A method for heating and welding repair of large castings

By using a heated welding method, combined with ceramic electric heating blankets, coal stoves, and insulation structures, the problem of repairing local defects in large castings was solved, achieving stable welding and performance matching of high-strength castings, and avoiding cold cracks and deformation.

CN123060370APending Publication Date: 2026-11-10FUJIAN XINGHANG MECHANICAL CASTING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611337241.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Large castings are prone to local defects during the casting process, such as cracks and sand holes. In particular, welding repairs of high-strength steel are difficult, and room temperature welding can easily lead to cold cracks and deformation, which are difficult to repair effectively with existing technologies.

Method used

The heating welding repair method is adopted. After pre-detection and cleaning of defects, industrial ceramic electric heating blankets and coal stoves are used in conjunction with insulation cotton for heating. A heat insulation structure is set up, the temperature is monitored, matching welding materials are selected and tempering treatment is performed to ensure the temperature uniformity and stability of the welding position.

Benefits of technology

This effectively avoids rapid cooling at the welding site, reduces welding stress, improves the mechanical properties of the repaired area, prevents delayed cracking, and ensures the overall structural stability of the casting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123060370A_ABST
    Figure CN123060370A_ABST
Patent Text Reader

Abstract

This invention relates to a method for hot welding repair of large castings, comprising the following steps: (1) pre-inspecting the casting for defects and cleaning and marking the cracks and sand holes; (2) sending the casting into a heat treatment furnace for heating to above 300°C; (3) removing the casting after the temperature is uniform and transferring it to the work area; (4) covering the casting with an industrial ceramic electric heating blanket and insulation cotton, and simultaneously setting up a heating device below the location requiring welding repair; (5) having multiple operators simultaneously perform hot welding to fill cracks and sand holes in multiple areas, and setting up a heat insulation structure between adjacent operators; (6) after the hot welding of the casting is completed, sending the casting into a heat treatment furnace for tempering to relieve stress. This method can perform hot welding repair on large castings and can avoid the welding location cooling down too quickly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for heating and welding repair of large castings. Background Technology

[0002] After casting, large castings often exhibit surface or near-surface defects in certain areas due to various factors such as casting process, cooling rate, mold conditions, and raw materials. The most common defects include non-expanding simple cracks that do not affect the overall structural performance, as well as sand holes and porosity caused by gas entrapment or insufficient molten metal feeding. The most common and cost-effective repair method for these casting defects in the industry is welding.

[0003] However, for large castings with high strength requirements and special materials (such as 45 steel and alloy steel), the difficulty of welding repair increases significantly once cracks appear. This is mainly because high-strength steel is prone to cold cracking at room temperature due to its inherent hardening tendency, and the large size and complex restraint stress of large castings make them highly susceptible to cold cracking in the weld and heat-affected zone. Furthermore, rapid local heating and cooling during room temperature welding can lead to huge temperature gradients, resulting in severe welding deformation and even secondary cracking. This makes room temperature welding extremely difficult and places very high demands on welding processes and welder skills.

[0004] Therefore, the repair of cracks in such large high-strength steel castings usually requires hot welding, but the temperature can drop too quickly during the hot welding process. Therefore, a heat-welding repair method suitable for large castings is needed. Summary of the Invention

[0005] The purpose of this invention is to provide a method for heating and welding repair of large castings, which can heat and weld large castings and avoid excessive cooling at the welding position.

[0006] The technical solution of this invention is: a method for heating and welding repair of large castings, comprising the following steps: (1) The casting is inspected for defects in advance, and cracks and sand holes in the casting are cleaned and marked; (2) The casting is sent into a heat treatment furnace and heated to above 300°C; (3) After the casting temperature is uniform, remove the casting and transfer it to the work area; (4) Cover the casting with an industrial ceramic electric heating blanket and insulation cotton, and at the same time set up a heating device below the position where welding is required; (5) Multiple operators simultaneously perform hot welding to fill cracks and pinholes in multiple areas, and heat insulation structures are set up between two adjacent operators; (6) After the hot welding of the casting is completed, the casting is sent to the heat treatment furnace for tempering to relieve stress.

[0007] Furthermore, at room temperature, the cracked and sand-hole areas are polished by installing an alloy rotary file on a handheld straight grinder until the cracks and sand holes are no longer visible.

[0008] Furthermore, the casting is sent into a heat treatment furnace for heating to 350°C; before the casting is removed, the work area is cleaned and sand is laid, and support components are set in the work area to support the heated casting. The support points should be selected in areas where hot welding is not required.

[0009] Furthermore, multiple pieces of insulating cotton are laid on the casting and the insulating cotton covers the sides of the casting; the heating device is a coal stove set on the lower side of the casting, and the setting of the coal stove should avoid burning the insulating cotton.

[0010] Furthermore, during the hot welding filling operation, the operator partially lifts the insulation cotton of the area to be hot welded and supports the insulation cotton with a bracket to expose the area to be hot welded before carrying out the hot welding filling operation. After the hot welding filling is completed, the insulation cotton is quickly laid back down.

[0011] Furthermore, during the hot welding filling operation, the temperature is measured every 3-10 minutes using an infrared thermometer to ensure that the casting temperature is above 260℃; if the temperature is below 260℃, a blower is used to assist combustion and increase the heating temperature.

[0012] Furthermore, the coal stove includes a movable furnace body, with lifting lugs on both sides of the upper part of the furnace body, and radially protruding support parts on both sides of the lower part of the inner cavity of the furnace body. A furnace grid is supported on the support parts, and an air inlet is provided on one side wall of the furnace body below the furnace grid. Vertical slots are provided on both sides of the air inlet, and air control plates for adjusting the air intake are inserted therein. Adjusting bolts with locking control plates are screwed onto the vertical slots.

[0013] Furthermore, an arc-shaped guide plate that curves upwards is provided on the bottom side of the furnace body.

[0014] Furthermore, the heat insulation structure includes a heat insulation board, which is vertically arranged, and a pair of support frames are provided on both sides of the lower part of the heat insulation board, with a support plate fixed at the lower end of the support frame.

[0015] Furthermore, the heat insulation board is a 5-10mm thick steel plate with a height of 1.2-1.5m.

[0016] Compared with the prior art, the present invention has the following advantages: (1) Strict defect cleaning and flaw detection must be carried out before welding repair to facilitate subsequent hot welding treatment; and the casting is heated to reduce the cooling rate and welding stress.

[0017] (2) Select special welding materials that match the casting and temper the casting after welding to relieve stress, so as to ensure that the mechanical properties of the repaired area match the casting and avoid the generation of delayed cracks.

[0018] (3) Use industrial ceramic electric heating blankets in conjunction with insulation cotton to prevent the casting from cooling down too quickly; and use coal furnace heating to ensure the selected hot welding temperature; at the same time, use infrared thermometer to monitor the casting temperature so as to intervene in time.

[0019] (4) By setting up a heat insulation structure, adjacent workstations can be separated, reducing the impact of heat radiation between workstations. Attached Figure Description

[0020] Figure 1 This is a schematic diagram showing the state of the casting of the present invention placed in the work area.

[0021] Figure 2 This is a cross-sectional view of the heating device of the present invention.

[0022] Figure 3 For the present invention Figure 2 Enlarged view of area A; Figure 4 For the present invention Figure 2 Right view of area A.

[0023] Figure 5 This is a schematic diagram of the heat insulation structure of the present invention.

[0024] Figure 6 This is a side view of the heat insulation structure of the present invention.

[0025] In the diagram: 1-casting, 2-working area, 3-industrial ceramic electric heating blanket, 4-insulation cotton, 5-heating device, 51-furnace body, 52-lifting lug, 53-support part, 54-furnace grille, 55-air inlet, 56-vertical slot, 57-air control plate, 58-adjusting bolt, 59-arc guide plate, 6-insulation structure, 61-insulation plate, 62-support frame, 63-support plate, 7-sand lining, 8-supporting component. Detailed Implementation

[0026] To make the above features and advantages of the present invention more readily understood, specific embodiments are described below in conjunction with the accompanying drawings, but the present invention is not limited thereto.

[0027] Example 1 (Reference) Figures 1 to 6 A method for heating and welding repair of large castings includes the following steps: (1) Before casting 1 is subjected to flaw detection, the cracks and sand holes in casting 1 are cleaned and marked; (2) The casting 1 is sent into a heat treatment furnace and heated to 320°C; (3) After the temperature of casting 1 is uniform, take out casting 1 and transfer casting 1 to work area 2; (4) Cover the casting 1 with an industrial ceramic electric heating blanket 3 and insulation cotton 4, and at the same time, set up a heating device 5 below the position that needs to be welded for heating; (5) Select special welding materials that match the castings, and have multiple operators simultaneously perform hot welding to fill cracks and sand holes in multiple areas. Set up a heat insulation structure 6 between two adjacent operators to block the heat radiation from the adjacent work station to the operators. (6) After the hot welding of casting 1 is completed, casting 1 is sent to a heat treatment furnace for tempering to relieve stress, so as to ensure that the mechanical properties of the repaired area match those of the casting and avoid the generation of delayed cracks.

[0028] In this embodiment, at room temperature, the cracks and sand holes on casting 1 are ground using a handheld straight grinder equipped with an alloy rotary file until they are no longer visible. The handheld straight grinder can be a Dongcheng S1J-FF03-10 or a Bosch GRO12V series.

[0029] In this embodiment, between steps (2) and (3), before the casting 1 is removed from the heat treatment furnace, the work area 2 is cleaned and sand 7 is laid on it. The sand is laid on to prevent the bottom surface of the casting 1 from being damaged due to excessive heat. 2. Supporting components 8 are set in the work area to support the heated casting 1. The supporting parts should be selected in areas where hot welding is not required, while ensuring the stability of the gradual support.

[0030] In this embodiment, multiple pieces of thermal insulation cotton 4 are laid on the casting 1, and the thermal insulation cotton 4 covers the side of the casting 1, that is, the thermal insulation cotton should extend to the ground to reduce heat loss.

[0031] In this embodiment, the heating device is a coal stove located on the lower side of the casting. The coal stove includes a movable furnace body 51. Lifting lugs 52 are provided on both sides of the upper part of the furnace body 51. Radially protruding support portions 53 are provided on both sides of the lower part of the inner cavity of the furnace body 51. A furnace grille 54 is supported on the support portions 53. An air inlet 55 is provided on one side wall of the furnace body 51 below the furnace grille 54. Vertical slots 56 are provided on both sides of the air inlet, and air control plates 57 for adjusting the air intake are inserted into them. Adjusting bolts 58 with locking control plates are screwed onto the vertical slots 56. The air intake is controlled by adjusting the size of the air inlet.

[0032] To facilitate the movement of the furnace body 51, an arc-shaped guide plate 59 with an upward curve is provided on the bottom side of the furnace body 51. The hook rod is used to hang the lifting lug, and the furnace body is dragged and moved in the work area by manual pulling. The guide plate reduces the resistance during dragging; or it can be hoisted by a crane.

[0033] In this embodiment, during the hot welding filling operation, the operator partially lifts the insulation cotton 4 at the area to be hot welded and supports it with a bracket to expose the area to be hot welded. The coal stove is then moved to the underside of the area to be hot welded, and the stove is positioned to prevent the insulation cotton 4 from burning. The hot welding filling operation is then performed. After the hot welding filling is completed, the coal stove is removed and the insulation cotton 4 is quickly laid back down.

[0034] In this embodiment, during the hot welding filling operation, the assistant personnel use an infrared thermometer to measure the temperature every 5 minutes to ensure that the temperature of the casting is above 260°C; if the temperature is below 260°C, a fan is used to blow air into the air inlet 55 to assist combustion and increase the heating temperature.

[0035] In this embodiment, the heat insulation structure includes a heat insulation plate 61, which is vertically arranged and made of 6mm thick steel plate with a height of 1.2m. A pair of support frames 62 are provided on both sides of the lower part of the heat insulation plate 61, and a support plate 63 is fixed to the lower end of each support frame 62. Each support plate has an area of ​​15cm². The support plates increase the support area of ​​the support frame 62 and ensure support stability.

[0036] Operators should take heat insulation measures (such as wearing heat-insulating clothing) during operation to reduce the impact of heat waves on personnel.

[0037] Example 2 (Reference) Figures 1 to 6 A method for heating and welding repair of large castings includes the following steps: (1) Before casting 1 is subjected to flaw detection, the cracks and sand holes in casting 1 are cleaned and marked; (2) The casting 1 is sent into a heat treatment furnace and heated to 350°C; (3) After the temperature of casting 1 is uniform, take out casting 1 and transfer casting 1 to work area 2; (4) Cover the casting 1 with an industrial ceramic electric heating blanket 3 and insulation cotton 4, and at the same time, set up a heating device 5 below the position that needs to be welded for heating; (5) Select special welding materials that match the castings, and have multiple operators simultaneously perform hot welding to fill cracks and sand holes in multiple areas. Set up a heat insulation structure 6 between two adjacent operators to block the heat radiation from the adjacent work station to the operators. (6) After the hot welding of casting 1 is completed, casting 1 is sent to a heat treatment furnace for tempering to relieve stress, so as to ensure that the mechanical properties of the repaired area match those of the casting and avoid the generation of delayed cracks.

[0038] In this embodiment, at room temperature, the cracks and sand holes on casting 1 are ground using a handheld straight grinder equipped with an alloy rotary file until they are no longer visible. The handheld straight grinder can be a Bosch GRO12V series.

[0039] In this embodiment, between steps (2) and (3), before the casting 1 is removed from the heat treatment furnace, the work area 2 is cleaned and sand 7 is laid on it. The sand is laid on to prevent the bottom surface of the casting 1 from being damaged due to excessive heat. 2. Supporting components 8 are set in the work area to support the heated casting 1. The supporting parts should be selected in areas where hot welding is not required, while ensuring the stability of the gradual support.

[0040] In this embodiment, multiple pieces of thermal insulation cotton 4 are laid on the casting 1, and the thermal insulation cotton 4 covers the side of the casting 1, that is, the thermal insulation cotton should extend to the ground to reduce heat loss.

[0041] In this embodiment, the heating device is a coal stove located on the lower side of the casting. The coal stove includes a movable furnace body 51. Lifting lugs 52 are provided on both sides of the upper part of the furnace body 51. Radially protruding support portions 53 are provided on both sides of the lower part of the inner cavity of the furnace body 51. A furnace grille 54 is supported on the support portions 53. An air inlet 55 is provided on one side wall of the furnace body 51 below the furnace grille 54. Vertical slots 56 are provided on both sides of the air inlet, and air control plates 57 for adjusting the air intake are inserted into them. Adjusting bolts 58 with locking control plates are screwed onto the vertical slots 56. The air intake is controlled by adjusting the size of the air inlet.

[0042] To facilitate the movement of the furnace body 51, an arc-shaped guide plate 59 with an upward curve is provided on the bottom side of the furnace body 51. The hook rod is used to hang the lifting lug, and the furnace body is dragged and moved in the work area by manual pulling. The guide plate reduces the resistance during dragging; or it can be hoisted by a crane.

[0043] In this embodiment, during the hot welding filling operation, the operator partially lifts the insulation cotton 4 at the area to be hot welded and supports it with a bracket to expose the area to be hot welded. The coal stove is then moved to the underside of the area to be hot welded, and the stove is positioned to prevent the insulation cotton 4 from burning. The hot welding filling operation is then performed. After the hot welding filling is completed, the coal stove is removed and the insulation cotton 4 is quickly laid back down.

[0044] In this embodiment, during the hot welding filling operation, the assistant personnel use an infrared thermometer to measure the temperature every 8 minutes to ensure that the temperature of the casting is above 275°C; if the temperature is below 275°C, a fan is used to blow air into the air inlet 55 to assist combustion and increase the heating temperature.

[0045] In this embodiment, the heat insulation structure includes a heat insulation plate 61, which is vertically arranged and made of 8mm thick steel plate with a height of 1.4m. A pair of support frames 62 are provided on both sides of the lower part of the heat insulation plate 61, and a support plate 63 is fixed to the lower end of each support frame 62. Each support plate has an area of ​​20cm². The support plates increase the support area of ​​the support frame 62 and ensure support stability.

[0046] Operators should take heat insulation measures (such as wearing heat-insulating clothing) during operation to reduce the impact of heat waves on personnel.

[0047] Example 3 (Reference) Figures 1 to 6 A method for heating and welding repair of large castings includes the following steps: (1) Before casting 1 is subjected to flaw detection, the cracks and sand holes in casting 1 are cleaned and marked; (2) The casting 1 is sent into a heat treatment furnace and heated to 380°C; (3) After the temperature of casting 1 is uniform, take out casting 1 and transfer casting 1 to work area 2; (4) Cover the casting 1 with an industrial ceramic electric heating blanket 3 and insulation cotton 4, and at the same time, set up a heating device 5 below the position that needs to be welded for heating; (5) Select special welding materials that match the castings, and have multiple operators simultaneously perform hot welding to fill cracks and sand holes in multiple areas. Set up a heat insulation structure 6 between two adjacent operators to block the heat radiation from the adjacent work station to the operators. (6) After the hot welding of casting 1 is completed, casting 1 is sent to a heat treatment furnace for tempering to relieve stress, so as to ensure that the mechanical properties of the repaired area match those of the casting and avoid the generation of delayed cracks.

[0048] In this embodiment, at room temperature, the cracks and sand holes on casting 1 are ground using a handheld straight grinder equipped with an alloy rotary file until they are no longer visible. The handheld straight grinder can be a Dongcheng S1J-FF03-10.

[0049] In this embodiment, between steps (2) and (3), before the casting 1 is removed from the heat treatment furnace, the work area 2 is cleaned and sand 7 is laid on it. The sand is laid on to prevent the bottom surface of the casting 1 from being damaged due to excessive heat. 2. Supporting components 8 are set in the work area to support the heated casting 1. The supporting parts should be selected in areas where hot welding is not required, while ensuring the stability of the gradual support.

[0050] In this embodiment, multiple pieces of thermal insulation cotton 4 are laid on the casting 1, and the thermal insulation cotton 4 covers the side of the casting 1, that is, the thermal insulation cotton should extend to the ground to reduce heat loss.

[0051] In this embodiment, the heating device is a coal stove located on the lower side of the casting. The coal stove includes a movable furnace body 51. Lifting lugs 52 are provided on both sides of the upper part of the furnace body 51. Radially protruding support portions 53 are provided on both sides of the lower part of the inner cavity of the furnace body 51. A furnace grille 54 is supported on the support portions 53. An air inlet 55 is provided on one side wall of the furnace body 51 below the furnace grille 54. Vertical slots 56 are provided on both sides of the air inlet, and air control plates 57 for adjusting the air intake are inserted into them. Adjusting bolts 58 with locking control plates are screwed onto the vertical slots 56. The air intake is controlled by adjusting the size of the air inlet.

[0052] To facilitate the movement of the furnace body 51, an arc-shaped guide plate 59 with an upward curve is provided on the bottom side of the furnace body 51. The hook rod is used to hang the lifting lug, and the furnace body is dragged and moved in the work area by manual pulling. The guide plate reduces the resistance during dragging; or it can be hoisted by a crane.

[0053] In this embodiment, during the hot welding filling operation, the operator partially lifts the insulation cotton 4 at the area to be hot welded and supports it with a bracket to expose the area to be hot welded. The coal stove is then moved to the underside of the area to be hot welded, and the stove is positioned to prevent the insulation cotton 4 from burning. The hot welding filling operation is then performed. After the hot welding filling is completed, the coal stove is removed and the insulation cotton 4 is quickly laid back down.

[0054] In this embodiment, during the hot welding filling operation, the assistant personnel use an infrared thermometer to measure the temperature every 6 minutes to ensure that the casting temperature is above 290°C; if the temperature is below 290°C, a fan is used to blow air into the air inlet 55 to assist combustion and increase the heating temperature.

[0055] In this embodiment, the heat insulation structure includes a heat insulation plate 61, which is vertically arranged and made of 10mm thick steel plate with a height of 1.2m. A pair of support frames 62 are provided on both sides of the lower part of the heat insulation plate 61, and a support plate 63 is fixed to the lower end of each support frame 62. Each support plate has an area of ​​25cm². The support plates increase the support area of ​​the support frame 62 and ensure support stability.

[0056] Operators should take heat insulation measures (such as wearing heat-insulating clothing) during operation to reduce the impact of heat waves on personnel.

[0057] The above description is only a preferred embodiment of the present invention. For those skilled in the art, designing different forms of heating and welding repair methods for large castings based on the teachings of the present invention does not require creative labor. All equivalent changes, modifications, substitutions and variations made in accordance with the scope of the patent application of the present invention without departing from the principles and spirit of the present invention shall be covered by the present invention.

Claims

1. A method for heating and welding repair of large castings, characterized in that, Includes the following steps: (1) The casting is inspected for defects in advance, and cracks and sand holes in the casting are cleaned and marked; (2) The casting is sent into a heat treatment furnace and heated to above 300°C; (3) After the casting temperature is uniform, remove the casting and transfer it to the work area; (4) Cover the casting with an industrial ceramic electric heating blanket and insulation cotton, and at the same time set up a heating device below the position where welding is required; (5) Multiple operators simultaneously perform hot welding to fill cracks and pinholes in multiple areas, and heat insulation structures are set up between two adjacent operators; (6) After the hot welding of the casting is completed, the casting is sent to the heat treatment furnace for tempering to relieve stress.

2. The method for heating and welding repair of large castings according to claim 1, characterized in that, At room temperature, use an alloy rotary file mounted on a handheld straight grinder to grind the cracked and sand-hole areas until the cracks and sand holes are no longer visible.

3. A method for heating and welding repair of large castings according to claim 1 or 2, characterized in that, The casting is sent into a heat treatment furnace and heated to 350°C. Before the casting is removed, the work area is cleaned and sand is laid. Supporting components are set up in the work area to support the heated casting. The supporting parts should be selected in areas where hot welding is not required.

4. The method for heating and welding repair of large castings according to claim 1, characterized in that, Multiple pieces of insulating cotton are laid on the casting and the sides of the casting are covered with the insulating cotton; the heating device is a coal stove set on the lower side of the casting, and the setting of the coal stove should avoid burning the insulating cotton.

5. A method for heating and welding repair of large castings according to claim 4, characterized in that, When performing hot welding filling operations, the operator partially lifts the insulation cotton in the area to be hot welded and supports the insulation cotton with a bracket to expose the area to be hot welded before performing the hot welding filling operation. After the hot welding filling is completed, the insulation cotton is quickly laid back down.

6. A method for heating and welding repair of large castings according to claim 5, characterized in that, During hot welding filling operations, the temperature is measured every 3-10 minutes using an infrared thermometer to ensure that the casting temperature is above 260℃; if the temperature is below 260℃, a blower is used to assist combustion and increase the heating temperature.

7. A method for heating and welding repair of large castings according to claim 4, 5, or 6, characterized in that, The coal stove includes a movable furnace body. The upper part of the furnace body is provided with lifting lugs on both sides. The lower part of the inner cavity of the furnace body is provided with radially protruding support parts on both sides. A furnace grid is supported on the support parts. An air inlet is provided on one side wall of the furnace body below the furnace grid. Vertical slots are provided on both sides of the air inlet and air control plates for adjusting the air intake are inserted. Adjusting bolts with locking control plates are screwed onto the vertical slots.

8. A method for heating and welding repair of large castings according to claim 7, characterized in that, The bottom side of the furnace body is provided with an arc-shaped guide plate that curves upwards.

9. A method for heating and welding repair of large castings according to claim 1, 4, 5, 6 or 8, characterized in that, The heat insulation structure includes a heat insulation board, which is vertically arranged, and a pair of support frames are provided on both sides of the lower part of the heat insulation board, with a support plate fixed to the lower end of the support frame.

10. A method for heating and welding repair of large castings according to claim 9, characterized in that, The insulation board is a 5-10mm thick steel plate with a height of 1.2-1.5m.