(BiLaSmNdGd)FeO3 Low Dielectric Constant Ceramic Materials and Their Preparation Methods
By preparing (BiLaSmNdGd)FeO3 low dielectric constant ceramic materials, the problem of high dielectric constant in high-entropy rare earth ferrite ceramics was solved, achieving both low dielectric constant and high electromagnetic wave transmittance, thus expanding its application range to wave-transparent materials.
Patent Information
- Application Number
- CN202611377444.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-07
- Publication Date
- 2026-11-10
AI Technical Summary
Existing high-entropy rare-earth ferrite ceramics have a high dielectric constant, which makes it difficult to meet the requirements of high-frequency, low-loss electronic devices, and the effect of traditional rare-earth doping is limited.
A method for preparing (BiLaSmNdGd)FeO3 low dielectric constant ceramic materials was adopted. Through specific element combinations and ratios, high entropy rare earth ferrite ceramics with low dielectric constant were prepared. The method includes steps such as weighing and dissolving metal nitrates, stirring with citric acid, adjusting pH with ammonia, heating in a water bath to generate wet gel, drying, and high-temperature sintering.
The prepared material has a dielectric constant of less than 3 and an electromagnetic wave transmittance of more than 88%, breaking through the application limitations of high-entropy rare earth ferrites and expanding into the field of wave-transparent materials.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of functional ceramic materials, specifically relating to a (BiLaSmNdGd)FeO3 low dielectric constant ceramic material and its preparation method. Background Technology
[0002] Ferrite ceramics, as important functional ceramic materials, are widely used in fields such as communications. In these applications, the dielectric constant of the material is a key performance indicator. An excessively high dielectric constant can lead to problems such as signal transmission delay, impedance matching difficulties, and increased parasitic capacitance, which are detrimental to the miniaturization and high-frequency development of devices. Therefore, developing ferrite ceramic materials with low dielectric constants and excellent overall performance has significant engineering value.
[0003] Rare earth elements, due to their unique 4f electron configuration, can effectively modulate the electromagnetic properties of ferrites. Existing technologies have reported on doping single or small amounts of rare earth ions into the ferrite lattice to improve dielectric or magnetic properties. However, most of these studies are limited to mono- or binary rare earth doping, resulting in materials with low entropy values, limited effectiveness in reducing the dielectric constant, and often accompanied by problems such as decreased magnetic loss or temperature stability.
[0004] High-entropy ceramics are a rapidly developing new type of ceramic material system in recent years. They typically consist of five or more metal cations occupying the same lattice sites in equimolar or near-equimolar ratios, forming a stable single-phase solid solution. Compared to traditional ceramics, high-entropy ceramics exhibit significant thermodynamic stability, lattice distortion effects, and tunable electronic structures, showing broad application prospects in mechanics, thermodynamics, and electromagnetics. In recent years, researchers have begun exploring the simultaneous introduction of multiple rare earth elements into ferrite lattices to construct high-entropy rare earth ferrite ceramics. For example, some literature reports high-entropy garnet-type or perovskite-type ceramics based on rare earth elements such as yttrium (Y), lanthanum (La), samarium (Sm), and gadolinium (Gd), primarily focusing on their magnetic properties and thermal stability.
[0005] However, existing high-entropy rare-earth ferrite ceramics generally suffer from a high dielectric constant, making it difficult to meet the demand for low dielectric constant materials in high-frequency, low-loss electronic devices. Furthermore, how to effectively reduce the dielectric constant while maintaining a single-phase high-entropy structure through the rational selection of rare-earth element combinations and ratios remains a pressing technical problem to be solved in this field. Summary of the Invention
[0006] This invention addresses the shortcomings of existing technologies by providing a (BiLaSmNdGd)FeO3 low dielectric constant ceramic material and its preparation method.
[0007] To achieve the above objectives, the technical solution of the present invention is as follows:
[0008] A method for preparing a (BiLaSmNdGd)FeO3 low dielectric constant ceramic material includes the following steps:
[0009] 1) According to the general chemical formula (Bi) x La (1-x) / 4 Nd (1-x) / 4 Sm (1-x) / 4 Gd (1-x) / 4 FeO3 is prepared by weighing out the nitrates of each metal and dissolving them in water to obtain a nitrate solution; wherein 0.10≤x≤0.30, the sum of the mole fractions of the A-site elements Bi, La, Nd, Sm and Gd is 1, and the ratio of the total molar amount of Fe to the total molar amount of the A-site elements is 1:1.
[0010] 2) Add citric acid to the nitrate solution and stir to obtain a mixed solution; 3) Add ammonia to adjust the mixed solution to alkalinity;
[0011] 4) After heating the alkaline mixed solution in a water bath until a wet gel is formed, dry it;
[0012] 5) The dried product is ground and pressed into shape, and then sintered at high temperature in air atmosphere at a temperature of 600-900 ℃ for 1-2 h. After cooling, (BiLaSmNdGd)FeO3 low dielectric constant ceramic material is obtained.
[0013] Optionally, in step (1), x is 0.10, 0.152, 0.20, 0.252 or 0.30.
[0014] Optionally, the concentration of the nitrate solution is 0.05-0.6 mol / L, based on the total molar amount of metal nitrates.
[0015] Optionally, in step 2), the molar ratio of citric acid to the total amount of nitrate is 1-1.5:1; and the stirring time is 15-30 min.
[0016] Optionally, in step 3), the pH of the mixed solution is adjusted to 8-10.
[0017] Optionally, in step 4), the water bath heating temperature is 70-90 ℃, the duration is 6-7 h, and the reaction is continuously stirred.
[0018] Optionally, in step 4), the drying temperature is 80-120 ℃ and the duration is 12-15 h.
[0019] Optionally, in step 5), the heating rate of the high-temperature sintering is 1-10 ℃ / min, and the cooling is either furnace cooling or a cooling rate of 1-10 ℃ / min.
[0020] A (BiLaSmNdGd)FeO3 low dielectric constant ceramic material is prepared by the above-mentioned preparation method of (BiLaSmNdGd)FeO3 low dielectric constant ceramic material.
[0021] Optionally, the dielectric constant of the (BiLaSmNdGd)FeO3 low dielectric constant ceramic material is less than 3, and the electromagnetic wave transmittance is greater than 88%.
[0022] The beneficial effects of this invention are as follows:
[0023] The material composition design prepared by this invention is extremely simplified. There is no need to introduce doping elements at the B site or add sintering aids, thereby significantly reducing raw material costs and process complexity.
[0024] The material prepared by this invention exhibits extremely low dielectric constant (ε'<3.0) and extremely high electromagnetic wave transmittance (>88%) in the 1-18 GHz frequency band, with wave transmission performance far exceeding that of traditional high-entropy rare earth ferrites.
[0025] This invention breaks through the limitation of existing technologies that only use high-entropy rare-earth ferrites for microwave absorption or magnetic devices, and can extend their application to the field of microwave-transparent materials, which has significant application novelty and broad prospects.
[0026] Other features and beneficial effects of the invention will be set forth in the description which follows, and will be apparent in part from the description, or may be learned by practicing the invention. Attached Figure Description
[0027] Figure 1 The X-ray diffraction pattern of the (BiLaSmNdGd)FeO3 low dielectric constant ceramic material prepared in Example 1 is shown.
[0028] Figure 2 This is an EDS image of the (BiLaSmNdGd)FeO3 low dielectric constant ceramic material prepared in Example 1.
[0029] Figure 3 The transmittance of the (BiLaSmNdGd)FeO3 low dielectric constant ceramic materials prepared in Examples 2, 3, and 4 in the frequency range of 1-18 GHz. Detailed Implementation
[0030] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments.
[0031] It should be noted that: for conditions not specifically specified in the examples, standard conditions or conditions recommended by the manufacturer should be followed. Reagents or instruments whose manufacturers are not specified are all commercially available products.
[0032] The embodiment provides a high-entropy rare-earth ferrite ceramic material with lanthanide metals as the main A-site elements. Through specific element combinations and formulation design, a low dielectric constant is achieved while maintaining good phase structure stability and process compatibility, providing a new option for the field of wave-transparent materials.
[0033] Specifically, the preparation method of the (BiLaSmNdGd)FeO3 low dielectric constant ceramic material in the embodiment is as follows:
[0034] 1) According to the general chemical formula (Bi) x La (1-x) / 4 Nd (1-x) / 4 Sm (1-x) / 4 Gd (1-x) / 4 FeO3 is prepared by weighing out various metal nitrate raw materials and dissolving them in distilled water to obtain a nitrate solution; wherein 0.10≤x≤0.30, the sum of the mole fractions of the A-site elements Bi, La, Nd, Sm and Gd is 1, and the ratio of the total molar amount of Fe to the total molar amount of the A-site elements is 1:1; the metal nitrate raw materials are bismuth nitrate, lanthanum nitrate, neodymium nitrate, samarium nitrate, gadolinium nitrate, and ferric nitrate, including but not limited to anhydrous or hydrated forms; the concentration of the nitrate solution is 0.05-0.6 mol / L based on the total molar amount of the metal nitrates;
[0035] 2) Add the complexing agent citric acid to the nitrate solution and stir for 15-30 minutes to obtain a mixed solution; wherein the molar ratio of citric acid to the total amount of nitrate is 1-1.5:1;
[0036] 3) Add ammonia to the above mixed solution to adjust the pH to 8-10;
[0037] 4) Place the alkaline mixed solution in a water bath for 6-7 hours at a temperature of 70-90 ℃, and stir continuously until a wet gel is formed. Then place it in an oven to dry at a temperature of 80-120 ℃ for 12-15 hours.
[0038] 5) After grinding the dried product, weigh 0.05-0.1g of powder and place it into a mold to press it into shape. Then, sinter it at high temperature in an air atmosphere. The heating rate is 1-10 ℃ / min, preferably 5 ℃ / min, the sintering temperature is 600-900 ℃, and the holding time is 1-2 h. The subsequent temperature is either programmed cooling or furnace cooling to obtain (BiLaSmNdGd)FeO3 low dielectric constant ceramic material. The temperature of the programmed cooling is 1-10 ℃ / min, preferably 5 ℃ / min.
[0039] Theoretically, a material's wave transmission capability mainly depends on the "reflection" of electromagnetic waves at the material's surface and the "attenuation" during propagation within the material. When a material has a low dielectric constant, its electromagnetic parameters are closer to those of air, resulting in better interfacial impedance matching. Consequently, the reflection of incident electromagnetic waves at the surface decreases, allowing more energy to enter and penetrate the material. Simultaneously, materials with low dielectric constants typically exhibit weaker polarization responses. If the dielectric loss is also low, the energy dissipation during electromagnetic wave propagation is even lower, making it easier to achieve higher wave transmission overall. Therefore, the obtained (BiLaSmNdGd)FeO3 low dielectric constant ceramic material has significant application prospects in the field of wave-transmitting materials.
[0040] Example 1
[0041] Weigh out 1.103 g of bismuth nitrate pentahydrate, 0.985 g of lanthanum nitrate hexahydrate, 0.997 g of neodymium nitrate hexahydrate, 1.011 g of samarium nitrate hexahydrate, 1.027 g of gadolinium nitrate hexahydrate, and 4.594 g of ferric nitrate nonahydrate powder. Dissolve all the powders together in 100 ml of distilled water in a container and mix thoroughly to obtain a mixed nitrate solution of metals. The molar ratio of Bi:La:Sm:Nd:Gd:Fe = 0.20:0.20:0.20:0.20:1. Weigh out 4.37 g of citric acid powder and add it to the above nitrate solution. Stir for 15 min to obtain a mixed solution. Add ammonia water to the above mixed solution to adjust the pH to 8. Cover the container of the alkaline mixed solution with plastic wrap and poke holes. Place it in an 80 ℃ water bath for 6 h to generate a wet gel, stirring continuously during the reaction. Place the reaction product in an oven and dry at 80 ℃. Dry at ℃ for 12 h; grind the dried sample, weigh 0.05 g of powder and put it into a mold to press it into shape, heat it to 700 ℃ in air at a heating rate of 5 ℃ / min, hold it for 2 h, and then cool it with the furnace to obtain (BiLaSmNdGd)FeO3 ceramic material.
[0042] Figure 1The image shows the X-ray diffraction pattern of the prepared (BiLaSmNdGd)FeO3 low-dielectric-constant ceramic material. Multiple distinct diffraction peaks are visible in the 2θ range of approximately 20°–80°, and some of these peaks can be attributed to related phases such as "BiFeO3", "NdFeO3", "(La,Sm)FeO3", and "(Bi,Nd)4FeO3". This indicates that perovskite-related crystalline phases were formed in the sample at a sintering temperature of 700 °C, and a certain degree of multiphase coexistence exists. Considering the intensity of the main peak, the sample exhibits good crystallinity.
[0043] Figure 2 The images show EDS (Electron Microscopy) scans of the (BiLaSmNdGd)FeO3 low dielectric constant ceramic material prepared in Example 1 at different magnifications. As can be seen from the images, (a) shows the SEM morphology of the sample, where the particles exhibit a clearly agglomerated flocculent structure with a rough surface and numerous pores, indicating that the sample exists as a porous agglomerated powder after preparation. (b)–(h) show the EDS surface scan results of Fe, O, La, Gd, Sm, Nd, and Bi. The elements are relatively uniformly distributed within the field of view, with no obvious enrichment or segregation, indicating that the components have entered the same matrix well, and the sample has good chemical homogeneity and solid solution characteristics.
[0044] The above-mentioned (BiLaSmNdGd)FeO3 ceramic material was ground into powder and mixed with paraffin at a mass ratio of sample:paraffin = 3:7 to obtain a ring-shaped sample. Then, the wave transmission performance of the sample was tested using a vector network analyzer. The sample showed extremely low dielectric constant and extremely high electromagnetic wave transmittance in the 1-18 GHz frequency band. The dielectric constant was 2.7, which is about 50% lower than that of traditional low dielectric materials (such as SiO2).
[0045] Example 2
[0046] 0.848 g of bismuth nitrate pentahydrate, 1.056 g of lanthanum nitrate hexahydrate, 1.069 g of neodymium nitrate hexahydrate, 1.084 g of samarium nitrate hexahydrate, 1.101 g of gadolinium nitrate hexahydrate, and 4.646 g of ferric nitrate nonahydrate powder were weighed and dissolved in 100 ml of distilled water to obtain a mixed nitrate solution of metals; the molar ratio of Bi:La:Sm:Nd:Gd:Fe was 0.152:0.212:0.212:0.212:0.212:1. 4.834 g of citric acid powder was weighed and added to the solution, and the mixture was stirred for 20 min to obtain a mixed solution. Ammonia was added to the mixed solution to adjust the pH to 9. The container of the alkaline mixed solution was covered with plastic wrap and punctured, and placed in a water bath at 80 ℃ for 6 h to form a wet gel, with continuous stirring during the reaction. The product was then placed in an oven and dried at 100 ℃ for 12 hours. h; Grind the dried sample, weigh 0.05 g of powder and put it into a mold to press it into shape. Heat it to 600 ℃ in air at a heating rate of 5 ℃ / min, hold it for 2 h, and then cool it with the furnace to obtain (BiLaSmNdGd)FeO3 ceramic material.
[0047] Example 3
[0048] 0.565 g of bismuth nitrate pentahydrate, 1.134 g of lanthanum nitrate hexahydrate, 1.148 g of neodymium nitrate hexahydrate, 1.164 g of samarium nitrate hexahydrate, 1.183 g of gadolinium nitrate hexahydrate, and 4.704 g of ferric nitrate nonahydrate powder were weighed and dissolved in 200 ml of distilled water to obtain a mixed nitrate solution of metals; the molar ratio of Bi:La:Sm:Nd:Gd:Fe = 0.1:0.225:0.225:0.225:0.225:1; 4.894 g of citric acid powder was weighed and added to the solution, and stirred for 20 min to obtain a mixed solution; ammonia water was added to the above mixed solution to adjust the pH of the solution to 8; the container of the mixed solution after adjustment to alkalinity was covered with plastic wrap and punctured, and placed in a water bath at 80 ℃ for 6 h to form a wet gel, with continuous stirring during the reaction; the product after reaction was placed in an oven and dried at 90 ℃ for 12 hours. h; Grind the dried sample, weigh 0.05 g of powder and put it into a mold to press it into shape. Heat it to 800 ℃ in air at a heating rate of 5 ℃ / min, hold it for 2 h, and then cool it with the furnace to obtain (BiLaSmNdGd)FeO3 ceramic material.
[0049] Example 4
[0050] 1.617 g of bismuth nitrate pentahydrate, 0.842 g of lanthanum nitrate hexahydrate, 0.853 g of neodymium nitrate hexahydrate, 0.865 g of samarium nitrate hexahydrate, 0.878 g of gadolinium nitrate hexahydrate, and 4.490 g of ferric nitrate nonahydrate powder were weighed and dissolved in 300 ml of distilled water to obtain a mixed nitrate solution of metals; the molar ratio of Bi:La:Sm:Nd:Gd:Fe = 0.3:0.175:0.175:0.175:0.175:1. 4.67 g of citric acid powder was weighed and added to the solution, and the mixture was stirred for 30 min to obtain a mixed solution. Ammonia was added to the mixed solution to adjust the pH to 10. The container of the alkaline mixed solution was covered with plastic wrap and punctured, and placed in a water bath at 80 ℃ for 6 h to generate a wet gel, with continuous stirring during the reaction. The product was then placed in an oven and dried at 90 ℃ for 12 hours. h; Grind the dried sample, weigh 0.07 g of powder and put it into a mold to press it into shape. Heat it to 900 ℃ in air at a heating rate of 5 ℃ / min, hold it for 2 h, and then cool it with the furnace to obtain (BiLaSmNdGd)FeO3 ceramic material.
[0051] Figure 3 The figure shows the transmittance of the (BiLaSmNdGd)FeO3 low dielectric constant ceramic materials prepared in Examples 2, 3, and 4 in the 1-18 GHz frequency range. As can be seen from the figure, all three groups of samples maintain high transmittance in the 1-18 GHz range, with values generally above 88%, indicating that the materials have good overall transmittance performance. With increasing frequency, the transmittance generally shows a fluctuating downward trend, with obvious absorption troughs in several frequency bands, and a relatively high peak value near 17 GHz, indicating that the samples have a certain frequency selectivity in response to electromagnetic waves of different frequencies. Comparing different sintering temperatures, the 800℃ sample has a slightly higher overall transmittance, with the curve at the top for most frequency bands, indicating its relatively best transmittance performance; the 600℃ sample is second; the 900℃ sample has slightly lower transmittance in most frequency bands, especially with more pronounced fluctuations in the high-frequency band, indicating that higher sintering temperatures may cause changes in the internal structure or dielectric properties of the material, thus having a certain adverse effect on the transmittance performance. Overall, different sintering temperatures have a certain impact on transmittance, but the differences among the three are not particularly large, and all samples show good broadband transmittance characteristics.
[0052] The above embodiments are only used to further illustrate the (BiLaSmNdGd)FeO3 low dielectric constant ceramic material and its preparation method according to the present invention. However, the present invention is not limited to the embodiments. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention shall fall within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a (BiLaSmNdGd)FeO3 low dielectric constant ceramic material, characterized in that: Includes the following steps: 1) According to the general chemical formula (Bi) x La (1-x) / 4 Nd (1-x) / 4 Sm (1-x) / 4 Gd (1-x) / 4 FeO3 is prepared by weighing out various metal nitrates and dissolving them in water to obtain a nitrate solution; wherein 0.10≤x≤0.30, the sum of the mole fractions of the A-site elements Bi, La, Nd, Sm and Gd is 1, and the ratio of the total molar amount of Fe to the total molar amount of the A-site elements is 1:
1. 2) Add citric acid to the nitrate solution and stir to obtain a mixed solution; 3) Add ammonia to adjust the mixed solution to be alkaline; 4) After heating the alkaline mixed solution in a water bath until a wet gel is formed, dry it; 5) The dried product is ground and pressed into shape, and then sintered at high temperature in air atmosphere at a temperature of 600-900 ℃ for 1-2 h. After cooling, (BiLaSmNdGd)FeO3 low dielectric constant ceramic material is obtained.
2. The method for preparing (BiLaSmNdGd)FeO3 low dielectric constant ceramic material according to claim 1, characterized in that, In step 1), x is 0.10, 0.152, 0.20, 0.252 or 0.
30.
3. The method for preparing (BiLaSmNdGd)FeO3 low dielectric constant ceramic material according to claim 1, characterized in that: The concentration of the nitrate solution is 0.05-0.6 mol / L, based on the total molar amount of metallic nitrates.
4. The method for preparing (BiLaSmNdGd)FeO3 low dielectric constant ceramic material according to claim 1, characterized in that: In step 2), the molar ratio of citric acid to total nitrate is 1-1.5:1; the stirring time is 15-30 min.
5. The method for preparing (BiLaSmNdGd)FeO3 low dielectric constant ceramic material according to claim 1, characterized in that: In step 3), the pH of the mixed solution is adjusted to 8-10.
6. The method for preparing (BiLaSmNdGd)FeO3 low dielectric constant ceramic material according to claim 1, characterized in that: In step 4), the water bath heating temperature is 70-90 ℃, the duration is 6-7 h, and the reaction is continuously stirred.
7. The method for preparing (BiLaSmNdGd)FeO3 low dielectric constant ceramic material according to claim 1, characterized in that: In step 4), the drying temperature is 80-120 ℃ and the duration is 12-15 h.
8. The method for preparing (BiLaSmNdGd)FeO3 low dielectric constant ceramic material according to claim 1, characterized in that: In step 5), the heating rate of the high-temperature sintering is 1-10 ℃ / min, and the cooling is either furnace cooling or a cooling rate of 1-10 ℃ / min.
9. A (BiLaSmNdGd)FeO3 low dielectric constant ceramic material, characterized in that: It is prepared by the method for preparing (BiLaSmNdGd)FeO3 low dielectric constant ceramic material according to any one of claims 1-8.
10. The (BiLaSmNdGd)FeO3 low dielectric constant ceramic material according to claim 9, characterized in that: The dielectric constant of the (BiLaSmNdGd)FeO3 low dielectric constant ceramic material is less than 3, and the electromagnetic wave transmittance is greater than 88%.