A method for preparing cement blanket
The microbubble atomization spraying process for preparing cement blankets solves the problems of uneven mixing and poor seepage prevention in the traditional production of PVC cement blankets, and realizes the production of high-strength cement blankets with excellent seepage prevention performance, which are suitable for high-standard farmland and irrigation canals.
Patent Information
- Application Number
- CN202611578122.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-13
- Publication Date
- 2026-11-10
AI Technical Summary
Traditional PVC cement blanket production suffers from problems such as inaccurate manual feeding, uneven powder mixing, uneven PVC coating thickness, poor impermeability, low production efficiency, and harmful gas pollution, making it unable to meet the requirements for use in high-standard farmland and irrigation canals.
The microbubble atomization spraying process is adopted. The PVC composite adhesive is prepared by mixing sand, cement and additives evenly, combined with microbubble generator and ultrasonic cavitation method, and then evenly sprayed onto cement-based materials. The adhesive is then plasticized and cooled at high temperature to form a continuous and dense impermeable membrane layer.
It improves the mechanical strength, impermeability, and peel strength of cement blankets, solving the problems of poor strength and impermeability in traditional processes, realizing efficient and automated production, and reducing production costs and environmental pollution.
Smart Images

Figure CN123060818A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of building materials technology, and specifically relates to a method for preparing cement blankets. Background Technology
[0002] Traditional PVC cement blanket production processes mostly involve manual feeding and manual application of PVC. Existing technologies suffer from the following significant drawbacks: intermittent manual shovel feeding results in poor proportioning accuracy and uneven powder mixing, leading to poor cement blanket strength; inconsistent fabric density results in varying mechanical properties of the finished product, failing to meet the service life requirements of high-standard farmland and irrigation canals; the PVC coating, achieved through integral lamination or manual brushing, results in uneven coating thickness, high raw material consumption, insufficient interfacial adhesion strength, and poor impermeability; harmful gases generated during production cannot be recovered through equipment, posing a threat to operator health and the surrounding environment; and low production efficiency and high labor costs prevent continuous, automated, large-scale production.
[0003] Therefore, it is of great significance to develop an integrated molding preparation method for PVC-reinforced high-strength impermeable cement blankets, which transforms the three-layer structure of the film-coated cement blanket into a two-layer three-dimensional cement blanket. Summary of the Invention
[0004] Purpose of the invention: The technical problem to be solved by the present invention is to provide a method for preparing an integrally formed cement blanket based on microbubble atomization spraying process, which addresses the shortcomings of the prior art.
[0005] To solve the above-mentioned technical problems, the present invention adopts the following technical solution: The first aspect of this invention provides a method for preparing a cement blanket, comprising the following steps: Step 1: Mix sand, cement, and additives evenly to obtain a dry powder mixture; transport the dry powder mixture to the surface of the base mesh, level it, and then vibrate and compact it to obtain a cement-based material; Step 2: Pre-treat the cement-based material from Step 1 by cleaning with a three-stage brush; Step 3: Take polyvinyl chloride paste resin, DOTP plasticizer and viscosity reducer, stir evenly and then vacuum degas, add oil-soluble foam stabilizer and mix at low speed to obtain PVC composite adhesive liquid; Step 4: A uniform microbubble system is produced by a microbubble generator, and then fine bubble nuclei are precipitated by ultrasonic cavitation to obtain a PVC composite adhesive containing bubbles. The PVC composite adhesive containing bubbles is then uniformly sprayed onto the surface of the pretreated cement-based material to obtain a semi-finished product. Step 5: The semi-finished product obtained in Step 4 is plasticized at high temperature, cooled and molded into an integrated shape, and then packaged and rolled up to obtain the finished cement blanket.
[0006] In step 1, the sand, cement, and additives are mixed in a mass ratio of 51:48:1; the mixing conditions are: mixing time 6-15 minutes, mixing speed 1440 r / min.
[0007] In some embodiments of the present invention, the additives include water-reducing agents, cellulose, and other components, which are mixed in proportion to form an enhancing formula, which has a significant effect on improving the strength of cement blankets after water sprinkling and hardening.
[0008] In some embodiments of the present invention, by setting up sand silos, cement silos and independent storage silos for additives, sand, cement and additives are accurately measured in a mass ratio of 51:48:1 and transported to an independent small mixing plant for homogeneous mixing.
[0009] In step 1, the vibration compaction is performed under the following conditions: the excitation frequency is 50 Hz, the amplitude is 0.7~0.8 mm, and the width is 2300 mm; the thickness of the cement-based material is 5~15 mm.
[0010] In some embodiments of the present invention, the parameters of the base fabric are: basis weight 650~1000 g / m. 2 .
[0011] In some embodiments of the present invention, in step 1, the excess powder generated during the operation is blocked by two adjustable fixed baffles, and the excess powder on the surface of the base mesh is blocked in front. At the same time, the vibrating platform continuously vibrates and compacts the powder. The excess powder is returned to the front raw material silo through the U-shaped open screw conveyor recycling system to achieve closed-loop recycling and reuse.
[0012] In step 2, the three-stage brush cleaning is performed under the following conditions: the three-stage brushes are divided into coarse brushes, fine brushes, and fine brushes. The material of the three-stage brushes is any one of horsehair, nylon, and plastic. The gap between the brush bristles and the cement-based material surface is -3 to 0 mm. The coarse brush cleans the cement-based material surface at a frequency of 10 rpm or higher, while the fine and fine brushes perform fine sweeping and leveling at a frequency of 12 rpm or higher.
[0013] In step 3, the polyvinyl chloride paste resin, DOTP plasticizer, and viscosity reducer are in a mass ratio of 100:65:4; the stirring conditions are: stirring speed 2800 r / min; stirring time 8~20 minutes.
[0014] In some embodiments of the present invention, the viscosity reducer mainly comprises straight-chain saturated alkanes, cycloalkanes, trace amounts of isoalkanes, antioxidant stabilizers, and other components. It is also called deep-hydrogenated dearomatic D80 hydrocarbon solvent oil, which is an oil-based liquid hydrocarbon viscosity reducer and is a general-purpose liquid viscosity reducer for PVC paste resin and polymer slurry.
[0015] In step 3, the vacuum degassing is performed under the following conditions: maintaining a vacuum of -0.096 MPa for 15 minutes, adding an oil-soluble foam stabilizer after degassing, mixing at low speed, and heating to 35 ℃ for later use; the viscosity of the PVC composite adhesive at 25 ℃ is 8500 MPa·s.
[0016] In some embodiments of the present invention, the oil-soluble foam stabilizer is polyglycerol oleate.
[0017] In step 4, the microbubble generator consists of a static mixer and a microporous foaming tube with a pore diameter of 0.08 mm. Dry and clean compressed air is introduced into the microbubble generator at a pressure of 0.25 MPa and a gas-liquid volume ratio of 0.1:1 to form a uniform microbubble system with a diameter of 0.25 mm. The ultrasonic cavitation method uses the periodic negative pressure of high-frequency sound waves to cause the air dissolved in the PVC composite adhesive to precipitate in situ, forming a large number of tiny bubble nuclei, thus obtaining a PVC composite adhesive containing bubbles.
[0018] In some embodiments of the present invention, the ultrasonic cavitation method is performed under the following conditions: ultrasonic frequency of 20 kHz, ultrasonic rated power of 3000 W, operating mode of pulse intermittent, and power density of 0.8–2.5 W / cm³. 2 The peak-to-peak amplitude of the variable amplitude rod is 20~60 μm, the static pressure of the system is 0.06~0.10 MPa, the temperature of the PVC composite adhesive is 40~60 ℃, and the flow rate is 50~200 L / h.
[0019] In step 4, the spraying conditions are as follows: the PVC composite adhesive containing air bubbles is distributed to the spray gun array, with the spray guns evenly spaced 200 mm apart along the width direction, collectively covering a width of 1-3 m; each spray gun has a nozzle diameter of 1.2 mm, is angled at 15 degrees to the vertical direction, and has a spraying distance of 220 mm; under the condition of a conveyor belt speed of 2 m / min, the PVC composite adhesive containing air bubbles is applied at a coating amount of 200 g / m. 2 Spray evenly onto the surface of the pretreated cement-based material.
[0020] In step 5, the high-temperature plasticizing conditions are: temperature 178~203 ℃, time 5~9 minutes.
[0021] In some embodiments of the present invention, in step 5, the high-temperature plasticizing conditions are: temperature 190 ℃ and time 6 minutes.
[0022] In some embodiments of the present invention, in step 5, the integrated cooling molding is performed under the following conditions: the plasticized semi-finished product is taken out of the oven outlet and immediately enters the cold water roller cooling zone; the surface temperature of the cold water roller is 20°C, which is maintained by circulating cooling water; the semi-finished product is in close contact with the cold water roller, and the contact cooling time is 6 minutes, so that the surface temperature of the semi-finished product drops to below 40°C; after cooling, it is then cooled by air at room temperature for 2 to 3 minutes.
[0023] A second aspect of the present invention provides a cement blanket prepared using the above-described preparation method.
[0024] In some embodiments of the present invention, cement blankets integrally formed using a microbubble atomization spraying process were successfully prepared using the preparation method provided by the present invention. Performance comparisons between these cement blankets and those prepared using a traditional manual PVC film pasting process show that the cement blankets prepared by the method provided by the present invention possess better mechanical strength, impermeability, and peel strength. A three-day hardening experiment demonstrates that the cement blankets prepared by the present invention have a smooth surface and good visual quality; the edges are firmly and tightly bonded, with close-fitting edges, resulting in a significant quality improvement.
[0025] Beneficial effects: 1. This invention abandons the traditional manual shovel-based, extensive material feeding method, and adopts a three-compartment precise metering and automated mixing system for sand, cement, and additives. The proportions are stable and controllable, and the uniformity of dry powder mixing is greatly improved. Combined with the double-sided leveling by a scraper with 5 reciprocating strokes per minute and synchronous vibration by a vibrating platform, the dry powder is spread evenly and compacted on the base mesh, effectively improving the density of the cement blanket matrix. The compressive and flexural strength of the finished product is significantly enhanced, and the matrix itself can achieve the basic seepage prevention effect.
[0026] The staggered scrapers block excess dry powder after compaction, allowing for recycling during operation and reducing raw material loss; they also significantly suppress dust dispersion, improve the workshop working environment, and reduce dust pollution and occupational disease risks.
[0027] 2. This invention prepares a composite adhesive by mixing polyvinyl chloride paste resin, DOTP plasticizer, and viscosity reducer in a mass ratio of 100:65:4. The synergistic effect of the formulation components increases the interfacial bonding strength between the adhesive and the cement blanket substrate by at least 58%, solving the defects of traditional coating and manual brushing of PVC layers, such as easy delamination, peeling, and poor adhesion.
[0028] 3. A bubble generator is used to dissolve gas into the adhesive, and then ultrasonic cavitation is used to precipitate tiny bubble nuclei. The atomization spraying process transforms the bubble-containing liquid composite adhesive into uniform microbubble spraying, saving 65% of adhesive consumption, improving coating uniformity by 68%, improving surface smoothness by 75%, and resulting in a neat finished product with no bumps, missed coatings, or adhesive accumulation defects.
[0029] 4. Controllable high-temperature plasticizing within the range of 178~203 ℃ is employed, allowing the bubble-like PVC rubber coating to fully melt and cross-link, forming a continuous, dense, and pinhole-free impermeable reinforcing membrane layer. After plasticizing, it is rapidly shaped by uniform cooling with cold water rollers for 3~7 minutes. The membrane layer shrinks evenly during cooling, without warping, wrinkling, or delamination. The PVC impermeable layer and the cement substrate are simultaneously cured and integrally formed, eliminating the need for a secondary lamination process.
[0030] 5. The PVC composite cement blanket prepared by this process combines the advantages of high strength of the cement matrix and high impermeability of the PVC membrane, resulting in overall impermeability significantly better than that of ordinary cement blankets. The product's mechanical strength, interlayer adhesion, surface smoothness, and impermeability durability are simultaneously optimized, making it suitable for large-scale water conservancy projects such as high-standard farmland impermeable lining, irrigation canals, and water conservancy slope protection. Attached Figure Description
[0031] The present invention will be further described in detail below with reference to the accompanying drawings, and the advantages of the present invention in the above and / or other aspects will become clearer.
[0032] Figure 1 This is a flowchart of the cement blanket preparation method in an embodiment of the present invention.
[0033] Figure 2 This is a hardened appearance diagram of the cement blanket prepared by the bubble generator atomization spraying process and the traditional manual PVC film pasting process in an embodiment of the present invention. Detailed Implementation
[0034] The present invention will be further described in detail below with reference to specific embodiments, and the advantages of the present invention in the above and / or other aspects will become clearer.
[0035] Unless otherwise specified, the experimental methods described in the following examples are conventional methods; the reagents and materials described are commercially available unless otherwise specified.
[0036] Example 1:
[0037] This embodiment provides a method for preparing a cement blanket. Figure 1 This is a flowchart of the cement blanket preparation method in this embodiment, which specifically includes the following steps: Step 1: Preparation of cement-based materials Separate storage bins for sand, cement, and additives are set up. Sand, cement, and additives are precisely measured at a mass ratio of 51:48:1 and transported to an independent small-scale mixing plant for homogenization. The mixing time is 6-15 minutes, and the mixing speed is 1440 r / min, yielding a mixed dry powder. The mixed dry powder is then conveyed by a continuous conveyor belt to the base mesh fabric (650-1000 g / m²) output by the unwinding rollers. 2The base mesh is laid synchronously on the vibrating platform. The platform is equipped with two adjustable fixed baffles to block excess powder from the base mesh surface. Simultaneously, the vibrating platform continuously vibrates and compacts the material at a frequency of 50 Hz, an amplitude of 0.7~0.8 mm, and a width of 2300 mm, resulting in a cement-based material with a thickness of 5~15 mm. Excess powder generated during the operation is returned to the front-end raw material silo via a U-shaped open screw conveyor recycling system, achieving closed-loop recycling and reuse.
[0038] Step 2: Surface pretreatment of cement-based materials Before entering the spraying station, the cement-based material formed in step 1 undergoes a three-stage brush cleaning pretreatment: First, a coarse brush is used to clean the surface of the substrate at a frequency of 10 rpm or higher to remove excess thick powder layer. The coarse brush can be made of horsehair, nylon, or plastic, and the gap between the coarse brush and the surface of the cement-based material is -3 to 0 mm. Then, a fine brush and a fine brush are used in sequence at a frequency of 12 rpm or higher for fine sweeping and finishing. The fine brush and fine brush can be made of horsehair, nylon, or plastic, and the gap between the fine brush and the surface of the cement-based material is -3 to 0 mm.
[0039] Step 3: Preparation of PVC composite adhesive 100 parts by mass of polyvinyl chloride paste resin, 65 parts by mass of DOTP plasticizer, and 4 parts by mass of viscosity reducer were added to a high-speed dispersing mixer. The mixture was stirred at 2800 r / min for 8–20 minutes. After stirring, the solution was transferred to a vacuum degassing tank and kept under a vacuum of -0.096 MPa for 15 minutes to remove macroscopic air bubbles entrained during stirring. The degassed solution was then mixed with an oil-soluble foam stabilizer, polyglycerol oleate (oil-soluble foam stabilizer to degassed solution mass ratio 1:110), at low speed until homogeneous. The mixture was then transferred to a constant-temperature jacketed storage tank and heated to 35 °C for later use. The resulting PVC composite adhesive solution had a viscosity of 8500 MPa·s at 25 °C.
[0040] Step 4: Bubble generation and atomized spraying The PVC composite adhesive prepared in step 3 is fed into a microbubble generator, which consists of a static mixer and a microporous foaming tube with a pore size of 0.08 mm. Simultaneously, dry and clean compressed air is introduced into the microbubble generator at a pressure of 0.25 MPa and a gas-liquid volume ratio of 0.1:1, forming a uniform microbubble system with a diameter of 0.25 mm. Fine bubble nuclei are then precipitated using ultrasonic cavitation to obtain a PVC composite adhesive containing bubbles. Specifically, the periodic negative pressure of high-frequency sound waves causes the air originally dissolved in the PVC composite adhesive to precipitate in situ, forming a large number of fine bubble nuclei. Table 1 shows the process parameters for the ultrasonic cavitation method.
[0041] Table 1. Process parameters for ultrasonic cavitation method
[0042] After precipitating fine bubble nuclei using ultrasonic cavitation, a bubble-containing PVC composite adhesive was obtained. This bubble-containing PVC composite adhesive was then distributed to a spray gun array for atomized spraying. The spray guns were evenly spaced 200 mm apart along the width of the fabric, collectively covering a width of 2.1 m. Each spray gun had a nozzle diameter of 1.2 mm, was angled at 15 degrees to the vertical, and had a spraying distance of 220 mm. Under a conveyor belt speed of 2 m / min, the bubble-containing PVC composite adhesive was uniformly sprayed onto the surface of the cement-based material pretreated in step 2, with a wet film coating weight of 200 g / m². 2 .
[0043] Step 5: Oven plasticizing The semi-finished product obtained in step 4 is conveyed into a special oven with a length of 5-8 m and a width of 2.1 m. It is subjected to high-temperature plasticization at a controllable temperature range of 178-203 ℃. Each plasticization is completed every 6 minutes on average, so that the bubble-like PVC coating can be fully melted and cross-linked to form a continuous, dense, and pinhole-free anti-seepage reinforced membrane layer.
[0044] Step 6: Cooling and Shaping The semi-finished product, plasticized in step 5, is drawn out of the oven outlet and immediately enters the cooling zone of the cold water rollers. The surface temperature of the cold water rollers is 20°C, maintained by circulating cooling water. The semi-finished product is in close contact with the cold water rollers for 6 minutes, reducing the surface temperature of the semi-finished product to below 40°C. After cooling, it is further cooled by air at room temperature for 2-3 minutes to eliminate residual heat. Finally, it is rolled up and packaged to obtain the finished PVC-reinforced high-strength impermeable cement blanket.
[0045] Comparative Example 1: This comparative example provides a traditional method for preparing cement blankets by manually pasting PVC film, as a benchmark for comparison with Embodiment 1 of the present invention.
[0046] Step 1: Preparation of cement-based materials Using the same raw materials and proportions as in Example 1 (sand, cement, and additives in a mass ratio of 51:48:1), but employing a manual shovel-based intermittent mixing method to obtain a mixed dry powder. The mixed dry powder is then manually laid on a base mesh (650~1000 g / m²). 2 Vibration compaction is applied to obtain a cement-based material with a thickness of 5-15 mm.
[0047] Step 2: Surface pretreatment of cement-based materials The cement-based material obtained in step 1 was treated with the surface pretreatment process described in Example 1.
[0048] Step 3: Preparation of PVC geomembrane and adhesive Apply hot melt adhesive (polyolefin type) evenly to the surface of the cement-based material treated in step 2 using a manual brushing method. The amount of adhesive applied is approximately 180~300 g / m². 2 Subsequently, the PVC geomembrane (approximately 0.8 mm thick) is manually laid onto the surface of the cement-based material coated with adhesive. The roller pressure is controlled at 0.35 MPa, the roller gap is 5.5~16 mm, the lamination speed is 1 m / min, and the lamination is carried out at room temperature. Air bubbles are removed, and a traditional hand-pasted cement blanket is produced.
[0049] Performance comparison: Experimental samples were prepared according to the preparation method of Example 1. Three groups of samples were prepared by controlling the plasticizing temperature in step 5 to 178 ℃, 190 ℃ and 203 ℃ respectively. The plasticizing effect was observed and a hand bending test was performed. Then, the optimal temperature for mass production was determined based on the plasticizing effect.
[0050] Plasticizing temperature experiments confirmed that at 178 ℃, PVC undergoes almost no thermal decomposition, the fabric surface does not scorch, and damage to the base fabric fibers is minimal. However, plasticization is insufficient, the PVC melt has poor fluidity, and it cannot fully wet the pores of the base fabric. Furthermore, the peel strength between the film and the base fabric is low, making it prone to delamination and blistering during bending and dragging. Microscopic voids exist internally, resulting in a high permeability coefficient. Additionally, trace amounts of plasticizer slowly leach out during the production process, reducing production line capacity. Therefore, this temperature is suitable for low-end, simple, non-impermeable cement blankets and small-batch prototyping, and should not be used as the primary production temperature.
[0051] At 203 ℃, PVC reaches its instantaneous plasticization limit and approaches the critical line for rapid thermal decomposition of PVC, making the melt too thin to solidify. At the same time, a large amount of plasticizers volatilize at high temperatures, causing the finished PVC to harden and its low-temperature folding resistance to plummet, making it prone to cracking and leakage during long-term outdoor use. Furthermore, excessively high temperatures can scorch polyester and polypropylene base fabrics, reduce the strength of geotextiles, and decrease the overall tear and puncture resistance of cement blankets. Therefore, it is not recommended for regular mass production.
[0052] At 190 ℃, PVC is fully gelled and plasticized. After full plasticization, the polymer chains are fully cross-linked, the melt has sufficient fluidity, and after hot pressing, PVC is deeply embedded in the fiber fabric. The composite peel strength reaches its peak, and it does not delaminate after repeated bending, exhibiting optimal flexibility. The film surface is dense, without pinholes or bubbles, providing optimal impermeability and meeting high water-resistant requirements. With a qualified calcium-zinc composite heat stabilizer system, 190 ℃ is within a safe processing range, and PVC will not yellow or become brittle in large quantities. The production line can operate at full speed with high temperature control tolerance. Therefore, at this temperature, PVC is fully plasticized, has the strongest adhesion, and provides perfect impermeability; this temperature is the preferred and optimal temperature for controllable thermal decomposition.
[0053] The following performance tests were all conducted at a plasticizing temperature of 190 °C. The test specimens were prepared and cut into standard test specimens, which were numbered as follows: MAC-01, MAC-02, MAC-03, MAC-04, MAC-05 and MAC-06.
[0054] The control sample was prepared according to the preparation method of Comparative Example 1. After shaping and cooling, the standard test strips were cut and numbered S-A03, S-B03, S-C03, S-D03, S-E03 and S-F03 respectively.
[0055] The cement blankets numbered MAC-01, MAC-02, MAC-03 and S-A03, S-B03, S-C03 were hardened by sprinkling water. Samples of different numbers were taken after 24 hours, 48 hours, 72 hours and 28 days of hardening, respectively. The samples were cut into 40×160 mm size for flexural strength test and 100×100 mm size for compressive strength test. Table 2 shows the strength test results of the cement blankets prepared by the preparation method provided by the present invention and the traditional process.
[0056] Table 2. Strength test results of cement blankets prepared by the preparation method provided by the present invention and by traditional processes.
[0057] Place MAC-04 and S-D03 on the anti-seepage tank device frame, then spray water to harden them. After 72 hours, observe whether there is water seepage or bulging on the back of the anti-seepage device. Table 3 shows the anti-seepage performance of cement blankets prepared by the preparation method provided by this invention and by traditional processes.
[0058] Table 3. Impermeability of cement blankets prepared by the preparation method provided by this invention and by traditional processes.
[0059] The coatings numbered MAC-06, S-E03, and S-F03 were hardened by spraying water. After three days of hardening, the surface smoothness and coating uniformity were evaluated. Figure 2 Images of the front of the MAC-06 and S-E03, where... Figure 2 In the diagram, A represents the front side of S-E03. Figure 2 The B in the text refers to the front of MAC-06, which is... Figure 2 It can be seen that the cement blankets prepared by traditional processes have poor surface smoothness after PVC bonding, with irregularly distributed pits and punctate defects on the surface; there is slight edge curling at component splicing and material termination edges, with some edges detaching from the base surface. In contrast, the cement blankets prepared by this invention have a smooth surface and good visual quality; the edges are firmly bonded and tightly finished.
[0060] The PVC layer thickness of S-F03 and MAC-06 was characterized. After three days of curing, the PVC layer thickness in S-F03 was 0.8 mm, while the PVC layer thickness in MAC-06 was only 0.5 mm. Furthermore, the thickness of the PVC layer on the back of S-F03 was uneven.
[0061] The comparison of examples and comparative examples shows that the traditional manual adhesive application process is affected by human operation factors, making it difficult to guarantee the uniformity of the adhesive layer and easily resulting in uneven local adhesive thickness. After pasting the PVC film, the surface smoothness is poor; the bonding strength is low in areas with insufficient adhesive, and edge lifting is prone to occur, and the adhesive is also difficult to fully melt and wet. The overall consumption of adhesive is difficult to control, resulting in poor product quality stability. In addition to occasional quality defects such as bulging, the compressive and flexural mechanical properties of the samples are also relatively weak due to insufficient interfacial density.
[0062] With the aid of a bubble generator and ultrasonic cavitation, the atomized spraying process can uniformly spray materials onto the substrate surface. High temperatures then allow for melting and wetting, enabling the material to penetrate deep into the substrate and achieve a seamless, integrated molding process, transforming the three-layer structure of the film into a two-layer structure. Compared to traditional processes, the compressive, flexural, and peel strengths, as well as the surface smoothness of the samples, are significantly improved. This process is not merely a simple physical interface bonding; rather, it achieves the fusion of materials, resulting in a two-layer cement blanket.
[0063] Compared to traditional manual PVC film pasting, the new atomized spraying high-temperature plasticizing integrated molding process abandons the simple physical interface bonding mode. Through high-temperature melting and wetting, the coating material penetrates and fuses into the substrate, achieving seamless interface connection and integral molding. This completely solves the problems of uneven adhesive layer thickness and insufficient wetting caused by manual glue application, effectively eliminating quality defects such as edge curling, bulging, and uneven surface of finished products, and significantly improving the interfacial thermal bonding strength and structural integrity of the PVC composite layer.
[0064] Under the same unit area weight conditions, the atomized spraying process has significant advantages, enabling uniform spraying of materials across the entire surface, resulting in a uniform coating thickness and excellent surface smoothness, completely avoiding human error caused by manual construction. Simultaneously, the process allows for precise material control, effectively reducing adhesive waste and significantly improving material utilization. Compared to traditional processes, the new process produces products with higher structural density, significantly optimizing overall compressive, flexural, and peel strength. Furthermore, the coating is tightly bonded and free of voids, effectively improving the product's impermeability and durability, avoiding the performance degradation problems caused by localized adhesive layer deficiencies and insufficient density in traditional processes.
[0065] Tracking tests on the compressive strength of products manufactured using the new process at different ages (24h, 48h, and 72h) show that the products formed by the atomized spray coating integrated molding process have a uniform structure, good density, stable early strength growth, and a regular performance gradient. Compared with products formed by traditional manual processes, the compressive strength at all ages is significantly improved, the product molding quality is uniform, and the performance stability is strong. This effectively solves the shortcomings of inconsistent molding quality and weak mechanical properties of traditional processes, and fully meets the requirements of engineering construction quality and performance.
[0066] This invention provides a method for preparing cement blankets. Many methods and approaches exist for implementing this technical solution; the above description is merely a preferred embodiment of the invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of this invention, and these improvements and modifications should also be considered within the scope of protection of this invention. All components not explicitly stated in this embodiment can be implemented using existing technologies.
Claims
1. A method for preparing a cement blanket, characterized in that, Includes the following steps: Step 1: Mix sand, cement, and additives evenly to obtain a dry powder mixture; transport the dry powder mixture to the surface of the base mesh, level it, and then vibrate and compact it to obtain a cement-based material; Step 2: Pre-treat the cement-based material from Step 1 by cleaning with a three-stage brush; Step 3: Take polyvinyl chloride paste resin, DOTP plasticizer and viscosity reducer, stir evenly and then vacuum degas, add oil-soluble foam stabilizer and mix at low speed to obtain PVC composite adhesive liquid; Step 4: A uniform microbubble system is produced by a microbubble generator, and then fine bubble nuclei are precipitated by ultrasonic cavitation to obtain a PVC composite adhesive containing bubbles. The PVC composite adhesive containing bubbles is then uniformly sprayed onto the surface of the pretreated cement-based material to obtain a semi-finished product. Step 5: The semi-finished product obtained in Step 4 is plasticized at high temperature, cooled and molded into an integrated shape, and then packaged and rolled up to obtain the finished cement blanket.
2. The preparation method according to claim 1, characterized in that, In step 1, the sand, cement, and additives are mixed in a mass ratio of 51:48:1; the mixing conditions are: mixing time of 6-15 minutes and mixing speed of 1440 r / min.
3. The preparation method according to claim 1, characterized in that, In step 1, the vibration compaction is performed under the following conditions: the excitation frequency is 50 Hz, the amplitude is 0.7~0.8 mm, and the width is 2300 mm; the thickness of the cement-based material is 5~15 mm.
4. The preparation method according to claim 1, characterized in that, In step 2, the three-stage brush cleaning is performed under the following conditions: the three-stage brushes are divided into coarse brushes, fine brushes, and fine brushes. The material of the three-stage brushes is any one of horsehair, nylon, and plastic. The gap between the brush bristles and the cement-based material surface is -3 to 0 mm. The coarse brush cleans the cement-based material surface at a frequency of 10 rpm or higher, while the fine and fine brushes perform fine sweeping and leveling at a frequency of 12 rpm or higher.
5. The preparation method according to claim 1, characterized in that, In step 3, the polyvinyl chloride paste resin, DOTP plasticizer, and viscosity reducer are in a mass ratio of 100:65:4; the stirring conditions are: stirring speed 2800 r / min; stirring time 8~20 minutes.
6. The preparation method according to claim 1, characterized in that, In step 3, the vacuum degassing is performed under the following conditions: maintaining a vacuum of -0.096 MPa for 15 minutes, adding an oil-soluble foam stabilizer after degassing, mixing at low speed, and heating to 35 ℃ for later use; the viscosity of the PVC composite adhesive at 25 ℃ is 8500 MPa·s.
7. The preparation method according to claim 1, characterized in that, In step 4, the microbubble generator consists of a static mixer and a microporous foaming tube with a pore size of 0.08 mm. Dry and clean compressed air is introduced into the microbubble generator at a pressure of 0.25 MPa, and the gas-liquid volume ratio is controlled at 0.1:1, forming a uniform microbubble system with a diameter of 0.25 mm. The ultrasonic cavitation method uses the periodic negative pressure of high-frequency sound waves to cause air dissolved in the PVC composite adhesive to precipitate in situ, forming a large number of tiny bubble nuclei, resulting in a PVC composite adhesive containing bubbles. The conditions for the ultrasonic cavitation method are: ultrasonic frequency of 20 kHz, ultrasonic rated power of 3000 W, operating mode of pulse intermittent, and power density of 0.8–2.5 W / cm³. 2 The peak-to-peak amplitude of the variable amplitude rod is 20~60 μm, the static pressure of the system is 0.06~0.10 MPa, the temperature of the PVC composite adhesive is 40~60 ℃, and the flow rate is 50~200 L / h.
8. The preparation method according to claim 1, characterized in that, In step 4, the spraying conditions are as follows: the PVC composite adhesive containing air bubbles is distributed to the spray gun array, with the spray guns evenly spaced 200 mm apart along the width direction, collectively covering a width of 1-3 m; each spray gun has a nozzle diameter of 1.2 mm, is angled at 15 degrees to the vertical direction, and has a spraying distance of 220 mm; under the condition of a conveyor belt speed of 2 m / min, the PVC composite adhesive containing air bubbles is applied at a coating amount of 200 g / m. 2 Spray evenly onto the surface of the pretreated cement-based material.
9. The preparation method according to claim 1, characterized in that, In step 5, the high-temperature plasticizing conditions are: temperature 178~203 ℃, time 5~9 minutes.