A crystal-modified calcium carbonate fiberboard and its preparation method

By combining steel slag and calcium carbide slag and using staged crystal form regulators, aragonite-nepheline composite calcium carbonate is generated, which solves the mechanical properties and durability problems of steel slag-based fiberboard, improves flexural strength and density, reduces water absorption, and forms a high-efficiency fiberboard material.

CN123062201APending Publication Date: 2026-11-10CHINA BUILDING MATERIALS ACADEMY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611571907.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-12
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing steel slag-based fiberboards suffer from problems in terms of mechanical properties and durability, such as low tensile strength, easy cracking, weak interfacial bonding, insufficient matrix density, and mismatch between calcium dissolution rate and CO2 diffusion rate, resulting in decreased saturated flexural strength and high water absorption.

Method used

Using a steel slag-carbide slag composite system as the calcium source, combined with a staged crystal form regulator and vacuum impregnation technology, the carbonization process is controlled by the staged introduction of polyaspartic acid, magnesium source, strontium source and polyacrylic acid, generating aragonite-nepheline composite calcium carbonate, inhibiting calcite formation, forming a dense polyaspartic acid-Mg2+ co-occupying layer and Sr2+ anchor points, and promoting the directional distribution of aragonite and nepheline.

Benefits of technology

It significantly improves the dry and saturated flexural strength of fiberboard, reduces water absorption, enhances matrix density, and forms a dual-scale reinforcement system of micro-whiskers and macro-fibers, thereby improving the overall performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123062201A_ABST
    Figure CN123062201A_ABST
Patent Text Reader

Abstract

This invention discloses a crystal-modified calcium carbonate fiberboard and its preparation method. The crystal-modified calcium carbonate fiberboard comprises the following components: a cementing component, basalt fiber, bamboo powder, organic synthetic fiber, a first-stage regulator, a second-stage regulator, silica fume, limestone powder, expanded perlite, pigment, and water. The cementing component includes steel slag powder and carbide slag; the first-stage regulator includes polyaspartic acid and a magnesium source; and the second-stage regulator includes a strontium source and polyacrylic acid. This invention, through a staged crystal-modified agent and a stepwise carbonization process, in-situ directionally constructs aragonite-aragonite composite calcium carbonate in the fiberboard. The aragonite acicular skeleton and fiber form a dual-scale reinforcement; the aragonite stabilizes the aragonite skeleton and inhibits calcite crystallization; and the significant reduction in the calcite proportion significantly reduces the open pores formed by the accumulation of rhombohedral calcite, reducing the product's water absorption rate to 7.0%~8.5% and significantly improving its density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of comprehensive utilization of bulk industrial solid waste, and in particular to a crystal-modified calcium carbonate fiberboard and its preparation method. Background Technology

[0002] Steel slag is a major industrial solid waste generated during the iron and steel smelting process, and its comprehensive utilization rate has long been low. Steel slag is rich in active calcium components such as β-C2S, γ-C2S, and Ca(OH)2, and has the dual potential to achieve CO2 fixation and structural modification through carbonization reaction.

[0003] Fiberboard is prepared using steel slag as the calcium source and fiber as the reinforcement, through slurry preparation, pressing, demolding, static curing, and carbonization curing. This process integrates solid waste resource utilization with CO2 mineralization and carbon sequestration. However, existing steel slag-based fiberboards still have the following prominent problems in terms of mechanical properties and durability: (1) Steel slag carbonized materials have low tensile strength and are prone to cracking. The carbonization products are mainly calcium carbonate crystals with calcite as the main component. The rhombohedral morphology of the crystals has limited contribution to the flexural strength of the matrix, and the saturated flexural strength of the board is not sufficiently improved. At the same time, traditional wet papermaking or high water-solid ratio slurry processes require filtration, dewatering and grouting, which are complicated and can easily cause uneven fiber orientation and matrix delamination.

[0004] (2) The flexural strength decreases significantly under saturated conditions. Under saturated conditions, water penetrates the pores of the matrix and the fiber-matrix interface transition zone of the steel slag-based fiberboard, weakening the interfacial bonding force, resulting in a significantly lower saturated flexural strength than that in the dry state; especially in the high water-to-solid ratio papermaking process, a large number of open pores remain after dewatering and grouting, which further aggravates the decrease in saturated strength.

[0005] (3) The fiber-matrix interface is weak. The surface of basalt fiber is smooth and the interfacial bonding performance with inorganic matrix is ​​weak. The interfacial anchoring effect of calcite crystal is limited and the interfacial transition zone still has high porosity. During the traditional dewatering and grouting process, the fiber is easy to migrate with the water flow, resulting in local water enrichment and increased porosity in the interfacial transition zone.

[0006] (4) Insufficient matrix density and high water absorption rate. The existing steel slag carburization products are mainly calcite. When calcite rhombohedral grains are stacked, a large number of open pores are easily formed. Moreover, calcite has limited filling efficiency for micropores, resulting in high open porosity in the matrix and easy water intrusion. In traditional processes, it is difficult to achieve uniform density under low water-solid ratio by filtration dewatering and grouting. Water migration channels are easily formed inside the slab.

[0007] (5) The calcium dissolution rate and CO2 diffusion rate are difficult to match during the carbonization process of a single steel slag calcium source. In the initial stage of carbonization, Ca... 2+Rapid release leads to a sharp increase in system supersaturation, with calcite nucleation becoming dominant; insufficient calcium dissolution in the later stages of carbonization makes it difficult to continuously improve the carbonization conversion rate. Meanwhile, in traditional high water-to-solid ratio processes, a large amount of free water dilutes the Ca. 2+ Concentration and delayed CO2 diffusion further exacerbate the mismatch between calcium dissolution and carbonization rates. Summary of the Invention

[0008] To address the aforementioned technical problems, this invention provides a crystal-modified calcium carbonate fiberboard and its preparation method. This invention uses a steel slag-carbide slag composite system as the calcium source, and basalt fiber, bamboo powder fiber, and organic synthetic fiber as composite reinforcements. It employs a staged crystal-modifying additive and step-by-step carbonation curing. In the first stage, a dual-modifier of "polyaspartic acid + magnesium source" is premixed into the steel slag-carbide slag-fiber mixture. After slurry preparation, dewatering, pressing, and static curing, a first-stage CO2 carbonation is performed, controlling the carbonation conversion rate to 45%~65%. The rapid calcium dissolution characteristic of carbide slag provides a high concentration of Ca in the early stages of carbonation. 2+ This makes polyaspartic acid and Mg 2+ The crystal facet occupancy effect plays a role at higher supersaturation, generating high aspect ratio acicular aragonite and forming dense polyaspartic acid-Mg 2+ The first stage involves a co-occupying layer; the second stage involves introducing a dual-regulatory agent of "strontium source + polyacrylic acid" into the slab through vacuum impregnation, followed by a second stage of CO2 carbonization to allow Sr to... 2+ Using the first-stage occupant layer as an anchor point, selective adsorption on specific aragonite crystal faces induces heterogeneous nucleation and directional distribution of aragonite, while polyacrylic acid stabilizes the aragonite and inhibits crystal transformation. Ultimately, an aragonite-aragonite composite calcium carbonate is formed in situ within the matrix, with aragonite as the framework and aragonite dispersed between aragonite crystal faces, forming a dual-scale reinforcement system of "microscopic whiskers - macroscopic fibers" with the fibers. Simultaneously, the staged carbonization process effectively suppresses calcite formation: the first-stage carbonization occurs in polyaspartic acid-Mg... 2+ The co-occupation layer preferentially induces aragonite nucleation, and the second stage of carbonization occurs in Sr. 2+ The anchoring point and the stabilizing effect of polyacrylic acid induce heterogeneous nucleation of nepheline, and the two-stage synergy significantly reduces the proportion of calcite. Since the rhombohedral calcite grains tend to form a large number of open pores when they are packed together, while the acicular crystals of aragonite and the spherical grains of nepheline are packed more tightly, the reduction of the proportion of calcite directly leads to a decrease in the number of open pores in the matrix, a decrease in water absorption, and an increase in density.

[0009] In a first aspect, the present invention provides a crystal-modified calcium carbonate fiberboard, which is achieved by the following technical solution.

[0010] A crystal-modified calcium carbonate fiberboard comprises the following components in parts by weight: Cementitious component: 55~75 parts; the cementitious component consists of steel slag powder and carbide slag, of which carbide slag accounts for 5%~20% of the total mass of the cementitious component; Basalt fiber: 2-6 parts; Bamboo powder: 1-4 parts; Organic synthetic fibers: 0-4 parts; First-stage regulator: 0.1-1.5 parts polyaspartic acid, 0.5-3 parts magnesium source; Second-stage regulator: 0.5-3 parts strontium source, 0.1-1.5 parts polyacrylic acid; Silica fume: 4-8 parts; Limestone powder: 10-20 parts; Expanded perlite: 0-10 parts; Pigment: 0.1~0.2 parts; The water-to-solid ratio should be controlled between 0.10 and 0.15:1.

[0011] Furthermore, the steel slag powder is steel slag powder rich in calcium silicate mineral phase, the mineral phase composition includes γ-type dicalcium silicate, RO phase, calcium ferrite, tricalcium silicate, free calcium oxide and free magnesium oxide, wherein the total mass content of dicalcium silicate and tricalcium silicate is >40%; the carbide slag is a by-product of the hydrolysis of carbide to produce acetylene, and the mass fraction of CaO is ≥80%.

[0012] Furthermore, the basalt fiber is short-cut basalt fiber, with a length of 6~18 mm, a diameter of 10~20 μm, and a tensile strength ≥2000 MPa; the bamboo powder has a median particle size D50 of 354.27 μm and a cumulative particle size D90 of 876.17 μm; the organic synthetic fiber includes PVA fiber and / or glass fiber, with PVA fiber having a length of 6~12 mm, a diameter of 12~24 μm, and a tensile strength ≥1200 MPa, and the glass fiber being alkali-free glass fiber, with a length of 6~12 mm, a diameter of 10~16 μm, and a tensile strength ≥1700 MPa.

[0013] Furthermore, the magnesium source is one or more of magnesium oxide, magnesium hydroxide, magnesium chloride, or magnesium sulfate; the polyaspartic acid has a weight-average molecular weight of 2000-8000; the strontium source is strontium nitrate or strontium chloride; and the polyacrylic acid has a weight-average molecular weight of 3000-10000.

[0014] Furthermore, the silica fume has a particle size of 0.2~5 μm and a SiO2 mass content of ≥90%; the limestone powder has a particle size of 10~20 μm; the expanded perlite has a particle size of 50~300 μm; and the pigments include cadmium red, titanium nickel yellow, titanium chromium brown, cobalt blue or cobalt green, with a particle size of 10~20 μm.

[0015] Secondly, the present invention provides a method for preparing a crystal-modified calcium carbonate fiberboard, which is achieved by the following technical solution.

[0016] A method for preparing the above-mentioned crystal form-controlled calcium carbonate fiberboard includes the following steps: S1. Raw material pretreatment S2. Preparation of Mixtures Basalt fiber, bamboo powder and organic synthetic fiber, steel slag powder, carbide slag, silica fume, limestone powder, expanded perlite and pigment are mixed to obtain a mixture. S3. Slurry preparation, pressing, demolding and curing Add water to the mixture and stir to form a slurry; place the slurry in a mold and press it, demold to obtain a slab, and let it rest; S4. First vacuum impregnation A first impregnation solution containing polyaspartic acid and magnesium source was prepared, and the first-stage regulator was introduced into the interior of the cured slab using a vacuum impregnation method. S5. First stage carbonization The slab after the first vacuum impregnation is passed through CO2 for the first stage of carbonization. S6. Second vacuum impregnation A second impregnation solution containing strontium source and polyacrylic acid was prepared, and the second-stage regulator was introduced into the interior of the slab after the first-stage carbonization by vacuum impregnation. S7. Second Stage Carbonization The blank obtained in step S6 is passed through CO2 again for a second stage of carbonization. After carbonization, it is dried to obtain aragonite-spherulite composite calcium carbonate negative carbon fiber board.

[0017] Furthermore, in step S4, the concentration of polyaspartic acid in the first impregnation solution is 0.5%~2.0%, the concentration of magnesium source is 0.1~0.5mol / L, and the total volume of the impregnation solution is calculated to completely submerge the slab and ensure that the slab weight gain is 8%~15%; the vacuum degree is -0.08~-0.095MPa, and the impregnation time is 0.5~2h; after impregnation, it is pre-dried at 40~60℃ until the water to solid mass ratio is 0.05~0.2:1.

[0018] Furthermore, in step S5, the carbonization conditions in the first stage are: CO2 volume concentration 10%~30%, temperature 25~45℃, relative humidity 40%~70%, CO2 pressure 0.1~0.3MPa, and carbonization time 3~8h; the carbonization conversion rate is controlled to 45%~65% by CO2 absorption weight gain method.

[0019] Furthermore, in step S6, the concentration of strontium source in the second impregnation solution is 0.1~0.5 mol / L, the concentration of polyacrylic acid is 0.5%~2.0%, and the total volume of the impregnation solution is calculated to completely submerge the slab and ensure that the slab weight gain is 8%~15%; the vacuum degree is -0.08~-0.095 MPa, the impregnation time is 0.5~2 h, and after impregnation, it is pre-dried at 40~60℃ until the water to solid mass ratio is 0.05~0.2:1.

[0020] Furthermore, in step S7, the carbonization conditions for the second stage are: CO2 volume concentration of 30%~80%, temperature of 30~60℃, relative humidity of 40%~70%, CO2 pressure of 0.2~0.5MPa, and carbonization time of 8~20h, with the endpoint being that the weight gain from CO2 absorption is stable or the weight gain is <0.2% for 2 consecutive hours.

[0021] By adopting the above technical solution, this application uses a steel slag-calcium carbide slag composite calcium source and a two-stage vacuum impregnation and phased carbonation process to construct aragonite-nepheline composite calcium carbonate in situ in fiberboard. The technical mechanism is as follows: The introduction of carbide slag provides an additional active calcium source for the first stage of carbonization, forming a calcium source relay with the steel slag: the CaO content of carbide slag reaches 80%~90%, mainly existing in the form of Ca(OH)2, and its active calcium component can supplement the system with Ca in the early stage of the first stage of carbonization. 2+ The relay of time between the slow-release calcium formation of calcium silicate phases such as β-C2S and γ-C2S in steel slag and the carbonization process allows the first-stage carbonization to achieve a target conversion rate of 45% to 65% within 4 hours, providing a time window for the establishment of the aragonite occupancy layer. It should be noted that carbide slag in this invention mainly serves as an auxiliary calcium source for rapid calcium dissolution in the first stage, and its dosage of 5% to 20% can form an effective calcium source relay with steel slag. The core invention lies in the phased introduction of the first-stage regulator (polyaspartic acid + magnesium source) and the second-stage regulator (strontium source + polyacrylic acid), combined with stepwise carbonization, to achieve the directional construction of the aragonite-nepheline composite crystal form and the effective inhibition of calcite formation.

[0022] Steel slag continuously releases calcium in the middle and late stages, maintaining the dense growth of the crystal occupancy layer: The carbonization reaction rate of calcium silicate phases such as β-C2S and γ-C2S in steel slag is relatively slow, and it continuously releases Ca in the middle and late stages. 2+ This ensures a timely calcium source relay with the calcium carbide slag formation, preventing the aragonite-occupying layer from becoming "patchy" or its growth from being interrupted due to initial calcium depletion. The endogenous Mg from the slow dissolution of free MgO in the steel slag... 2+ In synergy with an external magnesium source, it fills the adsorption vacancies between polyaspartic acid molecules, enhancing the compactness and stability of the molecular-ion co-occupancy layer.

[0023] The first vacuum impregnation process ensures that the first-stage regulator penetrates evenly into the interior of the slab: After static curing, the slab is vacuum impregnated, allowing polyaspartic acid and magnesium source to enter the pores of the slab along with the impregnation solution, preventing the regulator from remaining only on the surface. After vacuum impregnation, the slab is pre-dried to a water-to-solid ratio of 0.05~0.2:1 to remove excess free water, allowing the regulator to form a uniform adsorption layer on the pore wall surface, providing sites for the directional growth of aragonite crystal nuclei during the subsequent carbonization process.

[0024] The second vacuum impregnation allows for the directional introduction of the second-stage regulator onto the aragonite occupant layer: After the first-stage carbonization is completed, an aragonite crystal occupant layer has formed inside the slab. At this point, strontium source and polyacrylic acid are introduced through vacuum impregnation, causing Sr... 2+ Using the first-stage occupancy layer as an anchor point, selective adsorption occurs on specific crystal planes of aragonite, inducing heterogeneous nucleation and directional distribution of nepheline along the aragonite crystal planes. Polyacrylic acid adsorbs onto the surface of the nepheline crystal nuclei, reducing the nepheline-solution interfacial energy and inhibiting the transformation of nepheline to calcite. If the two-stage regulators are premixed at once, Sr... 2+ Unable to use the first-stage aragonite occupant layer as an anchor point, the distribution of nepheline is uneven; if Sr is lacking 2+ Insufficient heterogeneous nucleation of nepheline; if polyacrylic acid is lacking, nepheline is prone to transcrystallization into calcite.

[0025] Steel slag plays a role in the slow release and replenishment of residual calcium in the second stage: the incompletely carbonized calcium silicate mineral phase in the steel slag continues to slowly release Ca in the second stage. 2+ Together with residual active calcium in carbide slag, it maintains local calcium levels. 2+ / Sr 2+ Compared to, promoting Sr 2+ Selective adsorption occurs using the aragonite crystal facets as anchor points, inducing nepheline to nucleate along the aragonite crystal faces. The slow-release properties of steel slag avoid the homogeneous nucleation caused by a sudden increase in local supersaturation when calcium is added solely by carbide slag.

[0026] In addition, the γ-C2S carbide products in steel slag themselves contain small amounts of aragonite and nepheline, which are polyaspartic acid and Mg. 2+ This invention provides a crystal template that eliminates the need for nucleation from scratch, reducing the nucleation barrier of aragonite. Inert mineral phases such as RO phase and calcium ferrite in steel slag serve as micro-aggregate fillers, forming a multi-level dense structure with the aragonite framework and the dispersed nepheline phase. It should be noted that the reduction in water absorption in this invention does not primarily rely on the filling of micropores by nepheline, but rather stems from a significant reduction in the proportion of calcite. Calcite has a rhombohedral crystal form, which easily forms rigid stacking and open pores between grains; aragonite has a acicular crystal form, while nepheline has a spherical crystal form. When these two are stacked, they more easily form a tightly interlocked structure, and the dispersed distribution of nepheline among the aragonite crystal faces avoids the pore channels caused by the stacking of calcite rhombohedral crystals. Therefore, one of the core effects of staged crystal form control is to "suppress calcite and promote aragonite-nepheline," thereby fundamentally reducing the open porosity of the matrix.

[0027] This application has the following beneficial effects: (1) Through the effect of steel slag-carbide slag compounding and the phased crystal distribution control, aragonite-aragonite composite calcium carbonate is formed in situ in fiberboard, with aragonite accounting for 48%~57%, aragonite accounting for 32%~40%, and calcite accounting for 6%~18%, and the proportion of the three crystal forms is controllable. (2) Aragonite needle-like framework and fibers form a dual-scale reinforcement, and spheroidal aragonite fills the micropores and strengthens the interface; (3) The water absorption rate of the product of the present invention is reduced to 7.0%~8.5%, and the density is significantly improved. Attached Figure Description

[0028] Figure 1 This is the XRD pattern of steel slag in an embodiment of the present invention; Figure 2 These are microscopic morphology images of steel slag in embodiments of the present invention; Figure 3 This is a particle size distribution diagram of steel slag (a) and bamboo powder (b) in an embodiment of the present invention. Detailed Implementation

[0029] The present invention will be further described below with reference to embodiments. Unless otherwise specified, the experimental methods used in the following embodiments are conventional methods. Unless otherwise specified, the materials used in the preparation process in the following embodiments have not undergone further processing and are all commercially available.

[0030] The steel slag powder used in the following embodiments of the present invention was obtained from Maanshan Iron & Steel Co., Ltd. Its chemical composition was determined by X-ray fluorescence spectroscopy (XRF), and the results, expressed as oxide mass fractions, were: CaO 41.86%, Fe2O3 20.74%, SiO2 12.82%, Al2O3 10.76%, MgO 6.39%, MnO 3.02%, P2O5 1.90%, TiO2 1.09%, SO3 0.46%, Na2O 0.09%, SrO 10.03%, Cl 0.02%, K2O 0.02%, and loss on ignition 0.02%.

[0031] like Figure 1 As shown, XRD analysis indicates that the main phase composition of steel slag includes C2S (β-C2S, γ-C2S), C3S, C2F, and RO phases, as well as small amounts of Ca(OH)2, MgO, and FeO. The median particle size D50 of the steel slag after ball milling is 15.79 μm, and the cumulative particle size D90 is 57.75 μm.

[0032] The embodiments of the present invention utilize byproducts generated in the acetylene production process via calcium carbide hydrolysis, which are residues after the acetylene production process via calcium carbide hydrolysis.

[0033] like Figure 3 As shown, the bamboo powder used in this embodiment of the invention has D50 and D90 values ​​of 354.27 μm and 876.17 μm, respectively. Compared with steel slag, bamboo powder has a larger particle size, which is beneficial for forming a heterogeneous fiber support structure in the composite matrix.

[0034] The basalt fibers used in the embodiments of the present invention have a length of 6~18mm and a diameter of 10~20μm.

[0035] The organic synthetic fibers used in the embodiments of the present invention include PVA fibers and / or glass fibers. The PVA fibers are 6-12 mm in length, 12-24 μm in diameter, and have a tensile strength ≥1200 MPa. The glass fibers are commercially available alkali-free glass fibers, 6-12 mm in length, 10-16 μm in diameter, and have a tensile strength ≥1700 MPa.

[0036] The polyaspartic acid used in the following embodiments of the present invention has a weight-average molecular weight of 2000-8000; The polyacrylic acid used in the following embodiments of the present invention has a weight-average molecular weight of 3000~10000; The expanded perlite used in the following embodiments of the present invention has a particle size of 50~300 μm.

[0037] In the following embodiments of the present invention, X-ray diffraction (XRD) + Rietveld full-spectrum fitting method was used to quantitatively analyze the relative mass fraction of calcium carbonate in the product of three crystal forms: aragonite, nepheline, and calcite.

[0038] Example 1 A type of calcium carbonate fiberboard with regulated crystal form, with the following raw material ratio: 600 g of steel slag powder (specific surface area 380 m²) 2 / kg), 150 g of carbide slag (CaO mass fraction 85%, specific surface area 400 m²), 2 / kg), basalt fiber 40 g, bamboo powder 20 g, PVA fiber 20 g, magnesium hydroxide 10 g, polyaspartic acid 5 g, silica fume 60 g, limestone powder 150 g, expanded perlite 50 g, cadmium red pigment 2 g, and water as needed.

[0039] The specific preparation method is as follows: (1) Raw material pretreatment: water content 4%, aging for 36 h; carbide slag pre-digestion: water content 6%, aging for 36 h; basalt fiber was treated with KH-550 ethanol solution, coupling agent mass fraction 0.8%, soaked for 45 min, and dried at 70℃.

[0040] (2) Mix basalt fiber, bamboo powder, PVA fiber, steel slag powder, carbide slag, silica fume, limestone powder, expanded perlite and pigment for 15 min to obtain a mixture.

[0041] (3) Place the mixture and water in a pulping machine and stir for 12 minutes to form a slurry; place the slurry in a mold and press it to obtain a slab; let it stand at 40℃ and relative humidity ≤50% for 3 hours until the water-to-solid ratio in the slab is 0.1:1.

[0042] (4) First vacuum impregnation: Prepare a first impregnation solution containing polyaspartic acid and magnesium hydroxide. The concentration of polyaspartic acid is 1.0% and the concentration of magnesium hydroxide is 0.3 mol / L. The total volume of the impregnation solution is calculated to completely submerge the slab and ensure that the slab weight increases by 10%. The first stage regulator is introduced into the slab after static curing by vacuum impregnation method. The vacuum degree is -0.09 MPa, and the impregnation is carried out for 1 hour. After impregnation, the slab is pre-dried at 50°C until the water-to-solid ratio is 0.1:1.

[0043] (5) First stage carbonization: CO2 volume concentration 20%, temperature 35℃, relative humidity 50%, pressure 0.15MPa, carbonization for 4h, and control carbonization conversion rate 55%.

[0044] (6) Second vacuum impregnation: The second impregnation solution is 0.2mol / L Sr(NO3)2 + 1.0% polyacrylic acid. The total volume of the impregnation solution is calculated to completely submerge the slab and ensure that the slab weight increases by 10%. The slab after the first stage carbonization is vacuum impregnated at a vacuum degree of -0.09MPa for 1 hour. After impregnation, it is pre-dried at 50℃ until the water-to-solid ratio is 0.1:1.

[0045] (7) Second stage carbonization: CO2 volume concentration 50%, temperature 40℃, relative humidity 50%, pressure 0.3MPa, carbonization for 16h, with the end point being the weight gain and stabilization of CO2 absorption.

[0046] (8) After carbonization, the board is dried at 50°C until the moisture content is ≤5%.

[0047] Performance testing The calcium carbonate crystal composition (based on the total mass of calcium carbonate in the carbonation products) is aragonite 52%, nepheline 37%, and calcite 11%; the dry flexural strength is 26 MPa, the saturated flexural strength is 21 MPa, the water absorption rate is 7.8%, the density is 1.85 g / cm3, and the moisture content is ≤5%.

[0048] Example 2 (medium-low calcium carbide slag + alternative magnesium / strontium source) Raw material ratio: 650 g steel slag powder, 100 g calcium carbide slag (CaO mass fraction 88%), 60 g basalt fiber, 20 g bamboo powder, 20 g glass fiber, 15 g magnesium sulfate, 8 g polyaspartic acid, 50 g silica fume, 180 g limestone powder, 20 g expanded perlite, 2 g titanium nickel yellow pigment, and appropriate amount of water.

[0049] The preparation method is as follows: the raw material pretreatment, fiber suspension and mixture preparation, slurry preparation and pressing and curing steps are the same as in Example 1. The difference from Example 1 is: First vacuum impregnation: The impregnation solution is 1.5% polyaspartic acid + 0.3 mol / L magnesium sulfate. The slab is completely submerged and the weight gain of the slab is guaranteed to be 10%. Vacuum impregnation lasts for 1.5 hours.

[0050] First stage carbonization: CO2 concentration 18%, temperature 35℃, relative humidity 55%, pressure 0.15 MPa, carbonization for 3.5 h, conversion rate controlled at 50%.

[0051] Second vacuum impregnation: The impregnation solution is 0.15 mol / L SrCl2 + 1.5% polyacrylic acid. The slab is completely submerged and the weight gain of the slab is guaranteed to be 10%. Vacuum impregnation is carried out for 1.5 h.

[0052] Second stage carbonization: CO2 concentration 55%, temperature 45℃, relative humidity 55%, pressure 0.35 MPa, carbonization for 18 h.

[0053] Performance testing: The calcium carbonate crystal composition (based on the total mass of calcium carbonate in the carbonation products) is 50% aragonite, 40% nepheline, and 10% calcite; the dry flexural strength is 25 MPa, the saturated flexural strength is 20 MPa, the water absorption rate is 7.5%, the density is 1.82 g / cm3, and the moisture content is ≤5%.

[0054] Example 3 (Lower limit boundary example of carbide slag, 5%) Raw material ratio: 712.5 g steel slag powder, 37.5 g calcium carbide slag (5% of the cementitious component), 40 g basalt fiber, 20 g bamboo powder, 20 g PVA fiber, 10 g magnesium hydroxide, 5 g polyaspartic acid, 60 g silica fume, 150 g limestone powder, 50 g expanded perlite, 2 g cadmium red pigment, and appropriate amount of water.

[0055] Preparation process: The raw material pretreatment, fiber suspension and mixture preparation, slurry preparation and pressing / curing steps are the same as in Example 1. The difference from Example 1 is: First vacuum impregnation: The impregnation solution is 1.0% polyaspartic acid + 0.3 mol / L magnesium hydroxide, and the slab is completely submerged and the weight gain of the slab is guaranteed to be 10%. Vacuum impregnation is carried out for 1 hour.

[0056] First stage carbonization: CO2 concentration 20%, temperature 35℃, relative humidity 50%, pressure 0.15 MPa, carbonization for 4 h, conversion rate controlled at 47%.

[0057] Second vacuum impregnation: The impregnation solution is 0.2 mol / L Sr(NO3)2+ 1.0% polyacrylic acid, and the blank is completely submerged and the blank weight gain is guaranteed to be 10%. Vacuum impregnation is carried out for 1 h.

[0058] Second stage carbonization: CO2 concentration 50%, temperature 40℃, relative humidity 50%, pressure 0.3 MPa, carbonization for 16 h.

[0059] Performance testing: The calcium carbonate crystal composition (based on the total mass of calcium carbonate in the carbonation products) is 48% aragonite, 33% nepheline, and 16% calcite; the dry flexural strength is 24 MPa, the saturated flexural strength is 19 MPa, the water absorption rate is 8.7%, the density is 1.78 g / cm3, and the moisture content is ≤5%.

[0060] Example 4 (Upper limit of calcium carbide slag + upper limit of regulator + high conversion rate) Raw material ratio: 600 g steel slag powder, 150 g calcium carbide slag (accounting for 20% of the cementitious component), 40 g basalt fiber, 20 g bamboo powder, 20 g PVA fiber, 30 g magnesium hydroxide, 15 g polyaspartic acid, 60 g silica fume, 150 g limestone powder, 50 g expanded perlite, 2 g cadmium red pigment, and appropriate amount of water.

[0061] Preparation process: The raw material pretreatment, fiber suspension and mixture preparation, slurry preparation and pressing / curing steps are the same as in Example 1. The difference from Example 1 is: First vacuum impregnation: The impregnation solution is 2.0% polyaspartic acid + 0.5 mol / L magnesium hydroxide, which is used to completely immerse the slab and ensure a 10% weight gain. The vacuum degree is -0.095 MPa, and the impregnation is carried out for 1 hour. The slab is then pre-dried at 50°C to a water-to-solid ratio of 0.1:1.

[0062] First stage carbonization: CO2 concentration 25%, temperature 35℃, relative humidity 50%, pressure 0.2 MPa, carbonization for 6 h, conversion rate controlled at 62%.

[0063] Second vacuum impregnation: The impregnation solution is 0.5 mol / L Sr(NO3)2+ 2.0% polyacrylic acid, which is used to completely immerse the slab and ensure a 10% weight gain. The vacuum degree is -0.095 MPa, and the impregnation is carried out for 1 h. The slab is then pre-dried at 50℃ to a water-to-solid ratio of 0.1:1.

[0064] Second stage carbonization: CO2 concentration 80%, temperature 50℃, relative humidity 50%, pressure 0.5 MPa, carbonization for 20 h.

[0065] Performance testing The calcium carbonate crystal composition (based on the total mass of calcium carbonate in the carbonation products) is aragonite 57%, nepheline 37%, and calcite 6%; the dry flexural strength is 27 MPa, the saturated flexural strength is 22 MPa, the water absorption rate is 7.2%, the density is 1.88 g / cm3, and the moisture content is ≤5%.

[0066] Example 5 (Lower Limit Example of Regulator) Raw material ratio: 600 g steel slag powder, 150 g calcium carbide slag, 40 g basalt fiber, 20 g bamboo powder, 20 g PVA fiber, 6.25 g magnesium hydroxide, 1.25 g polyaspartic acid, 60 g silica fume, 150 g limestone powder, 50 g expanded perlite, 2 g cadmium red pigment, and appropriate amount of water.

[0067] Preparation process: The raw material pretreatment, fiber suspension and mixture preparation, slurry preparation and pressing / curing steps are the same as in Example 1. The difference from Example 1 is: First vacuum impregnation: The impregnation solution is 0.5% polyaspartic acid + 0.1 mol / L magnesium hydroxide. The slab is completely submerged and the weight gain of the slab is guaranteed to be 10%. Vacuum impregnation is carried out for 1 hour.

[0068] First stage carbonization: CO2 concentration 20%, temperature 35℃, relative humidity 50%, pressure 0.15 MPa, carbonization for 4 h, conversion rate controlled at 47%.

[0069] Second vacuum impregnation: The impregnation solution is 0.1 mol / L Sr(NO3)2 + 0.5% polyacrylic acid. The slab is completely submerged and the weight gain of the slab is guaranteed to be 10%. Vacuum impregnation is performed for 1 h.

[0070] Second stage carbonization: CO2 concentration 50%, temperature 40℃, relative humidity 50%, pressure 0.3 MPa, carbonization for 16 h.

[0071] Performance testing The calcium carbonate crystal composition (based on the total mass of calcium carbonate in the carbonation products) is 47% aragonite, 32% nepheline, and 18% calcite; the dry flexural strength is 24 MPa, the saturated flexural strength is 19 MPa, the water absorption rate is 8.7%, the density is 1.77 g / cm3, and the moisture content is ≤5%.

[0072] Comparative Example 1 (pure steel slag, compounded without carbide slag) Raw material ratio: Calcium carbide slag is replaced by steel slag in equal amounts, i.e., 750 g of steel slag powder, and the rest is the same as in Example 1.

[0073] Preparation process: Same as in Example 1.

[0074] Performance testing: The calcium carbonate crystal composition (based on the total mass of calcium carbonate in the carbonation product) is aragonite 42%, nepheline 27%, and calcite 28%; the first stage of carbonation requires 6.5 hours to reach a 55% conversion rate, which is 62.5% longer than that of Example 1; the dry flexural strength is 21 MPa, the saturated flexural strength is 17 MPa, the water absorption rate is 10.0%, and the density is 1.68 g / cm3.

[0075] Comparative Example 2 (Complete replacement of steel slag with carbide slag) Raw material ratio: The cementing component is 750 g of carbide slag, and the rest is the same as in Example 1.

[0076] Preparation process: Same as in Example 1.

[0077] Performance testing: The calcium carbonate crystal composition (based on the total mass of calcium carbonate in the carbonation products) is aragonite 32%, nepheline 17%, and calcite 50%; the initial carbonation reaction is intense, the surface densifies prematurely, and the internal carbonization is incomplete; the dry flexural strength is 17 MPa, the saturated flexural strength is 13 MPa, the water absorption rate is 13.0%, and the density is 1.55 g / cm3.

[0078] Comparative Example 3 (excessive calcium carbide slag content, 30%) Raw material ratio: The total amount of cementitious components is 750 g, of which 225 g is calcium carbide slag, 525 g is steel slag powder, and the rest is the same as in Example 1.

[0079] Preparation process: Same as in Example 1.

[0080] Performance testing: The calcium carbonate crystal composition (based on the total mass of calcium carbonate in the carbonation products) is aragonite 47%, nepheline 32%, and calcite 22%; SEM observation shows that the aspect ratio of aragonite is approximately 8-12, and the polyaspartic acid-Mg2+ occupying layer covers approximately 60%, exhibiting a "patchy" distribution; in the early stage of carbonation, Ca2+... + The supersaturation is extremely high, with localized excessive thickness and voids in the occupying layer, and the aragonite growth direction is disordered; the dry flexural strength is 22 MPa, the saturated flexural strength is 17.5 MPa, the water absorption rate is 9.5%, and the density is 1.72 g / cm3.

[0081] Comparative Example 4 (calcium carbide slag content was too low, 3%) Raw material ratio: The total amount of cementitious components is 750 g, of which 22.5 g is calcium carbide slag, 727.5 g is steel slag powder, and the rest is the same as in Example 1.

[0082] Preparation process: Same as in Example 1.

[0083] Performance testing: The calcium carbonate crystal composition (based on the total mass of calcium carbonate in the carbonation products) is aragonite 45%, nepheline 27%, and calcite 28%. SEM observation shows that the aspect ratio of aragonite is about 15~20, the polyaspartic acid-Mg2+ site coverage is about 55%, and it is distributed in a "sparse" manner. The first stage of rapid calcium dissolution is insufficient, the establishment of high supersaturation is slow, the nucleation density of aragonite is low, and the site layer is incomplete. The dry flexural strength is 22MPa, the saturated flexural strength is 17MPa, the water absorption rate is 10.0%, and the density is 1.70g / cm3.

[0084] Comparative Example 5 (without the first-stage regulator) Raw material ratio: without polyaspartic acid and magnesium hydroxide, the rest is the same as in Example 1.

[0085] Preparation process: The first vacuum impregnation solution was changed to deionized water, and the rest was the same as in Example 1.

[0086] Performance testing: The calcium carbonate crystal composition (based on the total mass of calcium carbonate in the carbonation products) is aragonite 32%, nepheline 22%, and calcite 45%; the lack of polyaspartic acid-Mg2+ co-occupancy layer restricts aragonite nucleation; the dry flexural strength is 19 MPa, the saturated flexural strength is 15 MPa, the water absorption rate is 11.0%, and the density is 1.62 g / cm3.

[0087] Comparative Example 6 (polyaspartic acid only, no magnesium source added) Raw material ratio: retain 5 g of polyaspartic acid, do not add magnesium hydroxide, and the rest is the same as in Example 1.

[0088] Preparation process: The first vacuum impregnation solution was 1.0% polyaspartic acid, without magnesium hydroxide, and the rest was the same as in Example 1.

[0089] Performance testing: The calcium carbonate crystal composition (based on the total mass of calcium carbonate in the carbonation products) is aragonite 37%, nepheline 27%, and calcite 35%; lacking Mg2+ co-occupancy, the polyaspartic acid adsorption vacancies are not filled, and the density of the occupancy layer decreases; the dry flexural strength is 20 MPa, the saturated flexural strength is 16 MPa, the water absorption rate is 10.0%, and the density is 1.66 g / cm3.

[0090] Comparative Example 7 (without a second-stage regulator) Raw material ratio: Same as in Example 1.

[0091] Preparation process: The second vacuum impregnation solution was changed to deionized water, which does not contain Sr(NO3)2 and polyacrylic acid; the rest is the same as in Example 1.

[0092] Performance testing: The calcium carbonate crystal composition (based on the total mass of calcium carbonate in the carbide products) is aragonite 47%, nepheline 12%, and calcite 40%; lacking Sr. 2+The anchoring point and polyacrylic acid stabilize the nepheline heterogeneous nucleation, which leads to insufficient nucleation and easy crystal transformation. The dry flexural strength is 20 MPa, the saturated flexural strength is 16 MPa, the water absorption rate is 10.0%, and the density is 1.67 g / cm³. 3 .

[0093] Comparative Example 8 (polyacrylic acid only, no strontium source added) Raw material ratio: Same as in Example 1.

[0094] Preparation process: The second vacuum impregnation solution is 1.0% polyacrylic acid, which does not contain Sr(NO3)2; the rest is the same as in Example 1.

[0095] Performance testing: The calcium carbonate crystal composition (based on the total mass of calcium carbonate in the carbide products) is aragonite 47%, nepheline 17%, and calcite 35%; lacking Sr² + Selective adsorption anchors on aragonite crystal faces; poor directional nucleation of nepheline; dry flexural strength 21 MPa, saturated flexural strength 17 MPa, water absorption 9.5%, density 1.69 g / cm³. 3 .

[0096] Comparative Example 9 (Two-stage regulator premixed in one step) Raw material ratio: The equivalent amounts of polyaspartic acid, magnesium source, strontium source and polyacrylic acid of the two impregnation solutions in Example 1 are added to the mixture in step (2) at one time, and the rest is the same as in Example 1.

[0097] Preparation process: The first and second vacuum impregnation processes are omitted, and the second stage carbonization is carried out directly after the first stage carbonization; the rest is the same as in Example 1.

[0098] Performance testing: The calcium carbonate crystal composition (based on the total mass of calcium carbonate in the carbonation products) was aragonite 42%, nepheline 22%, and calcite 32%; the two-stage regulators interfered with each other, Sr 2+ Unable to use the first-stage aragonite occupancy layer as an anchor point, nepheline distribution is uneven; dry flexural strength is 21 MPa, saturated flexural strength is 17 MPa, water absorption is 9.5%, and density is 1.70 g / cm³. 3 .

[0099] Comparative Example 10 (only one stage of carbonization) Raw material ratio: Same as in Example 1.

[0100] Preparation process: The first vacuum impregnation, the second vacuum impregnation, and the second stage carbonization are eliminated; the first stage carbonization directly adopts the second stage carbonization conditions: CO2 volume concentration 50%, temperature 40℃, relative humidity 50%, pressure 0.3MPa, carbonization until CO2 absorption and weight gain are stable, about 19h.

[0101] Performance testing: The calcium carbonate crystal composition (based on the total mass of calcium carbonate in the carbonation products) is aragonite 37%, nepheline 17%, and calcite 45%; a composite crystal structure of "aragonite framework + nepheline dispersed phase" was not formed, and calcite has a high proportion; the dry flexural strength is 19 MPa, the saturated flexural strength is 15 MPa, the water absorption rate is 11.0%, and the density is 1.63 g / cm³. 3 .

[0102] The core effect of this invention lies in the directional control of calcium carbonate crystal form: In Examples 1-5, the carbonization products contained aragonite (48%-57%), nepheline (32%-40%), and calcite (6%-18%), demonstrating controllable proportions of the three crystal forms; in Comparative Examples 5-10, due to the lack of a staged control agent or stepwise carbonization, the aragonite proportion decreased to 32%-47%, while the calcite proportion increased to 32%-45%, proving that "staged crystal form control" is a necessary condition for obtaining the aragonite-nepheline composite crystal form. Data from the examples and comparative examples show that the calcite proportion in the carbonization products is significantly positively correlated with the overall water absorption rate of the slabs: when the calcite proportion increased from 6% to 50%, the water absorption rate increased from 7.2% to 13.0%, and the density increased from 1.88 g / cm³. 3 Reduced to 1.55 g / cm³ 3 (Correlation coefficient R²>0.9). Some data points showed fluctuations, which are related to factors such as the proportion of nepheline and the uniformity of fiber distribution. However, the overall pattern further confirms that the main mechanism of this invention in reducing water absorption is that the staged crystal form regulation significantly inhibits the formation of calcite, rather than simply relying on the filling of micropores by nepheline.

[0103] The embodiments described herein are preferred embodiments of the present invention and are not intended to limit the scope of protection of the present invention. Therefore, all equivalent changes made in accordance with the structure, shape, and principle of the present invention should be covered within the scope of protection of the present invention.

Claims

1. A crystal-modified calcium carbonate fiberboard, characterized in that: Includes the following components by weight: Cementitious component: 55~75 parts; the cementitious component consists of steel slag powder and carbide slag, of which carbide slag accounts for 5%~20% of the total mass of the cementitious component; Basalt fiber: 2-6 parts; Bamboo powder: 1-4 parts; Organic synthetic fibers: 0-4 parts; First-stage regulator: 0.1-1.5 parts polyaspartic acid, 0.5-3 parts magnesium source; Second-stage regulator: 0.5-3 parts strontium source, 0.1-1.5 parts polyacrylic acid; Silica fume: 4-8 parts; Limestone powder: 10-20 parts; Expanded perlite: 0-10 parts; Pigment: 0.1~0.2 parts; The water-to-solid ratio should be controlled between 0.10 and 0.15:

1.

2. The crystal form-controlled calcium carbonate fiberboard according to claim 1, characterized in that: Steel slag powder is steel slag powder rich in calcium silicate mineral phase. The mineral phase composition includes γ-type dicalcium silicate, RO phase, calcium ferrite, tricalcium silicate, free calcium oxide and free magnesium oxide. The total mass content of dicalcium silicate and tricalcium silicate is >40%. Calcium carbide slag is a by-product of calcium carbide hydrolysis to produce acetylene, with a CaO mass fraction ≥80%.

3. The crystal-modified calcium carbonate fiberboard according to claim 1, characterized in that: The basalt fiber is a short-cut basalt fiber with a length of 6~18 mm, a diameter of 10~20 μm, and a tensile strength ≥2000 MPa; the bamboo powder has a median particle size D50 of 354.27 μm and a cumulative particle size D90 of 876.17 μm; the organic synthetic fiber includes PVA fiber and / or glass fiber.

4. The crystal form-controlled calcium carbonate fiberboard according to claim 1, characterized in that: The magnesium source is one or more of magnesium oxide, magnesium hydroxide, magnesium chloride, or magnesium sulfate; the polyaspartic acid has a weight-average molecular weight of 2000-8000; the strontium source is strontium nitrate or strontium chloride; and the polyacrylic acid has a weight-average molecular weight of 3000-10000.

5. The crystal form-controlled calcium carbonate fiberboard according to claim 1, characterized in that: The particle size of silica fume is 0.2~5 μm, and the SiO2 mass content is ≥90%; the particle size of limestone powder is 10~20 μm; the particle size of expanded perlite is 50~300 μm; the pigments include cadmium red, titanium nickel yellow, titanium chromium brown, cobalt blue or cobalt green, with a particle size of 10~20 μm.

6. A method for preparing a crystal-modified calcium carbonate fiberboard according to any one of claims 1-5, characterized in that: Includes the following steps: S1. Raw material pretreatment S2. Preparation of Mixtures Basalt fiber, bamboo powder and organic synthetic fiber, steel slag powder, carbide slag, silica fume, limestone powder, expanded perlite and pigment are mixed to obtain a mixture. S3. Slurry preparation, pressing, demolding and curing Add water to the mixture and stir to form a slurry; place the slurry in a mold and press it, demold to obtain a slab, and let it rest; S4. First vacuum impregnation A first impregnation solution containing polyaspartic acid and magnesium source was prepared, and the first-stage regulator was introduced into the interior of the cured slab using a vacuum impregnation method. S5. First stage carbonization The slab after the first vacuum impregnation is passed through CO2 for the first stage of carbonization. S6. Second vacuum impregnation A second impregnation solution containing strontium source and polyacrylic acid was prepared, and the second-stage regulator was introduced into the interior of the slab after the first-stage carbonization by vacuum impregnation. S7. Second Stage Carbonization The blank obtained in step S6 is passed through CO2 again for a second stage of carbonization. After carbonization, it is dried to obtain aragonite-spherulite composite calcium carbonate negative carbon fiber board.

7. The method for preparing a crystal-modified calcium carbonate fiberboard according to claim 6, characterized in that: In step S4, the concentration of polyaspartic acid in the first impregnation solution is 0.5%~2.0%, the concentration of magnesium source is 0.1~0.5mol / L, and the total volume of the impregnation solution is calculated to completely submerge the slab and ensure that the slab weight gain is 8%~15%. The vacuum degree is -0.08 to -0.095 MPa, and the impregnation time is 0.5 to 2 hours. After impregnation, it is pre-dried at 40 to 60°C until the water to solid mass ratio is 0.05 to 0.2:

1.

8. The method for preparing a crystal-modified calcium carbonate fiberboard according to claim 6, characterized in that: In step S5, the first stage carbonization conditions are: CO2 volume concentration 10%~30%, temperature 25~45℃, relative humidity 40%~70%, CO2 pressure 0.1~0.3MPa, and carbonization time 3~8h; the carbonization conversion rate is controlled to 45%~65% by CO2 absorption weight gain method.

9. The method for preparing a crystal-modified calcium carbonate fiberboard according to claim 6, characterized in that: In step S6, the concentration of strontium source in the second impregnation solution is 0.1~0.5 mol / L, the concentration of polyacrylic acid is 0.5%~2.0%, and the total volume of the impregnation solution is calculated to completely submerge the slab and ensure that the slab weight gain is 8%~15%. The vacuum degree is -0.08 to -0.095 MPa, the impregnation time is 0.5 to 2 hours, and after impregnation, it is pre-dried at 40 to 60℃ until the water to solid mass ratio is 0.05 to 0.2:

1.

10. The method for preparing a crystal-modified calcium carbonate fiberboard according to claim 6, characterized in that: In step S7, the carbonization conditions for the second stage are: CO2 volume concentration 30%~80%, temperature 30~60℃, relative humidity 40%~70%, CO2 pressure 0.2~0.5MPa, carbonization time 8~20h, with the endpoint being that the weight gain from CO2 absorption is stable or the weight gain is <0.2% for 2 consecutive hours.