manual TIG locating spot welding, double-sided single-pass laser locating welding, laser deep penetration welding, and laser filler wire cover welding, along with vibration aging treatment, to control welding deformation and improve weld quality.

Benefits of technology

The overall post-weld tolerance was better than ISO 13920-BF, the weld quality passed the EN15614-1 physical and chemical property test, the deformation of the welded profile was controlled within 1.2mm/1m, the weld quality was high, the deformation caused by heat input was reduced, and the welding efficiency and reliability were improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123060263A_ABST
    Figure CN123060263A_ABST
Patent Text Reader

Abstract

This invention discloses a welding process and tooling for thin-plate austenitic stainless steel profiles with long welds, belonging to the field of stainless steel precision welding technology. The welding process includes the following steps: placing the welding tooling on a welding workbench; assembling the austenitic stainless steel sheet to be welded onto the welding tooling to obtain the structure to be welded; performing manual TIG tack welding on the structure to be welded; performing laser tack welding on the structure to be welded after manual TIG tack welding; performing laser deep penetration welding on the structure to be welded after laser tack welding; performing laser filler wire capping welding to reinforce the weld; and performing post-weld straightening and stress relief treatment on the welded profile after laser filler wire capping welding. The welded profile produced by this invention exhibits high weld quality, minimal welding deformation, and low post-weld magnetic permeability, making it suitable for the mass production of large-size precision structural profiles for nuclear fusion devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of stainless steel precision welding technology, specifically relating to a welding process and tooling for thin-plate long-weld austenitic stainless steel profiles, applicable to the manufacturing of large-size precision structural profiles for nuclear fusion devices. Background Technology

[0002] ITER (International Thermonuclear Experimental Reactor) is the world's largest international nuclear fusion research and cooperation project, aiming to verify the engineering feasibility and commercial application prospects of controlled nuclear fusion energy. Among its components, the integrated atmospheric diagnostic system is the core supporting structure of the ITER plasma diagnostic system, directly supporting various precision diagnostic equipment. Its structural forming precision, overall stability, and welding reliability directly determine the accuracy of plasma physics parameter acquisition and the safety of device operation, making it a key component for the stable operation of the tokamak device.

[0003] The ITER diagnostic integrated atmospheric side system comprises multiple precision positioning support structures and nuclear shielding structures, with an overall weight exceeding 100 tons. The main structure is primarily constructed from radiation-resistant austenitic stainless steel plates, profiles, and forgings such as 316L(N)-IG and SS660, with internal boron-concrete filling forming the shielding system. These stainless steel profiles are mostly large-sized structures ranging from 3m to 6m, with plate thicknesses ranging from 5mm to 20mm, exhibiting characteristics of large size, thin plates, and long welds. Furthermore, this fusion-grade stainless steel material must meet stringent nuclear-grade performance requirements, including extremely low activation, radiation resistance, and the ability to withstand extreme operating loads. The overall structure also requires non-standard customization based on the diagnostic equipment layout. Traditional integral forming processes such as integral extrusion and integral rolling are difficult to adapt to the production needs of customized large-sized profiles; therefore, the industry generally adopts thin-plate welding to complete the overall structural forming.

[0004] Currently, for large-size, thin-plate, long-weld nuclear-grade austenitic stainless steel profiles, the welded structures need to achieve welding processes with lengths of 3m-6m and plate thicknesses of 5mm-20mm. Existing conventional welding processes and general-purpose tooling have significant technical shortcomings. Conventional welding methods are prone to defects such as large welding deformation, uneven weld formation, residual stress concentration, weld porosity, and incomplete fusion during the welding of thin plates and long welds, making it difficult to meet the high-precision dimensional tolerances and high-reliability service requirements of fusion devices. At the same time, existing general-purpose tooling lacks specificity and cannot achieve precise positioning and efficient welding of large-size thin-plate profiles. There is a lack of dedicated welding processes and matching tooling adapted to ITER nuclear-grade large-size thin-plate profiles with long welds, which restricts the welding quality and mass production efficiency of such key fusion structural profiles.

[0005] In summary, given the shortcomings of existing technologies, there is an urgent need to develop a long-seam welding process and specialized tooling suitable for large-size thin-plate austenitic stainless steel profiles (length-to-thickness ratio of 1000 or more) to solve the technical problems of insufficient customization, poor process forming accuracy, numerous welding defects, and uncontrollable deformation, and to meet the high-precision and high-reliability manufacturing requirements of nuclear-grade structural profiles for nuclear fusion devices. Summary of the Invention

[0006] To solve the above-mentioned technical problems, the present invention provides a welding process for thin-plate austenitic stainless steel profiles with long welds. This process can effectively improve the weld quality and avoid welding deformation of long plates with low thickness.

[0007] A further technical problem to be solved by the present invention is to provide tooling suitable for the welding process of the above-mentioned thin-plate long-weld austenitic stainless steel profiles.

[0008] To achieve the above objectives, the present invention adopts the following technical solution:

[0009] A high-efficiency laser welding process for thin-plate austenitic stainless steel profiles with long welds is characterized in that the length-to-thickness ratio of the austenitic stainless steel plate to be welded is 1000~1500:1, and the length of the continuous full-penetration weld formed after welding is 6~10m.

[0010] The welding process includes the following steps:

[0011] S1: Place the welding device on the welding workbench;

[0012] S2: Assemble the austenitic stainless steel sheet to be welded onto the welding fixture, and control the gap between the butt joint surfaces to be ≤0.2mm to obtain the structure to be welded;

[0013] S3: Perform manual TIG tack welding on the structure to be welded; during operation, take the center of the butt joint area as the reference point, and tack weld symmetrically to both ends, alternating between the front and back sides, with a point spacing of 80~120mm.

[0014] S4: Laser tack welding for double-sided single-pass welding; laser tack welding is a multi-segment continuous weld, with a single segment length of 100~160mm, a spacing between adjacent segments of 400~600mm, and a penetration depth of 2~3mm;

[0015] S5: Laser deep penetration welding for double-sided single-pass welding; laser deep penetration welding is symmetrical welding from the middle reference point to both ends, with a single-pass penetration depth ≥3.5mm and a penetration depth ≥1.5mm in the overlapping area of ​​the weld on both sides;

[0016] S6: After laser deep penetration welding is completed, laser filler wire cover welding is performed on the local area where the weld is lower than the base material;

[0017] S7: After the laser filler wire cover welding is completed, vibration aging treatment and post-weld straightening treatment are carried out in sequence.

[0018] The beneficial effects of this invention are as follows:

[0019] (1) This invention proposes a new welding process for welding stainless steel plates with thin plates and long welds, resulting in welded profiles with overall tolerances better than ISO 13920-BF and overall deformation controlled within 1.2mm / 1m. The weld quality has passed the physical and chemical performance test according to EN15614-1 and various non-destructive testing requirements, resulting in high weld quality.

[0020] (2) This invention mainly employs laser welding, combined with welding fixtures, to achieve automatic welding of profiles, thereby reducing heat input during the welding process, controlling welding deformation, and reducing subsequent straightening and machining work in the profile manufacturing process, thus achieving high-precision forming and manufacturing of profiles. Through the design of the welding fixtures and the control of the welding sequence, this invention reduces the number of repeated clamping operations during the welding process, improving the efficiency of single-sided welding.

[0021] (3) This invention achieves significant improvements in the quality, precision, and efficiency of profile welding by employing a system solution that combines automated laser welding with specialized tooling fixtures. Compared to traditional manual welding, laser welding features high energy density and low heat input, effectively refining the weld structure and reducing the heat-affected zone, thereby obtaining welded joints with higher strength and more stable performance. Combined with the excellent properties of 316L(N)-IG material itself, the profiles manufactured by this invention are superior to traditional products in terms of load-bearing capacity and dimensional accuracy, providing more reliable technical support for the peripheral structure of fusion devices.

[0022] (4) In terms of process control, the laser automatic welding process is stable and has good repeatability, which significantly reduces the impact of human factors on the forming quality and improves product consistency and forming accuracy. At the same time, the process does not require beveling, and with its inherent high precision characteristics, it usually does not require machining after welding to meet assembly requirements, thereby improving product quality while simplifying the manufacturing process and improving efficiency.

[0023] (5) The present invention has outstanding advantages in terms of material utilization. Traditional profile manufacturing mostly adopts manual or submerged arc welding, which requires continuous consumption of additional materials such as welding wire and flux. However, the laser self-fusion welding adopted in the present invention does not require any additional welding materials, which not only saves material costs and improves material utilization, but also avoids metallurgical inhomogeneity that may be caused by the difference in composition between the filler metal and the base material through the self-fusion connection of the materials, further ensuring the performance and reliability of the welded joint.

[0024] (6) The present invention also uses vibration aging to partially release and homogenize the stress of the welded profile. Unlike traditional heat treatment to relieve stress, vibration aging mainly achieves the homogenization of residual stress in the profile, reduces the residual stress gradient, and slightly reduces the residual stress at some measuring points. This avoids the deterioration of the performance of austenitic stainless steel materials caused by high-temperature heat treatment, thereby further improving the stability of the profile in the application scenario. Attached Figure Description

[0025] Figure 1 This is a weld diagram showing the PA welding position in the welding process of the thin-plate long-weld austenitic stainless steel profile of the present invention; wherein... Figure 1 (a) in the figure is a macroscopic weld diagram of an 8mm thick L-shaped profile; Figure 1 (b) in the figure is a macroscopic weld diagram of an 8mm thick T-section; Figure 1 (c) in the figure is a macroscopic weld diagram of a 10mm thick L-shaped profile; Figure 1 (d) in the figure is a macroscopic weld diagram of a 10mm thick T-section.

[0026] Figure 2 This is a weld diagram showing the PC welding position of the welding process for the thin-plate long-weld austenitic stainless steel profile of the present invention; wherein... Figure 2 (a) in the figure is a macroscopic weld diagram of a 10mm thick T-section; Figure 2 (b) is a macroscopic weld diagram of an 8mm thick L-shaped profile.

[0027] Figure 3 This is a picture of a physical object using 5KW single-sided welding.

[0028] Figure 4 This is a picture of a physical object using 4KW single-sided welding.

[0029] Figure 5 This is a picture of a product using 3KW double-sided welding.

[0030] Figure 6 This is a photograph of a sample of laser deep penetration welding.

[0031] Figure 7 This is a photograph of a laser deep penetration weld combined with laser filler wire cover weld.

[0032] Figure 8 This is an overall schematic diagram of the welding fixture for the thin-plate long-weld austenitic stainless steel profile of the present invention.

[0033] Figure 9 for Figure 8 The diagram shown illustrates the welding fixture used for welding L-shaped angle steel.

[0034] Figure 10 for Figure 8 The diagram shows a welding fixture used for welding H-beams.

[0035] Figure 11 for Figure 8 The diagram shown illustrates the welding fixture used for welding C-shaped channel steel.

[0036] Figure 12 This is an overall schematic diagram of the straightening fixture for the thin-plate long-weld austenitic stainless steel H-beam profile of the present invention.

[0037] Figure 13 This is a schematic diagram of the welding equipment mounted on the welding work platform.

[0038] Figure 14 This is a schematic diagram of the overall assembly of the austenitic stainless steel sheet to be welded onto the welding fixture.

[0039] Figure 15 This is a schematic diagram of the multi-segment tack welding process in Example 1.

[0040] Figure 16 This is a schematic diagram of the welding sequence of the L-shaped angle steel profile in Example 1.

[0041] Figure 17 This is a comparison cloud diagram of the L-shaped angle steel profile obtained in Example 1 and the theoretical model.

[0042] Figure 18 The radiographic inspection results of the L-shaped angle steel profile obtained after laser cover welding in Example 1 are shown in the films at different locations of the weld. Figure 18 (a) is a radiograph of the weld seam of the L-shaped angle steel profile at the 1 / 4 position; Figure 18 (b) is a radiograph of the L-shaped angle steel profile at the 2 / 4 position of the weld seam; Figure 18 (c) is a radiograph of the L-shaped angle steel profile at the 3 / 4 position of the weld seam; Figure 18 (d) is a radiograph of the 4 / 4 position of the weld seam of the L-shaped angle steel profile.

[0043] Figure 19 These are before-and-after comparison images of the bending test of the welded joint obtained by the welding method described in this invention. Figure 19 (a) in the diagram is the test chart before the full experiment. Figure 19 (b) in the figure is the test diagram after the bending test.

[0044] Figure 20 These are before-and-after comparison images of room temperature tensile tests on welded joints obtained using the welding method described in this invention. Figure 20 (a) in the figure is the test diagram before the room temperature tensile test. Figure 20 (b) in the figure is the test diagram after the room temperature tensile test.

[0045] Figure 21These are before-and-after comparison images of the high-temperature tensile test results of the welded joint obtained using the welding method described in this invention. Figure 21 (a) in the figure is the test diagram before the high temperature tensile test. Figure 21 (b) in the figure is the test diagram after the high temperature tensile test.

[0046] Figure 22 These are before-and-after comparison images of the impact test results of the welded joint obtained using the welding method described in this invention; wherein... Figure 22 (a) in the diagram is the test diagram before the impact test. Figure 22 (b) in the figure is the test diagram after the impact test.

[0047] Figure 23 This is a schematic diagram showing the relative permeability test results of the welded joint obtained using the welding method described in this invention; wherein... Figure 23 (a) shows the relative permeability test results of the weld zone. Figure 23 (b) in the figure shows the magnetic permeability test results of the heat-affected zone.

[0048] Figure 24 This is a schematic diagram of the welding sequence for C-shaped profiles.

[0049] Figure 25 This is a schematic diagram of the welding sequence for T-shaped profiles.

[0050] Figure 26 This is a physical image of the C-shaped channel steel profile obtained in Example 2.

[0051] The attached diagram is labeled as follows: 1-Fixed base plate; 2-Fixed base; 3-Side top mounting bolt; 4-Fixed nut; 5-Upper limit bolt; 6-Side top plate; 7-Vertical plate; 8-Horizontal plate; 9-Internal support plate; 10-Top limit plate; 11-Bolt sleeve; 100-Correcting fixture; 200-Profile to be corrected; 300-Hydraulic pressure head. Detailed Implementation

[0052] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention. Furthermore, the technical features involved in the various embodiments of this invention described below can be combined with each other as long as they do not conflict with each other.

[0053] A welding process for thin-plate austenitic stainless steel profiles with long welds, wherein the length-to-thickness ratio of the austenitic stainless steel plate to be welded is 1000~1500:1, and the weld length is 6~10m. The length-to-thickness ratio is the ratio of the total effective weld length of a single plate to the nominal thickness of the plate, and the nominal thickness of the plate is 5~20mm. The welding process includes the following steps:

[0054] S1: Place the welding device on the welding workbench;

[0055] S2: Assemble the austenitic stainless steel sheet to be welded onto the welding fixture, and control the gap between the butt joint surfaces to be ≤0.2mm to obtain the structure to be welded;

[0056] S3: Argon gas protection is used to perform manual TIG positioning spot welding on the structure to be welded to achieve pre-fixation of assembly; specifically, the center of the docking area is used as the reference point, and spot welding is performed symmetrically and alternately on both sides, with a spot spacing of 80~120mm.

[0057] S4: Laser tack welding is performed under nitrogen protection after manual TIG tack welding, with double-sided single-pass welding. Laser tack welding consists of multiple continuous welds, with a single segment length of 100~160mm, a spacing between adjacent segments of 400~600mm, and a penetration depth of 2~3mm. Laser tack welding is used to increase structural rigidity and constrain deep penetration weld deformation.

[0058] S5: After laser tack welding, double-sided single-pass laser deep penetration welding is performed under nitrogen protection; laser deep penetration welding is symmetrically welded from the middle reference to both ends, with a single-pass penetration depth ≥3.5mm, and a penetration depth ≥1.5mm in the overlapping area of ​​the positive and negative welds, achieving full penetration of the entire weld length.

[0059] S6: After laser deep penetration welding is completed, laser filler wire cover welding is performed on the local area where the weld is lower than the base material to ensure that the weld surface is not lower than the base material;

[0060] S7: After the laser filler wire cover welding is completed, vibration aging treatment and post-weld straightening treatment are carried out in sequence.

[0061] The austenitic stainless steel sheet used in this invention is 316L(N)-IG.

[0062] The inventive concept of this invention is as follows:

[0063] I. Selection of welding position.

[0064] Welding position is one of the important variables in welding scheme, and it plays a decisive role in weld formation and molten pool flow.

[0065] This embodiment tested three welding positions: PA, PB, and PC. The PA welding position refers to the welding position where the laser beam welds the workpiece surface from top to bottom. The welding torch angle range, centered at vertically downwards and capable of rotating ±30°, is considered the PA welding position. The PB welding position is at a 45° left or right tilt; the welding position is within a range of +15° / -10° centered on this point. The PC welding position is at a horizontal 0° angle; the welding position is within a range of +35° / -10° centered on this point.

[0066] In comparison, in both PB vertical welding and PC horizontal welding, the molten metal flows along the workpiece surface in the direction other than the weld seam under the influence of gravity. Therefore, additional measures are needed to suppress the gravity effect of the molten pool, which is difficult to control and prone to weld inhomogeneity. However, in PA welding, the gravity direction of the molten pool is vertically downward, and gravity assists the molten pool to naturally fill the bevel gap, which perfectly meets the filling direction of weld formation.

[0067] Figure 1 This is a weld diagram showing the PA welding position in the welding process of the thin-plate long-weld austenitic stainless steel profile of the present invention; wherein... Figure 1 (a) in the figure is a macroscopic weld diagram of an 8mm thick L-shaped profile; Figure 1 (b) in the figure is a macroscopic weld diagram of an 8mm thick T-section; Figure 1 (c) in the figure is a macroscopic weld diagram of a 10mm thick L-shaped profile; Figure 1 (d) in the figure is a macroscopic weld diagram of a 10mm thick T-section. Figure 2 This is a weld diagram showing the PC welding position of the welding process for the thin-plate long-weld austenitic stainless steel profile of the present invention; wherein... Figure 2 (a) in the figure is a macroscopic weld diagram of a 10mm thick T-section; Figure 2 (b) in the diagram is a macroscopic weld view of an 8mm thick L-shaped profile. From... Figure 1 and Figure 2 The comparison results show that the PA welding position has a better welding effect.

[0068] In addition, at the PA welding position, the gravity direction of the liquid molten pool metal is vertically downward. Gravity assists the molten pool metal to naturally fill the groove gap, which perfectly meets the filling direction of weld formation (red text repeated). This works in synergy with the keyhole effect formed by laser welding. It avoids keyhole collapse caused by gravity and the opposite direction of molten pool flow at non-PA welding positions. At the same time, the gas in the molten pool (such as metallurgical reaction gas and protective gas) can escape smoothly along the direction of gravity, reducing porosity defects from the root.

[0069] Furthermore, at the PA welding position, the molten pool exhibits uniform crystallization direction under the combined constraints of gravity and surface tension, suppressing columnar crystal growth and resulting in high weld metal density. Additionally, the slag, due to its density difference, can smoothly float to the weld surface, avoiding slag inclusions. Ultimately, the tensile strength and fatigue resistance of the weld are significantly superior to welds welded at non-PA welding positions, and the weld quality is easier to control and optimize.

[0070] Meanwhile, the PA welding position allows for high laser power and high welding speed process parameters without sacrificing deposition efficiency to suppress molten pool flow; and the laser head posture is stable during the welding process, eliminating the need to frequently adjust key parameters such as defocusing amount and shielding gas direction, which greatly improves the consistency of weld formation.

[0071] Based on the above analysis and experimental structure, for the welding structure of thin-walled long plates, which is the subject of this study, the control of welding deformation is quite difficult, and the quality consistency requirements of long welds are high. Therefore, the PA flat welding position is selected, which can effectively ensure the uniformity of the weld. At the same time, the PA welding position ensures good flow and solidification of the molten pool, and has a large adjustment range for welding parameters, which is conducive to the control of welding deformation in the later stage by welding parameters and welding sequence.

[0072] Compared with other welding positions, PA has significant advantages for welding such thin-walled long plates. Therefore, from the perspective of welding quality, the welding position for this technical solution is determined to be the PA welding position.

[0073] II. Selection of welding methods in laser tack welding and laser deep penetration welding.

[0074] For welding thin plates, both single-sided and double-sided welding can achieve weld formation. Welding tests are used to select the welding method for practical application.

[0075] Welding tests were conducted using an 8mm L-shaped joint as an example.

[0076] Single-sided welding: 5KW laser power is selected, with the laser beam directed from the flat welding area, achieving single-sided welding and double-sided forming. Metallographic images of the welded samples are shown below. Figure 3 As shown; from Figure 3 It can be seen that there are areas of incomplete penetration in the sample. Figure 3 (The two red lines in the image). Further increasing the power to 6KW, the metallographic photograph of the welded sample is shown below. Figure 4 As shown, from Figure 4 It can be seen that there are no incomplete penetration areas in the sample, but due to the high power of the laser beam, a large amount of base material is melted, and the weld surface appears to be lower than the base material, resulting in an incomplete weld shape.

[0077] Double-sided welding: A 3KW laser power was selected, with the laser beam directed from the flat welding area, resulting in double-sided welding and forming. Metallographic images of the welded samples are shown below. Figure 5As shown. From Figure 5 It can be seen that double-sided welding achieves weld formation, and the weld on the front side has a relatively full shape.

[0078] In summary, while single-sided welding can achieve the effect of double-sided forming, excessive heat input can lead to the weld seam being lower than the base material, and excessive heat input in the final product can also cause significant welding deformation. Therefore, this invention employs double-sided welding to reduce welding heat input and minimize welding deformation while ensuring weld quality.

[0079] III. Determination of Welding Parameters.

[0080] This invention provides different welding parameters for different joints to obtain welds with good welding effects.

[0081] According to ISO industry standards, welding procedure qualification must be performed before welding production activities to ensure that welding parameters and process plans can achieve the welding quality required for the product.

[0082] The ISO-15614 industry standard specifies the relevant requirements for welding procedure qualification. The object of welding procedure qualification is not the product itself, but rather the weld joint structure corresponding to each welding position. Therefore, the determination of all welding process parameters will revolve around the design and verification of the weld joints. For this product, analysis shows that the main weld joints are divided into 6mm L-shaped angle steel joints, 8mm L-shaped angle steel joints, 6mm L-shaped joints, 8mm L-shaped joints, 10mm L-shaped joints, and 14mm L-shaped joints. Therefore, appropriate welding parameters will be determined to achieve the welding of these six joint structures.

[0083] According to the standard, the nine categories of factors that constitute important elements for welding procedure qualification in laser welding processes are weld joint, base material, filler metal, welding position, preheating, post-weld heat treatment, gas, electrical properties, and welding techniques. This means that the determination of welding parameters must take all nine variables into account.

[0084] In this invention, the welding position is determined to be PA, and the base material and shielding gas are also determined. Therefore, the welding parameters (electrical properties) are mainly determined based on the existing base material, weld joint, and weld thickness. Through various experiments, the laser welding power and defocusing amount are determined to ensure the thickness of the weld penetration; the welding speed and wire feed speed are determined to ensure the uniformity and consistency of the weld. The determination of welding parameters is based on various mechanical property tests of the plate material in the welding process qualification test, and the final test results serve as the main basis for supporting the qualification of the welding parameters.

[0085] The final welding parameters are as follows:

[0086] (1) For T-shaped profiles, the welding power of laser tack welding is 1800±200W, the rising distance (length of the arc transition section) is 15~25mm, the falling distance (length of the arc termination section) is 20~30mm, there is no overlap, the defocusing amount is 0mm, the longitudinal beam angle is 12±2°, the transverse beam angle is 90°; the welding speed is 0.5~0.7m / min; the front shielding gas flow rate is 35~45 L / min; the angle between the gas shielding nozzle and the surface of the structure to be welded is 60°, and the distance between the gas shielding nozzle and the surface of the structure to be welded is ≤25mm.

[0087] For T-shaped profiles, the welding power of laser deep penetration welding is 3800~5200W (3800~4200W for 6mm thickness and 4800~5200W for 8mm thickness), the rise distance is 15~50mm, the fall distance is 20~100mm, the overlap distance is 0~50mm, the defocusing amount is 0mm, the longitudinal beam angle is 12±2°, and the transverse beam angle is 90°; the welding speed is 0.5~0.7m / min; the front shielding gas flow rate is 35~45 L / min; the angle between the gas shielding nozzle and the surface of the structure to be welded is 60°, and the distance between the gas shielding nozzle and the surface of the structure to be welded is ≤25mm.

[0088] For T-shaped profiles, the welding power for laser filler wire cover welding is 4100~4500W, the rise distance is 15~50mm, the fall distance is 20~100mm, the overlap distance is 0~50mm, the defocusing amount is 50-100mm, the longitudinal beam angle is 26±2°, and the transverse beam angle is 90°; the welding speed is 0.4~0.6m / min; the wire feed speed is 2.7~3.7 m / min; the front shielding gas flow rate is 35~45 L / min; the angle between the gas shielding nozzle and the surface of the structure to be welded is 60°, and the distance between the gas shielding nozzle and the surface of the structure to be welded is ≤25mm.

[0089] (2) For L-shaped angle steel profiles, the welding power of laser positioning welding is 1600~3200W (of which the welding power of 6mm thickness is 1600~2200W, the welding power of 8mm is 1800~2200W, and the welding power of 10mm and above is 2800~3200W), the rising distance is 15~25mm, the falling distance is 20~30mm, there is no overlap, the defocusing amount is 0mm, the longitudinal beam angle is 0±1° when welding on the front side, the longitudinal beam angle is 12±2° when welding on the back side, and the transverse beam angle is 90° (both front and back welding are 90°); the welding speed is 0.5~0.7m / min; the front shielding gas flow rate is 35~45 L / min; the angle between the gas shielding nozzle and the surface of the structure to be welded is 60°, and the distance between the gas shielding nozzle and the surface of the structure to be welded is ≤25mm.

[0090] For L-shaped angle steel profiles, the specific welding power for laser deep penetration welding is as follows: 3800~4200W for 6mm thickness; 4800~5200W for the front side and 3800~4200W for the back side for 8mm thickness; 5800~6200W for the front side and 4800~5200W for the back side for 10mm thickness; and 7800~8200W for the front side and 5800~6200W for the back side for 14mm thickness. The laser deep penetration welding has an ascent distance of 15~50mm, a descent distance of 20~100mm, an overlap distance of 0~50mm, a defocusing amount of 0mm, a longitudinal beam angle of 0±1° for front welding and 12±2° for back welding, and a transverse beam angle of 90° (90° for both front and back welding); a welding speed of 0.5~0.7m / min; a front shielding gas flow rate of 35~45 L / min; an angle of 60° between the gas shielding nozzle and the surface of the structure to be welded; and a distance of ≤25mm between the gas shielding nozzle and the surface of the structure to be welded.

[0091] For L-shaped angle steel profiles, the welding power for laser filler wire cover welding is 4100~4500W, the rise distance is 15~50mm, the fall distance is 20~100mm, the overlap distance is 0~50mm, the defocusing amount is 50-100mm, the longitudinal beam angle is 26±2°, and the transverse beam angle is 90°; the welding speed is 0.4~0.6m / min; the wire feed speed is 2.7~3.7 m / min; the front shielding gas flow rate is 35~45 L / min; the angle between the gas shielding nozzle and the surface of the structure to be welded is 60°, and the distance between the gas shielding nozzle and the surface of the structure to be welded is ≤25mm.

[0092] In addition, the austenitic stainless steel used in this invention is 316L(N)-IG stainless steel, which contains 0.06~0.08% nitrogen. During welding, porosity and intergranular corrosion are prone to occur. It is necessary to strictly control the purity of the protective gas (Ar purity ≥99.99%) and the welding heat input parameters (including welding power, welding position, welding speed and other parameters).

[0093] This invention adds laser filler wire capping after laser deep penetration welding, based on the discovery that laser deep penetration welding results in... Figure 6 The phenomenon shown in the diagram where the surface of several weld joint areas is slightly lower than the base metal surface is attributed to the downward flow of molten metal along the weld seam. Therefore, laser filler wire capping welding is used to fill the weld seam, which not only ensures the weld seam shape but also provides reinforcement. The effect of laser filler wire capping welding is as follows: Figure 7 As shown, from Figure 7As can be seen, the resulting weld formation is good and can meet the reinforcement requirements of the weld. Preferably, this invention only requires one filler wire.

[0094] This invention employs a comprehensive welding process combining manual TIG locating spot welding, laser locating welding, laser deep penetration welding, and laser filler wire cover welding. Manual TIG locating spot welding is convenient and efficient, with the spot weld ultimately fused into the weld seam without affecting its quality. It effectively provides fixing force for subsequent laser locating welding, preventing deformation of the sheet metal caused by heat input during laser locating welding (preventing assembled products from cracking due to deformation). Laser locating welding is a regional locating welding process, arranging continuous locating welds with equal spacing and small penetration depths according to the weld seam length, forming a locating constraint area to prevent relative displacement of the profile during the thermal expansion and contraction process of subsequent deep penetration welding. Simultaneously, laser locating welding offers higher precision, achieving accurate welding reference points and providing a solid foundation for subsequent deep penetration welding. Laser deep penetration welding primarily serves to penetrate the weld and enhance its strength and fixation; determining the parameters for laser deep penetration welding ensures that the mechanical properties and morphology of the weld meet the actual working conditions and technical requirements of the product. Laser filler wire cover welding, to a certain extent, achieves a reinforcement effect on the weld seam.

[0095] Preferably, in step S2, the gap between the butt joint surfaces of the austenitic stainless steel plates to be welded is controlled to be ≤0.2mm.

[0096] Preferably, during the manual TIG positioning spot welding in step S3, argon gas protection (purity ≥99.99%) is turned on in advance, the argon gas flow rate is 11L / min, the welding voltage is 10V, and the welding current is 80A.

[0097] Preferably, in step S3, when performing manual TIG positioning spot welding, spot welding is performed symmetrically to the left and right ends with the reference point as the center, alternating between the front and back sides, and the distance between each spot is controlled at 80-120mm. Spot welding is performed to cover the entire butt joint area of ​​the austenitic stainless steel plate to be welded, and finally, one point is reinforced at each end of the austenitic stainless steel plate to be welded.

[0098] Manual TIG tack welding is preferably performed using argon arc filler wire welding. The welding current for argon arc filler wire welding is 80-100A, and the welding wire used for argon arc filler wire welding can be ER317L with a diameter of 1.0mm.

[0099] Preferably, the laser positioning welding in step S4 employs a multi-segment positioning welding process, specifically:

[0100] The first laser positioning weld starts from the reference point in step S3 and is performed at a distance of 50-80mm before and after the reference point. The weld length of the laser positioning weld is 100-160mm.

[0101] Using the center of the first laser tack weld as a reference, laser tack welding is performed symmetrically and segmentally towards both ends of the weld. The spacing between each tack weld is evenly distributed, and the distance between adjacent tack welds is 400-600mm.

[0102] Preferably, the laser deep penetration welding in step S5 has a welding depth of 1200-1500 mm.

[0103] Preferably, in step S5, the laser deep penetration welding is performed with the central reference as the center. Step S5 employs a welding method of welding the middle section first, followed by symmetrical welding on both sides. The process parameters for laser deep penetration welding in step S5 are: single-segment welding length 1200~1500mm, welding speed 0.5~0.7m / min, defocusing amount 0mm, and welding position is PA flat welding. The welding sequence is symmetrical segmented welding from the middle to both ends, with an overlap length of 80~120mm between adjacent welds. Specifically, a welding robot is used for laser deep penetration welding. The robot's movement path is adjusted, and the starting and ending points of the laser are set to the middle position of the butt joint gap between the plates to be welded. The welding process parameters are set, and welding begins after introducing the front shielding gas, the side shielding gas, and the back shielding gas. The welding robot's movement path is linear.

[0104] Preferably, the process parameters for laser filler wire cover welding in step S6 are: welding wire diameter 1.0 mm, longitudinal beam angle for welding the front and back sides is 26±2°, and transverse beam angle is 90°; welding speed 500±50 mm / min, wire feeding speed 2700~3700 mm / min, and defocusing amount 50~100 mm.

[0105] Preferably, the local weld of the laser filler wire cover weld in step S6 specifically refers to the weld area of ​​the welded joint being lower than the weld area of ​​the austenitic stainless steel plate to be welded.

[0106] Preferably, in step S7:

[0107] Vibration aging treatment includes: installing a vibrator and vibration pickup after supporting the profile, and starting the vibration program to achieve residual stress homogenization;

[0108] The corrective treatment includes: first, allowing the plate to stand for ≥12 hours, and then alternating the shrinkage of the wing plate, the plane of the wing plate, and the web plate in stages from the middle to both ends.

[0109] Preferably, the process also includes a pretreatment step for the welding surface of the austenitic stainless steel sheet to be welded. Specifically, this involves initial leveling, machining, and non-destructive testing (NDT), where the NDT includes visual inspection and liquid penetrant testing of the welding surface. This pretreatment is standard practice in the art and generally includes machining and cleaning of the welding surface. Preferably, the cleaning method involves wiping the welding surface with ethanol.

[0110] The base material (i.e., the austenitic stainless steel sheet to be welded) of the present invention needs to be cut by laser cutting. The heat-affected zone of laser cutting is removed by a large gantry planer in the material factory. After cleaning, the resulting sheet can be directly used for profile welding.

[0111] To achieve better welding results, this invention also provides a tooling for thin-plate austenitic stainless steel profiles with long weld seams, see [link to tooling]. Figure 8 This fixture includes a welding fixture for fixing austenitic stainless steel sheets to be welded. The welding fixture includes a fixed base plate 1, a fixed base 2, a side top plate 6, vertical plates 7, and a horizontal plate 8. Two fixed bases 2 are symmetrically mounted on the fixed base plate 1; two vertical plates 7 are symmetrically mounted on the two fixed bases 2 respectively; and the horizontal plate 8 is installed between the two vertical plates 7. A top limiting plate 10 is also provided at the top of each vertical plate 7 to limit its movement. The top limiting plate 10 is fixed to the fixed base 2 by bolt sleeves 11 and upper limiting bolts 5. Multiple welding fixtures can be configured in use, with a minimum distance of 250 mm between adjacent welding fixtures, suitable for clamping profiles 6-10 m long.

[0112] Preferably, an internal support plate 9 for supporting the horizontal plate 8 is provided below the horizontal plate 8; a side top plate 6 is provided on the outside of the vertical plate 7, and the side top bolt 3 passes through the fixing nut 4 and abuts against the side top plate 6 to fix the vertical plate 7 on the fixed base 2.

[0113] The schematic diagram of the welding fixture used for L-shaped angle steel is as follows: Figure 9 As shown, the fixed bases 2 on both sides are used to fix the L-shaped angle steel laterally by the side top bolts 3 and the vertical plate 7. The fixed base plate 1 used in this invention includes, but is not limited to, a special chassis (with bolt positioning holes) and a chassis with calibrated bolt holes. The fixed bases 2 on both sides can be adjusted according to different sizes of profiles. The internal support plate 9 supports the horizontal plate 8, and the side top plate 6 supports the vertical plate 7 to ensure that the height of the plates remains consistent during the welding process. The top uses bolt sleeves 11 and top limiting plate 10 to limit the longitudinal direction of the L-shaped angle steel. In the actual manufacturing process, the position of the top limiting plate 10 moves with the welding process to ensure that there is no positional interference with the laser welding gun.

[0114] A schematic diagram of I-beams installed on welding fixtures is shown below. Figure 10 As shown, the fixed bases 2 on both sides use side top bolts 3 and vertical plates 7 to laterally limit the I-beam workpiece. The upper end of the fixed base 2 is connected to the top limiting plate 10 through bolt sleeve 11 to limit the inward bending deformation of the wing plate caused by weld shrinkage. During the processing, the position of the pressure bar is arranged according to the actual welding needs to avoid positional interference with the welding equipment during the welding process.

[0115] Channel steel welding fixtures, such as Figure 11 As shown, the fixed bases 2 on both sides use side top bolts 3 and vertical plates 7 to laterally limit the channel steel; the bottom is supported by multiple sets of internal support plates 9; the pressure rods are arranged according to the actual welding process; after the channel steel is reversed, the bottom is replaced with temporary stainless steel support or stainless steel shims for support, the upper part is welded with the I-beam, and the top limiting plate 10 is installed to reduce the shrinkage deformation of the wing plate.

[0116] Preferably, the above welding fixture is optimized according to the angle of the welding torch. By designing the chamfer of the top limiting plate 10, interference between the top limiting plate 10 and the welding torch is avoided, ensuring smooth welding while reducing thermal deformation during the welding process.

[0117] Figure 12 This is a schematic diagram of the overall straightening fixture for the thin-plate long-weld austenitic stainless steel H-beam profile of the present invention (C-type and L-type have similar structures). The straightening fixture 100 is used for straightening treatment. In use, the profile 200 to be straightened is placed in the straightening fixture 100, and the top hydraulic press is used to straighten the profile 200. The hydraulic pressure head 300 is used sequentially to straighten the flange, web, etc.

[0118] Example 1:

[0119] This embodiment uses the welding of L-shaped angle steel profiles as an example to illustrate the welding process of the present invention.

[0120] The base material for welding (i.e., austenitic stainless steel sheet) is 316L(N)-IG, with a thickness of 6mm, a length of 6m, and a quantity of 2; the welding material is ER317L, with a diameter of 1.0mm.

[0121] A welding process for thin-plate austenitic stainless steel profiles with long weld seams includes the following steps:

[0122] Part 1: Pre-treatment of the sheet material.

[0123] (1) Initial leveling of the board material.

[0124] The purchased austenitic stainless steel raw materials, especially plates, will undergo a certain amount of deformation after long-term storage and transportation. Therefore, the plates will be preliminarily leveled before production begins.

[0125] The austenitic stainless steel sheet is placed in a straightening press, using a combination of room temperature and localized point straightening. Depending on the sheet thickness (6mm-20mm), the initial pressure is approximately 5MPa. First, hydraulic pressure is applied to the middle area of ​​the sheet, holding the pressure for 2-3 seconds. Then, symmetrical, intermittent point pressure is applied to both sides of the sheet, again using 5MPa and holding the pressure for 2-3 seconds.

[0126] After straightening, the flatness of the board is measured, and the flatness of the board meets the following requirements:

[0127] The maximum gap should be ≤1.5mm / m when inspected along the length of the board.

[0128] Four-corner torsion detection, maximum gap ≤1mm / m;

[0129] Flatness deviation ≤1.5mm / m over the entire length.

[0130] (2) Sheet material processing.

[0131] The shaped boards are processed using a gantry planer to refine their dimensions and achieve dimensional control.

[0132] (3) Non-destructive testing before welding.

[0133] Before welding, liquid penetrant testing is performed on the surfaces of the two plates to be welded to determine the condition of the surfaces and prevent defects such as pores from affecting the weld quality. Welding is started after the liquid penetrant (PT) test is qualified. If the PT test is unqualified, the unqualified areas will be manually ground and repaired to make the plate surface meet the welding conditions.

[0134] (4) Cleaning of the board material.

[0135] After the non-destructive testing is completed, the base material is cleaned by wiping the plate with alcohol to ensure the surface is clean. The welding process of the present invention does not require beveling or preheating, so the pretreatment process can reduce the work of beveling and preheating.

[0136] Part Two: Welding of L-shaped Angle Steel Profiles.

[0137] S1: As Figure 13 As shown, the welding device is placed on the welding workbench.

[0138] S2: As Figure 14 As shown, the austenitic stainless steel sheet to be welded is assembled onto a welding fixture to obtain the structure to be welded; specifically, two welding base materials are placed on the welding fixture for L-shaped assembly. In this embodiment, the length of the welding base material is 6m, therefore multiple welding fixtures are required, and the distance between two adjacent welding fixtures is not less than 250mm.

[0139] Specifically, the height of the fixed base 2 and the internal support plate 9 is adjusted according to the specific profile dimensions. After adjustment, the fixed base 2 and the fixed base plate 1 are secured with bolts. After securing, the side top mounting bolts 3 and fixing nuts 4 are installed and rotated to lock according to the position of the L-shaped angle steel profile. The upper limit bolts 5 are installed and tightened according to the upper position of the structure to be welded, thereby limiting the upper part of the structure to be welded. After installation, the installation gap of the plates is measured and controlled to be ≤0.2mm. If the installation dimensions do not meet the requirements, the installation gap can be adjusted by the side top mounting bolts 3 or the upper limit bolts 5 until the dimensions meet the requirements.

[0140] S3: Perform manual TIG tack welding on the structure to be welded; the reference point for manual TIG tack welding is the exact center of the austenitic stainless steel sheet to be welded. The purpose of tack welding is to initially fix the structure to be welded.

[0141] The specific steps are as follows:

[0142] (1) Connect the manual TIG positioning spot welding power supply, turn on the argon gas protection in advance (Ar≥99.999%), control the flow rate of the protective gas at 11L / min, adjust the welding machine parameters, the welding voltage is 10V, and the welding current is 80A.

[0143] (2) After preparing the welding wire and welding gun, perform manual spot welding on the assembled plates. With the reference point in the middle of the assembled profile as the center, perform spot welding on the left and right sides symmetrically and alternately on the front and back sides. The distance between each spot is controlled at 80-120mm, and the spot welding length is 5-10mm. The plate is covered by spot welding in the entire butt area. Finally, spot weld one spot at each end of the plate for fixation.

[0144] S4: After manual TIG tack welding, laser tack welding is performed on the structure to be welded. Laser tack welding uses double-sided welding and nitrogen protection during the process. After the tack welding is completed, laser tack welding is performed on the structure to be welded. Laser tack welding uses multi-area segmented tack welding, which can achieve precise positioning and fixation of the workpiece and ensure the stability and reliability of the subsequent laser welding process.

[0145] The specific process is as follows:

[0146] (1) Check the assembly status of the workpiece to be welded and the welding fixture, and confirm that each fastener is in working condition;

[0147] (2) Adjust the welding torch and shielding gas position. The welding position is PA. Adjust the welding torch angle so that the longitudinal beam angle of the laser beam is 0±1° and the transverse beam angle is 90° when welding the front side penetration depth; the longitudinal beam angle of the laser beam is 12±2° and the transverse beam angle is 90° when welding the back side penetration depth to ensure that the laser beam energy acts perpendicularly on the workpiece surface. Adjust the shielding gas flow rate and position. Nitrogen shielding is used for laser welding (nitrogen composition ≥99.99%). Adjust the front shielding gas flow rate to 40L / min and adjust the shielding gas nozzle to an angle of about 60° with the workpiece surface. The nozzle outlet is obliquely aimed at the weld pool and the high-temperature area of ​​the weld, forming a continuous and stable laminar shielding gas curtain above the weld pool to achieve effective gas protection in the welding area. The welding parameters are as follows:

[0148] (3) Complete multi-segment tack welding:

[0149] See Figure 15 The first laser positioning weld starts from the reference point of manual welding, and positioning welding is carried out at a distance of 50-80mm before and after the point, with a weld length of 100-160mm.

[0150] Then, using the first tack weld as the center, laser tack welding is performed symmetrically and segmentally towards both ends of the weld. The spacing between each tack weld is evenly distributed, with the distance between adjacent tack welds adjusted to 400-600mm and the penetration depth 2-3mm. This ensures that the welding stress is evenly distributed, suppressing bending, warping, and angular deformation. For the double-sided welding process of this type of workpiece, due to the fixing effect of the actual welding fixture, after the tack weld is completed on the front side, laser tack welding is immediately and synchronously performed on the corresponding position on the back side to achieve symmetrical positioning, further offsetting stress and avoiding misalignment and deformation on both sides.

[0151] S5: After laser tack welding, laser deep penetration welding is performed on the structure to be welded; laser deep penetration welding adopts double-sided single-pass welding, and nitrogen protection is used during laser deep penetration welding. Laser deep penetration welding plays a decisive role in the weld strength.

[0152] The specific process is as follows:

[0153] (1) Check the condition of the workpiece after laser positioning welding and check the working condition of the welding fixture;

[0154] (2) Adjust the welding torch head and shielding gas position. The welding position is PA. Adjust the welding torch angle. Taking 8mm L-shaped angle steel as an example, when welding the front side with deep penetration, ensure that the longitudinal beam angle of the laser beam is 0±1° and the transverse beam angle is 90°; when welding the back side with deep penetration, ensure that the longitudinal beam angle of the laser beam is 12±2° and the transverse beam angle is 90°, that is, the laser beam energy acts perpendicularly on the workpiece surface; keep the shielding gas flow rate and angle consistent with the above-mentioned tack welding position.

[0155] (3) The length of each weld penetration section is 1200-1500mm. Welding should be performed with the middle reference as the center, with a single-pass penetration of ≥3.5mm and a penetration of ≥1.5mm in the overlapping area of ​​the positive and negative welds. First, start the shielding gas to ensure that the welding area is fully covered by the shielding gas; then start the welding power supply to complete the penetration welding of the workpiece. First, set the reference in the middle to ensure symmetrical shrinkage when welding the two ends and maintain low deformation of the weld plate; at the same time, welding the middle first and then the two sides can ensure that the overlapping area is on both sides of the middle weld. The overlapping area is remelted twice to ensure the consistency of the penetration.

[0156] (4) Based on the clamping and fixing of the welding fixture, welding deformation is minimized. Therefore, after the first section of the weld is completed, there is no need to cool to room temperature. The second section of the front weld with a penetration depth of 1200-1500mm can be repeated according to the above operation method. The coverage area of ​​the two sections of the weld is 80-120mm. Then the third section of the penetration depth is completed symmetrically.

[0157] (5) After the front welding is completed, the workpiece is cooled to a certain temperature of 30±10℃ before disassembly. After disassembly, the reverse side of the workpiece is clamped and fixed to prepare for subsequent reverse laser deep penetration welding.

[0158] (6) Check the working status of each fastener, the angle of the laser welding gun and the protective gas gun. After confirming that everything is correct, adjust the welding parameters to the reverse welding parameters of the structure. In this embodiment, 8mm L-shaped angle steel plates are used. The reverse welding parameters are: welding power 4±1KW, welding speed 0.6m / min, defocusing amount 0mm, and welding angle adjusted to 12°.

[0159] (7) Following the operation methods of (3) and (4), laser deep penetration welding is performed on the reverse side. The welding is carried out in three sections with priority to the middle and symmetrical welding on both sides to ensure the integrity of the weld in the weld overlap area.

[0160] (8) After the laser deep melting welding on both sides is completed, the workpiece is allowed to cool naturally.

[0161] S6: After laser deep penetration welding is completed, laser filler wire cover welding is performed on the local weld seam.

[0162] After laser deep penetration welding is completed, laser filler wire cover welding will be performed on the profile. The welding power will be set to 4±1KW, the defocusing amount will be adjusted to 50-100mm, the welding speed will be adjusted to 0.5m / min, the longitudinal beam angle of the front and back welding will be 26±2°, and the transverse beam angle will be 90°. Laser filler wire cover welding will be performed on the butt weld of the profile.

[0163] S7: After the laser filler wire cover welding is completed, vibration aging treatment and post-weld straightening treatment are carried out in sequence.

[0164] Post-weld treatment includes vibration aging treatment and straightening treatment;

[0165] The specific procedures for vibration aging treatment are as follows:

[0166] S711: Support the welded profile; specifically, divide the profile into 9 equal parts according to its length, and support it at approximately 2 / 9 and 7 / 9 of its length to ensure stability. Rubber pads are preferred for support, but wood or other elastic materials can be selected depending on the profile specifications. The materials chosen should meet cleanliness standards.

[0167] S712: Select appropriate clamping positions to install the vibrator and vibration pickup. Specifically, for L-shaped angle steel profiles, the vibrator should be installed at the 1 / 2 mark along its length, and the vibration pickup should be installed at the edge of the profile; for other L-shaped angle steel profiles, the vibrator should be installed at the edge, and the vibration pickup should be installed at the corresponding position. For I-shaped profiles, the vibrator should be installed at the edge, and the vibration pickup should be installed at the corresponding position.

[0168] S713: Start the vibration program to perform vibration aging treatment on the welded profile. The vibration program includes pre-vibration frequency sweep → vibration aging → post-vibration frequency sweep. The frequency used for vibration aging is determined by the natural frequency of the profile obtained from the pre-vibration frequency sweep, preferably slightly lower than the frequency point corresponding to the highest resonance peak.

[0169] The specific procedures for orthopedic treatment are as follows:

[0170] S721: Perform static aging treatment on the welded profiles; the static aging treatment time should be ≥12 hours; that is, after laser filler wire cover welding is completed, the profiles should first undergo static aging treatment to release some of the residual stress generated during the welding process, and the static aging time should be ≥12 hours; after static aging is completed, straightening treatment should be performed. Before straightening, the initial deformation amount and corresponding position of the profile / plate should be measured, and the measurement points should be marked for re-measurement after straightening, and the measurement records should be made.

[0171] S722: Use jacks to perform preliminary straightening of the shrinkage of the flanges of the welded profile, with the straightening direction alternating from the middle to both ends;

[0172] S723: Use a top hydraulic press to perform secondary straightening on the flange plane of the welded profile, with the straightening direction alternating from the middle to both ends;

[0173] S724: The web of the welded profile is straightened.

[0174] The specific procedures for the above-mentioned orthopedic treatment are as follows:

[0175] Adjust the pressure equipment or tooling, and align the hydraulic pressure head 300 with the area of ​​maximum deformation according to the deformation.

[0176] Start the equipment and apply pressure slowly. The amount of deformation (deformation δ) in a single press must not exceed 50mm. From the moment of contact with the workpiece, the single press distance should be gradually reduced as the correction amount increases;

[0177] After pressing down to the predetermined size, maintain the pressure for a period of time (the holding time T depends on the size and rigidity of the workpiece, and is generally 5~10s) before releasing the pressure.

[0178] After depressurization, let the workpiece stand for 1-2 minutes, measure the dimensional recovery, analyze the elastic recovery and record it;

[0179] Based on the response analysis results, adjust the pressure of the pressurizing equipment or the location of the pressurizing point, and re-pressurize and recalibrate. Repeat the above process of pressurizing-holding-remaining-measuring, continuously adjusting parameters to optimize the calibration effect;

[0180] After the overall orthodontic treatment is completed, any remaining unevenness in the local areas is fine-tuned.

[0181] When using a straightening press, apply pressure to the localized protruding area, and the amount of deformation in a single press should not exceed 20mm.

[0182] After depressurizing and letting it stand (1~2 minutes), use a straight ruler or right angle ruler to check the local plane.

[0183] Acceptance criteria: There is no obvious visible gap between the straight ruler and the plane;

[0184] If the local plane still does not meet the requirements, repeat the above fine-tuning steps until it is qualified.

[0185] The specific welding parameters for laser positioning welding of the L-shaped angle steel profile in this embodiment are as follows: the welding position is PA flat welding, the welding power is 1500~3000W (of which the welding power for 6mm thickness is 1600~2200W, the welding power for 8mm is 1800~2200W, and the welding power for 10mm and above is 2800~3200W), the rising distance is 15~25mm, the falling distance is 20~30mm, there is no overlap, the defocusing amount is 0mm, the welding speed is 0.5~0.7m / min; the front shielding gas flow rate is 35~45 L / min; the angle between the gas shielding nozzle and the surface of the structure to be welded is 60°, and the distance between the gas shielding nozzle and the surface of the structure to be welded is ≤25mm.

[0186] In this embodiment, the welding power of laser deep penetration welding of L-shaped angle steel profiles is as follows: the welding position is PA flat welding, the welding power of the front and back sides of 6mm thickness is 3800~4200W; the welding power of the front side of 8mm thickness is 4800~5200W, and the welding power of the back side of 8mm thickness is 3800~4200W; the welding power of the front side of 10mm thickness is 5800~6200W, and the welding power of the back side of 10mm thickness is 4800~5200W; the welding power of the front side of 14mm thickness is 7800~8200W, and the welding power of the back side of 14mm thickness is 5800~6200W. The laser deep penetration welding has an upward distance of 15~50mm, a downward distance of 20~100mm, an overlap distance of 0~50mm, and a defocusing amount of 0mm; the welding speed is 0.5~0.7m / min; the front shielding gas flow rate is 35~45 L / min; the angle between the gas shielding nozzle and the surface of the structure to be welded is 60°, and the distance between the gas shielding nozzle and the surface of the structure to be welded is ≤25mm.

[0187] In this embodiment, the laser filler wire cover welding of the L-shaped angle steel profile has a welding power of 3500~5000W, a rise distance of 15~50mm, a fall distance of 20~100mm, an overlap distance of 0~50mm, and a defocusing amount of 50-100mm; the welding speed is 0.4~0.6m / min; the wire feeding speed is 2.7~3.7 m / min; the front shielding gas flow rate is 35~45 L / min; the angle between the gas shielding nozzle and the surface of the structure to be welded is 60°, and the distance between the gas shielding nozzle and the surface of the structure to be welded is ≤25mm.

[0188] In this embodiment of laser deep penetration welding, the nozzle outlet is obliquely aligned with the weld pool and the high-temperature area of ​​the weld, forming a continuous and stable laminar protective gas curtain above the weld pool, thereby achieving effective gas protection for the welding area.

[0189] In this embodiment of laser deep penetration welding, each segment of the welding depth is 1200-1500mm long, and the welding depth is preferentially centered on the middle reference. First, the shielding gas is activated to ensure the welding area is fully covered; then, the welding power is activated to complete the deep penetration welding of the workpiece. Establishing a reference in the middle first ensures symmetrical shrinkage during welding at both ends, maintaining low deformation of the welded plate. Simultaneously, welding the middle first, then the sides, ensures that the lap area is on both sides of the middle weld, and this lap area undergoes secondary stable remelting, guaranteeing consistent penetration depth.

[0190] In this embodiment of laser deep penetration welding, since the clamping and fixing of the welding fixture can minimize welding deformation, after the first weld section is completed, there is no need to cool to room temperature. The second section of deep penetration welding on the front side can be repeated according to the above operation method, with a length of 1200-1500mm. The coverage area of ​​the two weld sections is 80-120mm. Then, the third section of deep penetration welding is completed symmetrically.

[0191] In this embodiment of laser deep penetration welding, after the front side welding is completed, the workpiece is cooled to a temperature of 30±10℃ before disassembly. After disassembly, the reverse side of the workpiece is clamped and fixed to prepare for subsequent reverse side laser deep penetration welding.

[0192] When performing reverse welding, check the working status of each fastener, the angle of the laser welding gun, and the shielding gas gun. After confirming that everything is correct, adjust the welding parameters to the reverse welding parameters for this structure. When performing reverse laser deep penetration welding on the workpiece, perform three-stage welding by prioritizing the middle and then welding symmetrically on both sides to ensure the integrity of the weld in the weld overlap area.

[0193] After the laser deep melting welding on both sides is completed, the workpiece is allowed to cool naturally.

[0194] See Figure 16 In this embodiment, the welding sequence of the L-shaped angle steel profile is as follows: spot welding for fixation + laser positioning welding → flipping → spot welding for fixation + laser positioning welding → flipping → laser deep penetration welding → flipping → laser deep penetration welding + laser filler wire cover welding. This embodiment only requires three flipping operations to achieve weld formation, resulting in high efficiency.

[0195] After laser deep penetration welding is completed, laser filler wire capping welding will be performed on the profile. For L-shaped profiles, the filler wire will only be applied to the reverse side once. The welding power will be set to 4±1KW, the defocusing amount will be adjusted to 50-100mm, and the welding speed will be adjusted to 0.5m / min according to the above process parameters. Laser filler wire capping welding will be performed on the butt weld of the profile. The filler wire is applied in one go from start to finish.

[0196] Part Three: Post-Welding Inspection.

[0197] After the correction is completed, given that the application scenario of this invention is high-precision nuclear fusion, laser scanning measurement is selected for dimensional detection. Based on the theoretical model, the welded profile is laser-scanned, and the surface state of the profile is reconstructed by software and compared with the theoretical model. Figure 17 This is a comparison cloud diagram of the L-shaped angle steel profile obtained in this embodiment and the theoretical model.

[0198] from Figure 17As can be seen, the profiles manufactured using the process of this invention, compared with the theoretical model, have an overall dimensional deviation that can be controlled within ±2mm, which is more consistent than the dimensional consistency of profiles manufactured by traditional manual welding methods. Furthermore, by repeating the straightening step, the dimensional index can be further improved to ±1.5mm.

[0199] After dimensional inspection, the profiles were subjected to liquid penetrant testing and 100% radiographic testing of the welds (see radiographic film). Figure 18 ), permeability detection. The above detection order can be adjusted according to the available detection resources.

[0200] Welded joints shall undergo process qualification and mechanical property testing according to EN ISO 15614-1 standard: bending test (see...) Figure 19 The joint showed no cracks, and both positive and negative bends met the requirements; room temperature tensile test (see...) Figure 20 The tensile strength of the weld is not lower than that of the base metal, and the fracture point is always located in the base metal; high-temperature tensile test (see...) Figure 21 The specimen fractured at the location in the parent material; impact test (see...) Figure 22 The impact energy of the weld zone meets the toughness index of nuclear-grade structures.

[0201] The relative permeability test results are shown in Figure 23 ;in Figure 23 (a) shows the relative permeability test results of the weld zone. Figure 23 (b) shows the magnetic permeability test results of the heat-affected zone. Figure 23 It can be seen that the overall relative magnetic permeability of the welded profile is ≤1.03, which meets the low magnetic permeability design requirements of nuclear fusion devices.

[0202] Table 1 shows a comparison of the internal residual stress at the weld location of the profile after vibration aging treatment:

[0203] Table 1 Comparison of internal residual stresses after vibration aging treatment

[0204]

[0205] As shown in Table 1, the core function of vibration aging is to homogenize residual stress, reduce stress gradient, and avoid stress concentration. After vibration aging, the stress at high stress points decreases significantly, and the stress distribution becomes more uniform. Subsequent static aging combined with mechanical straightening can further reduce the overall residual stress level.

[0206] Example 2:

[0207] This embodiment uses a C-shaped channel steel profile as an example to illustrate the welding process of the present invention.

[0208] In this embodiment, the base material is 316L(N)-IG, with a thickness of 6mm and a quantity of 3; the welding material is ER317L, with a diameter of 1.0mm.

[0209] The welding process is the same as in Example 1, except for the welding parameters and the flipping order of the structure to be welded.

[0210] The specific welding parameters for laser positioning welding of C-shaped channel steel profiles are as follows: welding position is PA flat welding; welding power is 1500~3000W (1600~2200W for 6mm thickness, 1800~2200W for 8mm thickness, and 2800~3200W for 10mm and above thickness); rising distance is 15~25mm; falling distance is 20~30mm; no overlap; defocusing amount is 0mm; longitudinal beam angle is 0±1° for front welding and 12±2° for back welding; transverse beam angle is 90° for both front and back welding; welding speed is 0.5~0.7m / min; front shielding gas flow rate is 35~45 L / min; the angle between the gas shielding nozzle and the surface of the structure to be welded is 60°; and the distance between the gas shielding nozzle and the surface of the structure to be welded is ≤25mm.

[0211] The specific welding power for laser deep penetration welding of C-shaped channel steel profiles is as follows: welding position is PA flat welding, welding power is 3000~6000W, laser deep penetration welding rise distance is 15~50mm, fall distance is 20~100mm, overlap distance is 0~50mm, defocusing amount is 0mm, longitudinal beam angle is 0±1° for front welding and 12±2° for back welding, transverse beam angle is 90° for both front and back welding; welding speed is 0.5~0.7m / min; front shielding gas flow rate is 35~45L / min; the angle between the gas shielding nozzle and the surface of the structure to be welded is 60°, and the distance between the gas shielding nozzle and the surface of the structure to be welded is ≤25mm.

[0212] The welding power for laser wire filler cover welding of C-shaped channel steel profiles is 3500~5000W, the rising distance is 15~50mm, the falling distance is 20~100mm, the overlap distance is 0~50mm, the defocusing amount is 50-100mm, the longitudinal beam angle for front and back welding is 26±2°, and the transverse beam angle for front and back welding is 90°; the welding speed is 0.4~0.6m / min; the wire feeding speed is 2.7~3.7 m / min; the front shielding gas flow rate is 35~45 L / min; the angle between the gas shielding nozzle and the surface of the structure to be welded is 60°, and the distance between the gas shielding nozzle and the surface of the structure to be welded is ≤25mm.

[0213] See Figure 24The welding sequence of the C-shaped channel steel in this embodiment is as follows: spot welding for fixation → laser positioning welding → flipping → laser positioning welding + laser deep penetration welding → flipping → laser deep penetration welding → flipping → laser filler wire cover welding. This embodiment only requires three flipping operations to achieve weld formation, resulting in high efficiency.

[0214] Since C-shaped channel steel involves two front-side welds and two back-side welds, the control of welding deformation must be fully considered. Therefore, during the double-sided welding of the same weld joint, the weld is flipped to achieve both front and back-side formation and to minimize deformation caused by unilateral welding. By designing the above welding sequence, welding deformation can be offset to the greatest extent, thereby reducing the amount of welding deformation and the post-weld processing work.

[0215] Figure 26 This is a photograph of the C-shaped channel steel profile obtained in Example 2. From... Figure 26 It can be seen that the welding process of the present invention produces high-quality welds on profiles, and this welding process is particularly suitable for welding long welds on thin plates.

[0216] Example 3:

[0217] This embodiment provides a welding process for obtaining T-shaped profiles by welding thin-plate austenitic stainless steel profiles with long weld seams.

[0218] The remaining operating steps are basically the same as in Example 1.

[0219] The specific welding parameters are as follows:

[0220] The laser tack welding power is 1800±200W, the rise distance is 15~25mm, the fall distance is 20~30mm, there is no overlap, the defocusing amount is 0mm, the longitudinal beam angle for both front and back welding is 12±2°, and the transverse beam angle for both front and back welding is 90°; the welding speed is 0.5~0.7m / min; the front shielding gas flow rate is 35~45 L / min; the angle between the gas shielding nozzle and the surface of the structure to be welded is 60°, and the distance between the gas shielding nozzle and the surface of the structure to be welded is ≤25mm.

[0221] For T-shaped structures, the welding power of laser deep penetration welding is 3800~5200W (3800~4200W for 6mm thickness and 4800~5200W for 8mm thickness), the rise distance is 15~50mm, the fall distance is 20~100mm, the overlap distance is 0~50mm, the defocusing amount is 0mm, the longitudinal beam angle for both front and back welding is 12±2°, and the transverse beam angle for both front and back welding is 90°; the welding speed is 0.5~0.7m / min; the front shielding gas flow rate is 35~45 L / min; the angle between the gas shielding nozzle and the surface of the structure to be welded is 60°, and the distance between the gas shielding nozzle and the surface of the structure to be welded is ≤25mm.

[0222] For T-shaped structures, the welding power of laser filler wire cover welding is 4100~4500W, the rise distance is 15~50mm, the fall distance is 20~100mm, the overlap distance is 0~50mm, the defocusing amount is 50-100mm, the longitudinal beam angle for both front and back welding is 26±2°, and the transverse beam angle for both front and back welding is 90°; the welding speed is 0.4~0.6m / min; the wire feed speed is 2.7~3.7 m / min; the front shielding gas flow rate is 35~45 L / min; the angle between the gas shielding nozzle and the surface of the structure to be welded is 60°, and the distance between the gas shielding nozzle and the surface of the structure to be welded is ≤25mm.

[0223] See Figure 25 The welding sequence of the T-shaped profile in this embodiment is as follows: spot welding for fixing → laser positioning welding → flipping → laser positioning welding + laser deep penetration welding → flipping → laser deep penetration welding + laser filler wire cover welding → flipping → laser filler wire cover welding.

[0224] Those skilled in the art will readily understand that the above description is merely a preferred embodiment of the present invention. The above embodiments are provided only for the purpose of describing the present invention and are not intended to limit the present invention. Parts not described in detail in this specification are well-known in the art and are not intended to limit the scope of the present invention. The scope of the present invention is defined by the appended claims. All equivalent substitutions and modifications made without departing from the spirit and principle of the present invention should be covered within the scope of the present invention.

Claims

1. A high-efficiency laser welding process for thin-plate austenitic stainless steel profiles with long weld seams, characterized in that, The length-to-thickness ratio of the austenitic stainless steel plates to be welded is 1000~1500:1, and the length of the continuous full penetration weld formed after welding is 6~10m. The welding process includes the following steps: S1: Place the welding device on the welding workbench; S2: Assemble the austenitic stainless steel sheet to be welded onto the welding fixture, and control the gap between the butt joint surfaces to be ≤0.2mm to obtain the structure to be welded; S3: Perform manual TIG tack welding on the structure to be welded; during operation, take the center of the butt joint area as the reference point, and tack weld symmetrically to both ends, alternating between the front and back sides, with a point spacing of 80~120mm. S4: Laser tack welding for double-sided single-pass welding; laser tack welding is a multi-segment continuous weld, with a single segment length of 100~160mm, a spacing between adjacent segments of 400~600mm, and a penetration depth of 2~3mm; S5: Laser deep penetration welding for double-sided single-pass welding; laser deep penetration welding is symmetrical welding from the middle reference point to both ends, with a single-pass penetration depth ≥3.5mm and a penetration depth ≥1.5mm in the overlapping area of ​​the weld on both sides; S6: After laser deep penetration welding is completed, laser filler wire cover welding is performed on the local area where the weld is lower than the base material; S7: After the laser filler wire cover welding is completed, vibration aging treatment and post-weld straightening treatment are carried out in sequence.

2. The high-efficiency laser welding process for thin-plate long-weld austenitic stainless steel profiles according to claim 1, characterized in that, The process parameters for manual TIG positioning spot welding in step S3 are: argon purity ≥99.99%, flow rate 10~20L / min, welding voltage 10±2V, welding current 80±5A; spot welding length 5~10mm, and one reinforcement weld point is added at each end of the structure.

3. The high-efficiency laser welding process for thin-plate long-weld austenitic stainless steel profiles according to claim 1, characterized in that, In steps S4 and S5, the laser beam angle is adjusted according to the cross-sectional shape of the profile: When the structure to be welded is T-shaped or I-shaped, the longitudinal beam angle for welding on both the front and back sides is 12±2° and the transverse beam angle is 90°. When the structure to be welded is L-shaped or C-shaped, the longitudinal beam angle for welding on the front side is 0±1°, the longitudinal beam angle for welding on the back side is 12±2°, and the transverse beam angle is 90°. The nitrogen protection flow rate is 35~45L / min, the nozzle angle with the workpiece surface is 60°, and the distance between the nozzle and the workpiece surface is ≤25mm.

4. The high-efficiency laser welding process for thin-plate long-weld austenitic stainless steel profiles according to claim 1, characterized in that, The implementation method of laser positioning welding in step S4 is as follows: the first positioning weld extends forward and backward by 50-80mm from the reference point in step S3; then, with the center of the first positioning weld as the reference, positioning welds are arranged symmetrically in segments towards both ends of the weld, with the spacing between each segment being evenly distributed.

5. The high-efficiency laser welding process for thin-plate long-weld austenitic stainless steel profiles according to claim 1, characterized in that, The process parameters for laser deep penetration welding in step S5 are as follows: single-segment welding length 1200~1500mm, welding speed 0.5~0.7m / min, defocusing amount 0mm, welding position is PA flat welding; welding sequence is symmetrical segmented welding from the middle to both ends, and the overlap length of adjacent welds is 80~120mm.

6. The high-efficiency laser welding process for thin-plate long-weld austenitic stainless steel profiles according to claim 1, characterized in that, The process parameters for laser filler wire cover welding in step S6 are as follows: welding wire diameter 1.0 mm, longitudinal beam angle of welding on both the front and back sides is 26±2°, and transverse beam angle is 90°; welding speed 500±50 mm / min, wire feeding speed 2700~3700 mm / min, and defocusing amount 50~100 mm.

7. The high-efficiency laser welding process for thin-plate long-weld austenitic stainless steel profiles according to claim 1, characterized in that, In step S7: Vibration aging treatment includes: installing a vibrator and vibration pickup after supporting the profile, and starting the vibration program to achieve residual stress homogenization; The corrective treatment includes: first, allowing the plate to stand for ≥12 hours, and then alternating the shrinkage of the wing plate, the plane of the wing plate, and the web plate in stages from the middle to both ends.

8. The high-efficiency laser welding process for thin-plate long-weld austenitic stainless steel profiles according to claim 1, characterized in that, Before step S1, the pre-welding material pretreatment includes initial leveling, machining and non-destructive testing of the material, including visual inspection of the surface to be welded and liquid penetration testing.

9. A welding fixture for thin-plate long weld austenitic stainless steel profiles used in the welding process described in any one of claims 1 to 8, characterized in that, Includes a fixed base plate, a fixed base, a side top plate, a vertical plate, a horizontal plate, and a top limiting plate; Two fixed bases are symmetrically installed on a fixed base plate, two vertical plates are respectively installed on the two fixed bases, and a horizontal plate is placed between the two vertical plates; an internal support plate is provided below the horizontal plate, and a side top plate is provided on the outside of the vertical plate. The side top bolts pass through the fixing nuts and abut against the side top plate to achieve horizontal fastening of the vertical plate. Each vertical plate is equipped with a top limiting plate, which is fixed to the fixed base by bolt sleeves and upper limiting bolts to achieve longitudinal limiting of the vertical plate.