A water-regulating waste AAC slag thin-layer mortar and its preparation method
By separating the flow into a combination of low-mineralized fine phase A and pore-mineralized coarse phase B, the contradiction between initial water grabbing and later water supply in thin-layer plastering is resolved, improving the bonding strength and water content stability of AAC/ALC base layer, and realizing a low-carbon and environmentally friendly mortar preparation method.
Patent Information
- Application Number
- CN202611328615.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-10
AI Technical Summary
In thin-layer plastering construction, the dry porous aggregate of AAC/ALC base layer absorbs a large amount of water in the early stage after mixing, which hinders the hydration reaction of cementitious materials. In addition, the carbonate activation reaction of slag requires a continuous supply of water. Existing technology cannot meet the dual time requirements of initial slow absorption and later storage and release at the same time. Furthermore, the moisture content of AAC/ALC base layer is highly sensitive, resulting in unstable bond strength.
Granulated blast furnace slag powder is used as the main cementitious precursor, which is divided into a low-mineralized fine phase A and a coarse phase B with orifice mineralization. The fine phase A mainly undertakes the wettable surface and alkali solution distribution, while the coarse phase B forms carbonate-enriched patches through orifice mineralization treatment to control water absorption characteristics and ensure continuous water supply for hydration reaction within 8 to 24 hours. Combined with the use of anhydrous sodium carbonate and quicklime, a single-component dry powder activation system is formed, avoiding the addition of gypsum and silicate cement clinker.
It achieves coordinated control of initial water replenishment and subsequent water supply in thin-layer plastering scenarios, improves bonding strength and stability across the base layer's moisture content, enhances the mortar's water retention and workability, reduces sensitivity to environmental conditions, and has low-carbon and environmentally friendly benefits.
Smart Images

Figure CN123062218A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of building materials technology, and in particular to a water-regulating waste AAC slag thin-layer mortar and its preparation method. Background Technology
[0002] Autoclaved aerated concrete (AAC) and aerated concrete (ALC) products generate a large amount of scrap material during production. It is common practice to crush the waste material and reuse it as aggregate in the matching plastering mortar.
[0003] Currently, the use of carbonate-activated slag to replace traditional cement in low-carbon cementitious systems is recognized in the industry. When dealing with the high water absorption characteristics of porous aggregates, the conventional approach is to reduce the water absorption rate of aggregates as much as possible through carbonation or coating treatment. The core logic is that the lower the water absorption rate, the better.
[0004] However, this logic is difficult to apply in thin-layer plastering scenarios. Thin-layer plastering is only 3-5 mm thick, with a very small water buffer capacity, which leads to a contradiction. On the one hand, dry porous aggregates and base layers will suddenly absorb a large amount of water within the first minute after mixing, causing the hydration reaction of the cementitious material to be hindered due to lack of water, and the interfacial bonding strength to be damaged. On the other hand, the carbonate-activated reaction of slag still requires a continuous supply of water to maintain the hydration process within 8-24 hours. If the pores of the aggregate are excessively blocked and lose their ability to store and release water, the bonding strength will also decrease in the later stage. Traditional water absorption reduction treatment methods cannot simultaneously meet the dual time requirements of "initial slow absorption" and "later storage and release".
[0005] In addition, the moisture content of the AAC / ALC base layer fluctuates significantly due to differences in environmental conditions, and thin-layer mortar is highly sensitive to this. At present, it is still difficult to reduce the bonding sensitivity across the moisture content of the base layer.
[0006] Therefore, a water-regulating waste AAC slag thin-layer mortar and its preparation method are proposed to solve the above problems. Summary of the Invention
[0007] The purpose of this invention is to provide a water-regulating waste AAC slag thin-layer mortar and its preparation method, which can solve the contradiction between initial water grabbing and later water supply, and improve the bonding stability across the water-bearing state of the base layer.
[0008] The above-mentioned technical objective of this invention is achieved through the following technical solution: a water-regulating waste AAC slag thin-layer mortar, with granulated blast furnace slag powder as the main cementitious precursor, containing no silicate cement clinker and added gypsum, and comprising the following components:
[0009] Anhydrous sodium carbonate 20.0–21.0 kg / t;
[0010] The mortar contains 8.7–9.3 kg / t of quicklime.
[0011] Low-mineralized fine phase A is 42-48 kg / t. The low-mineralized fine phase A is a fine powder obtained by low-temperature drying and air classification of waste autoclaved aerated concrete from the same source. Its median particle size D50 is 40-70 μm, and its relative mineralization Dc ≤ 15%. The relative mineralization Dc is calculated by normalizing the carbon dioxide-related weight loss in thermogravimetric analysis at 550-900℃, with the untreated sample and the fully mineralized platform sample from the same batch as the two ends.
[0012] The coarse mineralized phase B at the pore opening is 72-78 kg / t. This coarse mineralized phase B is a coarse-grained precursor from the same parent batch as the low-mineralized fine phase A, derived from waste autoclaved aerated concrete. Its particle size is 0.30-0.80 mm, and it possesses the following characteristics:
[0013] Carbon dioxide weight gain on a dry basis: 0.45%–0.70%;
[0014] Residual calcium hydroxide ≤0.20%.
[0015] By adopting the above technical solution, the same batch of waste AAC is separated into two asymmetric states. The fine phase A maintains low mineralization and mainly undertakes the functions of wettable surface and alkali distribution. The coarse phase B is treated with orifice mineralization, which forms carbonate enrichment patches at the orifice while retaining internal interconnecting pores. This allows the carbon dioxide dry basis weight gain and residual calcium hydroxide of the coarse phase B to be controlled within a specific range, laying the foundation for further limiting the water absorption kinetics.
[0016] A further feature of the present invention is that the water absorption ratio of the mineralized coarse phase B at the orifice is ≤0.80 within 1 minute, and the capacity retention rate is 75% to 95% within 24 hours.
[0017] By adopting the above technical solution, the water absorption ratio of coarse phase B in 1 minute is reduced to below 0.80, which suppresses the initial water grabbing phenomenon. At the same time, the 24-hour capacity retention rate is maintained at 75% to 95%, ensuring that the slag hydration reaction can obtain a continuous water supply within 8 to 24 hours, thus resolving the contradiction between the initial water grabbing and the later water supply in the thin-layer plastering scenario.
[0018] The present invention is further configured such that: the anhydrous sodium carbonate is 20.0–20.8 kg / t, the quicklime in the mortar matrix is 8.8–9.2 kg / t, the low-mineralized fine phase A is 44–46 kg / t, and the pore-mineralized coarse phase B is 74–76 kg / t; the median particle size D50 of the low-mineralized fine phase A is 50–58 μm, and the relative mineralization Dc is 11%–13%.
[0019] By adopting the above technical solution, the specific surface area and alkali distribution capacity of fine phase A are within the ideal range. Among them, the D50 of batches A-01 to A-03 is 51.9 to 56.1 μm, the specific surface area is 11.8 to 12.5 m² / g, and the relative mineralization is 11.1% to 12.3%. This is conducive to the rapid establishment of a uniform alkali distribution network after mortar mixing. The mortar using this preferred formula achieves a tensile bond strength of over 0.440 MPa on autoclaved aerated concrete base layer after 28 days.
[0020] A further feature of the present invention is that the carbon dioxide dry basis weight gain of the mineralized coarse phase B at the pore opening is 0.52% to 0.64%, the water absorption ratio in 1 minute is 0.68 to 0.80, and the capacity retention rate in 24 hours is 79% to 94%.
[0021] By adopting the above technical solution, the moisture regulation function of coarse phase B is further enhanced.
[0022] A further feature of the present invention is that the surface of the mineralized coarse phase B at the pore opening has spatially discontinuous carbonate enrichment patches, the carbonate coverage is 53% to 60%, the carbonate penetration depth is 38 to 47 μm, and the retention rate of internally distinguishable interconnected pores relative to the untreated state is not less than 85%.
[0023] By adopting the above technical solution, the spatially discontinuous carbonate patches play a role of partially covering rather than sealing the pore openings. This can reduce the initial rate of water entering the pores without blocking water from entering and exiting the particle through the retained connecting pores in the subsequent reaction stage, thereby simultaneously meeting the dual time requirements of initial slow absorption and later storage and release.
[0024] A further provision of the present invention is that the granulated blast furnace slag powder is S95 grade slag powder, with a dosage of 290-310 kg / t; the mortar also contains 13-17 kg / t of alkali-resistant redispersible latex powder, 3.0-3.4 kg / t of hydroxyethyl methyl cellulose ether, 0.30-0.40 kg / t of starch ether, 0.50-0.70 kg / t of polypropylene fiber, 0.70-0.90 kg / t of powder defoamer, 0.10-0.80 mm quartz sand, 440-480 kg / t of quartz powder with a D50 of 23-28 μm, and 65-75 kg / t of quartz powder.
[0025] By adopting the above technical solution, S95 slag powder, sodium carbonate, and quicklime form a single-component dry powder activation system, eliminating the need for external gypsum and silicate cement clinker. Hydroxyethyl methyl cellulose ether imparts good water retention and workability to the mortar. Tests show that the water retention rate of the mortar can be maintained above 99% in the range of 3.0 to 3.4 kg / t, with 3.2 kg / t being the optimal economic balance point. Polypropylene fibers effectively inhibit plastic cracking of the thin layer.
[0026] The invention is further configured such that the proportions of each component are as follows: granulated blast furnace slag powder 300.00 kg / t, anhydrous sodium carbonate 20.50 kg / t, quicklime in the mortar matrix 9.00 kg / t, alkali-resistant redispersible latex powder 15.00 kg / t, hydroxyethyl methyl cellulose ether 3.20 kg / t, starch ether 0.35 kg / t, polypropylene fiber 0.60 kg / t, powder defoamer 0.80 kg / t, low-mineralized fine phase A 45.00 kg / t, pore-mineralized coarse phase B 75.00 kg / t, quartz sand 0.10~0.80 mm 460.00 kg / t, and quartz powder D50 of 25 μm 70.55 kg / t.
[0027] By adopting the above technical solution, the water retention rate under standard curing conditions is ≥99.3%, the 14-day tensile bond strength is ≥0.42 MPa, and the bond stability across the water content state of the base layer is better.
[0028] A further feature of the present invention is that the low-mineralized fine phase A is obtained by air classification of the same source waste autoclaved aerated concrete after drying at a low temperature of 55-65℃ to a moisture content of ≤0.5%, without the use of a high-energy ball mill, and the energy consumption for classification is ≤5 kWh / t.
[0029] By adopting the above technical solutions, low-temperature drying avoids the dehydration and transformation of the tobermorite phase in AAC, and airflow classification achieves efficient separation of the fine phase without destroying the original pore structure of the particles.
[0030] A further provision of the present invention is that, in the mortar, all components except the coarse mineralized phase B at the pore opening are premixed first, and the coarse mineralized phase B at the pore opening is added later in a low-shear manner after the premixing is completed, with a mixing speed ≤30 r / min and a mixing time of 45 to 60 s.
[0031] By adopting the above technical solution, post-addition and low-shear mixing effectively protect the discontinuous carbonate patch structure on the surface of the coarse phase B, avoiding patch spalling and the generation of new fine powder caused by high shear force. Actual measurements showed that after adopting this mixing regime, the retention rate of B particles larger than 0.30 mm in the mixture did not decrease significantly compared to before addition, and the rate of newly added fine powder smaller than 0.15 mm was controlled within an acceptable range.
[0032] This invention also provides a method for preparing water-adjusting waste AAC slag thin-layer mortar, which includes the following steps:
[0033] S1. Take clean autoclaved aerated concrete cutting scraps from the same production line and the same master batch, pre-crush them to less than 5mm, and dry them at a low temperature of 55-65℃ until the moisture content is ≤0.5%;
[0034] S2. The dried material is separated into the low-mineralized fine phase A and the coarse precursor by airflow classification.
[0035] S3. The coarse precursor is screened again, and the 0.30-0.80 mm particle size fraction is sprayed onto the surface of the coarse precursor with a lime slurry of 10%-14% by mass, so that the calcium hydroxide solid is 0.8%-1.2% of the dry mass of the coarse precursor. It is then treated under the conditions of 4%-6% carbon dioxide volume fraction and 20-30℃ until the following four endpoints are met: carbon dioxide dry basis weight gain 0.45%-0.70%, residual calcium hydroxide ≤0.20%, water absorption ratio ≤0.80% in 1 minute, and capacity retention rate 75%-95% in 24 hours. After low-temperature drying and re-screening, the pore mineralized coarse phase B is obtained.
[0036] S4. Weigh all components except the mineralized coarse phase B at the orifice according to the proportion and put them into a dry mixer to mix evenly.
[0037] S5. After stopping the machine and scraping the wall, add the mineralized coarse phase B from the orifice, mix evenly in a low-shear manner, and then discharge and package.
[0038] The beneficial effects of this invention are:
[0039] 1. By separating the waste AAC from the same source into low-mineralized fine phase A and pore-mineralized coarse phase B, the coordinated regulation of moisture in time and space was achieved, which solved the contradiction between the initial water rush and the later water supply in the thin-layer plastering scenario.
[0040] 2. Using four endpoints instead of a single processing time as the release criterion for coarse phase B ensures the repeatability of functional endpoints and applicability across parent batches.
[0041] 3. It uses granulated blast furnace slag powder as the main cementitious precursor, does not contain silicate cement clinker or added gypsum, and utilizes industrial solid waste. While achieving excellent performance, it also has significant low-carbon and environmental protection benefits. Attached Figure Description
[0042] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0043] Figure 1 This is a schematic diagram of the overall process flow provided for an embodiment of the present invention;
[0044] Figure 2 This is a schematic diagram illustrating the separation of homologous waste AAC into fine-phase A and coarse-phase precursors provided in an embodiment of the present invention;
[0045] Figure 3 A schematic diagram of the bonding of biphase fusion under fixed water addition and equal spread provided in an embodiment of the present invention;
[0046] Figure 4 This is a schematic diagram illustrating the robustness of AAC / ALC source batches provided in an embodiment of the present invention.
[0047] Figure 5 This is a schematic diagram of the dynamic water absorption curve of coarse phase B provided in an embodiment of the present invention.
[0048] In the diagram, 100 is the same source of waste AAC raw material; 110 is the pre-crusher; 120 is the classifier; 130 is the low-mineralized fine phase A; 140 is the coarse phase precursor; 210 is the lime slurry tank and nozzle; 220 is the carbon dioxide mineralization chamber; 250 is the low-temperature dryer; 260 is the double screener; 270 is the finished coarse phase B; and 340 is the packaging end. Detailed Implementation
[0049] The technical solution of the present invention will now be clearly and completely described with reference to specific embodiments. Obviously, the described embodiments are merely some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0050] This invention specifically provides a water-regulating waste AAC slag thin-layer mortar and its preparation method, please refer to the attached document. Figure 1-2 The present invention will be further illustrated by the examples and comparative examples.
[0051] Example 1
[0052] Weigh each component according to the proportions in Table 1 (total amount 1000 kg / t, based on oven-dry standard at 105℃):
[0053] Table 1: Formulation of Example 1
[0054]
[0055] The mortar contains CL90-S standard quicklime, 3mm polypropylene fibers, low-mineralized fine phase A (batch A-02) with a D50 of 54.2 μm, a specific surface area of 12.1 m² / g, and a relative mineralization Dc of 11.8%, coarse phase B (batch TB-03) with a particle size of 0.30–0.80 mm, a carbon dioxide dry basis weight gain of 0.586%, residual calcium hydroxide of 0.110%, a 1-minute water absorption ratio of 0.715, a 24-hour capacity retention rate of 90.5%, and quartz sand with a particle size of 0.10–0.80 mm and a D50 of approximately 25 μm.
[0056] Furthermore, this embodiment uses the following method for preparation:
[0057] S1. Take clean, homologous waste AAC raw material 100 from the same mother batch as A-02 and TB-03, pre-crush it to less than 5 mm using a jaw crusher 110, dry it at a low temperature of 60℃ to a moisture content of ≤0.5%, and perform air classification using a classifier 120. The classifier 120 is an air splitter to obtain a low-mineralized fine phase A130 without using a high-energy ball mill, and at the same time obtain a coarse phase precursor 140.
[0058] S2. The 0.30-0.80 mm particle size fraction is obtained from the coarse precursor of the same batch. In the spraying / turning treatment zone, 12% lime slurry is sprayed through the lime slurry tank and nozzle 210 to make the calcium hydroxide solid 1.0% of the oven-dry B precursor. It is then treated in the carbon dioxide mineralization chamber 220 at 25°C with a CO2 volume fraction of 5% (the treatment time required for this batch to reach the four-stage endpoint is about 30 minutes). After reaching the four-stage endpoint, it is dried in the low-temperature dryer 250 and screened again in the screener 260 to obtain the finished coarse phase B270.
[0059] S3. In the dry mixer, a 20 kg horizontal paddle mixer is preferred. All components except B are fed in through the cementitious material and aggregate inlet and the admixture inlet. The mixture is mixed at 60 r / min for 90 s, and then the machine is stopped and the wall is scraped for 20 s.
[0060] S4. Add the finished coarse phase B270. After low shearing of the coarse phase B, mix at 25 r / min for 45 s at the feeding port, and then discharge and package at 340 through the packaging end.
[0061] During on-site construction, determine the amount of water to add according to the standard consistency (approximately 304 kg / t dry material initially), apply it to the AAC / ALC base layer to form a thin layer of mortar (3 mm thick), without interface agent, and cure at 20±2℃ and 60±5% relative humidity.
[0062] Example 2
[0063] The batches of 20 kg and 100 kg were mixed according to the proportions in Example 1.
[0064] 20 kg batch: 40 L horizontal paddle mill, mix at 60 r / min for 90 s except for B, scrape the wall for 20 s, add B after mixing at 25 r / min for 45 s. A dosage is 0.900 kg, finished product B dosage is 1.500 kg, total dry material is 20.000 kg.
[0065] 100 kg batch: 200 L plow mill, mix at 75 r / min for 120 s except for B, stop for 30 s, add 30 r / min after B and mix for 60 s, do not use high-speed flying knife, A dosage 4.500 kg, finished product B dosage 7.500 kg, total dry material 100.000 kg.
[0066] Scale-up criteria: mass recovery rate ≥ 99.5%, five-point content coefficient of variation ≤ 3.0%, B phase retention rate greater than 0.30 mm ≥ 98% before feeding, and newly added fine powder less than 0.15 mm ≤ 0.5%. Both batches met the above criteria.
[0067] Example 3
[0068] In Example 1, the particle size of the coarse phase B was adjusted to 0.30–0.60 mm, the length of the polypropylene fiber was adjusted to 1.5 mm, and the remaining components and proportions remained unchanged. This variant was used for 2 mm thin-layer application. After testing, there was no particle jamming or exposed particle phenomenon at a thickness of 2 mm, and the flatness met the engineering requirements.
[0069] Comparative Example D4
[0070] The carbon dioxide treatment of coarse phase B was extended to 360 minutes to reach a fully mineralized plateau (total relative increase in inorganic carbon < 2.0% over two consecutive 60-minute supplementary cycles), otherwise identical to Example 1. The carbon dioxide dry basis weight gain of finished product B was approximately 1.5%, the water absorption ratio at 1 minute was approximately 0.35, and the capacity retention rate at 24 hours was approximately 55%, with the remaining formulation and process consistent with Example 1.
[0071] Comparative Example D5
[0072] Fine phase A was treated under the same spraying-carbon dioxide conditions as B (equal calcium treatment), while coarse phase B remained untreated. The rest was exactly the same as in Example 1.
[0073] Comparative Example D6
[0074] The coarse phase B remains untreated. The amount of calcium corresponding to the lime used for B treatment and the amount of fixed CO2 is added to the formula in balance with the quicklime and inert filler in the mortar body. The rest is exactly the same as in Example 1.
[0075] Comparative Example C2
[0076] The low-mineralized fine phase A and the coarse phase B are in an untreated state, and the rest is exactly the same as in Example 1.
[0077] Comparative Example C3
[0078] Fine phase A is in a deep carbonization state, coarse phase B is the target pore mineralization B, and the rest is exactly the same as in Example 1.
[0079] Comparative Example C4
[0080] Both fine phase A and coarse phase B are in a state of deep carbonization treatment, and the rest are exactly the same as in Example 1.
[0081] Furthermore, the experiment was conducted and the results were obtained in the following manner.
[0082] Regarding the testing method for coarse phase B characteristic parameters
[0083] Carbon dioxide dry basis weight gain: Take the treated oven-dry B sample and the oven-dry B sample before treatment in the same batch, weigh them after constant weight at 105℃, calculate the percentage of mass increase, and correct the background carbonization contribution of AAC with blank samples of the same master batch that have not been sprayed with ash, and under the same temperature, humidity and CO2 conditions.
[0084] Residual calcium hydroxide: Thermogravimetric analysis (TG) was used to test under nitrogen atmosphere and heating rate of 10℃ / min. The weight loss peak in the temperature range of 450-550℃ was attributed to Ca(OH)2 dehydration. The quantitative calculation was performed after subtracting the baseline of untreated B from the same parent batch.
[0085] 1-minute water absorption ratio and 24-hour capacity retention rate: Take 100.0 g of oven-dried B sample, water temperature 20.0±0.5℃, immersion depth 50±2 mm, take it out after 1 minute and 24 hours respectively, let it drain freely in a standard mesh basket for 30±1 s and then weigh it. Each treated B is paired with untreated B of the same batch and particle size. 1-minute water absorption ratio = 1-minute water absorption of treated B / 1-minute water absorption of untreated B; 24-hour capacity retention rate = 24-hour water absorption of treated B / 24-hour water absorption of untreated B × 100%.
[0086] Regarding the five-order mineralization gradient test of coarse B phase
[0087] The water absorption and binding properties of the five mineralization gradients (B0 untreated, B1 slightly treated, B2 target, B3 over-treated, and B4 fully mineralized) are shown in Table 2.
[0088] Table 2: Coarse Phase B Mineralization Gradient and Transmatrix Bonding Properties
[0089]
[0090] As shown in Table 2, Target B2 achieved the best balance between water absorption ratio in 1 minute (0.716) and capacity retention in 24 hours (90.9%), and had the highest bonding performance (0.440 MPa), exhibiting non-monotonic optimal characteristics.
[0091] 2×2 factorial test
[0092] Two regimes were established: a fixed water addition (300 kg / t) and an equal spread (170±5 mm). The tensile bond strength of C4 (two-phase deep treatment), C2 (A optimization only), C3 (B optimization only), and C7 (A+B target scheme) was tested under three base layer moisture contents (approximately 3% dry, approximately 18% normal, and approximately 45% high moisture content) for 28 days. The results are shown in Table 3.
[0093] Table 3: Bonding behavior of biphase quating factors under fixed water addition and equal spread conditions
[0094]
[0095] It can be seen that, under a fixed water addition regime, the worst-state adhesion of C7 is increased by (0.435-0.375) / 0.375=16.00% compared with the best single factor (C3), and the cross-state coefficient of variation decreases from 4.92% to 2.43%.
[0096] Under the equal expansion regime, the worst-case adhesion of C7 relative to the best single-factor (C3) increased by (0.426-0.368) / 0.368=15.76%, and the cross-state coefficient of variation decreased from 5.03% to 2.49%. The A×B interaction significance probability was 0.0128 under the fixed water addition regime and 0.0026 under the equal expansion regime.
[0097] Traditional processing comparison
[0098] The bonding performance of C7 with D4 (fully mineralized platform B), D5 (reverse treatment), and D6 (equal total calcium) under engineering drying and normal substrate conditions for 28 days was compared with that of conventional treatment methods. The results are shown in Table 4.
[0099] Table 4: Comparison of Traditional Processing Methods
[0100]
[0101] It can be seen that the lower limit of the 95% confidence interval for all controls is greater than 0, and the p-value is less than 0.001. Traditional treatment methods such as full carbonization and simple treatment position swapping are difficult to achieve the desired effect.
[0102] Standard performance testing
[0103] The standard performance of Example 1 was tested according to JC / T 890-2017 "Special Mortar for Autoclaved Aerated Concrete Walls". The water retention rate was also verified according to JGJ / T 70. The results are shown in Table 5.
[0104] Table 5: Standard Performance Test Results
[0105]
[0106] Temperature and base source boundary test
[0107] Under curing conditions of 10℃: 24-hour compressive strength 0.57 MPa, final setting time 667 min, 14-day bond strength 0.352 MPa.
[0108] Under curing conditions of 30℃: initial setting time is 119 min, and setting is accelerated.
[0109] Among the four AAC / ALC source batches, C7 showed a 15.13%–21.50% improvement in 28-day bond strength relative to the best single-factor result, without any reversal of direction.
[0110] Spatial structure confirmed
[0111] Raman spectroscopy, micron-scale CT, and cross-sectional backscattered electron imaging were performed on target B, untreated B, and fully mineralized platform B. A blind evaluation was conducted on 15 independent process batches (30 grains per batch), totaling 450 grains; 430 grains were correctly identified, resulting in an overall identification rate of 95.6%.
[0112] Raman spectroscopy confirmed that target B had approximately 53%–60% carbonate coverage and an invasion depth of 38–47 μm. Micron-scale CT showed that approximately 85% of the connecting holes were retained relative to untreated B (the retention rate changed by no more than 0.9 percentage points when the threshold was ±5 gray levels).
[0113] Calorimetry and Interface Analysis
[0114] The measured average values of the main exothermic peaks for C4, C2, C3, and C7 were approximately 23.2 h, 16.2 h, 17.7 h, and 12.4 h, respectively. The cumulative heat of C7 over 24 hours was approximately 36.8 J / g slag, which was higher than that of each single-factor scheme. C7 showed improvement in terms of interfacial porosity, microcrack density, interfacial layer thickness, and unreacted slag area over 28 days.
[0115] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A water-regulating waste AAC slag thin-layer mortar, characterized in that: It is based on granulated blast furnace slag powder as the main cementitious precursor, and does not contain silicate cement clinker or added gypsum. It contains the following components: Anhydrous sodium carbonate 20.0–21.0 kg / t; The mortar contains 8.7–9.3 kg / t of quicklime. Low-mineralized fine phase A is 42-48 kg / t. The low-mineralized fine phase A is a fine powder obtained by low-temperature drying and air classification of waste autoclaved aerated concrete from the same source. Its median particle size D50 is 40-70 μm, and its relative mineralization Dc ≤ 15%. The relative mineralization Dc is calculated by normalizing the carbon dioxide-related weight loss in thermogravimetric analysis at 550-900℃, with the untreated sample and the fully mineralized platform sample from the same batch as the two ends. The coarse mineralized phase B at the pore opening is 72-78 kg / t. This coarse mineralized phase B is a coarse-grained precursor from the same parent batch as the low-mineralized fine phase A, derived from waste autoclaved aerated concrete. Its particle size is 0.30-0.80 mm, and it possesses the following characteristics: carbon dioxide Weight gain on a dry basis: 0.45%–0.70%; Residual calcium hydroxide ≤0.20%.
2. The water-regulating waste AAC slag thin-layer mortar according to claim 1, characterized in that: The water absorption ratio of the coarse phase B mineralized at the orifice is ≤0.80 in 1 minute, and the capacity retention rate is 75% to 95% in 24 hours.
3. The water-regulating waste AAC slag thin-layer mortar according to claim 1, characterized in that: The anhydrous sodium carbonate content is 20.0–20.8 kg / t, the quicklime content in the mortar matrix is 8.8–9.2 kg / t, the low-mineralized fine phase A content is 44–46 kg / t, the pore-mineralized coarse phase B content is 74–76 kg / t, the median particle size D50 of the low-mineralized fine phase A is 50–58 μm, and the relative mineralization Dc is 11%–13%.
4. The water-regulating waste AAC slag thin-layer mortar according to claim 1, characterized in that: The carbon dioxide dry basis weight gain of the mineralized coarse phase B at the orifice is 0.52% to 0.64%, the water absorption ratio in 1 minute is 0.68 to 0.80, and the capacity retention rate in 24 hours is 79% to 94%.
5. The water-regulating waste AAC slag thin-layer mortar according to claim 1, characterized in that: The surface of the mineralized coarse phase B at the pore opening has spatially discontinuous carbonate-enriched patches with a carbonate coverage of 53%–60% and a carbonate penetration depth of 38–47 μm. The retention rate of the internally distinguishable interconnected pores relative to the untreated state is not less than 85%.
6. The water-regulating waste AAC slag thin-layer mortar according to claim 1, characterized in that: The granulated blast furnace slag powder is S95 grade slag powder, and the dosage is 290-310 kg / t. The mortar also contains 13-17 kg / t of alkali-resistant redispersible latex powder, 3.0-3.4 kg / t of hydroxyethyl methyl cellulose ether, 0.30-0.40 kg / t of starch ether, 0.50-0.70 kg / t of polypropylene fiber, 0.70-0.90 kg / t of powder defoamer, 440-480 kg / t of quartz sand (0.10-0.80 mm), and 65-75 kg / t of quartz powder with a D50 of 23-28 μm.
7. The water-regulating waste AAC slag thin-layer mortar according to claim 1, characterized in that: The proportions of each component are as follows: granulated blast furnace slag powder 300.00 kg / t, anhydrous sodium carbonate 20.50 kg / t, quicklime in the mortar matrix 9.00 kg / t, alkali-resistant redispersible latex powder 15.00 kg / t, hydroxyethyl methyl cellulose ether 3.20 kg / t, starch ether 0.35 kg / t, polypropylene fiber 0.60 kg / t, powder defoamer 0.80 kg / t, low-mineralized fine phase A 45.00 kg / t, pore-mineralized coarse phase B 75.00 kg / t, quartz sand 0.10~0.80 mm 460.00 kg / t, and quartz powder D50 of 25 μm 70.55 kg / t.
8. The water-regulating waste AAC slag thin-layer mortar according to claim 1, characterized in that: The low-mineralized fine phase A is obtained by air classification of the same source waste autoclaved aerated concrete after drying at a low temperature of 55-65℃ to a moisture content of ≤0.5%, without the use of a high-energy ball mill, and the energy consumption for classification is ≤5 kWh / t.
9. A water-regulating waste AAC slag thin-layer mortar according to claim 1, characterized in that: In the mortar, all components except the coarse mineralized phase B at the pore opening are premixed first. The coarse mineralized phase B at the pore opening is added later in a low-shear manner after the premixing is completed, with a mixing speed ≤30 r / min and a mixing time of 45 to 60 s.
10. A method for preparing water-adjusting waste AAC slag thin-layer mortar, used to prepare the water-adjusting waste AAC slag thin-layer mortar as described in any one of claims 1-9, characterized in that: Includes the following steps: S1. Take clean autoclaved aerated concrete cutting scraps from the same production line and the same master batch, pre-crush them to less than 5 mm, and dry them at a low temperature of 55-65℃ until the moisture content is ≤0.5%; S2. The dried material is separated into the low-mineralized fine phase A and the coarse precursor by airflow classification. S3. The coarse precursor is screened again, and the 0.30-0.80 mm particle size fraction is sprayed onto the surface of the coarse precursor with a lime slurry of 10%-14% by mass, so that the calcium hydroxide solid is 0.8%-1.2% of the dry mass of the coarse precursor. It is then treated under the conditions of 4%-6% carbon dioxide volume fraction and 20-30℃ until the following four endpoints are met: carbon dioxide dry basis weight gain 0.45%-0.70%, residual calcium hydroxide ≤0.20%, water absorption ratio ≤0.80% in 1 minute, and capacity retention rate 75%-95% in 24 hours. After low-temperature drying and re-screening, the pore mineralized coarse phase B is obtained. S4. Weigh all components except the mineralized coarse phase B at the orifice according to the proportion and put them into a dry mixer to mix evenly. S5. After stopping the machine and scraping the wall, add the mineralized coarse phase B from the orifice, mix evenly in a low-shear manner, and then discharge and package.